Robot multi-layer and multi-pass welding method and device, electronic equipment and storage medium

By adjusting welding parameters in real time and using curve equations in welding database, the problems of welding position and bevel factors in medium and thick plate welding are solved, the welding quality and efficiency are improved, and the development cost is reduced.

CN119057175APending Publication Date: 2024-12-03CHINA RAILWAY CONSTR HEAVY IND
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411253971.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the welding of medium and thick plates, the existing technology fails to effectively consider factors such as the robot welding position, bevel gap and blunt edge, resulting in the risk of unqualified welding quality, which increases the development workload and cost.

Method used

By adjusting the welding current and welding speed in real time, correcting the welding layer morphology according to the actual bevel size, so that it is unified with the theoretical bevel welding layer morphology, and using the weld curve equation in the welding database to determine the robot welding position to realize welding Precise arrangement of channels.

Benefits of technology

It reduces the development workload and cost, eliminates welding errors, improves welding quality and operating efficiency, and ensures welding accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057175A_ABST
    Figure CN119057175A_ABST
Patent Text Reader

Abstract

The invention discloses a robot multi-layer and multi-pass welding method, device and equipment and a storage medium, and the method comprises the following steps: when a base layer is welded, according to the actual size of a measured groove, the welding current or the welding speed read from a welding database is adjusted in real time; the welding layer morphology of the actual groove is corrected so that the welding layer morphology of the actual groove can be unified with the theoretical groove welding layer morphology read in the welding database; the method comprises the following steps: after welding of a priming coat is finished, when welding beads of a filling layer and a capping layer are arranged, acquiring a welding seam curve equation of each welding seam of a theoretical sample piece closest to the shape and the angle of a groove to be welded from a welding database; and solving the intersection points of the weld curve equation of each weld and the groove straight edge, the groove bevel edge and / or the related weld curve equation in the established to-be-welded groove coordinate system to determine the robot welding position of each to-be-welded weld in the filling layer and the cover surface layer so as to complete the weld bead arrangement. The operation efficiency of multi-layer and multi-pass welding of the robot is improved, and the welding quality is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of welding technology, and in particular to a robot multi-layer multi-pass welding method, device, equipment and storage medium. Background Art

[0002] Medium and thick plate welding is common in engineering machinery, mining equipment and other industries. Due to the high weld strength requirements, multi-layer and multi-pass welding methods are usually required, among which groove welding is one of the common designs in medium and thick plate welding. At present, the common medium and thick plate automated welding method is usually to establish a groove weld arrangement or welding database, and then use the industrial robot multi-layer and multi-pass welding method to call the groove weld arrangement or welding database to achieve groove automated welding.

[0003] In practical applications, the arrangement of welds for multi-layer and multi-pass welding of medium and thick plates often does not take into account the determination of robot welding positions. The weld arrangement method tends to be based on theoretical groove calculations, and does not consider the influence of factors such as groove gap and groove blunt edge in actual workpieces. Therefore, theoretical multi-layer and multi-pass welding parameters and weld arrangement information often have errors in practical applications. Groove welds usually have higher welding quality requirements. Once the error is too large, it will increase the risk of unqualified welding quality and hinder the automated application of multi-layer and multi-pass welding.

[0004] In response to the error problem in the actual application of multi-layer and multi-pass robot welding, the current common method is to optimize the database algorithm to adapt to the influence of other size factors of the groove. Another method is to use sensors to collect data of the welding layer during the multi-layer and multi-pass welding process, and re-arrange the welds and select welding parameters by comparing with the database. The first method requires a large amount of groove welding data for database intelligent learning training, and considering that the robot welding position changes with the groove size, the development workload is large; the second method performs real-time database processing, and also faces the problems of sensor development and robot welding position adjustment. Summary of the invention

[0005] On one hand, the present invention provides a robot multi-layer and multi-pass welding method to solve the technical problems of existing medium and thick plate welding technology, such as large development workload and cost, and welding errors affecting quality.

[0006] The present invention is achieved through the following scheme:

[0007] A robot multi-layer multi-pass welding method, comprising the steps of:

[0008] When welding the base layer, according to the measured actual size of the groove, the welding current or welding speed read from the welding database is adjusted in real time, and the welding layer morphology of the actual groove is corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, wherein the theoretical groove in the welding database has no gap and no blunt edge, and the actual size of the groove includes the groove gap c and the groove blunt edge value p, the groove angle α, the groove width w, and the plate thickness t;

[0009] After the base layer welding is completed, when arranging the welds of the filling layer and the cover layer, the weld curve equations of each weld of the theoretical sample that is closest to the shape and angle of the groove to be welded are obtained from the welding database, and the intersection of the weld curve equations of each weld with the straight edge of the groove, the inclined edge of the groove and / or the relevant weld curve equations in the established coordinate system of the groove to be welded is obtained to determine the robot welding position of each weld to be welded in the filling layer and the cover layer, and complete the precise arrangement of the welds.

[0010] Preferably, before welding the base layer, the method further comprises the following steps:

[0011] A welding database is established, wherein the welding database includes groove input parameters and welding parameters. The groove input parameters include groove width and groove angle. The welding parameters include welding current, welding voltage, welding speed, weaving welding parameters, dry extension and robot welding position. The welding database includes theoretical samples without gaps and blunt edges, and weld curve equations of each weld of each theoretical sample. Considering the quality requirements of medium and thick plate welding, it is preferred to obtain the database program by welding actual samples.

[0012] Preferably, when welding the base layer, the welding current or welding speed read from the welding database is adjusted in real time according to the actual size of the groove, and the welding layer morphology of the actual groove is corrected to be consistent with the theoretical groove welding layer morphology read from the welding database, which specifically includes the steps of:

[0013] The formula S for calculating the theoretical cross-sectional area of ​​the base layer required for the theoretical groove is:

[0014]

[0015] Among them, h is the theoretical thickness of the base layer under the theoretical groove condition;

[0016] The back penetration of the groove is set to 1mm, and the back penetration cross-sectional area model is set to a triangle. When the theoretical thickness of the base layer h remains unchanged, the actual filling cross-sectional area S' of the base layer in the actual groove is calculated as follows:

[0017]

[0018] Under the premise that the weld length remains unchanged, the base layer area ratio k = S' / S is calculated based on the proportional relationship between the actual filling cross-sectional area and the theoretical cross-sectional area;

[0019] According to the base layer area ratio k, the base layer theoretical welding current, and the base layer theoretical welding speed, the actual base layer welding current I1 and welding speed v1 are calculated:

[0020] I1=k*I (3)

[0021] v1=v / k (4)

[0022] Among them, I is the theoretical welding current of the base layer, and v is the theoretical welding speed of the base layer;

[0023] The actual welding current I1 of the base layer or the actual welding speed v1 of the base layer is selected as a welding parameter to weld the base layer, and the welding layer morphology of the actual groove is corrected to be consistent with the theoretical groove welding layer morphology read from the welding database.

[0024] Preferably, when welding the base layer, according to the actual size of the groove obtained, the welding current or welding speed read from the welding database is adjusted in real time, and the welding layer morphology of the actual groove is corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, which specifically also includes the steps of:

[0025] If the welding current or welding speed read from the welding database is adjusted in real time after the base layer welding, the actual groove welding layer morphology cannot be corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, then the cross-sectional area S1 of the theoretical first filling layer is calculated:

[0026]

[0027] Among them, h2 is the total thickness of the welding layer after welding the theoretical first filling layer, and h1 is the thickness of the welding layer of the theoretical base layer;

[0028] When actually welding the first filling layer, due to the different thickness of the base layer, calculate the actual cross-sectional area S11 of the first filling layer:

[0029]

[0030] Among them, h 1s It is the actual thickness of the welding layer of the base layer;

[0031] Under the premise that the weld length remains unchanged, the filling layer area ratio k1=S11 / S1 is calculated based on the proportional relationship between the cross-sectional area of ​​the actual first filling layer and the cross-sectional area of ​​the theoretical first filling layer;

[0032] Since the filling amount is proportional to the welding current and inversely proportional to the welding speed, the actual welding current I3 and welding speed v3 of the filling layer are calculated according to the filling layer area ratio k1, the theoretical welding current of the filling layer, and the theoretical welding speed of the filling layer:

[0033] I3= k1×I2 (6)

[0034] v3= v2 / k1 (7)

[0035] Among them, I2 is the theoretical welding current, v2 is the theoretical welding speed;

[0036] The actual welding current I3 of the filling layer or the actual welding speed v3 of the filling layer is selected as a welding parameter to weld the first filling layer, and the welding layer morphology of the actual groove is corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database.

[0037] Preferably, after selecting the actual welding current I1 of the base layer or the actual welding speed v1 of the base layer as the welding parameter to weld the base layer and correcting the actual groove welding layer morphology to make it consistent with the theoretical groove welding layer morphology read in the welding database, the following steps are also included:

[0038] The actual welding current I4 during the actual welding of the base layer is obtained by using the welding machine communication or the arc tracking function of the robot;

[0039] Based on the theoretical welding current I of the base layer and the calculated actual welding speed v1 of the base layer, the actual welding speed v2 of the base layer after secondary adjustment is calculated:

[0040] v2= I / I4×v1 (8);

[0041] The actual welding speed v2 of the base layer after the secondary adjustment is used as the final welding parameter to weld the base layer, and the welding layer morphology of the actual groove is corrected to be consistent with the theoretical groove welding layer morphology read from the welding database.

[0042] Preferably, after the base layer welding is completed, when arranging the welds of the filling layer and the capping layer, the weld curve equations of each weld of the theoretical sample that is closest to the shape and angle of the groove to be welded are obtained from the welding database, and the intersection of the weld curve equations of each weld with the straight edge of the groove, the inclined edge of the groove and / or the relevant weld curve equations in the established coordinate system of the groove to be welded is obtained to determine the robot welding position of each weld to be welded in the filling layer and the capping layer, and complete the accurate arrangement of the welds, which specifically includes the steps of:

[0043] When the number of welding layers of the groove to be welded is less than or equal to the number of welding layers of the theoretical sample in the welding database that is closest to the shape and angle of the groove to be welded, the straight edge equations of the straight edge and the bevel edge of the groove in the coordinate system of the groove to be welded are obtained as y r =f(x), hypotenuse equation y h =f(x), the equation for obtaining the base weld morphology from the closest theoretical sample in the welding database is y0=f(x), where, due to the limitation of groove morphology parameters, the x-coordinate interval range is (0, w), and the y-coordinate interval range is (0, t);

[0044] In the coordinate region, solve the bottom layer weld morphology equation y0 = f(x) and the straight edge equation y r = the coordinates of the intersection point p0 of f(x), then the coordinates of the intersection point p0 are used as the robot welding position of the nearly straight edge weld of the first filling layer;

[0045] In the coordinate region, solve the bottom layer weld morphology equation y0 = f(x) and the hypotenuse equation y h =The coordinates of the intersection point p1 of f(x), and the x-coordinate interval of the equation y0=f(x) of the base weld morphology is obtained by using the coordinates of the intersection points p0 and p1;

[0046] Arrange the welding points of the first filling layer, wherein the weld types of the first filling layer include three types of welds: near straight edge welds, middle welds and near bevel edge welds. When arranging, first obtain the near straight edge weld curve equation y of the first filling layer weld according to the closest theoretical sample from the welding database r1 = f(x) and the straight edge equation y r =f(x) to find the intersection point p (0,1) , the intersection point p (0,1) To fill the robot welding position of the second layer of the nearly straight edge weld, then according to the nearly straight edge weld curve equation y r1 =f(x) and the bottom weld curve equation y0=f(x) to find the intersection point p (m1,1) , the intersection point p (m1,1) The robot welding position of the first intermediate weld adjacent to the nearly straight edge weld is (0,1) and p (m1,1) Get the equation of the nearly straight edge weld curve y r1 = the x-coordinate interval of f(x); then, calculate p (m1,1) The distance from p1 is d1. Under the standard groove model, the distance is d s , then when d1≤d s *C, only the near-bevel weld, where C is the tolerance factor, when d1>d s *C, including the middle weld, using the first middle weld curve equation y m1-1=f(x) and the equation of the nearly straight edge weld curve y r1 =f(x) to find the intersection point p (0 ,1,1), and find the intersection point p with the base weld y0=f(x) (m2,1) , calculate the intersection point p (m2,1) The distance d2 from p1, if d2>d s *C, then the intersection point p (m2,1) is the robot welding position of the second middle weld, if d2≤d s *C, then the intersection point p (m2,1) The midpoint p with p1 z1 As a robot welding position for near bevel welds, while using p (0,1,1) With p (m2,1) Get the equation y for the first intermediate weld m1-1 =f(x)'s x-mark interval; if there is a second middle weld, repeat the solution process for the first middle weld; if there is no second middle weld, only the near bevel weld y h1 =f(x), then the first middle weld curve equation y m1-1 =f(x) to find the intersection point p (1,1,1) , and the hypotenuse equation y h1 =f(x) to find the intersection point p (1,1) ;

[0047] Arrange the welding points of the i-th filling layer, and assume that the equation of the straight edge weld curve of the i-th filling layer is y ri =f(x), the equation of the first middle weld curve is y m1-i =f(x), the equation of the second middle weld curve is y m2-i =f(x), the equation of the nth middle weld curve is y mn-i =f(x), the equation of the weld near the bevel is y hi =f(x), equation of the nearly straight weld curve y ri = f(x) and the straight edge equation y r =f(x) to find the intersection point p (0,i) , the intersection point p of the two weld shapes of the nearly straight edge weld and the first middle weld adjacent to the weld shape of the i-1 filling layer is obtained (mi,1) , p (mi,1) Satisfy the x interval of the two welds and the y value is the largest, using p (0,i) With p (mi,1) Determine the x-coordinate interval of the nearly straight edge weld, p (mi,1) The robot welding position associated with the next weld, p (mi,1) The distance between the intersection of the hypotenuse and the i-1th filling layer is di. If di≤ds*C, there is no intermediate weld, p (mi,1) With p (1,i-1) The midpoint p ziis the arc starting point of the near-bevel weld, and the intersection point p between the near-bevel weld and the bevel is obtained. (1,i) , and find the intersection point p with the adjacent weld on the same layer (1,1,i) , p (1,i) With p (1,1,i) Determine the x-coordinate interval of the near-bevel weld. If di>ds*C, repeat the above process to obtain the arc starting position p of the first middle weld and the first middle weld and the second middle weld of the i-1st filling layer. (m2,1) , and find the intersection point p with the nearly straight edge weld of the same layer (0,i) ,p (m2,1) With p (0,i) Determine the x-coordinate interval of the second middle weld and calculate p (m2,1) The distance between the intersection point of the hypotenuse and the i-1th filling layer is calculated as di, until di≤ds*C. Once the intersection point of the near-hypotenuse weld is obtained, the arrangement of the welds in the same layer is completed.

[0048] Preferably, after the base layer welding is completed, when arranging the welds of the filling layer and the capping layer, the weld curve equations of each weld of the theoretical sample that is closest to the groove shape and groove angle to be welded are obtained from the welding database, and the intersection of the weld curve equations of each weld with the groove straight edge, the groove bevel and / or the relevant weld curve equations in the established groove coordinate system to be welded is obtained to determine the robot welding position of each weld to be welded in the filling layer and the capping layer, and complete the accurate arrangement of the welds, which specifically also includes the steps of:

[0049] When the number of welding layers of the groove to be welded is greater than the number of welding layers of the theoretical sample in the welding database that is closest to the shape and angle of the groove to be welded, the welds of the other welding layers exceeding the number of welding layers of the theoretical sample and the welds of the same type in the welding layer of the theoretical sample are in an offset relationship. If the curve equation of the i-th layer weld of the top layer of the closest theoretical sample in the welding database is y i =f(x), then the equation for the same type of weld in the i+1th layer is expressed as y i -b=f(xa), where coordinates a and b are the offsets of the arc starting positions of the two welds along the x and y directions respectively. The offset b along the y direction reflects the thickness of the weld layer, and the offset along the x direction is determined by the x offset between two adjacent welds of the same type in the theoretical sample.

[0050] Another aspect of the present invention provides a robot multi-layer multi-pass welding device, comprising:

[0051] The base layer welding correction module is used to adjust the welding current or welding speed read from the welding database in real time according to the measured actual size of the groove when welding the base layer, and correct the welding layer morphology of the actual groove to make it consistent with the theoretical groove welding layer morphology read from the welding database, wherein the theoretical groove in the welding database has no gap and no blunt edge, and the actual size of the groove includes the groove gap c and the groove blunt edge value p, the groove angle α, the groove width w, and the plate thickness t;

[0052] The weld bead arrangement module is used to obtain the weld curve equations of each weld of the theoretical sample that is closest to the shape and angle of the groove to be welded from the welding database when arranging the weld bead of the filling layer and the cover layer after the base layer welding is completed, and to obtain the intersection of the weld curve equation of each weld with the straight edge of the groove, the inclined edge of the groove and / or the relevant weld curve equation in the established coordinate system of the groove to be welded, so as to determine the robot welding position of each weld to be welded in the filling layer and the cover layer, and complete the precise arrangement of the weld bead.

[0053] On the other hand, the present invention also provides an electronic device, including a memory, a processor, and a computer program stored in the memory and executable on the processor, wherein the processor implements the steps of the robot multi-layer and multi-pass welding method when executing the computer program.

[0054] Another aspect of the present invention provides a storage medium, which includes a stored program, and when the program is run, controls the device where the storage medium is located to execute the steps of the robot multi-layer and multi-pass welding method.

[0055] The present invention has the following beneficial effects:

[0056] The present invention provides a robot multi-layer and multi-pass welding method, a device, an electronic device and a storage medium. The robot multi-layer and multi-pass welding method can accurately obtain the robot welding position through weld bead arrangement, and at the same time consider the influence of factors such as groove gap and groove blunt edge on groove welding in actual welding. During actual robot multi-layer and multi-pass welding, the influence of factors such as groove gap and groove blunt edge is removed by adjusting the base layer alone or adjusting the base layer and the first filling layer, so that the robot multi-layer and multi-pass welding of the actual groove meets the requirements of theoretical weld bead arrangement and welding parameters, reduces development workload and cost, eliminates the influence of welding errors on welding quality, and improves the operating efficiency and accuracy of robot multi-layer and multi-pass welding and its practicality in actual welding applications.

[0057] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] The accompanying drawings, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0059] Figure 1 1 is a schematic flow chart of a robot multi-layer multi-pass welding method according to a preferred embodiment of the present invention;

[0060] Figure 2 is a schematic diagram of a bottom weld in a preferred embodiment of the present invention;

[0061] Figure 3 Schematic diagram of the base and first filling layer welds of a preferred embodiment of the present invention;

[0062] Figure 4 It is a flow chart of a method for preaching a layer of a preferred embodiment of the present invention;

[0063] Figure 5 1. It is a schematic diagram of the distribution of single-sided V-shaped groove welds in a preferred embodiment of the present invention;

[0064] Figure 6 It is a schematic diagram of the actual structural dimensions of a single-sided V-shaped groove in a preferred embodiment of the present invention;

[0065] Figure 7 It is a schematic diagram of the cross-sectional area of ​​the theoretical bottom layer slope;

[0066] Figure 8 Schematic diagram of the cross-sectional area of ​​the actual groove base layer of the preferred embodiment of the present invention;

[0067] Fig. 9 It is a schematic diagram of the cross-sectional area of ​​the theoretical first welding layer groove;

[0068] Fig.10 Schematic diagram of groove angle measurement points in a preferred embodiment of the present invention;

[0069] Fig.11 Schematic diagram of measuring the thickness of the welding wire in contact with the welding bead according to a preferred embodiment of the present invention;

[0070] Fig.12 Schematic diagram of measuring the dry extension length of welding wire according to a preferred embodiment of the present invention;

[0071] Fig.13 Schematic diagram of a robot multi-layer multi-pass welding device module according to a preferred embodiment of the present invention;

[0072] Fig.14 It is a schematic diagram of a module of a robot multi-layer multi-pass welding device according to another preferred embodiment of the present invention;

[0073] Fig.15 is a schematic block diagram of an electronic device entity according to a preferred embodiment of the present invention;

[0074] Fig.16 It is a diagram of the internal structure of a computer device according to a preferred embodiment of the present invention. DETAILED DESCRIPTION

[0075] The embodiments of the present invention are described in detail below with reference to the accompanying drawings. However, the present invention can be implemented in many different ways as defined and covered below.

[0076] like Figure 1 As shown, a preferred embodiment of the present invention provides a robot multi-layer multi-pass welding method, comprising the steps of:

[0077] S1. When welding the base layer, according to the measured actual size of the groove, the welding current or welding speed read from the welding database is adjusted in real time, and the welding layer morphology of the actual groove is corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, wherein the theoretical groove in the welding database has no gap and no blunt edge, and the actual size of the groove includes the groove gap c and the groove blunt edge value p, the groove angle α, the groove width w, and the plate thickness t;

[0078] S2. After the base layer welding is completed, when arranging the welds of the filling layer and the cover layer, the weld curve equations of each weld of the theoretical sample that is closest to the shape and angle of the groove to be welded are obtained from the welding database, and the intersection of the weld curve equations of each weld with the straight edge of the groove, the inclined edge of the groove and / or the relevant weld curve equations in the established coordinate system of the groove to be welded is obtained to determine the robot welding position of each weld to be welded in the filling layer and the cover layer, and complete the precise arrangement of the welds.

[0079] The present embodiment provides a robot multi-layer and multi-pass welding method. The robot multi-layer and multi-pass welding method can accurately obtain the robot welding position through weld bead arrangement, and at the same time consider the influence of factors such as groove gap and groove blunt edge on groove welding in actual welding. During actual robot multi-layer and multi-pass welding, the influence of factors such as groove gap and groove blunt edge is removed by adjusting the base layer alone or adjusting the base layer and the first filling layer, so that the robot multi-layer and multi-pass welding of the actual groove meets the requirements of theoretical weld bead arrangement and welding parameters, reduces development workload and cost, eliminates the influence of welding errors on welding quality, and improves the operating efficiency and accuracy of robot multi-layer and multi-pass welding.

[0080] Preferably, before welding the base layer, the method further comprises the following steps:

[0081] S0. Establish a welding database, wherein the welding database includes groove input parameters and welding parameters. The groove input parameters include groove width and groove angle. The welding parameters include welding current, welding voltage, welding speed, weaving welding parameters, dry extension and robot welding position. The welding database includes theoretical samples without gaps and blunt edges, and weld curve equations of each weld of each theoretical sample. Considering the quality requirements of medium and thick plate welding, it is preferred to obtain the database program by welding actual samples.

[0082] Among them, when calculating the weld curve equation of each weld, the welding parameters of the medium and thick plate that meet the welding quality requirements are obtained through welding experiments; when the base weld is completed, the image morphology of the weld can be obtained through metallographic preparation, and the curve equation of the weld layer can be obtained using the image morphology. The specific method can be manual measurement method or image processing technology. Similarly, the weld curve equation of each weld can be obtained.

[0083] Preferably, Figure 6 Taking the actual single-sided V-shaped groove size parameters shown in the figure as an example, when welding the base layer, according to the actual size of the groove obtained, the welding current or welding speed read from the welding database is adjusted in real time, and the welding layer morphology of the actual groove is corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, which specifically includes the following steps:

[0084] S10. For the base layer, the theoretical groove section model is approximately fan-shaped, such as Figure 7 As shown in the figure, the formula S for calculating the theoretical cross-sectional area of ​​the base layer required for the theoretical groove is:

[0085]

[0086] Among them, h is the theoretical thickness of the base layer under the theoretical groove condition;

[0087] S11, Figure 8 The figure shows the actual groove cross-sectional area. The groove back is set to be melted through 1mm, and the back melt-through cross-sectional area model is set to a triangle. When the theoretical thickness of the base layer h remains unchanged, the actual filling cross-sectional area S' of the base layer in the actual groove is:

[0088]

[0089] S12. Under the premise that the weld length remains unchanged, the base layer area ratio k = S' / S is calculated based on the proportional relationship between the actual filling cross-sectional area and the theoretical cross-sectional area;

[0090] S13. In the actual welding process, the filling amount is proportional to the welding current and inversely proportional to the welding speed. Therefore, in the actual groove welding, if the requirements of the theoretical database are met, the welding current or welding speed needs to be adjusted. Therefore, the actual welding current I1 and welding speed v1 of the base layer are calculated according to the base layer area ratio k, the theoretical welding current of the base layer, and the theoretical welding speed of the base layer:

[0091] I1=k*I (3)

[0092] v1=v / k (4)

[0093] Among them, I is the theoretical welding current of the base layer, and v is the theoretical welding speed of the base layer;

[0094] S14, selecting the actual welding current I1 of the base layer or the actual welding speed v1 of the base layer as the welding parameter to weld the base layer, correcting the welding layer morphology of the actual groove to make it consistent with the theoretical groove welding layer morphology read in the welding database, and in the actual application process, choosing to adjust the welding current or welding speed, with the one with less actual impact and lower operating difficulty as the priority.

[0095] This embodiment uses Figure 6 Taking the actual single-sided V-groove size parameters shown as an example, considering the processing accuracy and measurement operability, the actual size of the groove includes the groove gap c and the groove blunt edge value p, the groove angle α, the groove width w, and the plate thickness t. During actual groove welding, due to the existence of the groove blunt edge value p and the gap c, the actual groove cannot be consistent with the theoretical database. Therefore, in view of the influence of the groove blunt edge value p and the gap c, this embodiment adjusts the welding current or welding speed of the base layer in real time to correct the welding layer morphology of the actual groove to make it consistent with the theoretical groove welding layer morphology read in the welding database, thereby ensuring the welding quality.

[0096] Preferably, when welding the base layer, according to the actual size of the groove obtained, the welding current or welding speed read from the welding database is adjusted in real time, and the welding layer morphology of the actual groove is corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, which specifically also includes the steps of:

[0097] S15. If the welding current or welding speed read from the welding database is adjusted in real time after the base layer welding, the actual groove welding layer morphology cannot be corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, such as Fig. 9 As shown, the cross-sectional area S1 of the theoretical first filling layer is calculated as:

[0098]

[0099] Among them, h2 is the total thickness of the welding layer after welding the theoretical first filling layer, and h1 is the thickness of the welding layer of the theoretical base layer;

[0100] S16. When actually welding the first filling layer, due to the different thickness of the base layer, calculate the actual cross-sectional area of ​​the first filling layer S11:

[0101]

[0102] Among them, h 1s It is the actual thickness of the welding layer of the base layer;

[0103] S17, under the premise that the weld length remains unchanged, the filling layer area ratio k1=S11 / S1 is calculated according to the proportional relationship between the cross-sectional area of ​​the actual first filling layer and the cross-sectional area of ​​the theoretical first filling layer;

[0104] S18. Since the filling amount is proportional to the welding current and inversely proportional to the welding speed, the actual welding current I3 and welding speed v3 of the filling layer are calculated according to the filling layer area ratio k1, the theoretical welding current of the filling layer, and the theoretical welding speed of the filling layer:

[0105] I3= k1×I2 (6)

[0106] v3= v2 / k1 (7)

[0107] Among them, I2 is the theoretical welding current, v2 is the theoretical welding speed;

[0108] S19, selecting the actual welding current I3 of the filling layer or the actual welding speed v3 of the filling layer as the welding parameter to weld the first filling layer, and correcting the welding layer morphology of the actual groove to make it consistent with the theoretical groove welding layer morphology read from the welding database.

[0109] In this embodiment, after the welding current or welding speed read from the welding database is adjusted in real time for the base layer welding, if the actual groove welding layer morphology cannot be corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, the welding current or welding speed of the first filling layer is adjusted again so that during the actual groove welding, the groove welding layer after welding the first filling layer meets the requirements of the theoretical database, thereby ensuring the welding quality.

[0110] In practical applications, if the actual groove is adjusted by laying the base layer and welding the first filling layer, and there is still a deviation from the theoretical database, the parameters can be adjusted in the subsequent filling in the same way as the adjustment of the first filling layer.

[0111] Preferably, after selecting the actual welding current I1 of the base layer or the actual welding speed v1 of the base layer as the welding parameter to weld the base layer and correcting the actual groove welding layer morphology to make it consistent with the theoretical groove welding layer morphology read in the welding database, the following steps are also included:

[0112] S110, using welding machine communication or using the arc tracking function of the robot to obtain the actual measured welding current I4 during the actual welding of the base layer;

[0113] S111, based on the theoretical welding current I of the base layer and the calculated actual welding speed v1 of the base layer, calculate the actual welding speed v2 of the base layer after secondary adjustment:

[0114] v2= I / I4×v1 (8);

[0115] S112, using the actual welding speed v2 of the base layer after the secondary adjustment as the final welding parameter welding base layer, and correcting the actual groove welding layer morphology to make it consistent with the theoretical groove welding layer morphology read from the welding database.

[0116] In order to make the welding layer thickness of the base layer the same as that of the theoretical database, the welding current or welding speed of the base layer is adjusted. At this time, the theoretical welding current is kept unchanged by default. Due to the existence of factors such as the actual base layer welding gap, the actual welding current is difficult to be consistent with the theoretical current. At this time, errors are prone to occur when the base layer adjusts the welding current or welding speed. Therefore, the solution provided in this embodiment is to use the ratio of the actual groove base layer cross-sectional area to the theoretical groove cross-sectional area, assuming that the welding current is the same as the theoretical current during actual welding, to adjust the welding speed; the welding current needs to be collected during actual welding, and compared with the welding current in the database. On the basis that the welding speed has been adjusted, the welding speed is adjusted in real time for the second time, so as to avoid errors when the base layer adjusts the welding current or welding speed, and improve the welding quality. The method for collecting welding current is to obtain real-time current using welding machine communication, or to obtain welding real-time current using the robot arc tracking function.

[0117] Preferably, if Figure 4 As shown, after the base layer welding is completed, when arranging the welds of the filling layer and the cover layer, the weld curve equations of each weld of the theoretical sample that is closest to the shape and angle of the groove to be welded are obtained from the welding database, and the intersection of the weld curve equations of each weld with the straight edge of the groove, the inclined edge of the groove and / or the relevant weld curve equations in the established coordinate system of the groove to be welded is obtained to determine the robot welding position of each weld to be welded in the filling layer and the cover layer, and complete the accurate arrangement of the welds, which specifically includes the steps of:

[0118] S21. When the number of welding layers of the groove to be welded is less than or equal to the number of welding layers of the theoretical sample in the welding database that is closest to the shape and angle of the groove to be welded, establish a coordinate system for the single-sided V-shaped groove such as Figure 2 As shown in the figure, the straight edge equations of the groove straight edge and the groove bevel edge in the groove coordinate system to be welded are obtained as y r =f(x), hypotenuse equation y h =f(x), and the equation for obtaining the base weld morphology from the closest theoretical sample in the welding database is y0=f(x), where, due to the limitation of the groove morphology parameters, the x-coordinate interval range is (0, w), and the y-coordinate interval range is (0, t).

[0119] S22. Solve the bottom weld morphology equation y0=f(x) and the straight edge equation y within the coordinate region. r = the coordinates of the intersection point p0 of f(x), then the coordinates of the intersection point p0 are used as the robot welding position of the nearly straight edge weld of the first filling layer;

[0120] S23. In the coordinate region, solve the bottom layer weld morphology equation y0=f(x) and the hypotenuse equation y h =The coordinates of the intersection point p1 of f(x), and the x-coordinate interval of the equation y0=f(x) of the base weld morphology is obtained by using the coordinates of the intersection points p0 and p1;

[0121] S24, arranging the welding points of the first filling layer, wherein Figure 3 As shown, the weld types of the first filling layer include three types of welds: near straight edge welds, middle welds and near bevel edge welds. Assume that the equation of the near straight edge weld is y r1 =f(x), the curve equation of the first middle weld is y m1-1 =f(x), the curve equation of the second middle weld is y m1-2 =f(x)……, the curve equation of the nth middle weld is y m1-n =f(x), the equation of the weld near the bevel is y h1 =f(x); When arranging, first obtain the nearly straight edge weld curve equation y of the first filling layer weld according to the closest theoretical sample from the welding database r1 = f(x) and the straight edge equation y r =f(x) to find the intersection point p (0,1) , the intersection point p (0,1) To fill the robot welding position of the second layer of the nearly straight edge weld (or offset the intersection by a certain distance), then according to the nearly straight edge weld curve equation y r1 =f(x) and the bottom weld curve equation y0=f(x) to find the intersection point p (m1,1) , the intersection point p (m1,1)is the robot welding position of the first intermediate weld adjacent to the nearly straight edge weld (or the intersection is offset by a certain distance), and p is used to (0,1) and p (m1,1) Get the equation of the nearly straight edge weld curve y r1 = the x-coordinate interval of f(x); then, calculate p (m1,1) The distance from p1 is d1. Under the standard groove model, the distance is d s , then when d1≤d s *C, only the near-bevel weld, where C is the tolerance factor, when d1>d s *C, including the middle weld, using the first middle weld curve equation y m1-1 =f(x) and the equation of the nearly straight edge weld curve y r1 =f(x) to find the intersection point p (0,1,1) , and the bottom layer weld y0 = f(x) to find the intersection point p (m2,1) , calculate the intersection point p (m2,1) The distance d2 from p1, if d2>d s *C, then the intersection point p (m2,1) is the robot welding position of the second middle weld (or offset the intersection by a certain distance), if d2≤d s *C, then the intersection point p (m2,1) The midpoint p with p1 z1 As a robot welding position for near bevel welds, while using p (0,1,1) With p (m2,1) Get the equation y for the first intermediate weld m1-1 =f(x)'s x-mark interval; if there is a second middle weld, repeat the solution process for the first middle weld; if there is no second middle weld, only the near bevel weld y h1 =f(x), then the first middle weld curve equation y m1-1 =f(x) to find the intersection point p (1,1,1) , and the hypotenuse equation y h1 =f(x) to find the intersection point p (1,1) ;

[0122] S25, arrange the welding points of the i-th filling layer, and assume that the equation of the straight edge weld curve of the i-th filling layer is y ri =f(x), the equation of the first middle weld curve is y m1-i =f(x), the equation of the second middle weld curve is y m2-i =f(x)……, the equation of the nth middle weld curve is y mn-i =f(x), the equation of the weld near the bevel is y hi =f(x), equation of the nearly straight weld curve y ri = f(x) and the straight edge equation y r=f(x) to find the intersection point p (0,i) , the intersection point p of the two weld shapes of the nearly straight edge weld and the first middle weld adjacent to the weld shape of the i-1 filling layer is obtained (mi,1) , p (mi,1) Satisfy the x interval of the two welds and the y value is the largest, using p (0,i) With p (mi,1) Determine the x-coordinate interval of the nearly straight edge weld, p (mi,1) The robot welding position associated with the next weld, p (mi,1) The distance between the intersection of the hypotenuse and the i-1th filling layer is di. If di≤ds*C, there is no intermediate weld, p (mi,1) With p (1,i-1) The midpoint p zi is the arc starting point of the near-bevel weld, and the intersection point p between the near-bevel weld and the bevel is obtained. (1,i) , and find the intersection point p with the adjacent weld on the same layer (1,1,i) , p (1,i) With p (1,1,i) Determine the x-coordinate interval of the near-bevel weld. If di>ds*C, repeat the above process to obtain the arc starting position p of the first middle weld and the first middle weld and the second middle weld of the i-1st filling layer. (m2,1) , and find the intersection point p with the nearly straight edge weld of the same layer (0,i) ,p (m2,1) With p (0,i) Determine the x-coordinate interval of the second middle weld and calculate p (m2,1) The distance between the intersection point of the hypotenuse and the i-1th filling layer is calculated as di, until di≤ds*C. Once the intersection point of the near-hypotenuse weld is obtained, the arrangement of the welds in the same layer is completed.

[0123] This embodiment uses the relevant weld data of similar theoretical samples in the database to solve the weld intersection points to obtain the robot welding position of each weld and complete the weld arrangement. The data reliability and accuracy are guaranteed, which improves the operating efficiency of the robot's multi-layer and multi-pass welding and ensures the welding quality.

[0124] Taking a single-sided V-groove as an example, the actual weld bead arrangement is as follows: Figure 5 If the amount of base layer filling is too much, it will lead to poor welding quality at the root of the groove. In actual welding, keep the robot position unchanged, that is, the welding position unchanged, weld the base layer and the first filling layer separately, at this time, only the dry extension length, welding current, welding speed and other parameters can be adjusted.

[0125] Preferably, after the base layer welding is completed, when arranging the welds of the filling layer and the capping layer, the weld curve equations of each weld of the theoretical sample that is closest to the groove shape and groove angle to be welded are obtained from the welding database, and the intersection of the weld curve equations of each weld with the groove straight edge, the groove bevel and / or the relevant weld curve equations in the established groove coordinate system to be welded is obtained to determine the robot welding position of each weld to be welded in the filling layer and the capping layer, and complete the accurate arrangement of the welds, which specifically also includes the steps of:

[0126] S26. When the number of welding layers of the groove to be welded is greater than the number of welding layers of the theoretical sample in the welding database that is closest to the shape and angle of the groove to be welded, the welds of the other welding layers exceeding the number of welding layers of the theoretical sample and the welds of the same type in the welding layer of the theoretical sample are in an offset relationship. If the curve equation of the i-th layer weld of the top layer of the closest theoretical sample in the welding database is y i =f(x), then the equation for the same type of weld in the i+1th layer is expressed as y i -b=f(xa), where coordinates a and b are the offsets of the arc starting positions of the two welds along the x and y directions respectively. The offset b along the y direction reflects the thickness of the weld layer, and the offset along the x direction is determined by the x offset between two adjacent welds of the same type in the theoretical sample.

[0127] In this embodiment, for the first few layers of welds, theoretical sample data with similar groove shapes and angles are found in the database. For example, if the theoretical sample has four layers of welds with known curve equations (excluding the base layer), then based on the known curve equations, the intersection of the welds with the known curve equations of the four layers of the theoretical sample is used to solve the starting points of the welds of the first four layers of the groove to be welded. For the exceeding part (such as the fifth layer of weld), since there is no ready-made weld curve equation, the present embodiment adopts an offset method to obtain the robot welding position of the other layers of welds. For example, the nearly straight edge weld of the fifth layer has an offset in the X and Y directions equal to the X and Y offsets of the nearly straight edge weld between the third and fourth layers. For the X and Y offsets of the middle weld, the Y offset is calculated by the X and Y offsets of the weld between the third and fourth layers. The thickness of the seam is determined, and the X offset is first obtained by the X-direction offset between the starting point of the first middle weld of the third layer and the starting point of the middle weld of the fourth layer, so as to obtain the curve equation of the first middle weld of the fifth layer. Then, the intersection of the curve equation of the first middle weld of the fifth layer and the fourth layer weld is obtained. If the distance between the intersection and the intersection of the fourth layer near bevel weld and the bevel is greater than the threshold, the intersection is used as the starting point of the second middle weld of the fifth layer. If the distance is less than the threshold, the midpoint position of the two points is used as the starting point of the fifth layer near bevel weld to complete the arrangement of the fifth layer weld, and so on, so as to obtain the accurate arrangement of the welds of other layers. Even if the relevant curve equations are missing in the database, the robot welding positions of other welds can be obtained, which improves the applicability of weld bead arrangement.

[0128] When obtaining the actual groove size, the groove gap and groove blunt edge values ​​are estimated manually. In order to conform to the database, the groove angle needs to be measured. The measurement method is to use sensors for measurement. This method uses the method of obtaining the groove position by the robot welding wire to measure the groove angle, such as Fig.10 shown.

[0129] When the robot moves, the welding wire contacts the groove. At this time, the welding system is turned on to form a circuit, and the robot records the position at this time. This method is a common function of contact sensing of arc welding robots. By measuring the coordinates of the four positions of the groove, p1 (x1, y1, z1), p2 (x2, y2, z2), p3 (x3, y3, z3), and p4 (x4, y4, z4), one of the three directions of X, Y, and Z is selected as the default direction, and the groove angle is obtained by using the method of finding the angle between two straight lines. If the Z direction is selected as the default direction, p1 and p2 form a straight line with a slope of k1, and p3 and p4 form a straight line with a slope of k2, then the formula for obtaining the groove angle α is:

[0130] k1=(y2-y1) / (x2-x1) (9)

[0131] k2=(y4-y3) / (x4-x3) (10)

[0132] tanα=|(k1-k2) / (1+k1*k2) (11)

[0133] For actual groove welding, it is necessary to measure the thickness of the base welding layer, and the measurement method is to convert it into the measurement of the dry extension length of the welding wire.

[0134] (1) Fig.11 The figure shows that after the base layer welding is completed, the robot runs to the position of the first filling layer according to the theoretical database. At this time, the dry extension length of the welding wire is short and does not touch the base layer weld. The robot starts feeding the wire by triggering the wire sending signal until the welding wire contacts the weld. At this time, the wire feeding stops because the power circuit is formed. Since the position of the robot is fixed, the dry extension length can be measured. If you want to improve the accuracy, you can repeatedly withdraw and feed the wire to obtain the dry extension length of the welding wire. Since the dry extension length of the theoretical database is fixed, the dry extension length at this time is subtracted from the theoretical dry extension length to calculate the welding thickness of the base layer.

[0135] (2) Measure the dry extension of the welding wire. Fig.12As shown, select the standard substrate position, compile the robot measurement program, and first record the robot position of the standard length of the wire extension. The extension length l1 is known, the robot initial position P0, at which time the wire is not in contact with the workpiece, and the robot moves along the Z-direction of the coordinate system toward the standard substrate until it contacts the standard substrate. At this time, the robot position is P1.

[0136] When the wire stickout length is unknown, the robot measurement program is executed. At this time, the robot moves from position P0 to P2, and the stickout length l can be calculated as:

[0137] l=l1+P2.z-P1.z.

[0138] like Fig.13 As shown, the preferred embodiment of the present invention also provides a robot multi-layer multi-pass welding device, comprising:

[0139] The base layer welding correction module is used to adjust the welding current or welding speed read from the welding database in real time according to the measured actual size of the groove when welding the base layer, and correct the welding layer morphology of the actual groove to make it consistent with the theoretical groove welding layer morphology read from the welding database, wherein the theoretical groove in the welding database has no gap and no blunt edge, and the actual size of the groove includes the groove gap c and the groove blunt edge value p, the groove angle α, the groove width w, and the plate thickness t;

[0140] The weld bead arrangement module is used to obtain the weld curve equations of each weld of the theoretical sample that is closest to the shape and angle of the groove to be welded from the welding database when arranging the weld bead of the filling layer and the cover layer after the base layer welding is completed, and to obtain the intersection of the weld curve equation of each weld with the straight edge of the groove, the inclined edge of the groove and / or the relevant weld curve equation in the established coordinate system of the groove to be welded, so as to determine the robot welding position of each weld to be welded in the filling layer and the cover layer, and complete the precise arrangement of the weld bead.

[0141] Preferably, if Fig.14 The robot multi-layer multi-pass welding device also includes:

[0142] A welding database establishment module is used to establish a welding database, wherein the welding database includes groove input parameters and welding parameters. The groove input parameters include groove width and groove angle. The welding parameters include welding current, welding voltage, welding speed, weaving welding parameters, dry extension and robot welding position. The welding database includes theoretical samples without gaps and blunt edges, and weld curve equations of each weld of each theoretical sample. Considering the quality requirements of medium and thick plate welding, it is preferred to obtain the database program by welding actual samples.

[0143] like Fig.15As shown, a preferred embodiment of the present invention also provides an electronic device, including a memory, a processor, and a computer program stored in the memory and executable on the processor, wherein the processor implements the steps of the robot multi-layer and multi-pass welding method in the above-mentioned embodiment when executing the computer program.

[0144] like Fig.16 As shown, the preferred embodiment of the present invention further provides a computer device, which can be a terminal or a liveness detection server, and its internal structure diagram can be as shown in Fig.16 As shown. The computer device includes a processor, a memory and a network interface connected through a system bus. Among them, the processor of the computer device is used to provide computing and control capabilities. The memory of the computer device includes a non-volatile storage medium and an internal memory. The non-volatile storage medium stores an operating system and a computer program. The internal memory provides an environment for the operation of the operating system and the computer program in the non-volatile storage medium. The network interface of the computer device is used to communicate with other external computer devices through a network connection. When the computer program is executed by the processor, the steps of the above-mentioned robot multi-layer multi-pass welding method are implemented.

[0145] Those skilled in the art will understand that Fig.16 The structure shown in the figure is only a block diagram of a part of the structure related to the solution of the present invention, and does not constitute a limitation on the computer device to which the solution of the present invention is applied. The specific computer device may include more or fewer components than those shown in the figure, or combine certain components, or have a different arrangement of components.

[0146] A preferred embodiment of the present invention further provides a storage medium, which includes a stored program, and when the program is run, controls the device where the storage medium is located to execute the steps of the robot multi-layer and multi-pass welding method in the above embodiment.

[0147] It should be noted that the steps shown in the flowcharts of the accompanying drawings can be executed in a computer system such as a set of computer executable instructions, and that, although a logical order is shown in the flowcharts, in some cases, the steps shown or described can be executed in an order different from that shown here.

[0148] If the functions described in the method of this embodiment are implemented in the form of software functional units and sold or used as independent products, they can be stored in one or more computing device readable storage media. Based on this understanding, the part of the embodiment of the present invention that contributes to the prior art or the part of the technical solution can be embodied in the form of a software product, which is stored in a storage medium and includes several instructions for a computing device (which can be a personal computer, server, mobile computing device or network device, etc.) to perform all or part of the steps of the method described in each embodiment of the present invention. The aforementioned storage medium includes: U disk, mobile hard disk, read-only memory (ROM, Read-Only Memory), random access memory (RAM, Random Access Memory), disk or optical disk and other media that can store program codes.

[0149] It will be appreciated by those skilled in the art that embodiments of the present invention may be provided as methods, systems, or computer program products. Therefore, the present invention may take the form of a complete hardware embodiment, a complete software embodiment, or an embodiment combining software and hardware. Moreover, the present invention may take the form of a computer program product implemented on one or more computer-usable storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) containing computer-usable program codes. The schemes in the embodiments of the present invention may be implemented in various computer languages, for example, object-oriented programming language Java and literal scripting language JavaScript, etc.

[0150] The present invention is described with reference to flowcharts and / or block diagrams of methods, devices (systems), and computer program products according to embodiments of the present invention. It should be understood that each process and / or block in the flowchart and / or block diagram, as well as the combination of processes and / or blocks in the flowchart and / or block diagram, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, a special-purpose computer, an embedded processor, or other programmable data processing device to produce a machine, so that the instructions executed by the processor of the computer or other programmable data processing device generate instructions for implementing the processes in the flowchart and / or block diagram. Figure 1 A process or multiple processes and / or boxes Figure 1 A device that provides the functions specified in a block or multiple blocks.

[0151] These computer program instructions may also be stored in a computer readable memory capable of directing a computer or other programmable data processing device to operate in a specific manner, so that the instructions stored in the computer readable memory produce an article of manufacture including an instruction device, which implements the process Figure 1 A process or multiple processes and / or boxes Figure 1A function specified in one or more boxes.

[0152] These computer program instructions can also be loaded onto a computer or other programmable data processing device so that a series of operating steps are executed on the computer or other programmable device to produce a computer-implemented process, thereby providing instructions for implementing the process. Figure 1 A process or multiple processes and / or boxes Figure 1 The steps for the functions specified in one or more boxes.

[0153] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0154] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A robot multi-layer multi-pass welding method, characterized in that: Includes steps: When welding the base layer, according to the measured actual size of the groove, the welding current or welding speed read from the welding database is adjusted in real time, and the welding layer morphology of the actual groove is corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, wherein the theoretical groove in the welding database has no gap and no blunt edge, and the actual size of the groove includes the groove gap c and the groove blunt edge value p, the groove angle α, the groove width w, and the plate thickness t; After the base layer welding is completed, when arranging the welds of the filling layer and the cover layer, the weld curve equations of each weld of the theoretical sample that is closest to the shape and angle of the groove to be welded are obtained from the welding database, and the intersection of the weld curve equations of each weld with the straight edge of the groove, the inclined edge of the groove and / or the relevant weld curve equations in the established coordinate system of the groove to be welded is obtained to determine the robot welding position of each weld to be welded in the filling layer and the cover layer, and complete the precise arrangement of the welds.

2. The robot multi-layer multi-pass welding method according to claim 1, characterized in that: Before welding the base layer, the following steps are also included: A welding database is established, wherein the welding database includes groove input parameters and welding parameters. The groove input parameters include groove width and groove angle. The welding parameters include welding current, welding voltage, welding speed, weaving welding parameters, dry extension and robot welding position. The welding database includes theoretical samples without gaps and blunt edges, and weld curve equations of each weld of each theoretical sample. Considering the quality requirements of medium and thick plate welding, it is preferred to obtain the database program by welding actual samples.

3. The robot multi-layer multi-pass welding method according to claim 1, characterized in that: When welding the base layer, according to the actual size of the groove obtained, the welding current or welding speed read from the welding database is adjusted in real time, and the welding layer morphology of the actual groove is corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, which specifically includes the steps of: The formula S for calculating the theoretical cross-sectional area of ​​the base layer required for the theoretical groove is: Among them, h is the theoretical thickness of the base layer under the theoretical groove condition; The back penetration of the groove is set to 1mm, and the back penetration cross-sectional area model is set to a triangle. When the theoretical thickness of the base layer h remains unchanged, the actual filling cross-sectional area S' of the base layer in the actual groove is calculated as follows: Under the premise that the weld length remains unchanged, the base layer area ratio k = S' / S is calculated based on the proportional relationship between the actual filling cross-sectional area and the theoretical cross-sectional area; According to the base layer area ratio k, the base layer theoretical welding current, and the base layer theoretical welding speed, the actual base layer welding current I1 and welding speed v1 are calculated: I1=k*I (3) v1=v / k (4) Among them, I is the theoretical welding current of the base layer, and v is the theoretical welding speed of the base layer; The actual welding current I1 of the base layer or the actual welding speed v1 of the base layer is selected as a welding parameter to weld the base layer, and the welding layer morphology of the actual groove is corrected to be consistent with the theoretical groove welding layer morphology read from the welding database.

4. The robot multi-layer multi-pass welding method according to claim 3, characterized in that: When welding the base layer, according to the actual size of the groove obtained, the welding current or welding speed read from the welding database is adjusted in real time, and the welding layer morphology of the actual groove is corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, which specifically includes the steps of: If the welding current or welding speed read from the welding database is adjusted in real time after the base layer welding, the actual groove welding layer morphology cannot be corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database, then the cross-sectional area S1 of the theoretical first filling layer is calculated: Among them, h2 is the total thickness of the welding layer after welding the theoretical first filling layer, and h1 is the thickness of the welding layer of the theoretical base layer; When actually welding the first filling layer, due to the different thickness of the base layer, calculate the actual cross-sectional area S11 of the first filling layer: Among them, h 1s It is the actual thickness of the welding layer of the base layer; Under the premise that the weld length remains unchanged, the filling layer area ratio k1=S11 / S1 is calculated based on the proportional relationship between the cross-sectional area of ​​the actual first filling layer and the cross-sectional area of ​​the theoretical first filling layer; Since the filling amount is proportional to the welding current and inversely proportional to the welding speed, the actual welding current I3 and welding speed v3 of the filling layer are calculated according to the filling layer area ratio k1, the theoretical welding current of the filling layer, and the theoretical welding speed of the filling layer: I3= k1×I2 (6) v3= v2 / k1 (7) Among them, I2 is the theoretical welding current, v2 is the theoretical welding speed; The actual welding current I3 of the filling layer or the actual welding speed v3 of the filling layer is selected as a welding parameter to weld the first filling layer, and the welding layer morphology of the actual groove is corrected to make it consistent with the theoretical groove welding layer morphology read from the welding database.

5. The robot multi-layer multi-pass welding method according to claim 3, characterized in that: After selecting the actual welding current I1 of the base layer or the actual welding speed v1 of the base layer as the welding parameter to weld the base layer and correcting the actual groove welding layer morphology to make it consistent with the theoretical groove welding layer morphology read from the welding database, the following steps are also included: The actual welding current I4 during the actual welding of the base layer is obtained by using the welding machine communication or the arc tracking function of the robot; Based on the theoretical welding current I of the base layer and the calculated actual welding speed v1 of the base layer, the actual welding speed v2 of the base layer after secondary adjustment is calculated: v2= I / I4×v1 (8); The actual welding speed v2 of the base layer after the secondary adjustment is used as the final welding parameter to weld the base layer, and the welding layer morphology of the actual groove is corrected to be consistent with the theoretical groove welding layer morphology read from the welding database.

6. The robot multi-layer multi-pass welding method according to claim 1, characterized in that: After the base layer welding is completed, when arranging the welds of the filling layer and the capping layer, the weld curve equations of each weld of the theoretical sample that is closest to the shape and angle of the groove to be welded are obtained from the welding database, and the intersection of the weld curve equations of each weld with the straight edge of the groove, the inclined edge of the groove and / or the relevant weld curve equations in the established coordinate system of the groove to be welded is obtained to determine the robot welding position of each weld to be welded in the filling layer and the capping layer, and complete the accurate arrangement of the welds, which specifically includes the steps of: When the number of welding layers of the groove to be welded is less than or equal to the number of welding layers of the theoretical sample in the welding database that is closest to the shape and angle of the groove to be welded, the straight edge equations of the straight edge and the bevel edge of the groove in the coordinate system of the groove to be welded are obtained as y r =f(x), hypotenuse equation y h =f(x), the equation for obtaining the base weld morphology from the closest theoretical sample in the welding database is y0=f(x), where, due to the limitation of groove morphology parameters, the x-coordinate interval range is (0, w), and the y-coordinate interval range is (0, t); In the coordinate region, solve the bottom layer weld morphology equation y0 = f(x) and the straight edge equation y r = the coordinates of the intersection point p0 of f(x), then the coordinates of the intersection point p0 are used as the robot welding position of the nearly straight edge weld of the first filling layer; In the coordinate region, solve the bottom layer weld morphology equation y0 = f(x) and the hypotenuse equation y h =The coordinates of the intersection point p1 of f(x), and the x-coordinate interval of the equation y0=f(x) of the base weld morphology is obtained by using the coordinates of the intersection points p0 and p1; Arrange the welding points of the first filling layer, wherein the weld types of the first filling layer include three types of welds: near straight edge welds, middle welds and near bevel edge welds. When arranging, first obtain the near straight edge weld curve equation y of the first filling layer weld according to the closest theoretical sample from the welding database r1 = f(x) and the straight edge equation y r =f(x) to find the intersection point p (0,1) , the intersection point p (0,1) To fill the robot welding position of the second layer of the nearly straight edge weld, then according to the nearly straight edge weld curve equation y r1 =f(x) and the bottom weld curve equation y0=f(x) to find the intersection point p (m1,1) , the intersection point p (m1,1) The robot welding position of the first intermediate weld adjacent to the nearly straight edge weld is (0,1) and p (m1,1) Get the equation y of the nearly straight edge weld curve r1 = the x-coordinate interval of f(x); then, calculate p (m1,1) The distance from p1 is d1. Under the standard groove model, the distance is d s , then when d1≤d s *C, only the near-bevel weld, where C is the tolerance factor, when d1>d s *C, including the middle weld, using the first middle weld curve equation y m1-1 =f(x) and the equation of the nearly straight edge weld curve y r1 =f(x) to find the intersection point p (0,1,1) , and the bottom layer weld y0 = f(x) to find the intersection point p (m2,1) , calculate the intersection point p (m2,1) The distance d2 from p1, if d2>d s *C, then the intersection point p (m2,1) is the robot welding position of the second middle weld, if d2≤d s *C, then the intersection point p (m2,1) The midpoint p with p1 z1 As a robot welding position for near bevel welds, while using p (0,1,1) With p (m2,1) Get the equation y for the first intermediate weld m1-1 = f(x) x-mark interval; if there is a second middle weld, repeat the solution process of the first middle weld; if there is no second middle weld, only the near bevel weld y h1 =f(x), then the first middle weld curve equation y m1-1 =f(x) to find the intersection point p (1,1,1) , and the hypotenuse equation y h1 =f(x) to find the intersection point p (1,1) ; Arrange the welding points of the i-th filling layer, and assume that the equation of the straight edge weld curve of the i-th filling layer is y ri =f(x), the equation of the first middle weld curve is y m1-i =f(x), the equation of the second middle weld curve is y m2-i =f(x), the equation of the nth middle weld curve is y mn-i =f(x), the equation of the weld near the bevel is y hi =f(x), equation of the nearly straight weld curve y ri = f(x) and the straight edge equation y r =f(x) to find the intersection point p (0,i) , the intersection point p of the two weld shapes of the nearly straight edge weld and the first middle weld adjacent to the weld shape of the i-1 filling layer is obtained (mi,1) , p (mi,1) Satisfy the x interval of the two welds and the y value is the largest, using p (0,i) With p (mi,1) Determine the x-coordinate interval of the nearly straight edge weld, p (mi,1) The robot welding position associated with the next weld, p (mi,1) The distance between the intersection of the hypotenuse and the i-1th filling layer is di. If di≤ds*C, there is no intermediate weld, p (mi,1) With p (1,i-1) The midpoint p zi is the arc starting point of the near-bevel weld, and the intersection point p between the near-bevel weld and the bevel is obtained. (1,i) , and find the intersection point p with the adjacent weld on the same layer (1,1,i) , p (1,i) With p (1,1,i) Determine the x-coordinate interval of the near-bevel weld. If di>ds*C, repeat the above process to obtain the arc starting position p of the first middle weld and the first middle weld and the second middle weld of the i-1st filling layer. (m2,1) , and find the intersection point p with the nearly straight edge weld of the same layer (0,i) ,p (m2,1) With p (0,i) Determine the x-coordinate interval of the second middle weld and calculate p (m2,1) The distance between the intersection point of the hypotenuse and the i-1th filling layer is calculated as di, until di≤ds*C. Once the intersection point of the near-hypotenuse weld is obtained, the arrangement of the welds in the same layer is completed.

7. The robot multi-layer multi-pass welding method according to claim 6, characterized in that: After the base layer welding is completed, when arranging the welds of the filling layer and the capping layer, the weld curve equations of each weld of the theoretical sample that is closest to the shape and angle of the groove to be welded are obtained from the welding database, and the intersection of the weld curve equations of each weld with the straight edge of the groove, the inclined edge of the groove and / or the relevant weld curve equations in the established coordinate system of the groove to be welded is obtained to determine the robot welding position of each weld to be welded in the filling layer and the capping layer, and complete the accurate arrangement of the welds, which specifically also includes the steps of: When the number of welding layers of the groove to be welded is greater than the number of welding layers of the theoretical sample in the welding database that is closest to the shape and angle of the groove to be welded, the welds of the other welding layers exceeding the number of welding layers of the theoretical sample and the welds of the same type in the welding layer of the theoretical sample are in an offset relationship. If the curve equation of the i-th layer weld of the top layer of the closest theoretical sample in the welding database is y i =f(x), then the equation for the same type of weld in the i+1th layer is expressed as y i -b=f(xa), where coordinates a and b are the offsets of the arc starting positions of the two welds along the x and y directions respectively. The offset b along the y direction reflects the thickness of the weld layer, and the offset along the x direction is determined by the x offset between two adjacent welds of the same type in the theoretical sample.

8. A robot multi-layer multi-pass welding device, characterized in that: include: The base layer welding correction module is used to adjust the welding current or welding speed read from the welding database in real time according to the measured actual size of the groove when welding the base layer, and correct the welding layer morphology of the actual groove to make it consistent with the theoretical groove welding layer morphology read from the welding database, wherein the theoretical groove in the welding database has no gap and no blunt edge, and the actual size of the groove includes the groove gap c and the groove blunt edge value p, the groove angle α, the groove width w, and the plate thickness t; The weld bead arrangement module is used to obtain the weld curve equations of each weld of the theoretical sample that is closest to the shape and angle of the groove to be welded from the welding database when arranging the weld bead of the filling layer and the cover layer after the base layer welding is completed, and to obtain the intersection of the weld curve equation of each weld with the straight edge of the groove, the inclined edge of the groove and / or the relevant weld curve equation in the established coordinate system of the groove to be welded, so as to determine the robot welding position of each weld to be welded in the filling layer and the cover layer, and complete the precise arrangement of the weld bead.

9. An electronic device comprising a memory, a processor, and a computer program stored in the memory and executable on the processor, characterized in that: When the processor executes the computer program, the steps of the robot multi-layer multi-pass welding method according to any one of claims 1 to 7 are implemented.

10. A storage medium, comprising a stored program, which controls a device where the storage medium is located to execute the steps of the robot multi-layer and multi-pass welding method as claimed in any one of claims 1 to 7 when the program is executed.

Citation Information

Cited By

  • Robot medium and thick plate welding control method based on expert database and integrated welding system

    CN121468043A

  • A robot-based medium plate welding control method based on an expert database and an integrated welding system

    CN121468043B

  • Automated welding equipment

    TWI940111B