Ceramic tile with colorful crystal effect and preparation process of ceramic tile
By mixing color dry particles with molten dry particles to make glaze slurry and melting with protective dry particles during firing, the glaze uneven problem caused by the difficulty of melting color dry particles in the prior art is solved, and high The colorful crystal effects of flatness and low luminance reduce production costs.
Patent Information
- Application Number
- CN202411153185.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-21
AI Technical Summary
When existing imitation marble ceramic tiles use colored dry particles to replace traditional printed glaze, the difficulty of melting leads to uneven gloss and poor gloss, and require a lot of polishing and cutting to correct, increasing costs.
Use colored dry particles and molten dry particles to make glaze slurry, and melt with the protective dry particles before and after firing to form a transparent colorful crystal effect, avoiding dry particles accumulation and ensuring a flat glaze surface.
It achieves high flatness and low luminance difference in glaze surface, reduces production costs, improves production stability, and restores the colorful crystal effect of real stone.
Smart Images

Figure CN119039052A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of building ceramics, and in particular to a colorful crystal effect ceramic tile and a preparation process thereof. Background Art
[0002] Imitation natural marble ceramic tiles are widely sought after in the high-end ceramic market due to their exquisite patterns, lifelike effects, and rich and colorful surface craftsmanship. At present, in order to achieve a crystal texture effect closer to natural marble, most of the imitation marble ceramic tiles on the market directly use various color dry particles to replace screen printing glaze for coloring. Compared with traditional printing glaze, color dry particles are more colorful and three-dimensional, thus being able to restore the crystal effect of natural stone.
[0003] However, there are still some technical problems in directly using color dry particles to replace traditional printing glaze:
[0004] 1. It is difficult to melt the dry particles of various colors, and they cannot be well melted in the protective dry particles, making it difficult to form clear and bright colors in the stone, thus covering up the original inkjet color;
[0005] 2. Since the color dry particles cannot be completely melted, they will remain in a piled state during firing, which can easily cause an uneven glaze surface and a huge difference in glaze gloss, affecting the appearance of the kiln bricks;
[0006] 3. In order to solve the problem of uneven glaze surface, it is usually necessary to apply a large amount of protective dry particles. After firing, smooth marble tiles are cut through polishing. The cost of glaze and polishing is high. Summary of the invention
[0007] The main purpose of the present invention is to propose a preparation process of colorful crystal effect ceramic tiles, which can prepare colorful crystal effect ceramic tiles imitating natural stone by replacing traditional printed glaze with color dry particles, and the prepared ceramic tiles have high surface flatness and small brightness difference.
[0008] To achieve the above object, the present invention proposes a preparation process of a colorful crystal effect ceramic tile, comprising the following steps:
[0009] S1, mixing at least two kinds of color dry particles with flux dry particles respectively, adding printing paste and printing oil to mix to form at least two kinds of colored glaze slurries for standby use;
[0010] S2, mixing protective glaze powder, water, methyl cellulose, sodium tripolyphosphate and ceramic glue to prepare protective glaze slurry for later use;
[0011] S3, applying base glaze and inkjet printing patterns on the surface of the blank;
[0012] S4, screen-printing the various colored glaze slurries obtained in step S1 on the surface of the blank obtained in step S3 according to preset pattern textures;
[0013] S5, applying protective dry particles on the surface of the body after applying the colored glaze slurry;
[0014] S6, applying the protective glaze slurry prepared in step S2 to the surface of the green body obtained in step S5;
[0015] S7, firing the glazed body obtained in step S6 to obtain the colorful crystal effect ceramic tile.
[0016] The present invention uses a mixture of color dry particles and flux dry particles to form a glaze slurry to replace the traditional printed glaze, so that the glaze effect after firing is more restored to the stone texture and has a colorful crystal effect imitating marble. In this scheme, the color dry particles are applied by wet glaze slurry, which has the advantage of high production stability compared to the traditional dry method. By first melting the color dry particles and flux dry particles, and then melting them with the protective dry particles, a crystal stone effect with good color development, bright colors and transparency is formed, which further restores the real stone texture.
[0017] Preferably, the softening temperature of the color dry particles is 1040-1070° C., the softening temperature of the flux dry particles is 930-950° C., and the softening temperature of the protective dry particles is 1030-1050° C. Since the softening temperature of the flux dry particles is relatively low, the color dry particles are mixed with the flux dry particles to control the color dry particles to begin to melt before the protective dry particles, and the color dry particles are melted to develop color and form a transparent colorful crystal effect without covering the pattern effect of the original inkjet printing layer.
[0018] Preferably, the colored dry particles include at least two of blue dry particles, green dry particles and black dry particles.
[0019] Preferably, the blue dry particles include the following components by mass percentage: SiO 2 43.80~46.50%、Al 2 O 3 14.02~15.52%, CaO 15.04~16.65%, MgO 6.00~8.00%, K 2 O0.81~1.52%、Na 2 O0.60~1.00%、BaO 4.86~5.97%、ZrO 2 4.51~5.93%、P 2 O 5 0.21~0.41%, loss on ignition: 0.40~0.60%;
[0020] The green dry particles include the following components by mass percentage: SiO2 53.49~56.39%、Al 2 O 3 19.83~21.09%, CaO 12.93~14.54%, MgO 3.98~5.78%, K 2 O 1.03~2.52%、Na 2 O 0.98~2.17%, BaO 0.07~0.20%, ZrO 2 0.09~0.24%、P 2 O 5 0.16~0.38%, loss on ignition: 0.40~0.60%;
[0021] The black dry particles include the following components by mass percentage: SiO 2 42.10~45.04%、Al 2 O 3 12.40~14.96%,Fe 2 O 3 4.42~5.46%, CaO 14.89~16.86%, MgO 5.41~7.85%, K 2 O 0.97~1.93%、Na 2 O 0.35~0.95%, BaO 4.86~5.97%, ZrO 2 2.65~3.89%, P 2 O 5 0.16~0.38%, MnO 2.69~3.57%, ignition loss: 0.85~1.23%.
[0022] Preferably, the fluxing dry particles include the following components by mass percentage: SiO 2 63.19~65.98%、Al 2 O 3 13.54~15.87%, CaO 9.23~11.69%, MgO 3.98~5.26%, K 2 O0.97~2.34%、Na 2 O1.87~3.24%, loss on ignition: 0.21~0.51%;
[0023] The protective dry particles include the following components by mass percentage: SiO 2 56.03~59.12%、Al 2 O 3 6.01~7.98%, CaO 11.14~13.17%, MgO 0.14~0.39%, K 2O 6.12~8.21%、Na 2 O 0.10~0.32%, BaO 1.99~3.05%, ZnO 10.13~12.01%, loss on ignition: 0.02~0.13%;
[0024] The protective glaze powder comprises the following components by mass percentage: SiO 2 64.85~67.03%、Al 2 O 3 9.51~11.07%, CaO 9.02~10.97%, MgO 1.02~2.09%, K 2 O 0.56~1.24%、Na 2 O 4.97~6.05%, BaO 0.64~1.23%, ZnO 0.98~1.58%, loss on ignition: 1.42~1.97%.
[0025] Preferably, the particle size range of the color dry particles is 60-120 meshes, the particle size range of the flux dry particles is 60-120 meshes, and the particle size range of the protective dry particles is 60-150 meshes.
[0026] Preferably, in step S1, the color dry particles are 90 to 110 parts by mass and the flux dry particles are 10 to 25 parts by mass. By adjusting the ratio of color dry particles and flux dry particles, the melting equilibrium point among color dry particles, flux dry particles and protective dry particles can be precisely adjusted to avoid the uneven brick surface caused by the stacking of dry particles. The prepared marble tile has high flatness, the unevenness difference can be controlled within 0.3mm, and the brightness difference is small and can be controlled within 3°. Avoid the cost increase problem caused by a large amount of cutting and polishing after conventional dry laying.
[0027] Preferably, in step S2, the protective glaze powder comprises 90 to 110 parts by mass, water comprises 50 to 65 parts by mass, 0.2 to 0.4 parts by mass of methyl cellulose, and 0.4 to 0.6 parts by mass of sodium tripolyphosphate.
[0028] Preferably, in step S4, the glaze amount of the colored glaze slurry is 55-120 g / m 2 .
[0029] Preferably, in step S5, the amount of the protective dry particle cloth is 800-900 g / m 2 .
[0030] Preferably, in step S6, the specific gravity of the protective glaze slurry is 1.18-1.25 g / mL, and the glaze application amount is 240-260 g / m 2 .
[0031] The present invention also provides a preparation process of a colorful crystal effect ceramic tile, comprising the following steps:
[0032] S11, mixing the blue dry particles and the fluxing dry particles, adding printing paste and printing oil to mix to prepare blue glaze slurry for standby use;
[0033] S12, mixing the green dry particles and the fluxing dry particles, adding printing paste and printing oil to mix to prepare green glaze slurry for standby use;
[0034] S13, mixing the black dry particles and the fluxing dry particles, adding printing paste and printing oil to mix to prepare black glaze slurry for standby use;
[0035] S2, mixing protective glaze powder, water, methyl cellulose, sodium tripolyphosphate and ceramic glue to prepare protective glaze slurry for later use;
[0036] S3, applying base glaze and inkjet printing patterns on the surface of the blank;
[0037] S41, screen printing a layer of the blue glaze slurry on the surface of the blank according to a preset pattern texture;
[0038] S42, screen printing a layer of the green glaze slurry on the surface of the blank according to a preset pattern texture;
[0039] S43, screen printing a layer of the black glaze slurry on the surface of the blank according to a preset pattern texture;
[0040] S5, applying protective dry particles on the surface of the body after applying the colored glaze slurry;
[0041] S6, applying the protective glaze slurry prepared in step S2 to the surface of the green body obtained in step S5;
[0042] S7, firing the glazed body obtained in step S6 to obtain the colorful crystal effect ceramic tile.
[0043] By combining blue dry particles, green dry particles and black dry particles, ceramic tiles imitating cloisonné stone can be prepared. The texture of the ceramic tile surface is transparent jade texture as the base, supplemented by large areas of blue crystals and transparent jade crystals, and then supplemented with green and black crystals to form colorful and visually impactful imitation cloisonné ceramic tiles.
[0044] In addition, the present invention also provides a colorful crystal effect ceramic tile, which is prepared by using the above-mentioned preparation process of the colorful crystal effect ceramic tile.
[0045] Compared with the prior art, the present invention has at least the following beneficial effects: the present invention adopts wet glaze slurry to apply color dry particles, and by first melting the color dry particles and the fluxing dry particles and then melting them with the protective dry particles, the crystallization effects of various colors and jade crystals in real stone can be restored; and compared with the traditional dry spreading process, less material is used, the glaze surface is smoother, the lightness difference is low, and the production stability is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying any creative work.
[0047] Figure 1 is a panoramic view of the ceramic tile of Example 2;
[0048] Figure 2 , Figure 3 This is a partial view of the ceramic tile of Example 2.
[0049] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0050] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0051] The present invention provides a preparation process of a colorful crystal effect ceramic tile, comprising the following steps:
[0052] S1, after mixing at least two kinds of color dry particles with flux dry particles respectively, add 8-12 parts of printing paste and 45-55 parts of printing oil to mix and prepare at least two kinds of colored glaze slurries for standby use;
[0053] S2, mixing protective glaze powder, water, methyl cellulose, sodium tripolyphosphate and ceramic glue to prepare protective glaze slurry for later use;
[0054] S3, applying base glaze and inkjet printing patterns on the surface of the blank;
[0055] S4, screen-printing the various colored glaze slurries obtained in step S1 on the surface of the blank obtained in step S3 according to preset pattern textures;
[0056] S5, applying protective dry particles on the surface of the body after applying the colored glaze slurry;
[0057] S6, applying the protective glaze slurry prepared in step S2 to the surface of the green body obtained in step S5;
[0058] S7, firing the glazed body obtained in step S6 to obtain the colorful crystal effect ceramic tile.
[0059] The present invention adopts the above steps to prepare dry-grain decorative ceramic tiles by using a wet glaze slurry process instead of a dry-grain fabric process, which has high production stability and low production cost. The preparation method first mixes color dry particles and fluxing dry particles to form a glaze slurry, which is first melted during the firing process and then melted with the protective dry particles, thereby forming a colorful and transparent crystal effect, which can truly restore the colorful crystal texture of the stone.
[0060] In the prior art, dry-grain decorative ceramic tiles usually adopt a dry-laying process, where color dry particles are spread and positioned on the blanks forming the base glaze layer and the printed pattern layer, and then fixed with ceramic glue, and then transparent glaze is applied, fired and polished to finally prepare ceramic tiles with three-dimensional color texture effects. However, in order to prepare ceramic tiles with colorful crystal effects, the color dry particles need to be cleverly integrated into the transparent dry particles to form a transparent crystal effect. Therefore, in the dry-laying process, the color dry particles and the transparent protective dry particles cannot be well melted, and the melting of the dry particles of each color is difficult, making it difficult to form a clear and bright color in the stone, and it is easy to cover the color of the original printed pattern layer. At the same time, since the color dry particles cannot be completely melted, they will remain in a stacked state during firing, resulting in poor glaze flatness after firing, affecting the appearance of the kiln, and in order to avoid the unevenness caused by the stacking of dry particles, a large amount of protective dry particles need to be applied later to obtain a flat marble tile by polishing and cutting after firing, thereby increasing the cost.
[0061] In this scheme, different colors of glaze slurry are made by mixing fluxing dry particles with lower initial melting points with color dry particles, and the glaze slurries of different colors are printed layer by layer on the body by screen printing. During the application of protective dry particles and the firing process, the color dry particles and fluxing dry particles melt first, and the protective dry particles melt later, so that the protective dry particles wrap the color dry particles to form a transparent colorful crystal effect. By mixing different colors of glaze slurry and printing in multiple colors layer by layer, the texture of natural stone can be imitated, so that the fired ceramic tile has clear patterns, distinct layers, and a strong three-dimensional sense.
[0062] This solution adds ceramic glue to the protective glaze slurry, and applies the protective glaze slurry after the protective dry particles. On the one hand, it fills the gaps, and on the other hand, the protective glaze slurry protects and bonds the protective dry particles, which helps to form a glaze layer with a smooth surface and also has a wear-resistant function.
[0063] In some embodiments, the softening temperature of the color dry particles is 1040-1070°C, the softening temperature of the flux dry particles is 930-950°C, and the softening temperature of the protective dry particles is 1030-1050°C. By adjusting the melting equilibrium point among the color dry particles, the flux dry particles, and the protective dry particles, a colorful crystal effect with a stronger three-dimensional effect, a more crystal-like sense of transparency, and more colorful colors is effectively formed. At the same time, since the softening temperature of the color dry particles is slightly higher than that of the protective dry particles, the pores can be sealed in the color dry particle layer without floating to the protective dry particle layer, so that the glaze surface after firing and polishing can reduce the pores of the color dry particles.
[0064] In some embodiments, the colored dry particles include at least two of blue dry particles, green dry particles, and black dry particles.
[0065] In an optional embodiment, the blue dry particles may include the following components by mass percentage: SiO 2 43.80~46.50%、Al 2 O 3 14.02~15.52%, CaO 15.04~16.65%, MgO 6.00~8.00%, K 2 O 0.81~1.52%、Na 2 O 0.60~1.00%, BaO 4.86~5.97%, ZrO 2 4.51~5.93%、P 2 O 5 0.21~0.41%, loss on ignition: 0.40~0.60%;
[0066] Green dry particles can include the following components by mass percentage: SiO 2 53.49~56.39%、Al 2 O 3 19.83~21.09%, CaO 12.93~14.54%, MgO 3.98~5.78%, K 2 O 1.03~2.52%、Na 2 O 0.98~2.17%, BaO 0.07~0.20%, ZrO 2 0.09~0.24%、P 2 O 50.16~0.38%, loss on ignition: 0.40~0.60%;
[0067] The black dry particles can include the following components by mass percentage: SiO 2 42.10~45.04%、Al 2 O 3 12.40~14.96%,Fe 2 O 3 4.42~5.46%, CaO 14.89~16.86%, MgO 5.41~7.85%, K 2 O 0.97~1.93%、Na 2 O 0.35~0.95%, BaO 4.86~5.97%, ZrO 2 2.65~3.89%, P 2 O 5 0.16~0.38%, MnO 2.69~3.57%, ignition loss: 0.85~1.23%.
[0068] In some preferred embodiments, the fluxing dry particles may include the following components by mass percentage: SiO 2 63.19~65.98%、Al 2 O 3 13.54~15.87%, CaO 9.23~11.69%, MgO 3.98~5.26%, K 2 O0.97~2.34%、Na 2 O 1.87~3.24%, loss on ignition: 0.21~0.51%;
[0069] As an example, the protected dry particles include the following components by mass percentage: SiO 2 56.03~59.12%、Al 2 O 3 6.01~7.98%, CaO 11.14~13.17%, MgO 0.14~0.39%, K 2 O 6.12~8.21%、Na 2 O 0.10~0.32%, BaO 1.99~3.05%, ZnO 10.13~12.01%, loss on ignition: 0.02~0.13%;
[0070] The protective glaze powder includes the following components by mass percentage: SiO 2 64.85~67.03%、Al 2 O 39.51~11.07%, CaO 9.02~10.97%, MgO 1.02~2.09%, K 2 O 0.56~1.24%、Na 2 O 4.97~6.05%, BaO 0.64~1.23%, ZnO 0.98~1.58%, loss on ignition: 1.42~1.97%.
[0071] In some embodiments, the particle size range of the color dry particles is 60-120 mesh, the particle size range of the flux dry particles is 60-120 mesh, and the particle size range of the protective dry particles is 60-150 mesh. Adjusting the particle size range of the dry particles can effectively prevent the difficulty of the green body from being exhausted due to too small particles, and reduce the bubbles in the glaze layer of the fired product. At the same time, the appropriate particle size range can enable the glaze to obtain better fluidity during the high-temperature melting process, thereby making the fired glaze surface smoother.
[0072] Preferably, in step S1, the color dry particles are 90 to 110 parts by mass and the flux dry particles are 10 to 25 parts by mass. By adjusting the ratio of the color dry particles and the flux dry particles, a marble tile with higher flatness can be obtained after firing, the glaze surface unevenness difference can be controlled within 0.3 mm, and the brightness difference can be controlled within 3°.
[0073] Preferably, in step S2, the protective glaze powder comprises 90 to 110 parts by mass, water comprises 50 to 65 parts by mass, 0.2 to 0.4 parts by mass of methyl cellulose, and 0.4 to 0.6 parts by mass of sodium tripolyphosphate.
[0074] Preferably, in step S4, the amount of colored glaze slurry applied is 55-120 g / m 2 . It is understandable that the amount of glaze applied is related to the number of colored glazes used in actual production and the preset pattern effect. When two colored glazes are used for screen printing, the amount of glaze applied is relatively small; when three colored glazes are used for screen printing, the amount of glaze required is larger. Controlling the glaze amount within the appropriate range is more conducive to ensuring the uniformity and fluidity of the glaze, so that the color development effect and flatness are better after firing.
[0075] Preferably, in step S5, the amount of protective dry granular material is 800-900 g / m 2 The colored glaze slurry adopts the appropriate glazing amount and the amount of protective dry particles to form an effective dry particle layer thickness of 0.2-0.4mm. While minimizing the amount used, it can ensure that the color dry particles can still be well melted into the protective dry particles after polishing, with a good crystal effect and ensure the flatness of the glaze surface.
[0076] Preferably, in step S6, the specific gravity is 1.18-1.25 g / mL, and the glazing amount is 240-260 g / m 2 Control and protect the glaze slurry within the appropriate specific gravity range and glazing amount, effectively protect the color dry particles, ensure the uniformity of glaze spraying, thereby further improving the flatness of the glaze surface and avoiding the risks of glaze deficiency or brick explosion.
[0077] Specifically, in step S7, the firing temperature is 1210-1230° C., and the firing time is 65-70 min.
[0078] Exemplarily, the present invention also provides a process for preparing a colorful crystal effect ceramic tile, comprising the following steps:
[0079] S11, mixing 90-110 parts of blue dry particles and 15-25 parts of flux dry particles, adding 8-12 parts of printing paste and 45-55 parts of printing oil to make a blue glaze slurry for standby use;
[0080] S12, mixing 90-110 parts of green dry particles and 10-20 parts of flux dry particles, adding 8-12 parts of printing paste and 45-55 parts of printing oil to make a green glaze slurry for later use;
[0081] S13, mixing 90-110 parts of black dry particles and 15-25 parts of flux dry particles, adding 8-12 parts of printing paste and 45-55 parts of printing oil to make a black glaze slurry for later use;
[0082] S2, 90-110 parts of protective glaze powder, 50-65 parts of water, 0.2-0.4 parts of methyl cellulose, 0.4-0.6 parts of sodium tripolyphosphate and ceramic glue are mixed to prepare a protective glaze slurry with a specific gravity of 1.18-1.25 g / mL, and set aside;
[0083] S3, applying base glaze and inkjet printing patterns on the surface of the blank;
[0084] S41, print a layer of blue glaze slurry on the surface of the blank with a 40-mesh screen according to the preset pattern texture, and the glaze amount is 45-55g / m 2 ;
[0085] S42, print a layer of green glaze slurry on the surface of the blank with a 40-mesh screen according to the preset pattern texture, and the glaze amount is 35-45g / m 2 ;
[0086] S43, print a layer of black glaze slurry on the surface of the blank with a 40-mesh screen according to the preset pattern texture, and the glaze amount is 10-20g / m 2 ;
[0087] S5. Apply protective dry particles on the surface of the blank after applying the colored glaze slurry, with a spreading amount of 800-900g / m 2 ;
[0088] S6: Apply protective glaze slurry on the surface of the body obtained in step S5, with the glaze amount being 240-260 g / m 2 ;
[0089] S7, firing the glazed body obtained in step S6, with the firing temperature being 1210-1230° C. and the firing time being 65-70 min, to obtain the colorful crystal effect ceramic tile.
[0090] In the above preparation method, blue dry particles, green dry particles and black dry particles are selected and combined with each other. By selecting a specific ratio and glazing amount, marble tiles imitating cloisonné stone can be prepared. The glaze texture presents a transparent jade texture as a base, which is supplemented by a large area of blue crystals and transparent jade crystals, and is dotted with green and black crystals, forming imitation cloisonné ceramic tiles with colorful colors and strong visual impact.
[0091] The following examples are further listed to describe the present invention in detail. It should be understood that the following examples are only used to further illustrate the present invention and should not be construed as limiting the scope of the present invention. Some non-essential improvements and adjustments made by those skilled in the art according to the above content of the present invention all belong to the scope of the present invention. The specific process parameters of the following examples are also only an example in a suitable range, that is, those skilled in the art can make selections within a suitable range through the description of this article, and are not limited to the specific numerical values of the examples below. If the specific conditions are not indicated in the examples, proceed according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0092] In the following embodiments, the blue dry particles, green dry particles, and black dry particles used are all purchased from Foshan Linggao New Materials Co., Ltd.; the fluxing dry particles used are PY1408 transparent dry particles, which are purchased from Foshan Linggao New Materials Co., Ltd.; the protective dry particles are 609 protective dry particles, which are purchased from Guangdong Dow Technology Co., Ltd.; the protective glaze powder is PG01 glaze powder, which is purchased from Foshan Linggao New Materials Co., Ltd.; the ceramic glue is DS1200 ceramic glue, which is purchased from Guangdong Dow Technology Co., Ltd.
[0093] The specific chemical compositions of the raw materials in the following examples are shown in the following table (mass percentage):
[0094]
[0095]
[0096] Note: The chemical composition of the raw materials in the above table is less than 100%, mainly due to the presence of other undetected impurities.
[0097] The melting points of the raw materials in the following examples are shown in the following table (°C):
[0098]
[0099] Example 1
[0100] A preparation process of a colorful crystal effect ceramic tile comprises the following steps:
[0101] S11, mix 100 parts of blue dry particles and 20 parts of flux dry particles, add 10 parts of printing paste and 50 parts of printing oil to make a blue glaze slurry for standby use;
[0102] S12, mix 100 parts of black dry particles and 15 parts of flux dry particles, add 10 parts of printing paste and 50 parts of printing oil to make black glaze slurry for standby use;
[0103] S2, 100 parts of protective glaze powder, 58 parts of water, 0.3 parts of methyl cellulose, and 0.5 parts of sodium tripolyphosphate were fully mixed and ball-milled for 10 minutes, and then ceramic glue was added and mixed to prepare a protective glaze slurry with a specific gravity of 1.20 g / mL, which was set aside;
[0104] S3, applying base glaze and inkjet printing patterns on the surface of conventional ceramic green bodies;
[0105] S41, print a layer of blue glaze slurry on the surface of the blank with a 40-mesh screen according to the preset pattern texture, and the glaze amount is 50g / m 2 ;
[0106] S42, print a layer of black glaze slurry on the surface of the blank with a 40-mesh screen according to the preset pattern texture, and the glaze amount is 14g / m 2 ;
[0107] S5. Apply protective dry particles on the surface of the body after applying the colored glaze slurry, with a spreading amount of 830g / m 2 ;
[0108] S6: Apply protective glaze slurry on the surface of the body obtained in step S5, with the glaze amount being 250g / m 2 ;
[0109] S7, firing the glazed body obtained in step S6, with the firing temperature being 1215° C. and the firing time being 67 min, to obtain the colorful crystal effect ceramic tile.
[0110] Example 2
[0111] A preparation process of a colorful crystal effect ceramic tile comprises the following steps:
[0112] S11, mix 100 parts of blue dry particles and 20 parts of flux dry particles, add 10 parts of printing paste and 50 parts of printing oil to make a blue glaze slurry for standby use;
[0113] S12, mix 100 parts of green dry particles and 15 parts of flux dry particles, add 10 parts of printing paste and 50 parts of printing oil to make a green glaze slurry for standby use;
[0114] S13, mix 100 parts of black dry particles and 20 parts of flux dry particles, add 10 parts of printing paste and 50 parts of printing oil to make black glaze slurry for standby use;
[0115] S2, 100 parts of protective glaze powder, 58 parts of water, 0.3 parts of methyl cellulose, and 0.5 parts of sodium tripolyphosphate were fully mixed and ball-milled for 10 minutes, and then ceramic glue was added and mixed to prepare a protective glaze slurry with a specific gravity of 1.20 g / mL, which was set aside;
[0116] S3, applying base glaze and inkjet printing patterns on the surface of conventional ceramic green bodies;
[0117] S41, print a layer of blue glaze slurry on the surface of the blank with a 40-mesh screen according to the preset pattern texture, and the glaze amount is 50g / m 2 ;
[0118] S42, print a layer of green glaze slurry on the surface of the blank with a 40-mesh screen according to the preset pattern texture, and the glaze amount is 39g / m 2 ;
[0119] S43, print a layer of black glaze slurry on the surface of the blank with a 40-mesh screen according to the preset pattern texture, and the glaze amount is 14g / m 2 ;
[0120] S5. Apply protective dry particles on the surface of the body after applying the colored glaze slurry, with a spreading amount of 830g / m 2 ;
[0121] S6: Apply protective glaze slurry on the surface of the body obtained in step S5, with the glaze amount being 250g / m 2 ;
[0122] S7, firing the glazed body obtained in step S6, with the firing temperature being 1215° C. and the firing time being 67 min, to obtain the colorful crystal effect ceramic tile.
[0123] Comparative Example 1
[0124] This comparative example adopts the same preparation process and parameters as Example 2, except that no fluxing dry particles are added when preparing the colored glaze slurry.
[0125] Comparative Example 2
[0126] This comparative example adopts the same preparation process and parameters as Example 2, except that the addition ratio of color dry particles and flux dry particles is adjusted, as shown in the following table:
[0127]
[0128] The colorful crystal effect ceramic tiles prepared in Examples 1 to 2 and Comparative Examples 1 to 2 were subjected to performance tests to detect the glaze flatness and brightness difference, and compared with natural stone, the appearance of the three-dimensional color texture pattern of the glaze was observed, the color and crystal effect were judged, and the grades were divided into "poor", "average" and "good". The glaze flatness was measured by using a ceramic tile flatness measuring instrument to measure the maximum concave-convex difference of the glaze surface, and the instrument reading was the glaze flatness of the tile. The brightness difference was measured by using a ceramic gloss measuring instrument to measure the maximum and minimum brightness of the tile surface, and the difference was the brightness difference.
[0129] The test results are shown in Table 1.
[0130] Table 1 Test results
[0131] Appearance comparison Glaze surface smoothness (mm) Luminosity difference (°) Example 1 good 0.28 2.5 Example 2 good 0.29 2.8 Comparative Example 1 Poor 0.90 8.5 Comparative Example 2-1 Poor 0.85 8.0 Comparative Example 2-2 Poor 1.2 35
[0132] As can be seen from Table 1, in Comparative Example 1, the color dry particles were not blended with the fluxing dry particles, and the glaze was directly applied on the surface of the body. The color dry particles were not well melted with the protective dry particles, and there was a pile-up phenomenon, resulting in an uneven glaze surface, poor flatness, and a large difference in glossiness, which affected the appearance of the bricks out of the kiln. In Comparative Example 2-1, the amount of fluxing dry particles added in the addition ratio of green dry particles to fluxing dry particles was small, and the green dry particles were not well melted, resulting in a small amount of pile-up phenomenon, which resulted in poor flatness of the glaze surface after firing, a high difference in glossiness, and a poor overall appearance. In Comparative Example 2-2, the amount of fluxing dry particles added was too large, which would cause the glaze surface to be over-burned, resulting in large holes in the glaze surface, and a significant decrease in flatness and glossiness. In Example 1, two color dry particles were compounded, and the glaze surface of the obtained ceramic tile was transparent and crystal, with blue and black crystal stone effects, and at the same time, the glaze surface had high flatness and a small difference in glossiness. Example 2: Three kinds of color dry particles, namely blue dry particles, green dry particles and black dry particles, were selected, and a specific ratio and glaze amount were selected, and they were screen-printed on the blank layer by layer according to a specific pattern to prepare the following Figure 1 The ceramic tile imitating cloisonné stone shown is from Figures 2-3 From the partial picture, we can see that the glaze texture is delicate, with a transparent jade texture as the base, supplemented by large areas of blue crystals and transparent jade crystals, and dotted with a few green and black crystals, forming a colorful and visually impactful imitation cloisonné ceramic tile. At the same time, the glaze surface after firing is highly flat, with a glaze surface concave and convex value of 0.29mm and a lightness difference of 2.8°.
[0133] In summary, the present invention adopts a wet glaze slurry process instead of a dry spreading process to prepare dry particle decorative ceramic tiles. By mixing color dry particles and fluxing dry particles and then applying protective dry particles, colorful crystal imitation stone textures with bright colors and transparent crystals can be made. At the same time, the glaze surface can be ensured to have high flatness, a concave-convex value of less than 0.3mm, and a brightness difference of less than 3°, thereby reducing production costs and improving production stability.
[0134] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A preparation process of colorful crystal effect ceramic tiles, It is characterized in that The steps include: S1, mixing at least two kinds of color dry particles with flux dry particles respectively, adding printing paste and printing oil to mix to form at least two kinds of colored glaze slurries for standby use; S2, mixing protective glaze powder, water, methyl cellulose, sodium tripolyphosphate and ceramic glue to prepare protective glaze slurry for later use; S3, applying base glaze and inkjet printing patterns on the surface of the blank; S4, screen-printing the various colored glaze slurries obtained in step S1 on the surface of the blank obtained in step S3 according to preset pattern textures; S5, applying protective dry particles on the surface of the body after applying the colored glaze slurry; S6, applying the protective glaze slurry prepared in step S2 to the surface of the green body obtained in step S5; S7, firing the glazed body obtained in step S6 to obtain the colorful crystal effect ceramic tile.
2. A process for preparing a colorful crystal effect ceramic tile as claimed in claim 1, It is characterized in that The softening temperature of the color dry particles is 1040-1070°C, the softening temperature of the fluxing dry particles is 930-950°C, and the softening temperature of the protective dry particles is 1030-1050°C.
3. A process for preparing a colorful crystal effect ceramic tile as claimed in claim 1, It is characterized in that The color dry particles include at least two of blue dry particles, green dry particles and black dry particles; The blue dry particles include the following components by mass percentage: SiO 2 43.80~46.50%、Al 2 O 3 14.02~15.52%, CaO 15.04~16.65%, MgO 6.00~8.00%, K 2 O 0.81~1.52%、Na 2 O 0.60~1.00%, BaO 4.86~5.97%, ZrO 2 4.51~5.93%、P 2 O 5 0.21~0.41%, loss on ignition: 0.40~0.60%; The green dry particles include the following components by mass percentage: SiO 2 53.49~56.39%、Al 2 O 3 19.83~21.09%, CaO 12.93~14.54%, MgO 3.98~5.78%, K 2 O 1.03~2.52%、Na 2 O 0.98~2.17%, BaO 0.07~0.20%, ZrO 2 0.09~0.24%、P 2 O 5 0.16~0.38%, loss on ignition: 0.40~0.60%; The black dry particles include the following components by mass percentage: SiO 2 42.10~45.04%、Al 2 O 3 12.40~14.96%,Fe 2 O 3 4.42~5.46%, CaO 14.89~16.86%, MgO 5.41~7.85%, K 2 O 0.97~1.93%、Na 2 O 0.35~0.95%, BaO 4.86~5.97%, ZrO 2 2.65~3.89%, P 2 O 5 0.16~0.38%, MnO 2.69~3.57%, ignition loss: 0.85~1.23%.
4. A process for preparing a colorful crystal effect ceramic tile as claimed in claim 1, It is characterized in that The fluxing dry particles include the following components by mass percentage: SiO 2 63.19~65.98%、Al 2 O 3 13.54~15.87%, CaO 9.23~11.69%, MgO 3.98~5.26%, K 2 O 0.97~2.34%、Na 2 O 1.87~3.24%, loss on ignition: 0.21~0.51%; The protective dry particles include the following components by mass percentage: SiO 2 56.03~59.12%、Al 2 O 3 6.01~7.98%, CaO 11.14~13.17%, MgO 0.14~0.39%, K 2 O 6.12~8.21%、Na 2 O 0.10~0.32%, BaO 1.99~3.05%, ZnO 10.13~12.01%, loss on ignition: 0.02~0.13%; The protective glaze powder comprises the following components by mass percentage: SiO 2 64.85~67.03%、Al 2 O 3 9.51~11.07%, CaO 9.02~10.97%, MgO 1.02~2.09%, K 2 O 0.56~1.24%、Na 2 O 4.97~6.05%, BaO 0.64~1.23%, ZnO 0.98~1.58%, loss on ignition: 1.42~1.97%.
5. A process for preparing a colorful crystal effect ceramic tile as claimed in claim 1, It is characterized in that The particle size range of the color dry particles is 60-120 meshes, the particle size range of the flux dry particles is 60-120 meshes, and the particle size range of the protective dry particles is 60-150 meshes.
6. A process for preparing a colorful crystal effect ceramic tile according to claim 1, It is characterized in that In the step S1, the color dry particles are 90 to 110 parts by weight, and the flux dry particles are 10 to 25 parts by weight; In the step S2, the protective glaze powder is 90-110 parts, water is 50-65 parts, methyl cellulose is 0.2-0.4 parts, and sodium tripolyphosphate is 0.4-0.6 parts, calculated by weight.
7. A process for preparing a colorful crystal effect ceramic tile according to claim 1, It is characterized in that In step S4, the amount of the colored glaze slurry applied is 55-120 g / m 2 .
8. A process for preparing a colorful crystal effect ceramic tile according to claim 1, It is characterized in that In step S5, the amount of the protective dry particle cloth is 800-900 g / m 2 ; In step S6, the specific gravity of the protective glaze slurry is 1.18-1.25 g / mL, and the glaze application amount is 240-260 g / m 2 .
9. A process for preparing a colorful crystal effect ceramic tile as claimed in claim 3, It is characterized in that The steps include: S11, mixing the blue dry particles and the fluxing dry particles, adding printing paste and printing oil to mix to prepare blue glaze slurry for standby use; S12, mixing the green dry particles and the fluxing dry particles, adding printing paste and printing oil to mix to prepare green glaze slurry for standby use; S13, mixing the black dry particles and the fluxing dry particles, adding printing paste and printing oil to mix to prepare black glaze slurry for standby use; S2, mixing protective glaze powder, water, methyl cellulose, sodium tripolyphosphate and ceramic glue to prepare protective glaze slurry for later use; S3, applying base glaze and inkjet printing patterns on the surface of the blank; S41, screen printing a layer of the blue glaze slurry on the surface of the blank according to a preset pattern texture; S42, screen printing a layer of the green glaze slurry on the surface of the blank according to a preset pattern texture; S43, screen printing a layer of the black glaze slurry on the surface of the blank according to a preset pattern texture; S5, applying protective dry particles on the surface of the body after applying the colored glaze slurry; S6, applying the protective glaze slurry prepared in step S2 to the surface of the green body obtained in step S5; S7, firing the glazed body obtained in step S6 to obtain the colorful crystal effect ceramic tile.
10. A colorful crystal effect ceramic tile, It is characterized in that The colorful crystal effect ceramic tile is prepared by the preparation process of the colorful crystal effect ceramic tile according to any one of claims 1 to 9.
Citation Information
Patent Citations
Ceramic tile with dry particle glaze-decorated surface and manufacturing method thereof
CN103626523A
Fully-polished glaze ceramic tiles with granular flashing decoration and preparation method thereof
CN110357668A
Stereo-positioning effect dry granule complete-polished ceramic brick and preparation method thereof
CN110396005A
Preparation method of colored crystal glazed porcelain
CN112876290A
Low-light marble ceramic tile with uniform luminosity and preparation method of low-light marble ceramic tile
CN114276167A