Gradient rigid-flexible coupling solid electrolyte interface enhanced zinc ion battery and preparation method thereof

By adding ZnSiF6 additive to the zinc sulfate aqueous solution of zinc ion battery, a SEI film with a gradient rigid-flexible coupling structure is formed, which solves the problems of zinc ion battery performance and cycle stability, significantly improves the battery's cycle life and Coulomb efficiency, and suppresses the secondary Reactions and dendrites growth.

CN119050505APending Publication Date: 2024-11-29TSINGHUA SHENZHEN INTERNATIONAL GRADUATE SCHOOL
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411158933.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The performance and cycle stability of zinc ion batteries are affected by problems such as dendrites' growth and side reactions, and the existing technology is difficult to effectively solve.

Method used

Adding ZnSiF6 additive to the zinc sulfate aqueous solution electrolyte of zinc ion battery induced a solid electrolyte interface SEI film with a gradient rigid-flexible coupling structure, mainly consisting of porous basic zinc sulfate as the skeleton, and ZnF2 is embedded in it to form a nano-scale zinc ion transport channel.

Benefits of technology

It significantly improves the cycle life and Coulomb efficiency of zinc ion batteries, inhibits hydrogen evolution reaction and dendrite growth, enhances the desolvation and transfer speed of zinc ions, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050505A_ABST
    Figure CN119050505A_ABST
Patent Text Reader

Abstract

The invention relates to a gradient rigid-flexible coupling solid electrolyte interface enhanced zinc ion battery and a preparation method thereof, and the zinc ion battery comprises a positive electrode which comprises a vanadium oxide VO2 positive electrode material; a negative electrode including metal zinc; a separator interposed between the positive electrode and the negative electrode; and the electrolyte is a zinc sulfate aqueous solution containing a ZnSiF6 additive, and the ZnSiF6 additive is induced on the negative electrode to form a solid electrolyte interface SEI film with a gradient rigid-flexible coupling structure. According to the SEI film, porous basic zinc sulfate ZHS serves as a framework, ZnF2 is embedded in the framework, and a nanoscale zinc ion transmission channel is formed. The composite SEI structure effectively prevents water permeation and promotes desolvation of zinc ions, so that the driving force and transmission speed of zinc ion migration are enhanced, the problems of dendritic crystal growth, hydrogen evolution reaction, surface passivation and the like are finally inhibited, and the cycle life, coulombic efficiency and rate capability of the zinc ion battery are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of new energy materials, and in particular relates to a gradient rigid-flexible coupling solid electrolyte interface enhanced zinc ion battery and a preparation method thereof. Background Art

[0002] Zinc-ion batteries (ZIBs) have been widely used due to their low cost, environmental friendliness, high specific capacity (820 mAh g -1 and 5855mAhcm -3 ) and good safety performance, it has become a very promising energy storage system. However, problems such as dendrite growth and side reactions (including hydrogen evolution reaction and surface passivation) seriously affect the performance and cycle stability of zinc-ion batteries. To address these problems, researchers have explored a variety of strategies to stabilize the zinc anode, including the use of electrolyte additives, surface coatings, and three-dimensional anode structures.

[0003] It should be noted that the information disclosed in the above background technology section is only used for understanding the background of the present application, and therefore may include information that does not constitute prior art known to ordinary technicians in the field. Summary of the invention

[0004] The main purpose of the present invention is to solve the problems existing in the above-mentioned background technology and to provide a gradient rigid-flexible coupled solid electrolyte interface enhanced zinc ion battery and a preparation method thereof.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] A gradient rigid-flexible coupled solid electrolyte interface enhanced zinc ion battery, comprising:

[0007] A positive electrode comprising a vanadium oxide VO2 positive electrode material;

[0008] a negative electrode comprising metallic zinc;

[0009] a separator, which is placed between the positive and negative electrodes;

[0010] The electrolyte is an aqueous solution of zinc sulfate containing a ZnSiF6 additive, wherein the ZnSiF6 additive induces the formation of a solid electrolyte interface SEI film with a gradient rigid-flexible coupling structure on the negative electrode.

[0011] Furthermore, the SEI film is mainly composed of porous basic zinc sulfate ZHS as a skeleton, and ZnF2 is embedded therein to form a nano-scale zinc ion transmission channel.

[0012] Furthermore, the concentration of the ZnSiF6 additive is 0.5 mM.

[0013] Furthermore, the positive electrode comprises vanadium oxide VO2 positive electrode material.

[0014] Furthermore, the diaphragm is a glass fiber diaphragm.

[0015] An electrolyte for improving the negative electrode performance of a zinc ion battery, comprising the following components:

[0016] An aqueous solution of zinc sulfate (ZnSO4) as the main component of the electrolyte;

[0017] The ZnSiF6 additive is used to induce the formation of a solid electrolyte interface SEI film with a gradient rigid-flexible coupling structure on the negative electrode.

[0018] Furthermore, the concentration of the ZnSiF6 additive is 0.5 mM.

[0019] A method for preparing the electrolyte comprises adding ZnSiF6 to a ZnSO4 electrolyte and stirring the mixture until the mixture is completely dissolved. The concentration of ZnSiF6 is 0.5 mM, and a ZnSO4 electrolyte containing a ZnSiF6 additive is obtained.

[0020] A method for preparing a gradient rigid-flexible coupled solid electrolyte interface enhanced zinc ion battery comprises assembling a positive electrode, a negative electrode and a separator, injecting the electrolyte and sealing the battery.

[0021] The present invention has the following beneficial effects:

[0022] The present invention provides a new scheme for enhancing the negative electrode performance of zinc ion batteries by adding ZnSiF6 to a ZnSO4 (ZSO) electrolyte. The addition of the ZnSiF6 electrolyte additive induces the formation of a gradient rigid-flexible coupling structure solid electrolyte interface (SEI), thereby significantly enhancing the performance of the zinc ion battery. The ZnSiF6 additive can promote the formation of a stable, fluorine-rich solid electrolyte interface (SEI) on the negative electrode. The SEI has a unique gradient rigid-flexible coupling structure, which is mainly composed of porous basic zinc sulfate (ZHS) as a skeleton, and ZnF2 is embedded therein to form a nanoscale zinc ion transmission channel. This composite SEI structure effectively prevents water penetration and promotes the desolvation of zinc ions, thereby enhancing the driving force and transmission speed of zinc ion migration.

[0023] In the present invention, the ZnSiF6 additive can effectively inhibit the hydrogen evolution reaction and the generation of basic zinc sulfate (ZHS) by-products, promote uniform zinc deposition, and thus inhibit dendrite growth.

[0024] The electrolyte with ZnSiF6 additive of the present invention can significantly improve the electrochemical performance of zinc negative electrode, including:

[0025] a) Extend cycle life: at 0.5mA / cm 2 Cycling for more than 3000 hours at a current density of 10 mA / cm2 Cycling for more than 560 hours at high current density.

[0026] b) Improved Coulombic efficiency: In the Zn||Cu half-cell test, the average Coulombic efficiency reached 99.57%.

[0027] The Zn||VO2 full cell using ZnSO4+ZnSiF6 electrolyte exhibits excellent rate performance and cycle life.

[0028] Other beneficial effects of the embodiments of the present invention will be further described below. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The ZnSiF6 additive of the embodiment of the present invention is to Zn 2+ Regulatory role of the solvation sheath.

[0030] Figure 2 The present invention provides theoretical and experimental research on the inhibition of zinc negative electrode side reactions.

[0031] Figure 3 The electrochemical performance of ZSO and ZSO-ZnSiF6 as electrolytes in the embodiments of the present invention are shown.

[0032] Figure 4 The dynamic kinetics in ZSO and ZSO-ZnSiF6 electrolytes of the embodiments of the present invention and the morphology of the zinc negative electrode after different cycle times.

[0033] Figure 5 The structure and composition of the zinc negative electrode of the embodiment of the present invention are characterized.

[0034] Figure 6 The composition and microstructure of the SEI layer of the zinc negative electrode after cycling in an embodiment of the present invention.

[0035] Figure 7 Characterization of VO2 and the cycle performance of Zn||VO2 battery of the embodiment of the present invention. DETAILED DESCRIPTION

[0036] The following is a detailed description of the embodiments of the present invention. It should be emphasized that the following description is only exemplary and is not intended to limit the scope and application of the present invention.

[0037] The embodiment of the present invention provides a gradient rigid-flexible coupling solid electrolyte interface enhanced zinc ion battery, comprising: a positive electrode, which comprises a vanadium oxide VO2 positive electrode material; a negative electrode, which comprises metal zinc; a diaphragm, which is placed between the positive electrode and the negative electrode; an electrolyte, which is an aqueous solution of zinc sulfate containing a ZnSiF6 additive, wherein the ZnSiF6 additive induces the formation of a gradient rigid-flexible coupling structure solid electrolyte interface SEI film on the negative electrode. The SEI film is mainly composed of porous basic zinc sulfate ZHS as a skeleton, and ZnF2 is embedded therein to form a nanoscale zinc ion transmission channel. Preferably, the concentration of the ZnSiF6 additive is 0.5mM. The positive electrode may include a vanadium oxide VO2 positive electrode material.

[0038] The zinc ion battery is 0.5 mA / cm 2 At a current density of 10 mA / cm 2 At a current density of 1.5 kW, the cycle life exceeds 560 hours.

[0039] The present invention provides an electrolyte for improving the performance of the negative electrode of a zinc ion battery, comprising the following components: an aqueous solution of zinc sulfate (ZnSO4) as the main component of the electrolyte; and a ZnSiF6 additive for inducing the formation of a solid electrolyte interface SEI film with a gradient rigid-flexible coupling structure on the negative electrode. Preferably, the concentration of the ZnSiF6 additive is 0.5 mM.

[0040] In a method for preparing an electrolyte according to an embodiment of the present invention, ZnSiF6 is added to a ZnSO4 electrolyte and stirred thoroughly until it is completely dissolved. The concentration of ZnSiF6 is 0.5 mM, and a ZnSO4 electrolyte containing a ZnSiF6 additive is prepared.

[0041] The embodiment of the present invention discloses a method for preparing a gradient rigid-flexible coupled solid electrolyte interface enhanced zinc ion battery, which comprises assembling a positive electrode, a negative electrode and a separator, injecting the electrolyte and sealing the battery.

[0042] The present invention provides a method for improving the performance of the negative electrode of a zinc ion battery, wherein a ZnSiF6 electrolyte additive is added to a zinc sulfate aqueous solution electrolyte. The ZnSiF6 additive induces the formation of a unique gradient rigid-flexible coupling structure solid electrolyte interface (SEI) on the surface of the zinc negative electrode, wherein the SEI is composed of porous basic zinc sulfate (ZHS) as a skeleton, and ZnF2 is embedded therein to form a nanoscale zinc ion transmission channel. This composite SEI structure effectively prevents water penetration and promotes the desolvation of zinc ions, thereby enhancing the driving force and transmission speed of zinc ion migration, ultimately inhibiting problems such as dendrite growth, hydrogen evolution reaction and surface passivation, and significantly improving the cycle life, coulomb efficiency and rate performance of the zinc ion battery. Thus, the present invention provides a new method for stabilizing the zinc negative electrode, and provides an effective solution for the development of high-performance zinc ion batteries.

[0043] The specific embodiments of the present invention are further described below.

[0044] An electrolyte for improving the performance of the negative electrode of a zinc ion battery comprises the following components: a zinc sulfate (ZnSO4) aqueous solution as the main component of the electrolyte and a ZnSiF6 additive for inducing the formation of a SEI layer with a gradient rigid-flexible coupling structure on the negative electrode, wherein the concentration of the ZnSiF6 additive is preferably 0.5 mM.

[0045] A method for preparing the above-mentioned electrolyte includes the following steps: dissolving ZnSiF6 in a ZnSO4 aqueous solution and stirring thoroughly until it is completely dissolved.

[0046] A zinc ion battery using the above electrolyte comprises: a positive electrode comprising a vanadium oxide (VO2) positive electrode material; a negative electrode comprising metallic zinc; a diaphragm placed between the positive electrode and the negative electrode, preferably a glass fiber diaphragm; and an electrolyte, which is the above zinc sulfate aqueous solution containing the ZnSiF6 additive.

[0047] This embodiment provides a method for preparing a zinc ion battery using an aqueous zinc sulfate solution containing a ZnSiF6 additive as an electrolyte, the method comprising:

[0048] Preparation of positive electrode materials: VO2(B) powder was prepared by solvothermal method. The specific steps are as follows:

[0049] a) Dissolve 0.3 g of V2O5 powder in 20 mL of deionized water, add 4 mL of 30% hydrogen peroxide under magnetic stirring, and stir for 20 minutes until the solution turns orange-red.

[0050] b) 10 mL of the above solution was added to a mixture of 50 mL of n-butanol and 30 mg of sodium dodecylbenzene sulfonate.

[0051] c) The mixed solution was poured into a 100 mL polytetrafluoroethylene-lined hydrothermal reactor and heated at 180° C. for 24 hours.

[0052] d) After the reaction, the product was vacuum filtered, washed with deionized water and ethanol, and then dried at 60°C for 12 hours to obtain black VO2(B) powder.

[0053] Preparation of negative electrode materials: Commercially available zinc foil was used as the negative electrode material.

[0054] Preparation of electrolyte: Dissolve 0.5 mM ZnSiF6 in 2 M zinc sulfate aqueous solution to prepare the electrolyte.

[0055] Battery assembly: The prepared VO2 positive electrode, zinc foil negative electrode and glass fiber separator are assembled in sequence in a CR2032 button battery shell, the electrolyte is injected and the battery is sealed.

[0056] Electrochemical performance test:

[0057] The assembled battery was subjected to the following electrochemical performance tests:

[0058] Cyclic voltammetry (CV): scan rate was 0.1 mV / s.

[0059] Rate performance test: current densities are 0.5A / g, 1A / g, 2A / g, 5A / g and 10A / g respectively.

[0060] Long cycle performance test: current density is 1A / g, and cycle is 1000 times.

[0061] Result analysis:

[0062] The electrochemical performance test results show that the Zn||VO2 full battery with the addition of ZnSiF6 exhibits excellent electrochemical performance, including:

[0063] Excellent rate performance: It can maintain high discharge capacity at different current densities.

[0064] Ultra-long cycle life: After 1000 cycles at a current density of 1A / g, the capacity retention rate is 70.4%.

[0065] The above results show that the electrolyte and zinc ion battery provided by the present invention can effectively improve the cycle stability and rate performance of the battery and have good application prospects.

[0066] The above content is a further detailed description of the present invention in combination with specific / preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, it can also make several substitutions or modifications to these described embodiments, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention. In the description of this specification, the description of the reference terms "an embodiment", "some embodiments", "preferred embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in combination with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily target the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In the absence of mutual contradiction, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples. Although the embodiments of the present invention and their advantages have been described in detail, it should be understood that various changes, substitutions and modifications can be made herein without departing from the scope of protection of the patent application.

Claims

1. A gradient rigid-flexible coupled solid electrolyte interface enhanced zinc ion battery, characterized in that: include: A positive electrode comprising a vanadium oxide VO2 positive electrode material; a negative electrode comprising metallic zinc; a separator, which is placed between the positive and negative electrodes; The electrolyte is an aqueous solution of zinc sulfate containing a ZnSiF6 additive, wherein the ZnSiF6 additive induces the formation of a solid electrolyte interface SEI film with a gradient rigid-flexible coupling structure on the negative electrode.

2. The gradient rigid-flexible coupled solid electrolyte interface enhanced zinc ion battery according to claim 1, characterized in that: The SEI film is mainly composed of porous basic zinc sulfate ZHS as a skeleton, and ZnF2 is embedded therein to form a nano-scale zinc ion transmission channel.

3. The gradient rigid-flexible coupled solid electrolyte interface enhanced zinc ion battery according to claim 1 or 2, characterized in that: The concentration of the ZnSiF6 additive is 0.5 mM.

4. The gradient rigid-flexible coupled solid electrolyte interface enhanced zinc ion battery according to any one of claims 1 to 3, characterized in that: The positive electrode comprises vanadium oxide VO2 positive electrode material.

5. The gradient rigid-flexible coupled solid electrolyte interface enhanced zinc ion battery according to any one of claims 1 to 4, characterized in that: The diaphragm is a glass fiber diaphragm.

6. An electrolyte for improving the performance of a negative electrode of a zinc ion battery, characterized in that: Contains the following ingredients: An aqueous solution of zinc sulfate (ZnSO4) as the main component of the electrolyte; The ZnSiF6 additive is used to induce the formation of a solid electrolyte interface SEI film with a gradient rigid-flexible coupling structure on the negative electrode.

7. The electrolyte according to claim 6, characterized in that The concentration of the ZnSiF6 additive is 0.5 mM.

8. A method for preparing the electrolyte according to claim 6 or 7, characterized in that: Add ZnSiF6 to ZnSO4 electrolyte and stir thoroughly until it is completely dissolved. The concentration of ZnSiF6 is 0.5 mM to prepare ZnSO4 electrolyte containing ZnSiF6 additive.

9. A method for preparing a gradient rigid-flexible coupled solid electrolyte interface enhanced zinc ion battery, characterized in that: Assemble the positive electrode, the negative electrode and the separator, inject the electrolyte as described in claim 6 or 7, and seal the battery.

Citation Information

Cited By

  • Method for in-situ construction of ZnS-based solid electrolyte interface layer by using sulfur-free additive

    CN120165074A