Selective atomic layer deposition method
By setting a patterned metal layer on the substrate surface and forming a barrier layer using self-assembled molecular layer material, multiple cycles are performed to achieve selective deposition of metal oxides, the problem of traditional low selectivity is solved and the selectivity is improved Selectivity of atomic layer deposition and uniformity of material deposition.
Patent Information
- Application Number
- CN202411587405.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-08
- Publication Date
- 2024-12-20
AI Technical Summary
The traditional regioselective atomic layer deposition method has low selectivity and it is difficult to achieve high selectivity material deposition.
By providing a patterned metal layer on the substrate surface and forming a barrier layer using self-assembled molecular layer material, multiple cycles are performed to achieve selective deposition of metal oxides and removal of barrier layers, ensuring that the Barrier layer growth mass consistency and stability, thereby improving the selectivity of selective atomic layer deposition.
This method effectively improves the selectivity of selective atomic layer deposition, reduces surface damage and impurity contamination problems of barrier layers, achieves a good barrier effect and selective deposition, and improves the uniformity and conformity of material deposition.
Smart Images

Figure CN119162565A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of atomic layer deposition, and in particular to a selective atomic layer deposition method. Background Art
[0002] Atomic layer deposition (ALD) occurs by alternately injecting two or more precursors into a chamber for chemical reaction, in which the substrate is placed at a given temperature and pressure to deposit the material layer by layer on the surface of the substrate. Atomic layer deposition enables the preparation of highly conformal and highly uniform thin films. Among them, area-selective atomic layer deposition (AS-ALD) is a method of selective atomic layer deposition that controls the difference in the chemical properties of the surface to be deposited so that some areas can react with the precursor molecules while some areas are inert.
[0003] However, conventional area-selective atomic layer deposition methods suffer from low selectivity. Summary of the invention
[0004] Based on this, it is necessary to provide a selective atomic layer deposition method that can improve the selectivity of selective atomic layer deposition.
[0005] The present application provides a selective atomic layer deposition method, comprising the following steps:
[0006] Providing a substrate, wherein a patterned metal layer is disposed on a surface of the substrate;
[0007] performing a first cycle treatment on the substrate for multiple times;
[0008] The first cycle process comprises the following steps:
[0009] Using a self-assembled molecular layer material to form a barrier layer on the surface of the metal layer;
[0010] Depositing a metal oxide layer on the surface of the substrate not covered by the metal layer;
[0011] The barrier layer is removed.
[0012] In some embodiments, the self-assembled molecular layer material includes a benzene-containing self-assembled molecular material.
[0013] In some embodiments, the self-assembled molecular layer material includes 3,5-bis(trifluoromethyl)thiophenol.
[0014] In some embodiments, the substrate includes at least one of a silicon substrate, a silicon oxide substrate, a silicon nitride substrate, and a titanium dioxide substrate.
[0015] In some embodiments, the metal layer includes at least one of copper and cobalt.
[0016] In some embodiments, the metal oxide comprises aluminum oxide.
[0017] In some embodiments, the first cycle treatment is performed 7 to 12 times.
[0018] In some embodiments, the barrier layer has a thickness of 2 nm to 4 nm.
[0019] In some embodiments, forming a barrier layer on the surface of the metal layer using a self-assembled molecular layer material comprises the following steps:
[0020] The substrate is subjected to a second cycle treatment for multiple times, wherein the second cycle treatment comprises the following steps:
[0021] The temperature of the reaction chamber is maintained at a preset temperature, and the self-assembled molecular layer material is introduced into the reaction chamber under the action of a first carrier gas;
[0022] The first protective gas is used to purge the remaining self-assembled molecular layer material in the reaction chamber.
[0023] In some embodiments, the self-assembled molecular layer material includes a benzene-containing self-assembled molecular material.
[0024] In some embodiments, the preset temperature is 110°C to 150°C.
[0025] In some embodiments, the flow rate of the first carrier gas is 2 sccm~10 sccm.
[0026] In some embodiments, the first carrier gas is introduced for a time of 0.5 s to 1 s.
[0027] In some embodiments, the vacuum degree of the reaction chamber after the self-assembled molecular layer material is introduced is 140Pa-150Pa.
[0028] In some embodiments, the flow rate of the first protective gas is 150 sccm-250 sccm.
[0029] In some embodiments, the first protective gas is introduced for 5s to 10s.
[0030] In some embodiments, the second cycle treatment is performed 10 to 20 times.
[0031] In some embodiments, depositing a metal oxide layer on the surface of the substrate not covered by the metal layer comprises the following steps:
[0032] The substrate after forming the barrier layer is subjected to a third cycle treatment for multiple times, wherein the third cycle treatment comprises the following steps:
[0033] The temperature of the reaction chamber is maintained at the preset temperature, and a metal source is introduced into the reaction chamber under the action of a second carrier gas;
[0034] Using a second protective gas to purge the remaining metal source in the reaction chamber;
[0035] introducing an oxygen source into the reaction chamber;
[0036] The remaining oxygen source in the reaction chamber is purged using a third protective gas.
[0037] In some embodiments, the flow rate of the second carrier gas is 60 sccm-100 sccm.
[0038] In some embodiments, the introduction time of the second carrier gas is 0.5s~2s.
[0039] In some embodiments, after the metal source is introduced, the vacuum degree of the reaction chamber is 180Pa~190Pa.
[0040] In some embodiments, the metal source includes dimethylaluminum isopropoxide.
[0041] In some embodiments, the flow rate of the second protective gas is 150 sccm-250 sccm.
[0042] In some embodiments, the introduction time of the second protective gas is 2s to 8s.
[0043] In some embodiments, the oxygen source comprises ultrapure water.
[0044] In some embodiments, the oxygen source is introduced for a time of 0.5 s to 1 s.
[0045] In some embodiments, after the oxygen source is introduced, the vacuum degree of the reaction chamber is 250Pa~260Pa.
[0046] In some embodiments, the flow rate of the third protective gas is 150 sccm-250 sccm.
[0047] In some embodiments, the third protective gas is introduced for 5s to 15s.
[0048] In some embodiments, the third cycle treatment is performed for 15 to 25 times.
[0049] In some embodiments, removing the barrier layer comprises the following steps:
[0050] introducing a hydrogen source into the reaction chamber;
[0051] The hydrogen source generates hydrogen plasma, and the barrier layer is removed by the hydrogen plasma.
[0052] In some embodiments, the following steps are further included before the substrate is subjected to multiple first cycle treatments:
[0053] The substrate is plasma cleaned.
[0054] In the above-mentioned selective atomic layer deposition method, selective deposition is performed through the first cycle treatment. In a single first cycle treatment, a barrier layer is formed on the surface of the metal layer using a self-assembled molecular layer (SAMs) material, which enables the metal oxide to be selectively deposited on the surface of the substrate not covered by the self-assembled molecular layer material. At the same time, after completing the selective deposition of the metal oxide in one cycle, the barrier layer is removed, and then a new barrier layer is prepared in the next cycle of the first cycle treatment. This selective atomic layer deposition method can reduce the problem of surface damage or the introduction of impurities and contamination in the barrier layer, and can achieve consistency and stability in the growth quality of the barrier layer in each first cycle treatment cycle, thereby making the barrier layer have a better barrier effect and improving the selectivity of the selective atomic layer deposition. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] FIG1 is a schematic diagram of a selective atomic layer deposition method according to an embodiment of the present application;
[0056] Figure 2 is a schematic diagram of the results of Auger electron spectroscopy characterization of the sample after deposition in Example 1 of the present application, wherein a in Figure 2 is a schematic diagram of the results of Al element characterization, and b in Figure 2 is a schematic diagram of the results of Cu element characterization. DETAILED DESCRIPTION
[0057] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0058] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0059] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0060] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of this application, "plurality" means at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0061] 1 , an embodiment of the present application provides a selective atomic layer deposition method, comprising the following steps:
[0062] Providing a substrate, wherein a patterned metal layer is disposed on a surface of the substrate;
[0063] performing a first cycle treatment on the substrate multiple times;
[0064] The first cycle processing includes the following steps:
[0065] Using a self-assembled molecular layer material to form a barrier layer on the surface of the metal layer;
[0066] Depositing a metal oxide layer on the surface of the substrate not covered by the metal layer;
[0067] Remove the barrier layer.
[0068] In the above-mentioned selective atomic layer deposition method, selective deposition is performed through a first cycle treatment. In a single first cycle treatment, a barrier layer is formed on the surface of the metal layer using a self-assembled molecular layer material, which enables metal oxide to be selectively deposited on the surface of the substrate not covered by the self-assembled molecular layer material. At the same time, after completing the selective deposition of metal oxide in one cycle, the barrier layer is removed, and a new barrier layer is prepared in the next cycle of the first cycle treatment. The selective atomic layer deposition method can reduce the problem of surface damage or the introduction of impurities and contamination in the barrier layer, and can achieve consistency and stability in the growth quality of the barrier layer in each first cycle treatment cycle, thereby making the barrier layer have a better barrier effect and improving the selectivity of the selective atomic layer deposition.
[0069] In some embodiments, the self-assembled molecular layer material includes a benzene-containing self-assembled molecular material.
[0070] Benzene-containing self-assembled molecular materials have the following advantages:
[0071] 1. Structural stability: The conjugated structure of the benzene ring makes the molecules tightly arranged and has a strong π-π interaction, which can increase the mechanical strength and thermal stability of the monomolecular barrier layer. The chemical stability of the benzene ring is more stable than the chain-like SAMs structure, and SAMs are more difficult to be oxidized and inactivated during the reaction process.
[0072] 2. Excellent molecular arrangement: The planar structure of the benzene ring helps the SAMs material molecules to form a regular and orderly arrangement on the substrate surface, reducing the generation of defects and improving surface uniformity. At the same time, the interaction between the benzene rings can accurately control the molecular spacing, thereby optimizing the thickness and electrical properties of the barrier layer.
[0073] 3. Adjustable functions: The hydrogen atoms on the benzene ring can be replaced by different functional groups (such as amino, hydroxyl, nitro), giving the surface a variety of chemical functions. Self-assembled molecular materials containing benzene can reduce the free energy of the substrate surface, making its surface easier to combine with other materials and forming a stable barrier layer on the surface of the metal layer.
[0074] In some embodiments, the self-assembled molecular layer material includes 3,5-bis(trifluoromethyl)thiophenol.
[0075] In some embodiments, the substrate includes at least one of a silicon substrate, a silicon oxide substrate, a silicon nitride substrate, and a titanium dioxide substrate.
[0076] In some embodiments, the metal layer includes at least one of copper and cobalt.
[0077] In some embodiments, the metal oxide includes aluminum oxide.
[0078] In some embodiments, the number of first cycle treatments is 7 to 12 times.
[0079] Optionally, the number of times of the first cycle treatment is 7 times, 8 times, 9 times, 10 times, 11 times or 12 times. When the number of times of the first cycle treatment is too many, the effect of the selective deposition will decrease.
[0080] In some embodiments, the thickness of the barrier layer is 2 nm to 4 nm.
[0081] Within the above-mentioned thickness range of the barrier layer, a good barrier effect on metal oxides can be achieved, and the barrier layer can also be easily removed. Optionally, the thickness of the barrier layer is 2nm, 2.2nm, 2.4nm, 2.6nm, 2.8nm, 3nm, 3.2nm, 3.4nm, 3.6nm, 3.8nm or 4nm, or the thickness of the barrier layer can also be within the range between any two of the above thicknesses.
[0082] In some embodiments, forming a barrier layer on the surface of a metal layer using a self-assembled molecular layer material comprises the following steps:
[0083] The substrate is subjected to a plurality of second cycle treatments, wherein the second cycle treatments include the following steps:
[0084] The temperature of the reaction chamber is maintained at a preset temperature, and a self-assembled molecular layer material is introduced into the reaction chamber under the action of a first carrier gas;
[0085] The first protective gas is used to purge the remaining self-assembled molecular layer material in the reaction chamber.
[0086] In each cycle of the first cycle treatment, the barrier layer is prepared through multiple second cycle treatments, so that a better barrier layer can be prepared on the metal layer of the substrate. At the same time, the barrier layer is prepared directly in the reaction chamber of the selective atomic layer deposition. Compared with the traditional liquid phase method for growing SAMs, the above-mentioned barrier layer preparation method can be integrated with the steps of ALD preparation of metal oxides and removal of the barrier layer for easy operation. At the same time, it can also reduce the risk of damage or contamination of the barrier layer surface during the process of transferring the substrate to the reaction chamber after SAMs growth by the liquid phase method.
[0087] In some embodiments, the self-assembled molecular layer material includes a benzene-containing self-assembled molecular material.
[0088] In some embodiments, the preset temperature is 110°C to 150°C.
[0089] Optionally, the preset temperature is 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C or 150°C, or, the preset temperature may be within a range between any two of the above temperatures.
[0090] In some embodiments, the first carrier gas includes at least one of nitrogen, helium, and argon.
[0091] In some embodiments, the flow rate of the first carrier gas is 2 sccm-10 sccm.
[0092] Optionally, the flow rate of the first carrier gas is 2 sccm, 3 sccm, 4 sccm, 5 sccm, 6 sccm, 7 sccm, 8 sccm, 9 sccm or 10 sccm, or, the flow rate of the first carrier gas may also be within the range between any two of the above flow rates.
[0093] In some embodiments, the first carrier gas is introduced for a time period of 0.5 s to 1 s.
[0094] Optionally, the introduction time of the first carrier gas is 0.5s, 0.6s, 0.7s, 0.8s, 0.9s or 1s, or, the introduction time of the first carrier gas may also be within the range between any two of the above times.
[0095] In some embodiments, the vacuum degree of the reaction chamber is 140Pa-150Pa after the self-assembled molecular layer material is introduced.
[0096] Optionally, the vacuum degree of the reaction chamber after the self-assembled molecular layer material is introduced is 140Pa, 141Pa, 142Pa, 143Pa, 144Pa, 145Pa, 146Pa, 147Pa, 148Pa, 149Pa or 150Pa, or, the vacuum degree of the reaction chamber after the self-assembled molecular layer material is introduced can also be within the range between any two of the above vacuum degrees.
[0097] In some embodiments, the first protective gas includes at least one of nitrogen, helium, and argon.
[0098] In some embodiments, the flow rate of the first protective gas is 150 sccm-250 sccm.
[0099] Optionally, the flow rate of the first protective gas is 150 sccm, 160 sccm, 170 sccm, 180 sccm, 190 sccm, 200 sccm, 210 sccm, 220 sccm, 230 sccm, 240 sccm or 250 sccm, or, the flow rate of the first protective gas may be within the range between any two of the above flow rates.
[0100] In some embodiments, the first protective gas is introduced for 5s to 10s.
[0101] If the first protective gas is introduced for too short a time, it is difficult to purge the remaining self-assembled molecular layer material, which may result in physical adsorption residues on the substrate surface, which is not conducive to forming a dense coverage of the metal layer surface. Optionally, the first protective gas is introduced for 5s, 6s, 7s, 8s, 9s or 10s, or the first protective gas can also be introduced within the range between any two of the above times.
[0102] In some embodiments, the second cycle treatment is performed 10 to 20 times.
[0103] If the number of cycles of the second cycle treatment is too small, the quality of the self-assembled molecular layer will be affected, making it difficult to form a complete high-quality barrier layer on the surface of the metal layer. Optionally, the number of cycles of the second cycle treatment is 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20.
[0104] Within the above-mentioned parameter ranges of each second cycle treatment, a better barrier layer preparation effect can be achieved to achieve a better selective deposition effect of the metal oxide layer on the surface of the substrate not covered by the metal layer within a single cycle of the first cycle treatment.
[0105] In some embodiments, depositing a metal oxide layer on the surface of the substrate not covered by the metal layer comprises the following steps:
[0106] The substrate after forming the barrier layer is subjected to a third cycle treatment for multiple times, and the third cycle treatment includes the following steps:
[0107] The temperature of the reaction chamber is maintained at a preset temperature, and a metal source is introduced into the reaction chamber under the action of a second carrier gas;
[0108] Using a second protective gas to purge the remaining metal source in the reaction chamber;
[0109] introducing an oxygen source into the reaction chamber;
[0110] The third protective gas is used to purge the remaining oxygen source in the reaction chamber.
[0111] The metal source and the oxygen source are sequentially introduced in a pulsed manner to form a metal oxide layer on the surface of the substrate not covered by the metal layer. The second protective gas and the third protective gas are used for purging respectively to clean the remaining precursors and byproducts in the reaction chamber to achieve a better metal oxide deposition effect.
[0112] In some embodiments, the second carrier gas includes at least one of nitrogen, helium, and argon.
[0113] In some embodiments, the flow rate of the second carrier gas is 60 sccm-100 sccm.
[0114] Optionally, the flow rate of the second carrier gas is 60 sccm, 65 sccm, 70 sccm, 75 sccm, 80 sccm, 85 sccm, 90 sccm, 95 sccm or 100 sccm, or, the flow rate of the second carrier gas may also be within the range between any two of the above flow rates.
[0115] In some embodiments, the second carrier gas is introduced for a time period of 0.5 s to 2 s.
[0116] Optionally, the introduction time of the second carrier gas is 0.5s, 0.7s, 1s, 1.2s, 1.5s, 1.7s or 2s, or, the introduction time of the second carrier gas may also be within the range between any two of the above times.
[0117] In some embodiments, the vacuum degree of the reaction chamber is 180Pa~190Pa after the metal source is introduced.
[0118] Optionally, the vacuum degree of the reaction chamber after the metal source is introduced is 180Pa, 181Pa, 182Pa, 183Pa, 184Pa, 185Pa, 186Pa, 187Pa, 188Pa, 189Pa or 190Pa, or, the vacuum degree of the reaction chamber after the metal source is introduced may also be within the range between any two of the above vacuum degrees.
[0119] In some embodiments, the metal source includes dimethylaluminum isopropoxide.
[0120] In some embodiments, the second protective gas includes at least one of nitrogen, helium, and argon.
[0121] In some embodiments, the flow rate of the second protective gas is 150 sccm-250 sccm.
[0122] Optionally, the flow rate of the second protective gas is 150 sccm, 160 sccm, 170 sccm, 180 sccm, 190 sccm, 200 sccm, 210 sccm, 220 sccm, 230 sccm, 240 sccm or 250 sccm, or, the flow rate of the second protective gas may be within the range between any two of the above flow rates.
[0123] In some embodiments, the second protective gas is introduced for a time of 2s to 8s.
[0124] Optionally, the introduction time of the second protective gas is 2s, 3s, 4s, 5s, 6s, 7s or 8s, or, the introduction time of the second protective gas may also be within the range between any two of the above times.
[0125] In some embodiments, the oxygen source comprises ultrapure water.
[0126] In some embodiments, the oxygen source is introduced for a time of 0.5 s to 1 s.
[0127] Optionally, the oxygen source is introduced for 0.5 s, 0.6 s, 0.7 s, 0.8 s, 0.9 s or 1 s, or the oxygen source is introduced for a time within a range between any two of the above times.
[0128] In some embodiments, the vacuum degree of the reaction chamber is 250Pa-260Pa after the oxygen source is introduced.
[0129] Optionally, the vacuum degree of the reaction chamber after the oxygen source is introduced is 250Pa, 251Pa, 252Pa, 253Pa, 254Pa, 255Pa, 256Pa, 257Pa, 258Pa, 259Pa or 260Pa, or, the vacuum degree of the reaction chamber after the oxygen source is introduced may also be within the range between any two of the above vacuum degrees.
[0130] In some embodiments, the third protective gas includes at least one of nitrogen, helium, and argon.
[0131] In some embodiments, the flow rate of the third protective gas is 150 sccm-250 sccm.
[0132] Optionally, the flow rate of the third protective gas is 150sccm, 160sccm, 170sccm, 180sccm, 190sccm, 200sccm, 210sccm, 220sccm, 230sccm, 240sccm or 250sccm, or, the flow rate of the third protective gas may be within the range between any two of the above flow rates.
[0133] In some embodiments, the third protective gas is introduced for 5s to 15s.
[0134] Optionally, the introduction time of the third protective gas is 5s, 6s, 7s, 8s, 9s, 10s, 11s, 12s, 13s, 14s or 15s, or, the introduction time of the third protective gas may also be within the range between any two of the above times.
[0135] In some embodiments, the third cycle treatment is performed 15 to 25 times.
[0136] Optionally, the number of cycles of the third cycle treatment is 15 times, 16 times, 17 times, 18 times, 19 times, 20 times, 21 times, 22 times, 23 times, 24 times or 25 times.
[0137] Within the parameter range of each third cycle treatment, a better deposition effect of the metal oxide layer can be achieved, so as to achieve a better selective deposition effect of the metal oxide layer on the surface of the substrate not covered by the metal layer within a single cycle of the first cycle treatment.
[0138] In some of these embodiments, the barrier layer is removed by hydrogen plasma treatment.
[0139] In some embodiments, removing the barrier layer comprises the following steps:
[0140] introducing a hydrogen source into the reaction chamber;
[0141] A hydrogen source is used to generate hydrogen plasma, and the barrier layer is removed by the hydrogen plasma.
[0142] The barrier layer can be removed more effectively by hydrogen plasma treatment. At the same time, hydrogen plasma has reducing properties, and can achieve a more thorough reduction and removal of the residual SAMs molecules on the surface of the metal layer. At the same time, the surface of the substrate not covered by the metal layer will not react with the hydrogen plasma because it is covered with a dense metal oxide layer. Furthermore, hydrogen plasma treatment can also generate active hydroxyl sites on the surface of the metal layer to achieve a better deposition effect of self-assembled molecules in the next first cycle of treatment.
[0143] In some embodiments, the following steps are further included before the substrate is subjected to multiple first cycle treatments:
[0144] The substrate is plasma cleaned.
[0145] In some embodiments, plasma cleaning the substrate includes:
[0146] The substrate is cleaned with hydrogen plasma.
[0147] Hydrogen plasma cleaning of the substrate can have a good cleaning effect on the surface of the substrate and reduce the residual impurities. At the same time, hydrogen plasma has a reducing property and can remove the oxide layer on the surface of the metal layer, so that the self-assembled molecular material has a better deposition effect on the surface of the metal layer.
[0148] The following are specific embodiments
[0149] Example 1
[0150] In this embodiment, aluminum oxide is prepared on a substrate by a selective atomic layer deposition method, including the following steps:
[0151] (1) Plasma cleaning of substrate
[0152] 1) Heat the cavity of the tubular ALD equipment, and the cavity heating temperature is 80℃~200℃;
[0153] 2) Place the substrate on the sample stage of the tubular ALD equipment. The substrate is a P100 silicon wafer with a 100nm thick patterned copper layer evaporated on the surface, and the sample stage is placed in the center of the tubular furnace;
[0154] 3) The mechanical pump of the tubular ALD equipment is turned on to evacuate the chamber until the vacuum degree of the chamber is below 3Pa;
[0155] 4) Keep the hydrogen source (composition is 10% H2 + 90% Ar by volume) in the closed state, set the flow rate of the hydrogen source part mass flow meter (MFC) to 500sccm, and exhaust the gas in the air path until the vacuum degree reaches below 5Pa;
[0156] 5) Open the valve of the hydrogen source part, set the flow rate of the mass flow meter (MFC) of the hydrogen source part to 80ccm, wait for 2 minutes until the gas pressure in the chamber is stable, and ensure that the pressure is around 160Pa;
[0157] 6) Turn on the plasma power supply and matching device, set the power at 100W~400W, and continuously introduce hydrogen for 10 minutes. Under the action of the RF power supply, inductive coupling occurs in the inductor coil part to generate H plasma, and plasma cleaning is achieved on the substrate surface.
[0158] (2) Using self-assembled molecular layer materials to form a barrier layer on the surface of the metal layer
[0159] 1) Heat the pipeline, cavity and source bottle of the tubular ALD equipment to the preset temperature, where the pipeline temperature is 80°C, the cavity temperature is 130°C, and the source bottle temperature is 50°C;
[0160] 2) Keep the mechanical pump turned on and evacuate the cavity until the vacuum degree reaches below 3Pa;
[0161] 3) Keep the substrate inside the chamber and introduce 50 sccm of N2 during the heating process until the temperature stabilizes;
[0162] 4) Open the needle valve of the source bottle of the self-assembled molecular layer material;
[0163] 5) Under the action of carrier gas, 3,5-bis(trifluoromethyl)thiophenol was introduced into the tubular ALD reaction chamber for 0.5 s, with a carrier gas flow rate of 5 sccm. After the introduction of 3,5-bis(trifluoromethyl)thiophenol, the vacuum degree was 140 Pa~150 Pa;
[0164] 6) N2 was introduced to purge the unreacted 3,5-bis(trifluoromethyl)thiophenol for 5 s at a purge flow rate of 200 sccm;
[0165] 7) After 10 cycles of deposition, the barrier layer is grown and a self-assembled monolayer of about 2 nm grows on the surface of the metal layer.
[0166] (3) Depositing a metal oxide layer on the surface of the substrate not covered by the metal layer
[0167] 1) Keep the substrate inside the chamber and introduce 50 sccm of N2 during the heating process until the pressure is stable;
[0168] 2) Open the needle valves of the metal source and oxygen source bottles;
[0169] 3) Under the action of N2 carrier gas, dimethyl isopropoxyaluminum with a metal source is introduced into the tubular ALD reaction chamber for 1 second, the carrier gas flow rate is 80 sccm, and the vacuum degree is 180Pa~190Pa after the metal source is introduced;
[0170] 4) Introduce 200 sccm of N2 to purge the unreacted metal source and by-products for 5 seconds;
[0171] 5) Introduce oxygen source ultrapure water, the flow rate is set to 50sccm, and the vacuum degree is 250Pa~260Pa after the oxygen source is introduced;
[0172] 6) Introduce 200 sccm of N2 to purge the unreacted oxygen source and by-products for 10 s;
[0173] 7) The deposition rate is 0.6Å / cycle~0.7Å / cycle, and the deposition is repeated for 20 cycles.
[0174] (4) Removing the barrier layer
[0175] 1) Keep the substrate inside the chamber and introduce 50 sccm of N2 during the heating process until the pressure is stable;
[0176] 2) Keep the hydrogen source (10% H2 + 90% Ar by volume) in the closed state, set the flow rate of the hydrogen source mass flow meter (MFC) to 500sccm, and exhaust the gas in the air path until the vacuum degree reaches below 5Pa;
[0177] 3) Open the valve of the hydrogen source part, set the flow rate of the mass flow meter (MFC) of the hydrogen source part to 80sccm, wait for 2 minutes until the gas pressure in the chamber is stable, and ensure that the pressure is within 160Pa;
[0178] 4) Turn on the plasma power supply and matching device, set the power at 300W, and continuously introduce hydrogen for 3 minutes. The inductive coupling occurs in the inductor coil to generate H plasma, which removes the barrier layer on the copper surface.
[0179] (5) Repeat steps (2) to (4) 12 times.
[0180] The result of Auger electron spectroscopy characterization of the substrate after aluminum oxide was prepared by the selective atomic layer deposition method in Example 1 is shown in Figure 2, where a in Figure 2 is a schematic diagram of the result of Al element characterization, and b in Figure 2 is a schematic diagram of the result of Cu element characterization. It can be seen that highly selective atomic layer deposition of aluminum oxide is achieved in Example 1. According to the results of Auger electron spectroscopy characterization, it can be calculated that the selectivity of aluminum oxide prepared on the substrate by the selective atomic layer deposition method in Example 1 can reach 92.4%.
[0181] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0182] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims, and the description and drawings may be used to interpret the contents of the claims.
Claims
1. A selective atomic layer deposition method, It is characterized in that The steps include: Providing a substrate, wherein a patterned metal layer is disposed on a surface of the substrate; performing a first cycle treatment on the substrate for multiple times; The first cycle process comprises the following steps: Using a self-assembled molecular layer material to form a barrier layer on the surface of the metal layer; Depositing a metal oxide layer on the surface of the substrate not covered by the metal layer; The barrier layer is removed.
2. The selective atomic layer deposition method according to claim 1, It is characterized in that The self-assembled molecular layer material comprises a benzene-containing self-assembled molecular material.
3. The selective atomic layer deposition method according to claim 2, It is characterized in that The self-assembled molecular layer material includes 3,5-bis(trifluoromethyl)thiophenol.
4. The selective atomic layer deposition method according to claim 1, It is characterized in that The substrate comprises at least one of a silicon substrate, a silicon oxide substrate, a silicon nitride substrate and a titanium dioxide substrate; and / or, The metal layer comprises at least one of copper and cobalt; and / or, The metal oxide comprises aluminum oxide; and / or, The number of times of the first cycle treatment is 7 to 12 times; and / or, The thickness of the barrier layer is 2nm~4nm.
5. The selective atomic layer deposition method according to claim 1, It is characterized in that Forming a barrier layer on the surface of the metal layer using a self-assembled molecular layer material comprises the following steps: The substrate is subjected to a second cycle treatment for multiple times, wherein the second cycle treatment comprises the following steps: The temperature of the reaction chamber is maintained at a preset temperature, and the self-assembled molecular layer material is introduced into the reaction chamber under the action of a first carrier gas; The first protective gas is used to purge the remaining self-assembled molecular layer material in the reaction chamber.
6. The selective atomic layer deposition method according to claim 5, It is characterized in that The self-assembled molecular layer material includes a benzene-containing self-assembled molecular material; and / or, The preset temperature is 110°C to 150°C; and / or, The flow rate of the first carrier gas is 2 sccm to 10 sccm; and / or, The first carrier gas is introduced for a time of 0.5s to 1s; and / or, After the self-assembled molecular layer material is introduced, the vacuum degree of the reaction chamber is 140Pa-150Pa; and / or, The flow rate of the first protective gas is 150 sccm to 250 sccm; and / or, The first protective gas is introduced for 5s to 10s; and / or The number of cycles of the second cycle treatment is 10 to 20 times.
7. The selective atomic layer deposition method according to claim 5, It is characterized in that Depositing a metal oxide layer on the surface of the substrate not covered by the metal layer comprises the following steps: The substrate after forming the barrier layer is subjected to a third cycle treatment for multiple times, wherein the third cycle treatment comprises the following steps: The temperature of the reaction chamber is maintained at the preset temperature, and a metal source is introduced into the reaction chamber under the action of a second carrier gas; Using a second protective gas to purge the remaining metal source in the reaction chamber; introducing an oxygen source into the reaction chamber; The remaining oxygen source in the reaction chamber is purged using a third protective gas.
8. The selective atomic layer deposition method according to claim 7, It is characterized in that The flow rate of the second carrier gas is 60 sccm to 100 sccm; and / or, The second carrier gas is introduced for a time of 0.5s to 2s; and / or, After the metal source is introduced, the vacuum degree of the reaction chamber is 180Pa-190Pa; and / or, The metal source comprises dimethyl isopropoxide aluminum; and / or, The flow rate of the second protective gas is 150 sccm to 250 sccm; and / or, The second protective gas is introduced for a time of 2s to 8s; and / or, The oxygen source comprises ultrapure water; and / or, The oxygen source is introduced for a time of 0.5s to 1s; and / or, After the oxygen source is introduced, the vacuum degree of the reaction chamber is 250Pa-260Pa; and / or, The flow rate of the third protective gas is 150 sccm to 250 sccm; and / or, The third protective gas is introduced for 5s to 15s; and / or The number of cycles of the third cycle treatment is 15 to 25 times.
9. The selective atomic layer deposition method according to any one of claims 1 to 8, It is characterized in that Removing the barrier layer comprises the following steps: introducing a hydrogen source into the reaction chamber; The hydrogen source generates hydrogen plasma, and the barrier layer is removed by the hydrogen plasma.
10. The selective atomic layer deposition method according to any one of claims 1 to 8, It is characterized in that Before the substrate is subjected to multiple first cycle treatments, the following steps are also included: The substrate is plasma cleaned.