Washable texture-controllable wrinkled real silk or silk-containing fabric as well as preparation process and application thereof
Through the processes of additive pretreatment, embroidery wrinkling, machine pressing and shaping, the problem of unnatural and impermissible washing of silk fabric texture wrinkles is solved, and a long-lasting continuous and regular texture wrinkle style and soft and breathable effect is achieved. In a variety of textiles.
Patent Information
- Application Number
- CN202411284939.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-06
AI Technical Summary
The wrinkles formed by existing silk fabrics are relatively three-dimensional and regular, and unnatural. The texture wrinkles formed by high-temperature wrinkle pressing process are unstable and are not resistant to water washing, and are prone to fading and disappearing after washing.
Using additive pretreatment, embroidery wrinkling treatment, machine ironing and shaping treatment, the fabric surface is formed by chemical substances such as polymer additives and inorganic metal salts, and ensures that it is shaping fluid and penetrant. Permanence of texture wrinkles.
It realizes the long-lasting, continuous and controllable regular texture wrinkle style of silk fabrics. It maintains a good style after multiple washes. Combined with a soft and breathable comfortable feel, it is suitable for clothing and home textiles.
Smart Images

Figure CN119083183A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, and in particular to a washable, texture-controllable wrinkle real silk or silk-containing fabric, and a preparation process and application thereof. Background Art
[0002] In recent years, with the rapid economic development, people's living standards and consumption levels have been continuously improving, and the requirements for updates and iterations in the textile industry have become increasingly higher. The micro-texture style of clothing, underwear fabrics, and home textile products has become increasingly popular among consumers.
[0003] At present, chemical fiber fabrics such as nylon and polyester have special thermoplastic characteristics. Through processes such as wrinkling and high-temperature shaping, the fabrics can present various styles of texture wrinkles, which are very popular in the consumer market, especially for female consumers. Silk enjoys the reputation of "Queen of Fibers". Silk fabrics made of it are light, smooth, soft and skin-friendly, with good moisture absorption and breathability and soft luster. They have always been widely loved as high-end textile fabrics, and their skin feel and comfort have advantages that other fibers cannot achieve. However, silk fibers themselves are relatively soft. Although they are easy to wrinkle during wearing, they will basically flatten and disappear after washing. In addition, silk is not a thermoplastic material. It is difficult to truly form a permanent texture wrinkle style after wrinkling through heat shaping.
[0004] At present, there are also various kinds of silk wrinkle fabrics on the market, such as double crepe, seersucker, georgette, etc., but they are all achieved through yarn twisting or special weaving processes. For example, the Chinese patent with publication number CN116005319A discloses a silk fabric and weaving method that can maintain strip wrinkles. It uses interval-arranged wrinkle lines to partially gather the fabric body to form strip wrinkles. During use, the setting of the wrinkle lines prevents the wrinkles formed from disappearing and fading. But overall, the wrinkles formed by this weaving wrinkling method are relatively three-dimensional and regular, unnatural, and difficult to form linear textures. The transition between wrinkled and non-wrinkled areas is not soft enough. It belongs to two completely different styles from the high-temperature wrinkling of chemical fiber fabrics. Moreover, although chemical fiber texture wrinkle fabrics have the advantages of durability, not easy to deform, and easy to wash, the material itself has poor moisture absorption and air permeability, and the comfort of wearing is far less than that of natural fibers. At present, the barrier to achieving a long-lasting wrinkled style of silk fabrics through post-finishing high-temperature wrinkling technology is high and still difficult to achieve.
[0005] Therefore, how to superimpose various wrinkle styles on high-end silk fabrics has become one of the current research directions of the silk industry. Summary of the invention
[0006] The purpose of the present invention is to provide a washable controllable texture wrinkle real silk or silk-containing fabric, which solves the problem that the wrinkles formed by the weaving wrinkling method of the existing real silk fabric are relatively three-dimensional and regular, unnatural, and the texture wrinkles formed by the high-temperature wrinkling process cannot be fixed, are not washable, and the wrinkles are easy to fade and disappear after washing. The fabric is skin-friendly, soft, smooth and comfortable, breathable and not stuffy, and also has a long-lasting continuous controllable regular texture wrinkle style, and still maintains a good texture wrinkle style after multiple washings. In addition, the present invention also provides a preparation process for a simple and efficient process flow, a wide range of applicability, and the fabric can be formed into a long-lasting washable controllable texture wrinkle real silk or silk-containing fabric, and the fabric is applied in the fields of clothing (jackets, trousers, skirts), underwear, home textiles, etc.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A first aspect of the present invention provides a washable, controllable texture wrinkle silk or silk-containing fabric, wherein continuous regular texture wrinkles are distributed on the surface of the silk or silk-containing fabric, and the continuous regular texture wrinkles are shape-retaining after washing, and the continuous regular texture wrinkles will not disappear or deform after multiple washings.
[0009] Furthermore, the continuous regular texture wrinkles are distributed in one or more of line-like, pattern-like, and pattern-like shapes.
[0010] Furthermore, the distribution state of the continuous regular texture wrinkles is one or more of continuous, discontinuous, articulated, and cross distribution.
[0011] Furthermore, the silk or silk-containing fabric includes 100% silk fabric, silk interwoven fabric with a silk content of more than 30%, or silk blended fabric.
[0012] Preferably, 100% silk fabric or silk interwoven fabric with a silk content of more than 30% is selected.
[0013] The silk or silk-containing fabric is one of plain weave, twill weave and satin weave.
[0014] The second aspect of the present invention provides a process for preparing the above-mentioned washable controllable texture wrinkle silk or silk-containing fabric, comprising the following steps:
[0015] S1. Pretreatment of additives:
[0016] The silk or silk-containing fabric is rolled or soaked in an auxiliary agent solution, with a rolling rate of 40 to 100%, and then the rolled or soaked fabric is subjected to a heating and shaping treatment;
[0017] The mass content of the additive in the additive solution is 0.5 to 100 g / L, preferably 2 to 20 g / L, and the additive is one or more of polyurethane, polycarbonate, and silicone additive;
[0018] S2. Embroidery wrinkle treatment:
[0019] Embroidering the silk or silk-containing fabric processed in step S1 by manual or program-controlled embroidery equipment, and shrinking and wrinkling the embroidery area to form regular texture wrinkles on the surface of the fabric;
[0020] S3, machine pressing treatment:
[0021] The fabric after embroidery shrinkage in step S2 is subjected to pressing treatment, with a pressure of 0.1-1.0 MPa, a temperature of 120-180° C., and a speed of 10-100 m / min.
[0022] S4, shaping process:
[0023] The silk or silk-containing fabric subjected to the pressing treatment in step S3 is rolled or soaked in a post-setting liquid for secondary heating and setting treatment, and then washed with water and dried to set the wrinkled parts on the fabric into permanent wrinkles;
[0024] The setting liquid contains a penetrant, an inorganic metal salt and an alkali agent.
[0025] Using the above preparation process:
[0026] Since silk fabrics or silk-containing fabrics are relatively soft, wrinkles formed on the surface are relatively easy to recover. In the present invention, a polymer additive is used to pre-treat the silk fabrics or silk-containing fabrics, which reacts and solidifies on the surface of the fabrics, making the silk fabrics or silk-containing fabrics relatively stiff. In the subsequent wrinkling treatment, it is easier to form wrinkles on the surface of the fabrics under stress, and the wrinkles formed are not easy to recover.
[0027] After the fabric is pre-treated with auxiliary agents, the embroidery and shrinkage processes are controlled to achieve continuous and regular wrinkling of the fabric, and various wrinkle shapes are formed through various patterns. The fabric is then pressed by a machine to give the fabric a preliminary shape of its wrinkling style.
[0028] However, the fabric after the auxiliary agent pre-treatment, embroidery wrinkling treatment and pressing treatment cannot be washed. If the fabric is washed at this time, the wrinkles formed on the surface of the fabric cannot be effectively maintained. Therefore, the present application also adopts a shaping treatment process to shape the texture wrinkles formed on the surface of the fabric into permanent wrinkles. During the shaping process, the silk is treated with alkali to make it easier to moisten, and then the inorganic metal salt enters the interior of the silk fiber and bonds with the active group to shape the silk. At the same time, an appropriate amount of penetrant can be added to make it easier for the inorganic metal salt to enter the interior of the silk fiber, which helps to completely shape the wrinkles.
[0029] After the silk or silk-containing fabrics are pre-treated with the auxiliary agent → embroidery wrinkling → machine pressing → shaping treatment → washing, dyeing and finishing, they still have a smooth, breathable, soft and comfortable feel, and continuous and controllable regular texture wrinkles are formed on the fabric, and the folds are natural. Moreover, the fabric can still maintain the continuous and controllable regular texture wrinkle style after 10 washings.
[0030] Furthermore, in step S2, the fabric is directly embroidered or the fabric is placed between two layers of shrinkable films and then embroidered, and the fabric is shrunk by drawing the thread or controlling the shrinkage of the film to form regular texture wrinkles.
[0031] Furthermore, the shrinkable film is made of polyester, polyamide, polyethylene, polypropylene, polybutylene or polyvinyl chloride, and the shrinkage of the film is controlled by heating, with a shrinkage temperature of 90 to 180° C. and a shrinkage time of 0.1 to 10 min.
[0032] Furthermore, in step S4, the mass content of the penetrant is 0.5-20 g / L, the mass content of the inorganic metal salt is 0.1-50 g / L, the content of the alkali agent is 0.5-20 g / L, and the bath ratio is 1:5-1:50.
[0033] Specifically, the penetrant is TF-107D; the inorganic metal salt is sodium sulfate; and the alkali agent is sodium carbonate.
[0034] Furthermore, in step S1, the primary heating and shaping treatment adopts steam heating and shaping or hot air shaping; the treatment temperature of steam heating and shaping is 100-140°C, and the treatment time is 1-60 minutes; the treatment temperature of hot air shaping is 100-140°C, and the treatment time is 1-5 minutes.
[0035] Since the curing of the additive on the surface of the fabric requires a certain temperature and time, however, if the temperature is too high, the silk fabric will turn yellow easily, affecting the appearance. If the treatment time is too long, there is also a risk of affecting the strength and color of the silk. Therefore, in the process of heating and setting, the heating temperature is controlled between 100 and 140°C, steam heating is achieved by using water vapor over 100°C, the steam heating setting treatment time is controlled between 1 and 60 minutes, and the hot air setting treatment time is controlled between 1 and 5 minutes.
[0036] Furthermore, in step S4, the temperature of the secondary heating and shaping treatment is set to 30-100° C., and the treatment time is 10-60 min.
[0037] The secondary heating setting treatment also has requirements for temperature and time. Combined with the components selected in the setting liquid and the setting principle of this step, the temperature of the secondary heating setting treatment is set to 30-100°C, and the treatment time is 10-60 minutes. Too low temperature in the bath setting treatment is not conducive to the effect of penetrant treatment on silk, etc. Too high temperature may damage the silk fabric. Too short treatment time has limited effect. Too long treatment time may also damage the silk fabric.
[0038] Furthermore, after the shaping treatment, the silk or silk-containing fabric is post-treated, and the post-treatment process includes washing, dyeing and finishing.
[0039] Washing process: Wash the fabric with washing solution, and then rinse it several times with room temperature tap water. The washing temperature is 20-80℃ and the washing time is 10-60min.
[0040] The washing solution includes 0.5-20 g / L of soaping agent sodium stearate and 0.5-5 g / L of anti-ash oil GD-62, which can greatly improve the feel and air permeability of silk fabrics.
[0041] Dyeing-finishing process: Ordinary acid dyeing or reactive dyeing conditions are sufficient. Depending on the type of fabric, it can be softened or have other functionalities such as waterproofing and UV resistance added during the finishing stage.
[0042] The third aspect of the present invention provides an application of a washable, controllable-texture wrinkle silk or silk-containing fabric. The washable, controllable-texture wrinkle silk or silk-containing fabric obtained by the above-mentioned preparation process is used for processing clothing (jackets, trousers, skirts), underwear and home textile products.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] (1) After being treated by this process, the silk or silk-containing fabric still has a smooth, breathable, soft and comfortable feel. Continuous and controllable regular texture wrinkles are formed on the fabric, and the wrinkles are natural. Moreover, the fabric can still maintain the continuous and controllable regular texture wrinkle style after being washed 10 times.
[0045] (2) Since silk fabrics or silk-containing fabrics are relatively soft, wrinkles formed on the surface are relatively easy to recover. In the present invention, a polymer additive is used to pre-treat the silk fabrics or silk-containing fabrics, which reacts and solidifies on the surface of the fabrics, making the silk fabrics or silk-containing fabrics relatively stiff. In the subsequent wrinkling treatment, it is easier to form wrinkles on the surface of the fabrics under stress, and the wrinkles formed are not easy to recover.
[0046] (3) After the pre-treatment with auxiliary agents, the fabric can be controlled to have a continuous and regular wrinkling state by controlling the embroidery and shrinkage process, and various wrinkle shapes can be formed through various patterns. The fabric is then pressed by a machine to give the fabric a preliminary shape of its wrinkling style.
[0047] (4) However, the fabric after the auxiliary agent pre-treatment, embroidery wrinkling treatment and pressing treatment cannot be washed. If the fabric is washed at this time, the wrinkles formed on the surface of the fabric cannot be effectively maintained. Therefore, the present application also adopts a shaping treatment process to shape the texture wrinkles formed on the surface of the fabric into permanent wrinkles. During the shaping process, the silk is treated with alkali to make it easier to moisten, and then the inorganic metal salt enters the interior of the silk fiber and bonds with the active group to shape the silk. At the same time, an appropriate amount of penetrant can be added to make it easier for the inorganic metal salt to enter the interior of the silk fiber, which helps to completely shape the wrinkles. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0049] Figure 1 The following are the actual pictures of the finished fabric prepared in Example 1 before and after washing.
[0050] Figure 2 The following are the actual pictures of the finished fabric prepared in Comparative Example 1 before and after washing.
[0051] Figure 3 The following are the actual pictures of the finished fabric prepared in Comparative Example 2 before and after washing. DETAILED DESCRIPTION
[0052] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] The present invention is further described below by way of examples. Unless otherwise specified, the various reagents and raw materials used in the present invention are all commercially available products or products that can be prepared by known methods.
[0054] Example 1
[0055] Fabric: Silk electrospun (weight 52g / m 2 )
[0056] The process for forming a washable controllable texture wrinkle comprises the following steps:
[0057] S1. Pretreatment of additives:
[0058] The fabric is dipped into a 20 g / L polyurethane solution with a liquid rate of 80%, and then the dipped or soaked fabric is hot-air dried at 130° C. for 2 minutes.
[0059] S2. Embroidery wrinkle treatment:
[0060] Place the fabric between the upper and lower layers of polyester shrinkable film, use program-controlled embroidery equipment and polyvinyl alcohol thread to embroider the fabric and the upper and lower shrinkable films in an interval manner with a needle spacing of 0.5 cm in warp and weft and an area of 5 cm*5 cm, and shrink them in an oven at 140℃ for 2 minutes.
[0061] S3, machine pressing treatment:
[0062] The fabric after embroidery shrinkage in step S2 is pressed at a pressure of 0.5 MPa, a temperature of 140° C., and a speed of 20 m / min to remove the embroidery thread and the shrinkable film.
[0063] S4, shaping process:
[0064] The fabric after the pressing treatment in step S3 is dipped into the post-setting liquid for secondary heating and setting treatment, the liquid carrying rate is controlled at 80%, the setting liquid temperature is controlled at 30°C, the setting treatment time is 30 minutes, and then washed and dried, and the wrinkled parts on the fabric are set into permanent wrinkles.
[0065] The setting liquid contains 5g / L of penetrant, 20g / L of inorganic metal salt and 2g / L of alkali agent.
[0066] S4, washing treatment:
[0067] The fabric was washed with a washing solution containing 5g / L of soaping agent sodium stearate and 2g / L of anti-ash oil GD-62 at a washing temperature of 30°C for 30 minutes. After washing, the fabric was rinsed three times with room temperature tap water.
[0068] S5. Dyeing treatment:
[0069] Ordinary acid stain.
[0070] The surface of the finished fabric of Example 1 forms clear and natural continuous regular texture wrinkles. After being washed 10 times, the fabric can still maintain the style of continuous regular texture wrinkles. The fabric is soft, skin-friendly, breathable and smooth.
[0071] Example 2
[0072] Fabric: Silk-bonded 48% silk, 52% viscose, 65g / m 2
[0073] The process for forming a washable controllable texture wrinkle comprises the following steps:
[0074] S1. Pretreatment of additives:
[0075] The fabric is dipped into a 30 g / L polyurethane solution with a liquid rate of 80%, and then the dipped or soaked fabric is hot-air dried at 140°C for 2 minutes.
[0076] S2. Embroidery wrinkle treatment:
[0077] Using program-controlled embroidery equipment and polyvinyl alcohol thread, the fabric is dotted with embroidery at a needle spacing of 2.0 cm in the weft direction and 10 cm in the warp direction. Then 1 / 3 of the total length is manually pulled out and treated at 140°C for 1 min using a pressing machine.
[0078] S3, machine pressing treatment:
[0079] The fabric after embroidery shrinkage in step S2 is pressed at a pressure of 1 MPa, a temperature of 140° C., and a speed of 20 m / min to remove the embroidery thread.
[0080] S4, shaping process:
[0081] The fabric after the pressing treatment in step S3 is dipped into the post-setting liquid for secondary heating and setting treatment, the liquid carrying rate is controlled at 80%, the setting liquid temperature is controlled at 30°C, the setting treatment time is 30 minutes, and then washed and dried, and the wrinkled parts on the fabric are set into permanent wrinkles.
[0082] The setting liquid contains 10g / L of penetrant, 30g / L of inorganic metal salt and 5g / L of alkali agent.
[0083] S4, washing treatment:
[0084] The fabric was washed with a washing solution containing 5g / L of soaping agent sodium stearate and 2g / L of anti-ash oil GD-62 at a washing temperature of 30°C for 30 minutes. After washing, the fabric was rinsed three times with room temperature tap water.
[0085] S5. Dyeing treatment:
[0086] Ordinary acid stain.
[0087] The surface of the finished fabric of Example 2 forms clear and natural continuous regular texture wrinkles. After being washed 10 times, the fabric can still maintain the clear continuous regular texture wrinkle style. The fabric is soft, skin-friendly, breathable and smooth.
[0088] Example 3
[0089] Fabric: 82g / m 2 Silk Twill
[0090] The process for forming a washable controllable texture wrinkle comprises the following steps:
[0091] S1. Pretreatment of additives:
[0092] The fabric is dipped into a 40g / L polyurethane solution with a liquid rate of 80%, and then the dipped or soaked fabric is dried with hot air at 100°C for 5 minutes.
[0093] S2. Embroidery wrinkle treatment:
[0094] Place the fabric between the upper and lower layers of polyester shrinkable film, use program-controlled embroidery equipment and polyvinyl alcohol thread to embroider the fabric and the upper and lower shrinkable films in an interval manner with a needle spacing of 0.5 cm in warp and weft and an area of 5 cm*5 cm, and shrink them in an oven at 140℃ for 2 minutes.
[0095] S3, machine pressing treatment:
[0096] The fabric after embroidery shrinkage in step S2 is pressed at a pressure of 0.1 MPa, a temperature of 140° C., and a speed of 10 m / min to remove the embroidery thread and the shrinkable film.
[0097] S4, shaping process:
[0098] The fabric after the pressing treatment in step S3 is dipped into the post-setting liquid for secondary heating and setting treatment, the liquid carrying rate is controlled at 80%, the setting liquid temperature is controlled at 60°C, the setting treatment time is 10 minutes, and then washed and dried, the wrinkled parts on the fabric are set into permanent wrinkles.
[0099] The setting liquid contains 5g / L of penetrant, 20g / L of inorganic metal salt and 2g / L of alkali agent.
[0100] S4, washing treatment:
[0101] The fabric was washed with a washing solution containing 5g / L of soaping agent sodium stearate and 2g / L of anti-ash oil GD-62 at a washing temperature of 30°C for 30 minutes. After washing, the fabric was rinsed three times with room temperature tap water.
[0102] S5. Dyeing treatment:
[0103] Ordinary acid stain.
[0104] The surface of the finished fabric of Example 3 forms clear and natural continuous regular texture wrinkles. After being washed 10 times, the fabric can still maintain a good continuous regular texture wrinkle style. The fabric is soft, skin-friendly, breathable and smooth.
[0105] Example 4
[0106] Fabric: Silk electrospun (weight 65g / m 2 )
[0107] The process for forming a washable controllable texture wrinkle comprises the following steps:
[0108] S1. Pretreatment of additives:
[0109] The fabric is dipped into a 0.5 g / L polyurethane solution with a liquid rate of 80%, and then the fabric after the padding or soaking treatment is steam-heated at 100°C for 5 minutes.
[0110] S2. Embroidery wrinkle treatment:
[0111] Place the fabric between the upper and lower layers of polyester shrinkable film, use program-controlled embroidery equipment and polyvinyl alcohol thread to embroider the fabric and the upper and lower shrinkable films in an interval manner with a needle spacing of 0.5 cm in warp and weft and an area of 5 cm*5 cm, and shrink them in an oven at 140℃ for 2 minutes.
[0112] S3, machine pressing treatment:
[0113] The fabric after embroidery shrinkage in step S2 is pressed at a pressure of 0.5 MPa, a temperature of 140° C., and a speed of 20 m / min to remove the embroidery thread and the shrinkable film.
[0114] S4, shaping process:
[0115] The fabric after the pressing treatment in step S3 is dipped into the post-setting liquid for secondary heating and setting treatment, the liquid carrying rate is controlled at 80%, the setting liquid temperature is controlled at 40°C, the setting treatment time is 20 minutes, and then washed and dried, and the wrinkled parts on the fabric are set into permanent wrinkles.
[0116] The setting liquid contains 20g / L of penetrant, 50g / L of inorganic metal salt and 20g / L of alkali agent.
[0117] S4, washing treatment:
[0118] The fabric was washed with a washing solution containing 5g / L of soaping agent sodium stearate and 2g / L of anti-ash oil GD-62 at a washing temperature of 30°C for 30 minutes. After washing, the fabric was rinsed three times with room temperature tap water.
[0119] S5. Dyeing treatment:
[0120] Ordinary acid stain.
[0121] The surface of the finished fabric of Example 4 forms clear and natural continuous regular texture wrinkles. After being washed 10 times, the fabric can still maintain the clear continuous regular texture wrinkle style. The fabric is soft, skin-friendly, breathable and smooth.
[0122] Example 5
[0123] Fabric: Silk electrospun (weight 82g / m 2 )
[0124] The process for forming a washable controllable texture wrinkle comprises the following steps:
[0125] S1. Pretreatment of additives:
[0126] The fabric is dipped into a 100 g / L polyurethane solution with a liquid rate of 80%, and then the fabric after the padding or soaking treatment is steam-heated at 130°C for 10 minutes.
[0127] S2. Embroidery wrinkle treatment:
[0128] Place the fabric between the upper and lower layers of polyester shrinkable film, use program-controlled embroidery equipment and polyvinyl alcohol thread to embroider the fabric and the upper and lower shrinkable films in an interval manner with a needle spacing of 0.5 cm in warp and weft and an area of 5 cm*5 cm, and shrink them in an oven at 140℃ for 2 minutes.
[0129] S3, machine pressing treatment:
[0130] The fabric after embroidery shrinkage in step S2 is pressed at a pressure of 0.5 MPa, a temperature of 140° C., and a speed of 20 m / min to remove the embroidery thread and the shrinkable film.
[0131] S4, shaping process:
[0132] The fabric after the pressing treatment in step S3 is dipped into the post-setting liquid for secondary heating and setting treatment, the liquid carrying rate is controlled at 80%, the setting liquid temperature is controlled at 60°C, the setting treatment time is 30 minutes, and then washed and dried, the wrinkled parts on the fabric are set into permanent wrinkles.
[0133] The setting liquid contains 0.5g / L of penetrant, 0.1g / L of inorganic metal salt and 0.5g / L of alkali agent.
[0134] S4, washing treatment:
[0135] The fabric was washed with a washing solution containing 5g / L of soaping agent sodium stearate and 2g / L of anti-ash oil GD-62 at a washing temperature of 30°C for 30 minutes. After washing, the fabric was rinsed three times with room temperature tap water.
[0136] S5. Dyeing treatment:
[0137] Ordinary acid stain.
[0138] The surface of the finished fabric of Example 5 forms clear and natural continuous regular texture wrinkles. After being washed 10 times, the fabric can still maintain a relatively shallow continuous regular texture wrinkle style, but there is a tendency for the texture to fade. The fabric is soft, skin-friendly, breathable and smooth.
[0139] Example 6
[0140] Fabric: Silk electrospun (weight 90g / m 2 )
[0141] The process for forming a washable controllable texture wrinkle comprises the following steps:
[0142] S1. Pretreatment of additives:
[0143] The fabric is dipped into a 10g / L polyurethane solution with a liquid rate of 80%, and then the fabric after the padding or soaking treatment is steam-heated at 130°C for 5 minutes.
[0144] S2. Embroidery wrinkle treatment:
[0145] Using program-controlled embroidery equipment and polyvinyl alcohol thread, the fabric is dotted with embroidery at a needle spacing of 2.0 cm in the weft direction and 10 cm in the warp direction. Then 1 / 3 of the total length is manually pulled out and treated at 140°C for 1 min using a pressing machine.
[0146] S3, machine pressing treatment:
[0147] The fabric after embroidery shrinkage in step S2 is pressed at a pressure of 0.5 MPa, a temperature of 140° C., and a speed of 20 m / min to remove the embroidery thread.
[0148] S4, shaping process:
[0149] The fabric after the pressing treatment in step S3 is dipped into the post-setting liquid for secondary heating and setting treatment, the liquid carrying rate is controlled at 80%, the setting liquid temperature is controlled at 100°C, the setting treatment time is 10 minutes, and then it is washed and dried, and the wrinkled parts on the fabric are set into permanent wrinkles.
[0150] The setting liquid contains 2g / L of penetrant, 10g / L of inorganic metal salt and 1g / L of alkali agent.
[0151] S4, washing treatment:
[0152] The fabric was washed with a washing solution containing 5g / L of soaping agent sodium stearate and 2g / L of anti-ash oil GD-62 at a washing temperature of 30°C for 30 minutes. After washing, the fabric was rinsed three times with room temperature tap water.
[0153] S5. Dyeing treatment:
[0154] Ordinary acid stain.
[0155] The surface of the finished fabric of Example 6 forms clear and natural continuous regular texture wrinkles. The fabric can still maintain the clear continuous regular texture wrinkle style after being washed 10 times. The fabric is soft, skin-friendly, breathable and smooth.
[0156] Example 7
[0157] Fabric: Silk electrospun (weight 108g / m 2 )
[0158] The process for forming a washable controllable texture wrinkle comprises the following steps:
[0159] S1. Pretreatment of additives:
[0160] The fabric is dipped into a 60g / L polyurethane solution with a liquid rate of 80%, and then the dipped or soaked fabric is hot-air dried at 130°C for 2 minutes.
[0161] S2. Embroidery wrinkle treatment:
[0162] Place the fabric between the upper and lower layers of polyester shrinkable film, use program-controlled embroidery equipment and polyvinyl alcohol thread to embroider the fabric and the upper and lower shrinkable films in an interval manner with a needle spacing of 0.5 cm in warp and weft and an area of 5 cm*5 cm, and shrink them in an oven at 140℃ for 2 minutes.
[0163] S3, machine pressing treatment:
[0164] The fabric after embroidery shrinkage in step S2 is pressed at a pressure of 0.5 MPa, a temperature of 140° C., and a speed of 20 m / min to remove the embroidery thread and the shrinkable film.
[0165] S4, shaping process:
[0166] The fabric after the pressing treatment in step S3 is dipped into the post-setting liquid for secondary heating and setting treatment, the liquid carrying rate is controlled at 80%, the setting liquid temperature is controlled at 30°C, the setting treatment time is 30 minutes, and then washed and dried, and the wrinkled parts on the fabric are set into permanent wrinkles.
[0167] The setting liquid contains 15g / L of penetrant, 40g / L of inorganic metal salt and 10g / L of alkali agent.
[0168] S4, washing treatment:
[0169] The fabric was washed with a washing solution containing 5g / L of soaping agent sodium stearate and 2g / L of anti-ash oil GD-62 at a washing temperature of 30°C for 30 minutes. After washing, the fabric was rinsed three times with room temperature tap water.
[0170] S5. Dyeing treatment:
[0171] Ordinary acid stain.
[0172] The surface of the finished fabric of Example 7 forms clear and natural continuous regular texture wrinkles. After being washed 10 times, the fabric can still maintain the clear continuous regular texture wrinkle style. The fabric is soft, skin-friendly, breathable and smooth.
[0173] Comparative Example 1
[0174] Comparative Example 1 is a comparative test example of Example 1, and the difference between it and Example 1 is that:
[0175] The S4-setting treatment step is missing in this comparative example.
[0176] Although continuous and regular texture wrinkles are formed on the surface of the finished fabric of Comparative Example 1, the wrinkles are unclear and unnatural, the folds are shallow, and it is not suitable for washing. After washing once, the texture wrinkles disappear and the fabric surface becomes smooth.
[0177] Comparative Example 2
[0178] Comparative Example 2 is a comparative test example of Example 1, and the difference between it and Example 1 is that:
[0179] The S1-auxiliary agent pre-treatment step is missing in this comparative example.
[0180] The surface of the finished fabric of Comparative Example 2 cannot form continuous and regular texture wrinkles, or the continuous and regular texture wrinkles formed are unclear, unnatural, and the folds are shallow. Moreover, after washing once, the texture wrinkles disappear and the fabric surface becomes smooth.
[0181] Figure 1 A is a physical picture of the finished fabric obtained in Example 1, on which evenly distributed, clear, natural, continuous and regular texture wrinkles are formed, and the creases are clear, obvious and natural. Figure 1 B is a real picture of the finished fabric obtained in Example 1 after being washed 10 times. Although the creases of the texture wrinkles of the fabric become lighter after being washed 10 times, the fabric can still maintain a continuous and regular texture wrinkle style.
[0182] Figure 2 A is a physical picture of the finished fabric obtained in Comparative Example 1. Although continuous and regular texture wrinkles are formed on the fabric, the wrinkles are unclear and unnatural, the folds are shallow, and it is not suitable for washing. Figure 2 B is a real picture of the finished fabric prepared in comparative example 1 after being washed once. After washing once, the texture wrinkles on the fabric disappear and the fabric surface becomes smooth.
[0183] In Comparative Example 1, only the fabric is pre-treated with an auxiliary agent and then subjected to a wrinkle pressing treatment. Although continuous and regular texture wrinkles can be formed on the fabric, since the wrinkles formed on the fabric are not subjected to a shaping treatment, the wrinkles formed on the fabric cannot be effectively maintained during subsequent washing and dyeing treatments. Therefore, although continuous and regular texture wrinkles are formed on the finished fabric prepared in Comparative Example 1, the wrinkles are not clear, the creases are shallow, and the fabric is not resistant to water washing. After washing once, the texture wrinkles on the fabric disappear and the fabric surface becomes smooth.
[0184] Figure 3 A is the finished fabric surface of comparative example 2, which cannot form continuous and regular texture wrinkles or the formed texture wrinkles are unclear, uneven, and the creases are shallow. Figure 3 B is a real picture of the finished fabric obtained in Comparative Example 2 after being washed once. After washing once, the wrinkled part of the texture on the fabric disappears and the texture is not obvious.
[0185] In Comparative Example 2, the fabric was not pre-treated with auxiliary agents, and the fabric was directly subjected to embroidery wrinkling, machine pressing and shaping treatment. Because the fabric is relatively soft, the embroidery wrinkling treatment was directly performed. Although wrinkles can be formed on the surface of the fabric, even after the shaping treatment, the wrinkles on the fabric are relatively easy to recover, especially after subsequent washing and dyeing treatments, resulting in the wrinkles on the fabric cannot be effectively maintained. Therefore, the texture wrinkles formed on the finished fabric prepared in Comparative Example 2 are unclear and unnatural, the folds are shallow, and it is not resistant to washing. After washing once, the texture wrinkles on the fabric disappear and the cloth surface becomes smooth.
[0186] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A washable, controllable texture wrinkle silk or silk-containing fabric, characterized in that: Continuous regular texture wrinkles are distributed on the surface of the silk or silk-containing fabric, and the continuous regular texture wrinkles have water washing shape retention properties.
2. The washable controllable texture wrinkle silk or silk-containing fabric according to claim 1, characterized in that: The continuous regular texture wrinkles are distributed in one or more of line, pattern, and pattern shapes.
3. The washable, texture-controlled wrinkle-resistant silk or silk-containing fabric according to claim 2, characterized in that: The distribution state of the continuous regular texture wrinkles is one or more of continuous, discontinuous, articulated, and cross distribution.
4. The washable controllable texture wrinkle silk or silk-containing fabric according to claim 1, characterized in that: The silk or silk-containing fabrics include 100% silk fabrics, silk interwoven fabrics with a silk content of more than 30%, or silk blended fabrics.
5. A process for preparing the washable controllable texture wrinkle silk or silk-containing fabric according to any one of claims 1 to 4, characterized in that: The steps include: S1. Pretreatment of additives: The silk or silk-containing fabric is padded or soaked in an auxiliary agent solution, and then the padded or soaked fabric is subjected to a heating and setting treatment; The mass content of the additive in the additive solution is 0.5-100 g / L, and the additive is one or more of polyurethane, polycarbonate, and silicone additive; S2. Embroidery wrinkle treatment: Embroidering the silk or silk-containing fabric processed in step S1, and shrinking and wrinkling the embroidery area to form regular texture wrinkles on the surface of the fabric; S3, machine pressing treatment: The fabric that has shrunk after embroidery in step S2 is subjected to pressing treatment. S4, shaping process: The silk or silk-containing fabric subjected to the pressing treatment in step S3 is rolled or soaked in a post-setting liquid for secondary heating and setting treatment, and then washed with water and dried to set the wrinkled parts on the fabric into permanent wrinkles; The setting liquid contains a penetrant, an inorganic metal salt and an alkali agent.
6. The process for preparing the washable controllable texture wrinkle silk or silk-containing fabric according to claim 5, characterized in that: In step S2, embroidery is directly performed on the fabric or the fabric is placed between two layers of shrinkable films and then embroidered, and the fabric is shrunk by drawing threads or controlling the shrinkage of the film to form regular texture wrinkles.
7. The process for preparing the washable controllable texture wrinkle silk or silk-containing fabric according to claim 6, characterized in that: The shrinkable film is made of polyester, polyamide, polyethylene, polypropylene, polybutylene or polyvinyl chloride. The shrinkage of the film is controlled by heating, with a shrinking temperature of 90 to 180° C. and a shrinking time of 0.1 to 10 minutes.
8. The process for preparing the washable controllable texture wrinkle silk or silk-containing fabric according to claim 5, characterized in that: In the step S4, the mass content of the penetrant is 0.5-20 g / L, the mass content of the inorganic metal salt is 0.1-50 g / L, and the mass content of the alkali agent is 0.5-20 g / L.
9. The process for preparing the washable controllable texture wrinkle silk or silk-containing fabric according to claim 5, characterized in that: In step S1, the primary heating and shaping treatment adopts steam heating and shaping or hot air shaping; the treatment temperature of steam heating and shaping is 100-140° C., and the treatment time is 1-60 minutes; the treatment temperature of hot air shaping is 100-140° C., and the treatment time is 1-5 minutes.
10. The process for preparing the washable controllable texture wrinkle silk or silk-containing fabric according to claim 5, characterized in that: In step S4, the temperature of the secondary heating and shaping treatment is set to 30-100° C., and the treatment time is 10-60 minutes.
11. The process for preparing the washable controllable texture wrinkle silk or silk-containing fabric according to claim 5, characterized in that: In step S3, the pressure of the pressing treatment is 0.1-1.0 MPa, the temperature is 120-180° C., and the speed is 10-100 m / min.
12. The process for preparing the washable wrinkled silk or silk-containing fabric according to claim 5, characterized in that: After the shaping treatment, the silk or silk-containing fabric is post-treated, and the post-treatment process includes washing, dyeing and finishing.
13. An application of washable, controllable texture wrinkle silk or silk-containing fabric, characterized in that: The washable controllable texture wrinkle silk or silk-containing fabric according to any one of claims 1 to 4 is used for processing clothing, underwear and home textile products.