Positive pole piece and preparation method thereof, and secondary battery and electrochemical device comprising positive pole piece

By adopting a double-layer clad structure on the manganese-based positive electrode material, using the combination of oxide solid electrolyte and conductive polymer layer, the problem of decreasing capacity of manganese-based positive electrode material at high temperatures and manganese dissolution is solved, and the secondary battery is realized Improved high cycle performance and rate performance.

CN119050268APending Publication Date: 2024-11-29清陶(乌海)能源科技有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411182870.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The charge and discharge capacity of manganese-based positive electrode materials rapidly decreases in high temperature environments, and manganese dissolves and deposits during electrochemical cycles, affecting its application prospects. The existing oxide solid electrolyte coating cannot completely isolate the electrolyte, resulting in deterioration of rate performance.

Method used

Using a double-layer clad structure, including an oxide solid electrolyte layer and a conductive polymer layer, the complex barrier effect on manganese ions is enhanced through the selection of conductive polymers such as polyaniline and polypyrrole, and the ions are lifted in combination with the second solid electrolyte powder. Conductivity, the positive electrode sheet formed.

Benefits of technology

It significantly improves the circulation performance and capacity retention rate of the secondary battery, reduces the dissolution and deposition of manganese elements, and has both good rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012709290000091
    Figure BDA0005012709290000091
  • Figure BDA0005012709290000092
    Figure BDA0005012709290000092
  • Figure BDA0005012709290000161
    Figure BDA0005012709290000161
Patent Text Reader

Abstract

The invention belongs to the technical field of energy storage, and particularly provides a positive pole piece, a preparation method of the positive pole piece, a secondary battery comprising the positive pole piece and an electrochemical device comprising the positive pole piece. The positive electrode material particles comprise positive electrode active material particles, oxide solid electrolyte layers coating the outer surfaces of the positive electrode active material particles, and conductive polymer layers coating the surfaces of the sides, away from the positive electrode active material particles, of the oxide solid electrolyte layers. The positive electrode active material particles comprise a positive electrode active material; the positive electrode active material is selected from at least one of lithium manganate, a lithium-rich manganese-based positive electrode material and nickel cobalt lithium manganate. According to the positive pole piece provided by the invention, the cycle performance and the capacity retention ratio of the secondary battery comprising the positive pole piece can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of energy storage materials, and in particular to a positive electrode sheet and a preparation method thereof, as well as a secondary battery and an electrochemical device comprising the same. Background Art

[0002] Lithium-ion batteries have become the main solution for mobile energy due to their outstanding advantages such as high energy density, low self-discharge, and no memory effect, and have been widely used in mobile phones, tablets, electric vehicles, drones, etc. Manganese-based cathode materials have the advantages of low cost, excellent low-temperature performance, and good safety. However, under high temperature conditions, the charge and discharge capacity of manganese-based cathode materials decreases rapidly, which has become the main disadvantage restricting their development; during the electrochemical cycle, manganese will inevitably dissolve from the active material into the electrolyte, which greatly affects the application prospects of manganese-based cathode materials.

[0003] On the one hand, the loss of manganese in the active material can lead to the structural collapse of the positive electrode, and on the other hand, the manganese deposition on the negative electrode side driven by the electric field can affect the solid electrolyte interface (SEI) stability and capacity decay. The corrosion of the electrolyte is believed to be the cause of the manganese dissolution during the cycling process. During the cycling process, the high-valent manganese ions are easily reduced to Mn 3+ , even Mn 2+ In addition, through Mn 3+ The disproportionation reaction of Mn will promote the dissolution of Mn 4+ +e→Mn 3+ ;2Mn 3+ →Mn 4+ +Mn 2+ ). Therefore, it is considered to modify the surface of the manganese-based positive electrode material on the basis of composite doping to further improve the electrochemical performance of lithium manganese oxide. If only oxide solid electrolyte is used to coat the manganese-based positive electrode material, most of the electrolyte can be isolated. However, due to the high Young's modulus and hard texture of the oxide solid electrolyte, it is impossible to achieve dense coating and complete isolation. Some electrolyte will inevitably contact the manganese-based positive electrode material. Moreover, due to the low ionic conductivity of the oxide solid electrolyte itself, the oxide solid electrolyte coating will cause the battery's rate performance to deteriorate. Summary of the invention

[0004] The object of the present invention is to provide a positive electrode plate and a method for preparing the same, as well as a secondary battery and an electrochemical device comprising the same, for improving the cycle performance and capacity retention rate of the secondary battery.

[0005] To achieve the above-mentioned purpose of the invention, the technical solution of the present invention is as follows:

[0006] According to a first aspect of the present invention, a positive electrode plate is provided, the positive electrode plate comprising: a positive electrode material layer, the positive electrode material layer comprising positive electrode material particles, the positive electrode material particles comprising positive electrode active material particles, an oxide solid electrolyte layer coated on the outer surface of the positive electrode active material particles, and a conductive polymer layer coated on the surface of the oxide solid electrolyte layer on a side away from the positive electrode active material particles; the positive electrode active material particles comprising positive electrode active material; the positive electrode active material is selected from at least one of lithium manganese oxide, lithium-rich manganese-based positive electrode material and nickel cobalt lithium manganese oxide.

[0007] In one aspect of the present invention, the conductive polymer layer comprises a conductive polymer; the conductive polymer is selected from polyaniline and / or polypyrrole.

[0008] In one aspect of the present invention, the oxide solid state electrolyte layer includes an oxide solid state electrolyte.

[0009] In one aspect of the present invention, the oxide solid electrolyte is selected from lithium aluminum titanium phosphate (Li 1.3 Al 0.3 Ti 1.7 (PO4)3, LATP).

[0010] In one aspect of the present invention, the oxide solid electrolyte is selected from lithium lanthanum zirconium oxide (Li7La3Zr2O 12 , LLZO).

[0011] In one aspect of the present invention, the oxide solid electrolyte is selected from lithium lanthanum titanium oxide (Li 0.33 La 0.56 TiO3, LLTO).

[0012] In one aspect of the present invention, in the positive electrode material layer, the mass ratio of the oxide solid electrolyte layer to the positive electrode active material particles is (1-5): (95-99).

[0013] In one aspect of the present invention, the thickness of the oxide solid electrolyte layer is 0.01-2 μm.

[0014] In one aspect of the present invention, the conductive polymer is prepared by conductive polymer monomers; wherein the ratio of the mass of the conductive polymer monomers to the sum of the mass of the oxide solid electrolyte layer and the positive electrode active material particles in the positive electrode material layer is (1-5): (95-99). Specifically, the mass ratio of the oxide solid electrolyte layer to the positive electrode active material particles can be 1:99, 3:97 or 5:95.

[0015] In one aspect of the present invention, based on the total mass of the positive electrode material layer, the mass percentage of the positive electrode active material particles in the positive electrode material layer is 80%-99%.

[0016] In one aspect of the present invention, the positive electrode plate further includes a conductive agent and a binder; wherein, based on the total mass of the positive electrode plate, the mass percentage of the conductive agent is 1%-20%; the mass percentage of the binder is 1%-20%.

[0017] In one aspect of the present invention, the positive electrode material layer further includes a second solid electrolyte powder; the second solid electrolyte powder is used to improve the ionic conductivity of the composite positive electrode. The present invention does not limit the type of the second solid electrolyte powder, which can be at least one of an oxide solid electrolyte powder, a sulfide solid electrolyte powder and a second halide solid electrolyte powder.

[0018] In one aspect of the present invention, the material of the second oxide solid state electrolyte powder is the same as that of the oxide solid state electrolyte.

[0019] In one aspect of the present invention, based on the total mass of the positive electrode material layer, the mass percentage of the second solid electrolyte powder is 1%-20%, preferably 5%-20%.

[0020] According to a second aspect of the present invention, there is provided a method for preparing the aforementioned positive electrode sheet, the method comprising the following steps:

[0021] Step 1: fully and uniformly mixing the positive electrode active material and the oxide solid electrolyte to obtain a first mixture;

[0022] Step 2: placing the first mixture obtained in step 1 in water, adding a first acidic medium solution to adjust the pH to a first pH value, and then adding a conductive polymer monomer to obtain a first solution; placing the first mixture in the first solution;

[0023] Step 3: placing an oxidant in water, adding the second acidic medium solution to adjust the pH to a second pH value, and obtaining a second solution;

[0024] Step 4: lowering the temperatures of the first solution and the second solution, and then adding the second solution to the first solution in a stirring state, and continuing the reaction after the dropwise addition is completed to obtain a positive electrode material;

[0025] Step 5: coating the positive electrode slurry containing the positive electrode material on the positive electrode collector to obtain the positive electrode sheet.

[0026] In one aspect of the present invention, in step 4, after lowering the temperatures of the first solution and the second solution, the second solution is slowly added to the first solution in a stirring state.

[0027] In one aspect of the present invention, the first acidic medium solution and the second acidic medium solution are selected from hydrochloric acid solution or sulfuric acid solution; the molar concentration of the first acidic medium solution and the second acidic medium solution is selected from 0.8-1.5 mol / L.

[0028] In one aspect of the present invention, the first pH value and the second pH value are 2-4.

[0029] In one aspect of the present invention, the mass of the oxidant is 0.1%-1% of the mass of the conductive polymer monomer.

[0030] In one aspect of the present invention, the oxidant comprises at least one of ammonium persulfate, hydrogen peroxide, sodium vanadate and potassium dichromate.

[0031] In one aspect of the present invention, in the aforementioned method, the positive electrode active material is selected from at least one of lithium manganese oxide, lithium-rich manganese-based positive electrode materials and nickel cobalt lithium manganese oxide.

[0032] In one aspect of the present invention, in the aforementioned method, the conductive polymer layer comprises a conductive polymer; the conductive polymer is selected from polyaniline and / or polypyrrole.

[0033] In one aspect of the present invention, in the aforementioned method, the oxide solid electrolyte layer comprises an oxide solid electrolyte; the oxide solid electrolyte is selected from at least one of a NASICON-type solid electrolyte, a garnet-type solid electrolyte and a perovskite-type solid electrolyte, or a doped modified material selected from at least one of the NASICON-type solid electrolyte, the garnet-type solid electrolyte and the perovskite-type solid electrolyte.

[0034] In one aspect of the present invention, in the aforementioned method, the oxide solid electrolyte is selected from lithium aluminum titanium phosphate (Li 1.3 Al 0.3 Ti 1.7 (PO4)3, LATP).

[0035] In one aspect of the present invention, in the aforementioned method, the oxide solid electrolyte is selected from lithium lanthanum zirconium oxide (Li7La3Zr2O 12 , LLZO).

[0036] In one aspect of the present invention, in the aforementioned method, the oxide solid electrolyte is selected from lithium lanthanum titanium oxide (Li 0.33 La 0.56 TiO3, LLTO).

[0037] In one aspect of the present invention, in step 1 of the aforementioned method, the positive electrode active material and the oxide solid electrolyte are placed in a high-speed mixer for full and uniform mixing, so that friction and collision occur during the physical mixing process, so that the solid electrolyte is evenly dispersed and adsorbed on the surface of the manganese-based positive electrode material to form an inner coating layer.

[0038] In one aspect of the present invention, the speed of the high-speed mixer is 300-700 r / min; and the mixing time is 12-48 h.

[0039] In one aspect of the present invention, in step 4 of the aforementioned method, step 4 includes the following: placing the first solution and the second solution in an ice water bath, and then slowly adding the second solution to the first solution in a stirring state, and continuing the reaction for 2-4 hours after the dropwise addition is completed to obtain a positive electrode material.

[0040] According to a third aspect of the present invention, a secondary battery is provided, comprising a negative electrode plate, an electrolyte, and the positive electrode plate described above, or a positive electrode plate prepared by the method described above.

[0041] According to a fourth aspect of the present invention, there is provided an electrochemical device comprising the aforementioned secondary battery.

[0042] The beneficial effects of the present invention are as follows: by using the secondary battery with the positive electrode plate provided by the present invention, the isolation effect on the electrolyte is enhanced by double-layer coating of the manganese-based positive electrode material, and the secondary battery has good cycle performance and rate performance through the coordination of the conductive sublayer and the ion conductive layer. By selecting the conductive polymer, the complexing barrier effect on manganese ions is enhanced, so that the cycle performance and capacity retention rate of the secondary battery can be significantly improved, and the dissolution and deposition of the manganese element in its positive electrode active material can also be significantly reduced. DETAILED DESCRIPTION

[0043] The following non-limiting examples can enable those skilled in the art to more fully understand the present invention, but do not limit the present invention in any way. The following content is only an exemplary description of the scope of the present invention, and those skilled in the art can make various changes and modifications to the invention of the present invention based on the disclosed content, and they should also fall within the scope of the present application.

[0044] Positive electrode:

[0045] In some embodiments of the present invention, the secondary battery provided by the present invention includes a positive electrode, the positive electrode includes a positive electrode current collector and a positive electrode material layer disposed on the positive electrode current collector, the positive electrode material layer includes a positive electrode material, and the positive electrode material particles include positive electrode active material particles, an oxide solid electrolyte layer coated on the outer surface of the positive electrode active material particles, and a conductive polymer layer coated on the surface of the oxide solid electrolyte layer away from the positive electrode active material particles. The positive electrode active material includes a compound that reversibly embeds and deintercalates lithium ions. In the present invention, the positive electrode active material is selected from a manganese-based positive electrode material. Specifically, the positive electrode active material is selected from at least one of lithium manganate, lithium-rich manganese-based positive electrode material, and nickel cobalt lithium manganate. They can be used alone, or two or more can be used in any combination.

[0046] In some embodiments of the present invention, the positive electrode active material is selected from lithium manganese oxide.

[0047] In some embodiments of the present invention, the oxide solid electrolyte layer comprises an oxide solid electrolyte; the type of oxide solid electrolyte is not limited in the present application, and any oxide solid electrolyte with lithium ion conductivity in the art can be used in the present application. Exemplarily, the oxide solid electrolyte is at least one of a NASICON solid electrolyte, a garnet solid electrolyte, and a perovskite solid electrolyte, or a doped modified material selected from at least one of a NASICON solid electrolyte, a garnet solid electrolyte, and a perovskite solid electrolyte.

[0048] In some embodiments of the present invention, the conductive polymer is selected from polyaniline and / or polypyrrole.

[0049] In some preferred embodiments of the present invention, the positive electrode active material is selected from lithium manganese oxide, and the oxide solid electrolyte is selected from lithium titanium aluminum phosphate or lithium lanthanum zirconium oxide.

[0050] In some preferred embodiments of the present invention, the thickness of the oxide solid electrolyte is 0.01-2 μm.

[0051] In some embodiments of the present invention, the positive electrode material layer further includes a binder, which improves the bonding between the positive electrode active material particles and also improves the bonding between the positive electrode material layer and the positive electrode current collector.

[0052] In some embodiments of the present invention, non-limiting examples of binders include polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, and the like.

[0053] In some embodiments of the present invention, the cathode material layer includes a conductive agent to impart conductivity to the electrode. The conductive agent may include any conductive material as long as it does not cause chemical changes. Non-limiting examples of conductive materials include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., including, for example, copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives) and mixtures thereof.

[0054] In some embodiments of the present invention, the positive electrode sheet includes a positive electrode current collector. Exemplarily, the positive electrode current collector may be aluminum (Al), but is not limited thereto.

[0055] In some embodiments of the present invention, the positive electrode provided by the present invention is obtained by the following preparation method:

[0056] Step 1: fully and uniformly mixing the positive electrode active material and the oxide solid electrolyte to obtain a first mixture;

[0057] Step 2: placing the first mixture obtained in step 1 in water, adding a first acidic medium solution to adjust the pH to a first pH value, and then adding a conductive polymer monomer to obtain a first solution; placing the first mixture in the first solution;

[0058] Step 3: placing an oxidant in water, adding a second acidic medium solution to adjust the pH to a second pH value, and obtaining a second solution;

[0059] Step 4: lowering the temperatures of the first solution and the second solution, and then adding the second solution to the first solution in a stirring state, and continuing the reaction after the dropwise addition is completed to obtain a positive electrode material;

[0060] Step 5: Coat the positive electrode slurry containing the positive electrode material on the positive electrode collector to obtain a positive electrode sheet.

[0061] In some embodiments of the present invention, based on the total mass of the positive electrode material layer, the mass percentage of the positive electrode active material particles in the positive electrode material layer is 80%-99%.

[0062] In some embodiments of the present invention, the mass of the conductive agent accounts for 1%-20% of the mass of the positive electrode material layer.

[0063] In some embodiments of the present invention, the mass of the binder accounts for 1%-20% of the mass of the positive electrode material layer.

[0064] In some embodiments of the present invention, the positive electrode plate provided by the present invention further includes a second solid electrolyte powder for improving the ionic conductivity of the composite positive electrode. The present invention does not limit the type of the second solid electrolyte powder, which may be an oxide solid electrolyte powder, a sulfide solid electrolyte powder, or a halide solid electrolyte powder. Optionally, the mass of the second solid electrolyte powder accounts for 1%-20% of the mass of the positive electrode plate; preferably 5%-20%.

[0065] In some embodiments of the present invention, the thickness of the positive electrode material layer in the positive electrode plate provided by the present invention is 30-400 μm, for example, 30 μm, 40 μm, 50 μm, 80 μm, 110 μm, 200 μm, 300 μm, 400 μm, preferably 50-110 μm.

[0066] Negative electrode:

[0067] In some embodiments of the present invention, the negative electrode sheet includes a current collector and a negative electrode active material layer disposed on the current collector.

[0068] In the present invention, the specific types of negative electrode active materials are not subject to specific restrictions and can be selected according to needs. Specifically, the negative electrode active material is selected from natural graphite, artificial graphite, mesophase microcarbon beads (MCMB for short), hard carbon, soft carbon, silicon, silicon-carbon composites, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO2, spinel structured lithiated TiO2-Li4Ti5O 12 , Li-Al alloy. Non-limiting examples of carbon materials include crystalline carbon, amorphous carbon and mixtures thereof. Crystalline carbon can be amorphous or flake-shaped, platelet-shaped, spherical or fibrous natural graphite or artificial graphite. Amorphous carbon can be soft carbon, hard carbon, mesophase pitch carbide, calcined coke, etc.

[0069] In some embodiments of the present invention, metal elements and metal compounds can also be selected as negative electrode active materials, such as compounds containing metals or metalloids such as Li, Ag, Al, Bi, Cu, Ga, Ge, In, Ni, Pb, Sb, Si, Sn, Sr, and Zn.

[0070] In some embodiments of the present invention, the mass percentage of the negative electrode active material contained in the negative electrode active material layer can be 80%-99%, for example, 80%, 85%, 90%, 95%, 97%, 99%, etc., preferably 95%-97%.

[0071] In some embodiments of the present invention, the negative electrode material layer may include a binder; the binder improves the bonding between negative electrode active material particles and the bonding between the negative electrode active material and the current collector.

[0072] In some embodiments of the present invention, non-limiting examples of binders include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, and the like.

[0073] In some embodiments of the present invention, the negative electrode active material layer can be obtained by coating a negative electrode slurry on a negative electrode current collector and then drying the negative electrode slurry, wherein the negative electrode slurry includes at least a negative electrode active material and a negative electrode binder. When an aqueous solvent is used as a liquid medium for forming the negative electrode slurry, a thickener is preferably used for slurrying, and the thickener can generally be used to adjust the viscosity of the slurry.

[0074] In some embodiments of the present invention, the aforementioned thickener may be one or more of the following: carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein and salts thereof.

[0075] In some embodiments of the present invention, the mass proportion of the thickener in the negative electrode slurry can be 0.1%-5%, for example, 0.1%, 0.2%, 0.5%, 0.6%, 1%, 2%, 3%, 4%, 5%, etc., preferably 0.5%-3%, and more preferably 0.6%-2%.

[0076] In some embodiments of the present invention, the negative electrode active material layer includes a conductive material, so that the electrode has conductivity. The conductive material may include any conductive material as long as it does not cause chemical changes. Non-limiting examples of conductive materials include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., such as copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives) and mixtures thereof.

[0077] In some embodiments of the present invention, the negative electrode current collector may be selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0078] Diaphragm:

[0079] In some embodiments of the present invention, the lithium battery and electrochemical device of the present invention are provided with a separator between the positive electrode and the negative electrode to prevent short circuit. The material and shape of the separator used in the electrochemical device of the present invention are not particularly limited, and it can be any technology disclosed in the prior art.

[0080] In some embodiments of the present invention, the separator includes a polymer or an inorganic substance formed of a material that is stable to the electrolyte of the present application.

[0081] In some embodiments of the present invention, the separator may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film with a porous structure, and the material of the substrate layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide.

[0082] Electrolyte:

[0083] The lithium battery and electrochemical device of the present invention also include an electrolyte.

[0084] In some embodiments of the present invention, the electrolyte includes a lithium salt and a solvent.

[0085] In some embodiments of the present invention, the lithium salt includes at least one of an organic lithium salt or an inorganic lithium salt. In some embodiments of the present invention, the lithium salt includes, but is not limited to: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), bistrifluoromethanesulfonyl imide lithium LiN(CF3SO2)2 (LiTFSI), bis(fluorosulfonyl)imide lithium Li(N(SO2F)2) (LiFSI), lithium bis(oxalate borate) LiB(C2O4)2 (LiBOB) or lithium di(oxalate borate) LiBF2(C2O4) (LiDFOB).

[0086] In some embodiments of the present invention, the solvent can be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0087] In some embodiments of the present invention, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, additives that improve battery low temperature performance, etc.

[0088] In some embodiments of the present invention, the aforementioned additives include 1,3-propane sultone, 1,4-butane sultone, propenyl-1,3-sultone, vinyl sulfate, 4-methyl vinyl sulfate, propenyl sulfate,

[0089]

[0090] , at least one of saturated phosphate compounds and unsaturated phosphate compounds, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)borate, tris(triethylsilyl)borate, succinonitrile, glutaronitrile, ethylene glycol bis(propionitrile) ether, hexanetrinitrile, adiponitrile, pimelonitrile, suberonitrile, azelaic acid dinitrile, and sebaconitrile, and a compound comprising the following chemical formula:

[0091]

[0092] Among them, R 41 , R 42 , R 43 Each independently selected from a C1-C5 saturated hydrocarbon group, an unsaturated hydrocarbon group, a halogenated hydrocarbon group, -Si(C m H 2m+1 )3, m is a natural number from 1 to 3, and R 41 , R 42 , R 43 At least one of them is an unsaturated hydrocarbon group.

[0093] Secondary battery:

[0094] In some embodiments of the present invention, the secondary battery of the present invention comprises the above-mentioned positive electrode sheet, negative electrode sheet, separator, electrolyte, etc., but is not limited thereto.

[0095] In some embodiments of the present invention, the secondary battery of the present invention is made by stacking the above-mentioned positive and negative electrode sheets.

[0096] In some embodiments of the present invention, the secondary battery of the present invention may include an outer package, which may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.

[0097] In some embodiments of the present invention, the present invention further provides a battery module. The battery module includes the above-mentioned secondary battery. The number of secondary batteries contained in the battery module of the present invention can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module.

[0098] In some embodiments of the present invention, the present invention further provides a battery pack, which includes the above-mentioned battery module. The number of battery modules included in the battery pack can be adjusted according to the application and capacity of the battery pack.

[0099] Device:

[0100] The present invention also provides a device, which includes at least one of the above-mentioned secondary battery, battery module or battery pack.

[0101] In some embodiments of the present invention, the device includes, but is not limited to: electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, power storage systems, etc. In order to meet the device's requirements for high power and high energy density of lithium batteries, a battery pack or battery module can be used.

[0102] In other embodiments of the present invention, the device may be a mobile phone, a tablet computer, a notebook computer, etc. The device is usually required to be light and thin, and a lithium battery may be used as a power source.

[0103] The present invention will be further described below in conjunction with the examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0104] The present invention is further described below by way of specific examples. The various chemical reagents used in the examples of the present invention are obtained through conventional commercial channels unless otherwise specified. Unless otherwise specified, the contents described below are all weight contents. Unless otherwise specified, it is understood that the process is carried out at room temperature.

[0105] Embodiment 1:

[0106] Embodiment 1 comprises the following steps:

[0107] (1) Preparation of positive electrode sheet:

[0108] Step 1: placing an oxide solid electrolyte and a positive electrode active material in a high-speed mixer for mixing, the speed of the high-speed mixer is 600 r / min; the mixing time is 20 hours, and a first mixture is obtained; wherein the oxide solid electrolyte is lithium aluminum titanium phosphate (LATP), and the positive electrode active material is lithium manganate; the mass ratio of the oxide solid electrolyte to the positive electrode active material is 1:99;

[0109] Step 2: placing the obtained first mixture in deionized water, and slowly dropping a hydrochloric acid solution to adjust the pH to 2.5, and then adding aniline monomer, the whole process is in a stirring state, to obtain a first solution (the first mixture is still placed in the first solution); wherein the mass ratio of aniline monomer to the first mixture is 5:95;

[0110] Step 3: placing potassium dichromate in deionized water, stirring, and then adding hydrochloric acid solution to adjust the pH to 2.5 to obtain a second solution;

[0111] Step 4: Transfer the first solution and the second solution to an ice water bath, slowly drop the second solution into the first solution under stirring, and continue the reaction for 3 hours after the dropwise addition is completed to obtain the product;

[0112] Step 5: Weigh the product, the conductive agent Super-P, and the binder PVDF in a mass ratio of 95:2:3; mix with the solvent NMP to form a uniform positive electrode slurry, and apply the positive electrode slurry on the current collector and dry it to form a composite positive electrode. The positive electrode current collector is aluminum foil.

[0113] (2) Preparation of negative electrode sheet:

[0114] Artificial graphite, conductive agent superconducting carbon black, thickener sodium carboxymethyl cellulose (CMC), and binder styrene butadiene rubber (SBR) are fully stirred and mixed in a proper amount of deionized water solvent according to a weight ratio of 95.0:1.5:1.5:2 to form a uniform negative electrode slurry. The slurry is coated on the negative electrode current collector copper foil, dried and cold pressed to obtain a negative electrode active material layer, and then cut, slit, and welded to obtain a negative electrode sheet.

[0115] (3) Preparation of lithium batteries:

[0116] The prepared positive electrode sheet, negative electrode sheet and separator (composed of a 9 μm PE polyethylene-based film and a 2 μm boehmite ceramic coating on both sides) are stacked in order so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging foil aluminum-plastic film, and the electrolyte (50% EMC + 30% EC + 20% DEC + 1.1M LiPF6 + 1% LiPO2F2 + 1% VC (vinyl carbonate) + 1% FEC) is injected into the dried bare battery cell, and after vacuum packaging, standing, formation, shaping, capacity testing and other processes, the preparation of the lithium ion battery of Example 1 is completed.

[0117] Embodiment 2:

[0118] Embodiment 2 comprises the following steps:

[0119] (1) Preparation of positive electrode sheet:

[0120] Step 1: placing an oxide solid electrolyte and a positive electrode active material in a high-speed mixer for mixing, the speed of the high-speed mixer is 600 r / min; the mixing time is 20 hours, and a first mixture is obtained; wherein the oxide solid electrolyte is lithium aluminum titanium phosphate (LATP), and the positive electrode active material is lithium manganate; the mass ratio of the oxide solid electrolyte to the positive electrode active material is 1:99;

[0121] Step 2: placing the obtained first mixture in deionized water, and slowly dropping a hydrochloric acid solution to adjust the pH to 2.5, and then adding aniline monomer, the whole process is in a stirring state, to obtain a first solution (the first mixture is still placed in the first solution); wherein the mass ratio of aniline monomer to the first mixture is 1:99;

[0122] Step 3: placing potassium dichromate in deionized water, stirring, and then adding hydrochloric acid solution to adjust the pH to 2.5 to obtain a second solution;

[0123] Step 4: Transfer the first solution and the second solution to an ice water bath, slowly drop the second solution into the first solution under stirring, and continue the reaction for 3 hours after the dropwise addition is completed to obtain the product;

[0124] Step 5: Weigh the product, the conductive agent Super-P, and the binder PVDF in a mass ratio of 95:2:3; mix with the solvent NMP to form a uniform positive electrode slurry, and apply the positive electrode slurry on the current collector and dry it to form a composite positive electrode. The positive electrode current collector is aluminum foil.

[0125] (2) Preparation of negative electrode sheet:

[0126] Artificial graphite, conductive agent superconducting carbon black, thickener sodium carboxymethyl cellulose (CMC), and binder styrene butadiene rubber (SBR) are fully stirred and mixed in a proper amount of deionized water solvent according to a weight ratio of 95.0:1.5:1.5:2 to form a uniform negative electrode slurry. The slurry is coated on the negative electrode current collector copper foil, dried and cold pressed to obtain a negative electrode active material layer, and then cut, slit, and welded to obtain a negative electrode sheet.

[0127] (3) Preparation of lithium batteries:

[0128] The prepared positive electrode sheet, negative electrode sheet and separator (composed of a 9 μm PE polyethylene-based film and a 2 μm boehmite ceramic coating on both sides) are stacked in order so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging foil aluminum-plastic film, and the electrolyte (50% EMC + 30% EC + 20% DEC + 1.1M LiPF6 + 1% LiPO2F2 + 1% VC (vinyl carbonate) + 1% FEC) is injected into the dried bare battery cell, and after vacuum packaging, standing, formation, shaping, capacity testing and other processes, the preparation of the lithium ion battery of Example 2 is completed.

[0129] Embodiment 3:

[0130] The steps of Example 3 are the same as those of Example 1, except that in step 2 of preparing the positive electrode sheet, the mass ratio of the aniline monomer to the first mixture is 10:90.

[0131] Embodiment 4:

[0132] The steps of Example 4 are the same as those of Example 1, except that in step 1 of preparing the positive electrode sheet, the mass ratio of the oxide solid electrolyte to the positive electrode active material is 5:95.

[0133] Embodiment 5:

[0134] The steps of Example 5 are the same as those of Example 1, except that in step 1 of preparing the positive electrode sheet, the mass ratio of the oxide solid electrolyte to the positive electrode active material is 3:97.

[0135] Embodiment 6:

[0136] The steps of Example 6 are the same as those of Example 1, except that in step 1 of preparing the positive electrode plate, the oxide solid electrolyte is lithium lanthanum zirconium oxide (LLZO); and in step 2 of preparing the positive electrode plate, pyrrole monomer is used instead of aniline monomer.

[0137] Comparative Example 1:

[0138] Comparative Example 1 comprises the following steps:

[0139] (1) Preparation of positive electrode sheet:

[0140] Lithium manganate, conductive agent Super-P, and binder PVDF are weighed in a mass ratio of 95:2:3; and mixed with solvent NMP to form a uniform positive electrode slurry, and the positive electrode slurry is coated on the current collector and dried to form a composite positive electrode. Aluminum foil is used as the positive electrode current collector.

[0141] (2) Preparation of negative electrode sheet:

[0142] Artificial graphite, conductive agent superconducting carbon black, thickener sodium carboxymethyl cellulose (CMC), and binder styrene butadiene rubber (SBR) are fully stirred and mixed in a proper amount of deionized water solvent according to a weight ratio of 95.0:1.5:1.5:2 to form a uniform negative electrode slurry. The slurry is coated on the negative electrode current collector copper foil, dried and cold pressed to obtain a negative electrode active material layer, and then cut, slit, and welded to obtain a negative electrode sheet.

[0143] (3) Preparation of lithium batteries:

[0144] The prepared positive electrode sheet, negative electrode sheet and separator (composed of a 9 μm PE polyethylene-based film and a 2 μm boehmite ceramic coating on both sides) are stacked in order so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging foil aluminum-plastic film, and the electrolyte (50% EMC + 30% EC + 20% DEC + 1.1M LiPF6 + 1% LiPO2F2 + 1% VC (vinyl carbonate) + 1% FEC) is injected into the dried bare battery cell, and after vacuum packaging, standing, formation, shaping, capacity testing and other processes, the preparation of the lithium ion battery of Comparative Example 1 is completed.

[0145] Comparative Example 2:

[0146] Comparative Example 2 comprises the following steps:

[0147] (1) Preparation of positive electrode sheet:

[0148] Step 1: placing the positive electrode active material lithium manganate in deionized water, and slowly dropping a hydrochloric acid solution to adjust the pH to 2.5, and then adding aniline monomer, the whole process is in a stirring state, to obtain a first solution (the first mixture is still placed in the first solution); wherein the mass ratio of the aniline monomer to the first mixture is 5:95;

[0149] Step 2: placing potassium dichromate in deionized water, stirring, and then adding hydrochloric acid solution to adjust the pH to 2.5 to obtain a second solution;

[0150] Step 3: Transfer the first solution and the second solution to an ice water bath, slowly drop the second solution into the first solution under stirring, and continue the reaction for 3 hours after the dropwise addition is completed to obtain the product;

[0151] Step 4: The product is weighed with the conductive agent Super-P and the binder PVDF in a mass ratio of 95:2:3; and mixed with the solvent NMP to form a uniform positive electrode slurry, and the positive electrode slurry is coated on the current collector and dried to form a composite positive electrode. Aluminum foil is used as the positive electrode current collector.

[0152] (2) Preparation of negative electrode sheet:

[0153] Artificial graphite, conductive agent superconducting carbon black, thickener sodium carboxymethyl cellulose (CMC), and binder styrene butadiene rubber (SBR) are fully stirred and mixed in a proper amount of deionized water solvent according to a weight ratio of 95.0:1.5:1.5:2 to form a uniform negative electrode slurry. The slurry is coated on the negative electrode current collector copper foil, dried and cold pressed to obtain a negative electrode active material layer, and then cut, slit, and welded to obtain a negative electrode sheet.

[0154] (3) Preparation of lithium batteries:

[0155] The prepared positive electrode sheet, negative electrode sheet and separator (composed of a 9 μm PE polyethylene-based film and a 2 μm boehmite ceramic coating on both sides) are stacked in order so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging foil aluminum-plastic film, and the electrolyte (50% EMC + 30% EC + 20% DEC + 1.1M LiPF6 + 1% LiPO2F2 + 1% VC (vinyl carbonate) + 1% FEC) is injected into the dried bare battery cell, and after vacuum packaging, standing, formation, shaping, capacity testing and other processes, the preparation of the lithium ion battery of Comparative Example 2 is completed.

[0156] Comparative Example 3:

[0157] Comparative Example 3 comprises the following steps:

[0158] (1) Preparation of positive electrode sheet:

[0159] Step 1: placing an oxide solid electrolyte and a positive electrode active material in a high-speed mixer for mixing, the speed of the high-speed mixer is 600 r / min; the mixing time is 20 hours, and a first mixture is obtained; wherein the oxide solid electrolyte is lithium aluminum titanium phosphate (LATP), and the positive electrode active material is lithium manganate; the mass ratio of the oxide solid electrolyte to the positive electrode active material is 1:99;

[0160] Step 2: The first mixture, the conductive agent Super-P, and the binder PVDF are weighed in a mass ratio of 95:2:3; and mixed with the solvent NMP to form a uniform positive electrode slurry, and the positive electrode slurry is coated on the current collector and dried to form a composite positive electrode. The positive electrode current collector is aluminum foil.

[0161] (2) Preparation of negative electrode sheet:

[0162] Artificial graphite, conductive agent superconducting carbon black, thickener sodium carboxymethyl cellulose (CMC), and binder styrene butadiene rubber (SBR) are fully stirred and mixed in a proper amount of deionized water solvent according to a weight ratio of 95.0:1.5:1.5:2 to form a uniform negative electrode slurry. The slurry is coated on the negative electrode current collector copper foil, dried and cold pressed to obtain a negative electrode active material layer, and then cut, slit, and welded to obtain a negative electrode sheet.

[0163] (3) Preparation of lithium batteries:

[0164] The prepared positive electrode sheet, negative electrode sheet and separator (composed of a 9 μm PE polyethylene-based film and a 2 μm boehmite ceramic coating on both sides) are stacked in order so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging foil aluminum-plastic film, and the electrolyte (50% EMC + 30% EC + 20% DEC + 1.1M LiPF6 + 1% LiPO2F2 + 1% VC (vinyl carbonate) + 1% FEC) is injected into the dried bare battery cell, and after vacuum packaging, standing, formation, shaping, capacity testing and other processes, the preparation of the lithium ion battery of Comparative Example 3 is completed.

[0165] Electrochemical test method:

[0166] The following electrochemical tests were performed on Examples 1-7 and Comparative Examples 1-3:

[0167] Cycle life test with 80% capacity cutoff at room temperature: comprising the following steps: (1) charging at 0.3C to a cutoff voltage of 4.2V, a cutoff current of 0.05C, and standing for 30 minutes; (2) discharging at 0.3C to a discharge end voltage of 3.0V, recording the discharge capacity, and standing for 30 minutes; (3) cycling (1)-(2) to test the cycle life with 80% capacity cutoff at room temperature.

[0168] 2C discharge capacity retention rate test: At room temperature (25°C), charge the battery cell to 4.2V at 2C, then switch to constant voltage charging with a cut-off current of 0.05C. The capacity is C0 at this time. Discharge the fully charged battery to 3.0V at the required rate (2C). The capacity obtained by the test is C1. C1 / C0 is the 2C discharge capacity retention rate.

[0169] ICP test:

[0170] Weigh about 0.1g of negative electrode powder (accurate to ±0.0003g) of two portions of each embodiment, place in a 100ml beaker, add a small amount of distilled water to wet the bottom of the cup, then add 5ml12mol / L HCl (made in Shandong, GR) to dissolve, heat on an electric heating plate for 20min, remove and cool, dilute and test. Introduce the prepared series of standard solutions into an iCAP7000 inductively coupled plasma spectrometer (ICP) (made in the United States), and measure the intensity of manganese in the standard solution at the wavelength of the element manganese to be measured. When the linear correlation coefficient of the working curve r≥0.9995, the measurement can be performed.

[0171] The test results of Examples 1-7 and Comparative Examples 1-3 are shown in Table 1.

[0172] Table 1

[0173]

[0174]

[0175] It can be seen from the above table:

[0176] Compared with Examples 1-6 and Comparative Examples 1-3, the positive electrode plate provided in the present application can effectively improve the cycle performance of the battery, the capacity retention rate of the battery can also be maintained at more than 92%, and the dissolution and deposition of manganese elements can also be reduced.

[0177] The present invention is intended to cover any modifications, uses or adaptive changes of the present invention, which follow the general principles of the present invention and include common knowledge or customary technical means in the technical field not disclosed by the present invention.

Claims

1. A positive electrode sheet, characterized in that: The positive electrode sheet comprises: a positive electrode material layer, the positive electrode material layer comprises positive electrode material particles, the positive electrode material particles comprise positive electrode active material particles, an oxide solid electrolyte layer coated on the outer surface of the positive electrode active material particles, and a conductive polymer layer coated on the surface of the oxide solid electrolyte layer away from the positive electrode active material particles; The positive electrode active material particles contain positive electrode active materials; the positive electrode active material is selected from at least one of lithium manganese oxide, lithium-rich manganese-based positive electrode materials and nickel-cobalt lithium manganese oxide.

2. The positive electrode sheet according to claim 1, characterized in that: The conductive polymer layer comprises a conductive polymer; the conductive polymer is selected from polyaniline and / or polypyrrole.

3. The positive electrode sheet according to claim 1, characterized in that: In the positive electrode material layer, the mass ratio of the oxide solid electrolyte layer to the positive electrode active material particles is 1-5:95-99.

4. The positive electrode sheet according to claim 1, characterized in that: The thickness of the oxide solid electrolyte layer is 0.01-2 μm.

5. The positive electrode sheet according to claim 2, characterized in that: The conductive polymer is prepared from conductive polymer monomers; wherein the ratio of the mass of the conductive polymer monomer to the sum of the mass of the oxide solid electrolyte layer and the positive electrode active material particles in the positive electrode material layer is 1-5:95-99.

6. The positive electrode sheet according to claim 1, characterized in that: Based on the total mass of the positive electrode material layer, the mass percentage of the positive electrode active material particles in the positive electrode material layer is 80%-99%.

7. A method for preparing the positive electrode sheet according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: Step 1: fully and uniformly mixing the positive electrode active material and the oxide solid electrolyte to obtain a first mixture; Step 2: placing the first mixture obtained in step 1 in water, adding a first acidic medium solution to adjust the pH to a first pH value, and then adding a conductive polymer monomer to obtain a first solution; placing the first mixture in the first solution; Step 3: placing an oxidant in water, adding the second acidic medium solution to adjust the pH to a second pH value, and obtaining a second solution; Step 4: lowering the temperatures of the first solution and the second solution, and then adding the second solution to the first solution in a stirring state, and continuing the reaction after the dropwise addition is completed to obtain a positive electrode material; Step 5: coating the positive electrode slurry containing the positive electrode material on the positive electrode collector to obtain the positive electrode sheet.

8. The method according to claim 7, characterized in that The method satisfies at least one of the following conditions: (1) the first acidic medium solution and the second acidic medium solution are selected from hydrochloric acid solution or sulfuric acid solution; the molar concentration of the first acidic medium solution and the second acidic medium solution is selected from 0.8-1.5 mol / L; (2) the first pH value and the second pH value are selected from 2-4; (3) The mass of the oxidant is selected from 0.1% to 1% of the mass of the conductive polymer monomer; (4) The oxidant includes at least one of ammonium persulfate, hydrogen peroxide, sodium vanadate and potassium dichromate.

9. A secondary battery, characterized in that: The secondary battery comprises a negative electrode sheet, an electrolyte, and a positive electrode sheet according to any one of claims 1 to 6, or a positive electrode sheet prepared by the method according to claim 7 or 8.

10. An electrochemical device, characterized in that: The electrochemical device includes the secondary battery according to claim 9.

Citation Information