Environment-friendly low-phenol color fixing agent and preparation method thereof
By using lignin to replace bisphenol S and condensate with formaldehyde, combining phenol sulfonic acid and lignin sulfonate to form a color fixing agent with a three-dimensional network structure, the problems of high free phenol residues and color fastness in textile printing and dyeing are solved, and the problem of high free phenol residues and color fastness in textile printing and dyeing is achieved. It has high-efficiency color fixing effect of environmentally friendly low-phenol color fixing agent.
Patent Information
- Application Number
- CN202411440344.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-15
- Publication Date
- 2024-12-20
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The acid dye fixing agent used in existing textile printing and dyeing has a high residual problem of free phenol, which is difficult to reduce the amount of formaldehyde and the content of free phenol at the same time, affecting environmental protection and color fastness.
Lignon is used to replace part of bisphenol S, and by condensation reaction with formaldehyde under alkaline catalysis, lignin phenolic copolymer resin is formed, combining phenol sulfonic acid and lignin sulfonate to form a color fixing agent with a three-dimensional network structure. Improve color fixation effect and color fastness.
It effectively reduces the residue of bisphenol S, improves the color fixing effect and color fastness of the color fixing agent, and meets the dual requirements of environmental protection and performance.
Smart Images

Figure BDA0005086188040000031 
Figure BDA0005086188040000041 
Figure BDA0005086188040000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fabric color fixing, and in particular to an environmentally friendly low-phenol color fixing agent and a preparation method thereof. Background Art
[0002] With the development of textile printing and dyeing industry and the improvement of people's living standards, people not only pay attention to the color fastness of textiles in the printing and dyeing process, but also gradually put forward higher requirements for the safety and environmental protection of printing and dyeing fixing agents. The large-scale discharge of toxic and harmful textile chemicals has caused environmental pollution.
[0003] EU regulations on textiles focus on four aspects: pre-processing and pre-treatment, printing and dyeing, post-finishing and composite product processing, aiming to reduce the pollution of water environment caused by key processing steps in the entire textile production chain. Developed countries are at a high level of risk assessment and management of textile chemicals. As a textile power, my country has also further improved its requirements for environmental protection.
[0004] The mainstream acid dye fixing agents on the market are mainly aromatic sulfonate polymers synthesized by sulfonation, condensation and other process lines using bisphenol S and formaldehyde as raw materials, which can be classified as synthetic tannins, such as polyphenol compounds, condensates based on diphenyl sulfone, and condensates of phenol formaldehyde.
[0005] The fixing mechanism of synthetic tannin is as follows: it relies on the well-water-soluble sulfonate group in the fixing agent to ionize in water to form anions, which form electrostatic repulsion with the dye anions, prompting the dye molecules to diffuse into the fiber; inhibiting the dye desorbed from the fiber to diffuse to the outside of the fiber, blocking the pores for the dye to dissolve again, preventing the destruction of the ionic bond between the dye and the fiber, firmly fixing the dye on the fiber, and forming electrostatic attraction with the ionized amino groups on the fiber.
[0006] Affected by the process, the free phenol residue of the acid dye fixing agent currently synthesized with phenolic compounds as the main raw materials is generally at a high value. There are two main ways to reduce the free phenol content of synthetic tannins: one is to reduce the molar ratio of phenolic compounds and formaldehyde, but increasing the amount of formaldehyde to reduce free phenol will inevitably increase the free formaldehyde content. The second is to partially replace phenolic compounds with substances containing phenolic hydroxyl structures.
[0007] Prior art 1: Chinese patent application 201310745400.0 discloses a method for preparing a modified phenolic resin, comprising the following steps: under the action of an acidic catalyst, heating a phenolic compound and an activator under a constant pH value to undergo a first reaction to obtain a first reaction mixture; subjecting the reaction mixture obtained in the above steps, a phenolic compound and an aldehyde compound to a second reaction to obtain a second reaction mixture; mixing the second reaction mixture with a modifier to obtain a modified phenolic resin; the activator is lignin; and the modifier is xylene formaldehyde resin.
[0008] The grinding wheel prepared by the modified phenolic resin provided by the solution improves storage stability, delays the performance degradation of the grinding wheel during storage, and has high cutting resistance and cutting efficiency;
[0009] From the 24th paragraph of the specification of the scheme, it can be seen that the scheme uses lignin as an activator, and explains that the activator mainly functions to improve the toughness and water resistance of the resin, thereby enhancing the storage stability of the grinding wheel;
[0010] Prior art 2: Chinese patent application 202010774565.0 discloses an environmentally friendly acidic color fixing agent capable of one-bath dyeing and fixing treatment, a preparation method and an application thereof, which belongs to the field of textile printing and dyeing auxiliaries, and comprises, by weight percentage, 30-70% of an aromatic sulfonic acid compound, 1-5% of anionic polyurethane, 5-20% of a dispersant and 5-65% of deionized water;
[0011] The preparation method comprises: 1) adding a formulated amount of dispersant into a stirring kettle;
[0012] 2) Heat the stirring kettle to 60-65°C, then add the formulated amount of anionic polyurethane while stirring for 50-70 minutes, and stir for 20-40 minutes after the addition;
[0013] 3) Add the formulated amount of aromatic sulfonic acid compound and stir at 60° C. for 25-35 minutes;
[0014] 4) Add the formula amount of deionized water and mix for 25-35 minutes.
[0015] Further observation of this solution shows that lignin sulfonate is added as a dispersant in this solution.
[0016] The problem to be solved by this scheme is: how to provide an environmentally friendly color fixing agent with low formaldehyde dosage and low free phenol content. Summary of the invention
[0017] The purpose of this application is to provide an environmentally friendly low-phenol color fixing agent. This application uses lignin to replace part of bisphenol S. Lignin is a complex aromatic natural macromolecular polymer with a three-dimensional network structure and contains multiple functional groups. The structure of lignin is composed of multiple phenylpropane structural units. The phenoxyl coupling of p-hydroxycinnamyl alcohol, coniferyl alcohol or sinapyl alcohol with similar structures forms a heterogeneous polycrystalline natural macromolecular polymer. Using lignin to replace part of bisphenol S can not only reduce the residual bisphenol S, but also improve the color fixing effect of the color fixing agent to a certain extent.
[0018] In addition, the present application also provides a preparation method for preparing the above-mentioned environmentally friendly low-phenol fixing agent;
[0019] To achieve the above object, the present application discloses an environmentally friendly low-phenol color fixing agent, which comprises the following components by molar weight:
[0020]
[0021] The phenolic hydroxyl structure compound is selected from at least one of lignin and lignin sulfonate.
[0022] Lignin is a complex aromatic natural polymer with a three-dimensional network structure and contains a variety of functional groups. The structure of lignin is composed of multiple phenylpropane structural units. The phenoxyl groups of p-hydroxycinnamyl alcohol, coniferyl alcohol or sinapyl alcohol with similar structures are coupled to form a heterogeneous polycrystalline natural polymer. Lignin and formaldehyde can also undergo condensation reaction under alkaline catalysis. This reaction occurs at the C5 position of the guaiacol ring of lignin. The lignin structure contains both phenolic hydroxyl and alcoholic hydroxyl groups, as well as aldehyde and carboxyl groups, and has certain reactivity. Under alkaline conditions, the ortho position of the phenolic hydroxyl group of lignin can undergo addition reaction with formaldehyde to form hydroxymethyl, which can further undergo polymerization reaction with phenol, bisphenol S or the active groups of lignin to form lignin phenolic copolymer resin. Replacing part of bisphenol S with part of lignin can reduce the bisphenol S residue in phenolic resin. Due to the three-dimensional network structure of lignin, it can also enhance the bonding strength between the fixing agent and the fabric, thereby improving the fixing effect.
[0023] Preferably, the formaldehyde is added to the environmentally friendly low-phenol color fixing agent in the form of a formaldehyde aqueous solution, and the mass fraction of formaldehyde in the formaldehyde aqueous solution is 37-44%;
[0024] The auxiliary agent is composed of a formaldehyde remover, a pH regulator, and an initiator. The environmentally friendly low-phenol color fixing agent comprises the following components by molar weight:
[0025]
[0026] The formaldehyde remover is an amine compound, and the modifier is an alkaline hydroxide.
[0027] Preferably, the phenolic compound is selected from at least one of naphthol and bisphenol S;
[0028] The aromatic sulfonic acid compound is selected from at least one of phenolsulfonic acid, sodium phenolsulfonate, naphtholsulfonic acid and sodium naphtholsulfonate.
[0029] Preferably, the lignin sulfonate is selected from at least one of sodium lignin sulfonate, potassium lignin sulfonate, calcium lignin sulfonate and magnesium lignin sulfonate.
[0030] Preferably, the amine compound is selected from at least one of ammonia, urea and ethanolamine.
[0031] Preferably, the alkaline hydroxide is selected from at least one of sodium hydroxide, potassium hydroxide, barium hydroxide, lithium hydroxide and strontium hydroxide.
[0032] Preferably, the phenolic compound is bisphenol S;
[0033] The aromatic sulfonic acid compound is a mixture of phenolsulfonic acid and sodium phenolsulfonate.
[0034] In addition, the present application also discloses a method for preparing the above-mentioned environmentally friendly low-phenol fixing agent, comprising the following steps:
[0035] Step 1: Mix and stir a phenolic compound, an aromatic sulfonic acid compound, a phenolic hydroxyl structure compound, sodium sulfite and deionized water to obtain an intermediate;
[0036] Step 2: Add a pH adjuster to the intermediate 1 and heat it to 90-100° C., then dropwise add a formaldehyde aqueous solution, and keep the temperature at 100° C. for 10-20 hours to obtain the intermediate 2;
[0037] Step 3: Add formaldehyde remover to the intermediate 2 and stir, then degas under vacuum conditions to obtain an environmentally friendly low-phenol color fixing agent.
[0038] The beneficial effects of this application are:
[0039] Lignin is a complex aromatic natural polymer with a three-dimensional network structure and multiple functional groups. The structure of lignin is composed of multiple phenylpropane structural units. The phenoxy groups of p-hydroxycinnamyl alcohol, coniferyl alcohol or sinapyl alcohol with similar structures are coupled to form a heterogeneous polycrystalline natural polymer. Lignin and formaldehyde can also undergo condensation reaction under alkaline catalysis. This reaction occurs at the C5 position of the guaiacol ring of lignin. The lignin structure contains both phenolic hydroxyl and alcoholic hydroxyl groups, as well as aldehyde and carboxyl groups, and has certain reactivity. Under alkaline conditions, the ortho position of the phenolic hydroxyl group of lignin can undergo addition reaction with formaldehyde to form hydroxymethyl, which can further undergo polymerization reaction with phenol, bisphenol S or the active groups of lignin to form lignin phenolic copolymer resin. Replacing part of bisphenol S with part of lignin can reduce the residual bisphenol S in phenolic resin, and to a certain extent, it can also improve the fixing effect of the fixing agent. DETAILED DESCRIPTION
[0040] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. In the description of the present invention, it should be noted that, if no specific conditions are specified in the embodiments, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0041] Before presenting the examples, the raw materials involved in the examples are first described as follows:
[0042] The supplier information of the raw materials involved in the examples is shown in Table 1:
[0043] Table 1
[0044]
[0045]
[0046] Unless otherwise specified, the preparation methods of the embodiments and comparative examples are as follows:
[0047] Step 1: Mix and stir a phenolic compound, an aromatic sulfonic acid compound, a phenolic hydroxyl structure compound, sodium sulfite and deionized water to obtain an intermediate 1;
[0048] Step 2: Add a pH adjuster to the intermediate 1 and heat it to 95±5°C, then dropwise add a formaldehyde aqueous solution and keep it at 100°C for 15h to obtain the intermediate 2;
[0049] Step 3: Add formaldehyde remover to the intermediate 2 and stir, then degas under vacuum conditions to obtain an environmentally friendly low-phenol color fixing agent;
[0050] The specific selection and addition amount of each raw material in the embodiments and comparative examples are detailed in the formula tables of the embodiments and comparative examples. It should be noted that the raw materials involved in the formula tables are in the form of aqueous solutions, and the molar fractions refer to the molar fractions of the solute in the aqueous solution.
[0051] Examples 1-4
[0052] An environmentally friendly low-phenol fixing agent, the formula is shown in Table 2:
[0053] Table 2
[0054]
[0055] It should be noted that in Example 1, the amine compound is an ammonia solution with a mass fraction of 20%, the pH adjuster is sodium hydroxide, and the mass fraction of formaldehyde in the formaldehyde solution is 37%;
[0056] In Example 2, the amine compound is urea, the pH regulator is potassium hydroxide, and the mass fraction of formaldehyde in the formaldehyde aqueous solution is 39%;
[0057] In Example 3, the amine compound is ethanolamine, the pH regulator is barium hydroxide, and the mass fraction of formaldehyde in the formaldehyde aqueous solution is 41%;
[0058] In Example 4, the amine compound is an aqueous ammonia solution with a mass fraction of 20%, the pH regulator is strontium hydroxide, and the mass fraction of formaldehyde in the formaldehyde aqueous solution is 44%.
[0059] Example 5
[0060] The method is substantially the same as Example 1, except that the same molar amount of naphthol is used instead of bisphenol S.
[0061] Example 6
[0062] The process is substantially the same as Example 1, except that bisphenol S is replaced by phenol in the same molar amount.
[0063] Example 7
[0064] The method is substantially the same as Example 1, except that the same molar amount of sodium phenolsulfonate is used instead of phenolsulfonic acid.
[0065] Example 8
[0066] The method is substantially the same as Example 1, except that the same molar amount of sodium naphtholsulfonate is used instead of phenolsulfonic acid.
[0067] Example 9
[0068] The method is substantially the same as Example 1, except that a mixture of phenolsulfonic acid and sodium phenolsulfonate in the same molar amount is used instead of phenolsulfonic acid, and the molar ratio of phenolsulfonic acid to sodium phenolsulfonate is 1:1.
[0069] Example 10
[0070] The method is substantially the same as Example 1, except that the same molar amount of sodium lignin sulfonate is used instead of lignin.
[0071] Embodiment 11
[0072] The method is substantially the same as Example 1, except that a mixture of sodium lignin sulfonate and calcium lignin sulfonate in the same molar amount is used instead of lignin, and the molar ratio of sodium lignin sulfonate to calcium lignin sulfonate is 1:1.
[0073] Example 12
[0074] The method is substantially the same as Example 1, except that a mixture of sodium lignin sulfonate and potassium lignin sulfonate in the same molar amount is used instead of lignin, and the molar ratio of sodium lignin sulfonate to potassium lignin sulfonate is 1:1.
[0075] Example 13
[0076] The method is substantially the same as Example 1, except that the same molar amount of potassium lignin sulfonate is used instead of lignin.
[0077] Embodiment 14
[0078] The method is basically the same as Example 1, except that the mass fraction of formaldehyde in the formaldehyde aqueous solution is 30%.
[0079] Embodiment 15
[0080] The method is basically the same as Example 1, except that the mass fraction of formaldehyde in the formaldehyde aqueous solution is 50%.
[0081] Comparative Examples 1-4
[0082] A color fixing agent, the formula is shown in Table 3:
[0083] Table 3
[0084]
[0085]
[0086] Comparative Examples 5-6
[0087] A color fixing agent, the formula of which is shown in Table 4:
[0088] Table 4
[0089]
[0090] It should be noted that the phenolsulfonic acid substitute in Comparative Example 6 is prepared by mixing chlorosulfonic acid and phenol in a molar ratio of 1:1.
[0091] Black nylon
[0092] Dipping process → environmentally friendly color fixing agent (4.5-6%) owf → 80℃*30min → washing with water → drying
[0093] Washing test method
[0094] Color fastness to washing with soap: Determined in accordance with GB / T 3921-2008 "Textiles - Tests for Color Fastness - Color Fastness to Washing with Soap", the test results are shown in Table 5:
[0095] Table 5
[0096]
[0097] Result analysis:
[0098] 1. It can be seen from Examples 1-4 that when the amount of raw material added of the color fixing agent is slightly adjusted or the type of the auxiliary agent is partially changed, the color fastness to soaping of Examples 1-4 shows a certain change trend, but the overall change range is small;
[0099] 2. It can be added from Examples 1 and 5-8 that when naphthol or phenol is used instead of bisphenol S, the color fastness to soaping of Examples 5-6 is still superior to that of the blank group, but relative to Example 1, the performance of Examples 5 and 6 in the test process of cotton staining, nylon staining, polyester staining, acrylic staining, and wool staining is not as good as that of Example 1. It can be seen that when bisphenol S is used as a phenolic compound, the application effect on cotton, nylon, polyester, acrylic, and wool materials is significantly better than that of naphthol and phenol;
[0100] Further observation of Example 1 and Examples 7-8 shows that when phenolsulfonic acid is used as the aromatic sulfonic acid compound, the application effect of Example 1 on cotton, nylon, polyester, acrylic fiber, and wool materials is significantly better than that of Examples 7-8. It can be seen that the effect of phenolsulfonic acid as an aromatic sulfonic acid compound in the formula of the present application is more significant; further observation of Example 9 shows that when a mixture of phenolsulfonic acid and sodium phenolsulfonate is used to replace phenolsulfonic acid, the soap-resistant color fastness of Example 9 on wool materials is significantly improved relative to Example 1. We believe that the reason for this phenomenon may be that during the dyeing process, the fabric may carry a positive charge under acidic conditions, and the anions of sodium phenolsulfonate and phenolsulfonic acid can electrostatically attract these positive charges, thereby enhancing the binding force between the dye molecules and the fibers; at the same time, the mixture of sodium phenolsulfonate and phenolsulfonic acid may provide a wider charge distribution and stronger ionic interaction, and this synergistic effect can improve the adhesion and uniformity of the dye;
[0101] 3. It can be seen from Examples 1 and 10-13 that when sodium lignin sulfonate is used alone in Example 10 and potassium lignin sulfonate is used alone in Example 13, the application effects of the two on cotton, nylon, polyester, acrylic and wool materials show a certain downward trend compared with Example 1. However, it can be seen from Example 12 that the sodium lignin sulfonate in Example 10 and the potassium lignin sulfonate in Example 13 are compounded. Under the premise that the color fastness to soaping of Examples 10 and 13 relative to Example 1 both show a downward trend, Example 12 does not decrease but increases. It can be seen that a certain synergistic effect is produced between potassium lignin sulfonate and sodium lignin sulfonate, thereby causing the color fastness of Example 12 to increase instead of decrease. In this regard, the reason for this phenomenon may be that lignin is a complex aromatic natural high molecular polymer with a three-dimensional network space structure and contains a variety of functional groups. At the same time, potassium and sodium may further improve the dispersibility and solubility of lignin sulfonate, thereby improving the color fixing effect of the fixing agent.
[0102] 4. It can be seen from Example 1 and Comparative Examples 1-4 that when Comparative Examples 1-4 lack any one of bisphenol S, phenolsulfonic acid, lignin, and formaldehyde aqueous solution, the soap-resistant color fastness of Comparative Examples 1-4 relative to Example 1 shows a significant downward trend. It can be seen that any one of bisphenol S, phenolsulfonic acid, lignin, and formaldehyde aqueous solution in the formula of the present application is indispensable. At the same time, it can be seen from Comparative Examples 1 and Comparative Examples 3 that when the total mass parts of bisphenol S and lignin remain unchanged, using only one of the two as a color fixing agent still cannot obtain good color fastness. It can be seen that only when the two are used at the same time, the color fixing agent can produce a good color fixing effect;
[0103] 5. It can be seen from Example 1 and Comparative Examples 5-6 that when a mixture of chlorosulfonic acid and phenol is used to replace phenolsulfonic acid, it is difficult for Comparative Example 5 to achieve a good color fixation effect. It can be seen that even if benzene rings and sulfonic acid groups exist in the mixture, Comparative Example 5 achieves an effect similar to that of Example 1.
[0104] Further observation shows that after lignin is replaced by cellulose in Comparative Example 6, the soap-resistant color fixation of Comparative Example 6 shows an obvious downward trend, which shows that the lignin in this application is irreplaceable.
[0105] 6. It can be seen from Example 1 and Comparative Examples 7-8 that when the mass fraction of formaldehyde in the formaldehyde aqueous solution is greatly increased or decreased, the soap-resistant color fastness of Comparative Examples 7 and 8 is significantly reduced. The reason for this phenomenon may be that as the amount of formaldehyde increases, the molecular weight of the product increases, the film-forming property on the fabric surface is better, the affinity for the fabric is also better, and the dissolution channel of the dye can be better blocked, thereby improving the color fastness; but when the amount of formaldehyde is too much, the molecular weight of the color fixing agent is too large, and it is not easy to combine with the fiber, and the color fixing effect is not obvious. Therefore, too much or too little formaldehyde has a significant effect on the color fastness.
[0106] Nylon printed fabric
[0107] Color fixing process → environmentally friendly color fixing agent (4.5-6%) owf → 60℃*30min → washing with water → drying "Textile Color Fastness Test Color Fastness to Soaping" test, the test results are shown in Table 6:
[0108] Table 6
[0109]
[0110]
[0111] Result analysis:
[0112] 1. It can be seen from Examples 1-4 that when the amount of raw material added of the color fixing agent is slightly adjusted or the type of the auxiliary agent is partially changed, the color fastness to soaping of Examples 1-4 shows a certain change trend, but the overall change range is small;
[0113] 2. It can be added from Examples 1 and 5-8 that when naphthol or phenol is used instead of bisphenol S, the color fastness to soaping of Examples 5-6 is still superior to that of the blank group. However, relative to Example 1, the performance of Example 5 in the test process of cotton staining, nylon staining, acrylic staining, and wool staining; the performance of Example 6 in the test process of cotton staining, nylon staining, polyester staining, acrylic staining, and wool staining is not as good as that of Example 1. It can be seen that when bisphenol S is used as a phenolic compound, the application effect on cotton, nylon, polyester, acrylic, and wool materials is more advantageous overall.
[0114] Further observation of Example 1 and Examples 7-8 shows that when phenolsulfonic acid is used as the aromatic sulfonic acid compound, the application effect of Example 1 on only vinegar and cotton is significantly better than that of Example 7. It can be seen that in the application process of color fixation of printed cloth, there is no obvious difference between Examples 1, 7, and 8.
[0115] Further observation of Example 9 shows that when the mixture of phenolsulfonic acid and sodium phenolsulfonate is used to replace phenolsulfonic acid, the color fastness to soap washing of Example 9 is significantly improved relative to that of Example 1. We believe that the reason for this phenomenon may be that during the dyeing process, the fabric may have positive charges under acidic conditions, and the anions of sodium phenolsulfonate and phenolsulfonic acid can electrostatically attract these positive charges, thereby enhancing the binding force between the dye molecules and the fibers; at the same time, the mixture of sodium phenolsulfonate and phenolsulfonic acid may provide a wider charge distribution and stronger ionic interaction, and this synergistic effect can improve the adhesion and uniformity of the dye;
[0116] 3. It can be seen from Examples 1 and 10-13 that when sodium lignin sulfonate is used alone in Example 10 and potassium lignin sulfonate is used alone in Example 13, only Example 13 shows a certain downward trend in the application effect on polyester and acrylic materials compared with Example 1, while the rest show similar effects. However, it can be seen from Example 12 that the sodium lignin sulfonate in Example 10 and the potassium lignin sulfonate in Example 13 are compounded. When there is no obvious fluctuation in the soap-resistant color fastness of Examples 10 and 13 relative to Example 1, the multiple color fastnesses of Example 12 increase instead of decrease. It can be seen that a certain synergistic effect is produced between potassium lignin sulfonate and sodium lignin sulfonate, thereby causing the color fastness of Example 12 to increase instead of decrease. The reason for this phenomenon may be that lignin is a complex aromatic natural high molecular polymer with a three-dimensional network space structure and contains a variety of functional groups. At the same time, potassium and sodium may further improve the dispersibility and solubility of lignin sulfonate, thereby improving the color fixing effect of the color fixing agent.
[0117] 4. It can be seen from Example 1 and Comparative Examples 1-4 that when Comparative Examples 1-4 lack any one of bisphenol S, phenolsulfonic acid, lignin, and formaldehyde aqueous solution, the soap-resistant color fastness of Comparative Examples 1-4 relative to Example 1 shows a significant downward trend. It can be seen that any one of bisphenol S, phenolsulfonic acid, lignin, and formaldehyde aqueous solution in the formula of the present application is indispensable. At the same time, it can be seen from Comparative Examples 1 and Comparative Examples 3 that when the total mass parts of bisphenol S and lignin remain unchanged, using only one of the two as a color fixing agent still cannot obtain good color fastness. It can be seen that only when the two are used at the same time, the color fixing agent can produce a good color fixing effect;
[0118] 5. It can be seen from Example 1 and Comparative Examples 5-6 that when a mixture of chlorosulfonic acid and phenol is used to replace phenolsulfonic acid, it is difficult for Comparative Example 5 to achieve a good color fixation effect. It can be seen that even if benzene rings and sulfonic acid groups exist in the mixture, Comparative Example 5 achieves an effect similar to that of Example 1.
[0119] Further observation shows that after lignin is replaced by cellulose in Comparative Example 6, the soap-resistant color fixation of Comparative Example 6 shows an obvious downward trend, which shows that the lignin in this application is irreplaceable.
[0120] 6. It can be seen from Example 1 and Comparative Examples 7-8 that when the mass fraction of formaldehyde in the formaldehyde aqueous solution is greatly increased or decreased, the soap-resistant color fastness of Comparative Examples 7 and 8 is significantly reduced. The reason for this phenomenon may be that as the amount of formaldehyde increases, the molecular weight of the product increases, the film-forming property on the fabric surface is better, the affinity for the fabric is also better, and the dissolution channel of the dye can be better blocked, thereby improving the color fastness; but when the amount of formaldehyde is too much, the molecular weight of the color fixing agent is too large, and it is not easy to combine with the fiber, and the color fixing effect is not obvious. Therefore, too much or too little formaldehyde has a significant effect on the color fastness.
[0121] BPS residue test: The BPS residues of Examples 1-4 and Comparative Examples 1-8 were tested with reference to GB / T 16631-2008 General Rules for High Performance Liquid Chromatography. The results are shown in Table 7:
[0122] Table 7
[0123]
[0124] As shown in Table 7, compared with the examples, the overall BPS residual values of Comparative Examples 1-4 are significantly higher than any of Examples 1-4. It can be seen that when any of bisphenol S, phenolsulfonic acid, lignin, and formaldehyde aqueous solution is missing in the formula, the BPS residual will increase during the use of the fixing agent.
[0125] On the other hand, in Comparative Examples 5-6, when phenolsulfonic acid or lignin was replaced by a mixture of chlorosulfonic acid and phenol or by cellulose, the color fastness of the fixing agent when used showed an upward trend, and reducing the amount of formaldehyde aqueous solution added also led to an increase in the amount of BPS residue after the fixing agent was used.
Claims
1. An environmentally friendly low-phenol fixing agent, characterized in that: In terms of molar amounts, it comprises the following components: The phenolic hydroxyl structure compound is selected from at least one of lignin and lignin sulfonate.
2. The environmentally friendly low-phenol fixing agent according to claim 1, characterized in that: The formaldehyde is added to the environmentally friendly low-phenol color fixing agent in the form of a formaldehyde aqueous solution, and the mass fraction of formaldehyde in the formaldehyde aqueous solution is 37-44%; The auxiliary agent is composed of a formaldehyde remover, a pH regulator, and an initiator. The environmentally friendly low-phenol color fixing agent comprises the following components by molar weight: The formaldehyde remover is an amine compound, and the modifier is an alkaline hydroxide.
3. The environmentally friendly low-phenol fixing agent according to claim 1, characterized in that: The phenolic compound is selected from at least one of naphthol and bisphenol S; The aromatic sulfonic acid compound is selected from at least one of phenolsulfonic acid, sodium phenolsulfonate, naphtholsulfonic acid and sodium naphtholsulfonate.
4. The environmentally friendly low-phenol fixing agent according to claim 1, characterized in that: The lignin sulfonate is selected from at least one of sodium lignin sulfonate, potassium lignin sulfonate, calcium lignin sulfonate and magnesium lignin sulfonate.
5. The environmentally friendly low-phenol fixing agent according to claim 2, characterized in that: The amine compound is selected from at least one of ammonia water, urea and ethanolamine.
6. The environmentally friendly low-phenol fixing agent according to claim 2, characterized in that: The alkaline hydroxide is selected from at least one of sodium hydroxide, potassium hydroxide, barium hydroxide, lithium hydroxide and strontium hydroxide.
7. The environmentally friendly low-phenol fixing agent according to claim 1, characterized in that: The phenolic compound is bisphenol S; The aromatic sulfonic acid compound is a mixture of phenolsulfonic acid and sodium phenolsulfonate.
8. A method for preparing the environmentally friendly low-phenol fixing agent according to any one of claims 2 to 7, characterized in that: The following steps are involved: Step 1: Mix and stir a phenolic compound, an aromatic sulfonic acid compound, a phenolic hydroxyl structure compound, sodium sulfite and deionized water to obtain an intermediate 1; Step 2: Add a pH adjuster to the intermediate 1 and heat it to 90-100° C., then dropwise add a formaldehyde aqueous solution, and keep the temperature at 100° C. for 10-20 hours to obtain the intermediate 2; Step 3: Add formaldehyde remover to the intermediate 2 and stir, then degas under vacuum conditions to obtain an environmentally friendly low-phenol color fixing agent.
Citation Information
Patent Citations
Method for preparing lignin sulfonate dye dispersant
CN102174273A
Acid reaction resistant chinlon fixer and application thereof
CN102850500A
Environment-friendly type synthetic tannin color fixing agent as well as preparation method and application thereof
CN108442150A
Environmentally-friendly acidic color fixing agent capable of achieving dyeing and fixing one-bath treatment, manufacturing method and application
CN111826979A
Printing and dyeing processing method for improving wet treatment color fastness of nylon spandex elastic knitted fabric
CN118390317A