A method for preparing monoammonium phosphate using residual raffinate

By concentrating residual acid and combining it with a purification process using solvent and barium fluoride, the problem of low utilization rate of residual acid was solved, enabling the preparation of high-purity monoammonium phosphate, thereby increasing product added value and simplifying the process.

CN119461279BActive Publication Date: 2026-11-10GUIZHOU CHANHEN CHEM CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411601290.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-11
Publication Date
2026-11-10
Estimated Expiration
2044-11-11

AI Technical Summary

Technical Problem

Existing technologies are difficult to effectively utilize residual acid in the preparation of high-purity monoammonium phosphate. The impurity removal rate is low, the added value of the product is low, and the process is complex and the equipment is prone to corrosion and blockage.

Method used

The residual acid is extracted and concentrated using concentrated sulfuric acid. This is followed by primary purification with alcohols, ketones, or ethers and secondary purification with barium fluoride. The mixture is then neutralized with ammonia-based alkaline substances to prepare fire-resistant monoammonium phosphate.

Benefits of technology

The process improved phosphorus yield and impurity removal rate, and the obtained monoammonium phosphate met fire-fighting standards. It also simplified the process flow and reduced the risk of equipment corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119461279B_ABST
    Figure CN119461279B_ABST
Patent Text Reader

Abstract

This invention relates to the field of phosphorus chemical technology, and particularly to a method for preparing monoammonium phosphate using residual raffinate acid, comprising: S1) mixing residual raffinate acid with concentrated sulfuric acid, concentrating the mixture, and then separating the solid and liquid phases to obtain a concentrated solution; S2) adding solvent dropwise to the concentrated solution for primary solvent purification, and defining the solvent components; S3) allowing the light and heavy mixed phases obtained from the primary solvent purification to separate into an acid-containing solvent phase; S4) mixing the acid-containing solvent phase with barium fluoride, reacting the mixture, and then separating the solid and liquid phases to obtain a secondary purified acid-containing solvent and a purification residue; S5) performing vacuum distillation on the secondary purified acid-containing solvent to recover the solvent, with the residue in the distillation vessel being the purified acid; S6) diluting the purified acid, then mixing it with an ammonia-containing alkaline substance for a neutralization reaction, filtering the mixture after the reaction, drying and granulating the filter cake to obtain fire-fighting grade monoammonium phosphate product. The method provided by this invention has a high impurity removal rate, high phosphorus yield, and high product added value, and can produce fire-fighting grade monoammonium phosphate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of phosphorus chemical technology, and in particular to a method for preparing monoammonium phosphate using residual raffinate. Background Technology

[0002] Phosphoric acid is an important basic chemical raw material with a wide range of applications. It can be used to produce a series of other important products, playing a significant role in the development of the national economy. Currently, wet-process phosphoric acid is mainly obtained by decomposing phosphate rock with sulfuric acid and then separating it. This type of phosphoric acid has a relatively high impurity content, mainly consisting of calcium, magnesium, iron, aluminum, fluorine, silicon dioxide, sulfate, and organic matter. This wet-process phosphoric acid can be used directly in fertilizer production, but further purification and impurity removal are required for the production of high-purity industrial phosphoric acid or fine phosphates.

[0003] Based on the characteristics of impurities in wet-process phosphoric acid and the requirements for refined products, researchers have developed many purification methods for wet-process phosphoric acid. Among these, organic solvent extraction is the most widely used method for purifying phosphoric acid in industrial applications. In the solvent extraction process for purifying wet-process phosphoric acid, the purification rate is generally controlled at 50%–60%. This process inevitably produces residual raffinate (i.e., acid remaining in the aqueous phase after extraction), characterized by high P2O5 concentration and high impurity content (mainly metallic cations such as calcium, magnesium, iron, and aluminum). Effective utilization of this residual raffinate to prepare high-value-added products will bring greater economic benefits to enterprises.

[0004] For a long time, the recovery and utilization of residual raffinate has been a technical challenge, mainly limited by factors such as high impurity ion content, difficulty in purification and refining, and high cost. Directly using residual raffinate to replace ordinary wet-process phosphoric acid in monoammonium phosphate (MAP) production facilities results in adverse effects such as low main component content, high slurry viscosity, difficult reaction, low product yield, and easy scaling of process equipment and pipelines. Currently, the common method for producing MAP is to mix residual raffinate with ordinary wet-process phosphoric acid. This method involves mixing ordinary wet-process phosphoric acid with a P2O5 content of 25% with residual raffinate in a specific ratio to reduce the cation content, followed by neutralization with ammonia. MAP produced using this method only meets agricultural fertilizer quality standards, has low added value, and requires mixing residual raffinate with ordinary wet-process phosphoric acid in a specific ratio, which cannot meet the process requirements for producing MAP entirely with residual raffinate.

[0005] Some patents employ solvent precipitation to purify and utilize residual raffinate. For example, patent application CN101704518B discloses "a method for purifying residual raffinate," which involves adding alcohol while continuously stirring residual raffinate with a P2O5 mass concentration of 40.9%–47.0% and a magnesium mass concentration of 1.6%–2.8% at room temperature to 75°C. After mixing for 10 minutes, fluorosilicic acid is added, and the reaction continues for 20–30 minutes. After cooling to room temperature to 35°C, vacuum filtration is performed to separate the precipitate and obtain a clear liquid. The clear liquid is then vacuum distilled to recover the alcohol, yielding purified residual raffinate. This patent utilizes a combination of alcohol solvent and fluorosilicic acid, purifying residual raffinate through solvent precipitation, separation, and distillation concentration, enabling its reuse and improving the utilization rate of phosphoric acid, the raw material for solvent extraction. Simultaneously, the purified residual raffinate has a low magnesium ion content, with a magnesium removal rate reaching up to 77.6%. The purification effect is good, the process is simple, and the cost is low.

[0006] However, due to the high solubility of magnesium fluorosilicate, within the concentration range of the residual acid, even with the addition of excess fluorosilicic acid, only a small amount of precipitate can be formed to achieve magnesium separation, thus preventing further improvement in magnesium removal rate. The remaining large amount of fluorosilicic acid requires treatment with alkali metal salts (such as sodium carbonate) to form insoluble fluorosilicates for separation. However, sodium carbonate consumes phosphoric acid, leading to increased phosphorus loss, and the incomplete defluorination increases the risk of equipment corrosion and blockage during subsequent residual acid concentration. Summary of the Invention

[0007] In view of this, the technical problem to be solved by the present invention is to provide a method for preparing monoammonium phosphate using residual raffinate, which has a high impurity removal rate, high phosphorus yield, and high product added value, and can produce fire-fighting grade monoammonium phosphate.

[0008] This invention provides a method for preparing monoammonium phosphate using residual raffinate, comprising the following steps:

[0009] S1) Mix the residual acid with concentrated sulfuric acid, concentrate the mixture, and then separate the solid and liquid components to obtain the concentrated solution.

[0010] S2) Add solvent dropwise to the concentrate for primary solvent purification; the solvent includes at least one of alcohol solvents, ketone solvents, and ether solvents;

[0011] S3) The light and heavy mixed phase obtained by the purification of the primary solvent is allowed to stand and separate into two phases: the upper layer is the acid-containing solvent phase and the lower layer is the impurity-containing heavy phase.

[0012] S4) The acid-containing solvent phase is mixed with barium fluoride and reacted. After solid-liquid separation, secondary purified acid-containing solvent and purified residue are obtained.

[0013] S5) Vacuum distill the acidic solvent in the secondary purification process to recover the solvent. The resulting regenerated solvent is returned to the primary solvent purification process for recycling. The residue in the distillation kettle is the purified acid.

[0014] S6) The purified acid is diluted and then mixed with an ammonia-containing alkaline substance to carry out a neutralization reaction. After the reaction, the mixture is filtered, and the filter cake is dried and granulated to obtain fire-fighting grade monoammonium phosphate product.

[0015] Preferably, in step S1), concentrated sulfuric acid and residual raffinate are reacted according to SO42-. 2- Mix with P2O5 at a mass ratio of 4.2 to 30:100.

[0016] Preferably, in step S1), the concentration method includes vacuum concentration, atmospheric pressure concentration, or a single-stage atmospheric pressure concentration followed by a double-stage vacuum concentration.

[0017] The vacuum degree of the vacuum concentration is 80-90 kPa; after concentration, the mass concentration of P2O5 in the solution is 23%-54%.

[0018] Preferably, in step S2), the volume ratio of the solvent to the concentrate is 1 to 3.5:1;

[0019] The solvent is added dropwise over a period of 30–90 minutes; the temperature for primary solvent purification is 55–65°C; and the time for primary solvent purification after solvent addition is 10–90 minutes.

[0020] Preferably, in step S3), the pH value of the acid-containing solvent phase is 0.8 to 1.2.

[0021] Preferably, in step S3), after obtaining the impurity-containing heavy phase, the process further includes:

[0022] Superphosphate is prepared using a heavy phase containing impurities, calcium carbonate, and phosphogypsum; the phosphogypsum includes the precipitated phosphogypsum obtained in step S1).

[0023] The P2O5 in the impure heavy phase and the Ca in calcium carbonate 2+ The mass ratio is 4.8–5.2:1; the mass ratio of phosphogypsum to P2O5 in the impurity heavy phase is 18–22:100.

[0024] Preferably, in step S4), the Mg in the acid-containing solvent phase 2+ and the F in the barium fluoride - The molar ratio is 1:2.

[0025] Preferably, in step S4), mixing the acid-containing solvent phase with barium fluoride includes:

[0026] Barium fluoride is added dropwise to the acid-containing solvent phase; the dropwise addition time is 30–120 min.

[0027] The reaction temperature is 55–65°C; the reaction time after mixing is 10–60 min.

[0028] Preferably, in step S5), the temperature of the vacuum distillation is 60-80°C and the vacuum degree is 80-90 kPa.

[0029] Preferably, in step S6), the dilution is performed by adding water; the mass ratio of the purified acid to water is 0.8–1.2:0.8–1.2.

[0030] The ammonia-containing alkaline substances include ammonia water, ammonia gas, ammonium carbonate, or ammonium bicarbonate;

[0031] When the ammonia-containing alkaline substance is ammonia water, mixing with the ammonia-containing alkaline substance includes:

[0032] Ammonia water is added dropwise to the diluted purified acid until the pH value reaches 4.0–4.5; the dropwise addition time is 30–90 minutes.

[0033] The neutralization reaction temperature is 65–80°C; after mixing with ammonia-containing alkaline substances, the neutralization reaction time is 30–60 minutes.

[0034] This invention provides a method for preparing monoammonium phosphate using residual raffinate acid, comprising the following steps: S1) mixing residual raffinate acid with concentrated sulfuric acid, concentrating the mixture, and then separating the solid and liquid phases to obtain a concentrated solution; S2) adding solvent dropwise to the concentrated solution for primary solvent purification; the solvent includes at least one of alcohol solvents, ketone solvents, and ether solvents; S3) allowing the light and heavy mixed phases obtained from the primary solvent purification to stand and separate, with the upper layer being an acid-containing solvent phase and the lower layer being a heavy phase containing impurities; S4) mixing the acid-containing solvent phase with barium fluoride, reacting the mixture, and then separating the solid and liquid phases to obtain a secondary purified acid-containing solvent and a purification residue; S5) performing vacuum distillation on the secondary purified acid-containing solvent to recover the solvent, and returning the regenerated solvent obtained to the primary solvent purification process for recycling, with the residue in the distillation vessel being the purified acid; S6) diluting the purified acid, then mixing it with an ammonia-containing alkaline substance for a neutralization reaction, filtering the mixture after the reaction, drying and granulating the filter cake to obtain a fire-fighting grade monoammonium phosphate product. The method provided by this invention has a high impurity removal rate, high phosphorus yield, and high product added value, and can produce fire-fighting grade monoammonium phosphate. Attached Figure Description

[0035] Figure 1 A process flow diagram for preparing monoammonium phosphate using residual raffinate is provided for one embodiment of the present invention. Detailed Implementation

[0036] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0037] This invention provides a method for preparing monoammonium phosphate using residual raffinate, comprising the following steps:

[0038] S1) Mix the residual acid with concentrated sulfuric acid, concentrate the mixture, and then separate the solid and liquid components to obtain the concentrated solution.

[0039] S2) Add solvent dropwise to the concentrate for primary solvent purification; the solvent includes at least one of alcohol solvents, ketone solvents, and ether solvents;

[0040] S3) The light and heavy mixed phase obtained by the purification of the primary solvent is allowed to stand and separate into two phases: the upper layer is the acid-containing solvent phase and the lower layer is the impurity-containing heavy phase.

[0041] S4) The acid-containing solvent phase is mixed with barium fluoride and reacted. After solid-liquid separation, secondary purified acid-containing solvent and purified residue are obtained.

[0042] S5) Vacuum distill the acidic solvent in the secondary purification process to recover the solvent. The resulting regenerated solvent is returned to the primary solvent purification process for recycling. The residue in the distillation kettle is the purified acid.

[0043] S6) The purified acid is diluted and then mixed with an alkaline substance to carry out a neutralization reaction. After the reaction, the mixture is filtered, and the filter cake is dried and granulated to obtain fire-fighting grade monoammonium phosphate product.

[0044] Figure 1 A process flow diagram for preparing monoammonium phosphate using residual raffinate is provided for one embodiment of the present invention.

[0045] Regarding step S1):

[0046] The residual acid was mixed with concentrated sulfuric acid, concentrated, and then the solid and liquid were separated to obtain the concentrated solution.

[0047] In some embodiments of the present invention, the residual acid contains 21% to 23% P2O5 by mass and Ca... 2+ The mass content is 0.2% to 0.35%, Mg 2+ The mass content is 0.8% to 1.2%, Fe 3+ The mass content is 0.2% to 0.3%, Al 3+ The mass content is 0.2%–0.3%, the mass content of SiO2 is 80–200 ppm, and the mass content of SO4 is 0.2%–0.3%. 2-The mass content is 200-400 ppm, F - The mass content is 700-1100 ppm, Na + The mass content is 380-1000 ppm, K + The mass content is 500-1000 ppm, Cl - The mass content is 30-60 ppm, Cr 3+ The mass content is 20-55 ppm, Ba 2+ The mass content is 5-10 ppm. Specifically, in the residual acid, the mass content of P2O5 is 22.46%, and the mass content of Ca is... 2+ The mass content is 0.25%, Mg 2+ The mass content is 1.1%, Fe 3+ The mass content is 0.24%, Al 3+ The mass content is 0.28%, the mass content of SiO2 is 94ppm, and the mass content of SO4 is... 2- The mass content is 240 ppm, F - The mass content was 1085 ppm, Na + The mass content was 680 ppm, K + The mass content was 598 ppm, Cl - The mass content was 35 ppm, Cr 3+ The mass content was 22 ppm, Ba 2+ The mass content is 5.5 ppm.

[0048] In some embodiments of the present invention, concentrated sulfuric acid and residual raffinate are reacted according to SO4. 2- Mix with P2O5 at a mass ratio of 4.2 to 30:100; for example, 5:100, 10:100, 15:100, 20:100 or 30:100.

[0049] The concentration can be vacuum concentration, but is not limited to vacuum concentration; it can also be atmospheric pressure concentration or a single-stage atmospheric pressure concentration followed by a double-stage vacuum concentration. The vacuum degree of the vacuum concentration is 80–90 kPa, for example, 85 kPa. After concentration, the mass concentration of P2O5 in the solution is 23%–54%.

[0050] The solid-liquid separation method is filtration. After solid-liquid separation, precipitated phosphogypsum and concentrated liquid are obtained.

[0051] In step S1), adding concentrated sulfuric acid can increase the activity of hydrogen ions in the raffinate, thereby increasing the phosphorus yield during solvent extraction. At the same time, adding concentrated sulfuric acid can pre-remove calcium ions from the raffinate, as shown in formula (1):

[0052] Ca 2+ +SO42- =CaSO4 (1).

[0053] Regarding step S2):

[0054] A solvent is added dropwise to the concentrate for primary solvent purification; the solvent includes at least one of alcohol solvents, ketone solvents, and ether solvents, preferably an alcohol solvent. The alcohol solvent is selected from C1-C15 alcohol solvents, such as at least one of isopropanol, n-butanol, methanol, and ethanol; preferably isopropanol and / or n-butanol. The ketone solvent can be acetone. The ether solvent can be dimethyl ether.

[0055] In some embodiments of the present invention, the volume ratio of the solvent to the concentrate is 1 to 3.5:1, for example, 2:1.

[0056] The solvent is added dropwise over a period of 30–90 minutes, for example, 60 minutes. The temperature for primary solvent purification is 55–65°C, for example, 60°C; the time for primary solvent purification after adding the solvent is 10–90 minutes, for example, 50 minutes.

[0057] In step S2), a solvent, preferably a water-soluble solvent, is added. Utilizing the miscibility of the solvent and water, the "free water" in the residual acid system is drawn away. Most of the phosphoric acid and a small amount of cationic impurities follow into the solvent-water mixture, while the remaining cationic impurities are transferred to the heavy phase. Through primary solvent purification, the phosphorus yield can reach over 92%.

[0058] Regarding step S3):

[0059] The light and heavy mixed phase obtained by the purification of the primary solvent is allowed to stand and separate into two phases: the upper layer is the acid-containing solvent phase, and the lower layer is the impurity-containing heavy phase.

[0060] The pH value of the acid-containing solvent phase is 0.8 to 1.2.

[0061] The acid-containing solvent phase proceeds to the next purification step.

[0062] After obtaining the impure heavy phase, it also includes:

[0063] Superphosphate is prepared using a heavy phase containing impurities, calcium carbonate, and phosphogypsum; the phosphogypsum includes the precipitated phosphogypsum obtained in step S1).

[0064] Specifically, the method for preparing superphosphate includes the following steps:

[0065] a) Add the calcium carbonate slurry to the heated heavy phase containing impurities and mix well;

[0066] b) Add phosphogypsum to the slurry after mixing in step a) and mix well;

[0067] c) Dry, crush, and sieve the slurry after mixing in step b) to obtain the superphosphate product.

[0068] Regarding step a):

[0069] The temperature of the heavy phase containing impurities after heating is 90-100℃, for example, 95℃.

[0070] The calcium carbonate slurry has a mass concentration of 55% to 65%, for example, 60%. The solvent for the calcium carbonate slurry is water.

[0071] The P2O5 in the impure heavy phase and the Ca in calcium carbonate 2+ The mass ratio is 4.8 to 5.2:1, for example, 5:1.

[0072] The calcium carbonate slurry is added at a rate that prevents foam from overflowing. The mixing process involves stirring to achieve the desired consistency.

[0073] Regarding step b):

[0074] The mass ratio of phosphogypsum to P2O5 in the impurity heavy phase is 18–22:100, for example, 20:100. The phosphogypsum is first obtained from the precipitated phosphogypsum in step S1), and any insufficient amount is supplemented.

[0075] The mixing process involves stirring and mixing.

[0076] Regarding step c):

[0077] The drying temperature is 90–105°C, for example, 100°C.

[0078] Regarding step S4):

[0079] The acid-containing solvent phase is mixed with barium fluoride and reacted. After solid-liquid separation, a secondary purified acid-containing solvent and purified residue are obtained.

[0080] In some embodiments of the present invention, the barium fluoride is used as a precipitant to remove Mg from the acidic solvent phase. 2+ and SO4 2- The Mg in the acid-containing solvent phase 2+ and the F in the barium fluoride - The molar ratio is 1:2.

[0081] In some embodiments of the present invention, mixing the acid-containing solvent phase with barium fluoride includes:

[0082] Barium fluoride is added dropwise to the acid-containing solvent phase. The dropwise addition time is 30–120 min, for example, 60 min.

[0083] The reaction temperature is 55–65°C, for example, 60°C; the reaction time after mixing is 10–60 min, for example, 40 min.

[0084] The solid-liquid separation method is filtration.

[0085] In step S4), since barium fluoride is sparingly soluble in water but readily soluble in alcohol solvents, the F it dissociates releases... - and Ba 2+ Can be used with Mg 2+ and SO4 2- The SO4 is removed by forming a sparingly soluble precipitate. 2- Furthermore, it purifies the cationic impurities within. The reaction formulas are shown in formulas (2) and (3):

[0086] Ba 2+ +SO4 2- =BaSO4↓ Equation (2);

[0087] F - +Mg 2+ =MgF2↓ (3)

[0088] During the purification process of alcohol solvents, Mg 2+ and a small amount of Fe 3+ Al 3+ Both are dissolved in the solvent in the form of sulfates. Therefore, in the acidic solvent phase, Mg 2+ and SO4 2- With a molar ratio of 1:1.06, barium fluoride can effectively remove fluorine and barium residues. Through two-stage precipitation purification, Mg... 2+ The removal rate is as high as 95% or more, SO4 2- The removal rate is over 98%.

[0089] Regarding step S5):

[0090] The acidic solvent in the secondary purification process is vacuum distilled to recover the solvent. The resulting regenerated solvent is returned to the primary solvent purification process for recycling. The residue in the distillation vessel is the purified acid.

[0091] In some embodiments of the present invention, the temperature of the vacuum distillation is 60-80°C, for example 70°C; and the vacuum degree is 80-90 kPa, for example 85 kPa.

[0092] Regarding step S6):

[0093] The purified acid is diluted and then mixed with an ammonia-containing alkaline substance to carry out a neutralization reaction. After the reaction, the mixture is filtered, and the filter cake is dried and granulated to obtain fire-fighting grade monoammonium phosphate product.

[0094] In some embodiments of the present invention, the dilution can be achieved by adding water. The mass ratio of the purified acid to water is 0.8–1.2:0.8–1.2, for example, 1:1.

[0095] The ammonia-containing alkaline substances include ammonia water, ammonia gas, ammonium carbonate, or ammonium bicarbonate.

[0096] When the ammonia-containing alkaline substance is ammonia water, mixing with the ammonia-containing alkaline substance includes:

[0097] Add ammonia water dropwise to the diluted purified acid until the pH value reaches 4.0–4.5. The dropwise addition time is 30–90 minutes.

[0098] The neutralization reaction temperature is 65–80°C, for example, 70°C; after mixing with an ammonia-containing alkaline substance, the neutralization reaction time is 30–60 minutes, for example, 40 minutes.

[0099] The mother liquor obtained from filtration can be reused to dilute the purified acid or to prepare the calcium carbonate slurry in step a).

[0100] This invention adds concentrated sulfuric acid before concentration, which firstly increases the hydrogen ion activity of the residual acid, allowing more phosphoric acid to enter the solvent during purification and thus improving phosphorus yield; secondly, it pre-removes calcium during concentration, with the calcium existing in the form of calcium sulfate, reducing phosphorus loss during solvent purification. Using this invention, the final phosphorus yield can reach over 92%.

[0101] This invention is the first to use barium fluoride as a precipitant, utilizing the property of barium fluoride's easy solubility in alcohol solvents to precipitate Mg in acidic solvents. 2+ and SO4 2- Simultaneously remove, and leave residual F - and Ba 2+ The content is low. Furthermore, it avoids the need for stepwise addition of reagents for desulfurization and removal of metal cations at the later stages, simplifying the process. Using the technical solution of this invention, the final Mg content is... 2+ The removal rate of SO4 is over 95%. 2- With a removal rate of over 98%, the purified acid obtained can be used to prepare fire-grade monoammonium phosphate, and the product meets the standard requirements for fire-grade monoammonium phosphate.

[0102] This invention combines primary solvent purification and secondary precipitation purification. Primary solvent purification removes approximately 70% of impurities. The innovative use of barium fluoride also facilitates magnesium and sulfur removal. Secondary precipitation purification ultimately achieves an impurity removal rate exceeding 95%. This invention, combining solvent purification with precipitation purification, results in high impurity removal and phosphorus recovery rates, yielding a high-value fire-grade monoammonium phosphate product.

[0103] The present invention does not impose any special restrictions on the source of the raw materials used above, and they can be commercially available.

[0104] To further illustrate the present invention, the following detailed description of a method for preparing monoammonium phosphate using residual raffinate is provided in conjunction with embodiments, but it should not be construed as limiting the scope of protection of the present invention.

[0105] In the examples, the residual acid contained 22.46% P2O5 by mass and Ca... 2+ The mass content is 0.25%, Mg 2+ The mass content is 1.1%, Fe 3+ The mass content is 0.24%, Al 3+ The mass content is 0.28%, the mass content of SiO2 is 94ppm, and the mass content of SO4 is... 2- The mass content is 240 ppm, F - The mass content was 1085 ppm, Na + The mass content was 680 ppm, K + The mass content was 598 ppm, Cl - The mass content was 35 ppm, Cr 3+ The mass content was 22 ppm, Ba 2+ The mass content is 5.5 ppm.

[0106] Examples 1-5

[0107] Method for preparing monoammonium phosphate using the residual raffinate:

[0108] 1) Concentration and activation of residual acid: according to SO4 2- The mass ratio of P2O5 to P2O5 was R (see Table 1). Concentrated sulfuric acid was added to the residual raffinate and stirred until homogeneous. Then, vacuum concentration was carried out at 70℃ and 85 kPa. The concentration of P2O5 in the solution was as shown in Table 1. After filtration, precipitated phosphogypsum and concentrated solution were obtained. SO4 2- The mass ratio (R) of P2O5 and the properties of the resulting concentrate are shown in Table 1.

[0109] Table 1. R and the properties of the obtained concentrate (mass concentration, %)

[0110] R <![CDATA[P2O5 / %]]> Ca / % Mg / % Fe / % Al / % <![CDATA[SO4 2- / %]]> Example 1 5% 40.96 0.09 1.28 0.35 0.26 2.21 Example 2 10% 40.14 0.05 1.29 0.39 0.29 3.00 Example 3 15% 40.98 0.04 1.31 0.40 0.30 4.70 Example 4 20% 39.11 0.04 1.27 0.38 0.29 5.60 Example 5 30% 40.68 0.03 1.22 0.35 0.25 6.92

[0111] 2) Isopropanol is added dropwise to the concentrate (time controlled at 60 min), with a volume ratio of isopropanol to the concentrate of 2:1. After adding isopropanol, the mixture is reacted at 60°C for 50 min to complete the first-stage solvent purification. After the first-stage solvent purification, most of the phosphoric acid and a small amount of cationic impurities are transferred into the mixture of isopropanol and water (containing acid solvent). The remaining cationic impurities are transferred to the heavy phase. The distribution of each component in the acid solvent and the heavy phase is shown in Table 2. Due to detection errors, the sum of the ion or component distributions cannot reach an absolute 100%. Generally, a sum of 90% to 110% is considered acceptable.

[0112] After primary solvent purification, the phosphorus yield in Example 1 reached 75.44%, the phosphorus yield in Example 2 reached 84.31%, the phosphorus yield in Example 3 reached 87.81%, the phosphorus yield in Example 4 reached 92.95%, and the phosphorus yield in Example 5 reached 93.23%.

[0113] Table 2. Distribution of each component in acidic solvent and heavy phase.

[0114]

[0115] 3) The light and heavy mixed phase obtained from the primary solvent purification is allowed to stand and separate. The upper layer is the acid-containing solvent phase, and the lower layer is the impurity-containing heavy phase. The acid-containing solvent phase proceeds to the next purification step. Superphosphate is prepared using the impurity-containing heavy phase, calcium carbonate, and phosphogypsum:

[0116] a) Heating the heavy phase containing impurities to 95°C;

[0117] According to the P2O5 in the impure heavy phase and the Ca in calcium carbonate 2+ Weigh calcium carbonate at a mass ratio of 5:1 and add water to prepare a calcium carbonate slurry with a mass concentration of 60%.

[0118] The calcium carbonate slurry is added to the heavy phase containing impurities at a rate that prevents foam from overflowing, and then stirred until well mixed.

[0119] b) Weigh out phosphogypsum and add it to the slurry after mixing in step a) according to the mass ratio of phosphogypsum to P2O5 in the heavy phase containing impurities of 20:100, and stir until well mixed; the phosphogypsum is first obtained from the precipitated phosphogypsum in step 1), and the excess is added separately.

[0120] c) Dry the slurry after mixing in step b) at 100°C, crush and screen it to obtain the superphosphate product.

[0121] The parameters of the acid-containing solvent phase are shown in Table 3 (the "%" in Table 3 represents the mass concentration).

[0122] Table 3. Indicators of acid-containing solvent phases

[0123] <![CDATA[P2O5 / %]]> <![CDATA[Ca 2+ / ppm]]> <![CDATA[Mg 2+ / %]]> <![CDATA[Fe 3+ / %]]> <![CDATA[Al 3+ / %]]> <![CDATA[SO4 2- / %]]> Example 1 17.87 154 0.16 0.06 0.05 0.22 Example 2 19.95 62 0.21 0.10 0.06 0.68 Example 3 20.44 58 0.26 0.12 0.08 1.02 Example 4 19.95 64 0.29 0.12 0.08 1.2 Example 5 20.94 55 0.30 0.13 0.08 1.29

[0124] 4) Barium fluoride is added dropwise to the acid-containing solvent phase (the addition time is 60 min), and the Mg in the acid-containing solvent phase... 2+ and the F in the barium fluoride - The molar ratio was 1:2; after reacting at 60℃ for 40 min, the mixture was filtered to obtain a secondary purified acidic solvent and purified residue. Through secondary precipitation purification, in Example 1, Mg... 2+ The removal rate was 95.4%, SO42- 2- The removal rate was 96.5%; in Example 2, Mg 2+ The removal rate was 95.4%, SO42- 2- The removal rate was 98.6%; in Example 3, Mg 2+ The removal rate was 95.6% for SO4. 2- The removal rate was 98.9%; in Example 4, Mg 2+ The removal rate was 95.8%, SO42- 2- The removal rate was 98.8%; in Example 5, Mg 2+ The removal rate was 95.4%, SO42- 2- The removal rate was 98.5%.

[0125] 5) The secondary purified acidic solvent is vacuum distilled at 70℃ and 85KPa to recover the solvent. The resulting regenerated solvent is returned to the primary solvent purification process for recycling. The residue in the distillation vessel is the purified acid. The indicators of the purified acid are shown in Table 4 (the "%" in Table 4 represents the mass concentration).

[0126] Table 4 Indicators for Purified Acid

[0127] <![CDATA[P2O5 / %]]> <![CDATA[Ca 2+ / ppm]]> <![CDATA[Mg 2+ / ppm]]> <![CDATA[Fe 3+ / ppm]]> <![CDATA[Al 3+ / ppm]]> <![CDATA[SO4 2- / ppm]]> <![CDATA[F - / ppm]]> <![CDATA[Ba 2+ / ppm]]> Example 1 50.23 25 390 184 655 124 155 273 Example 2 50.19 21 540 200 800 220 142 245 Example 3 49.53 24 640 210 820 263 166 249 Example 4 50.05 24 620 202 800 327 176 275 Example 5 50.45 18 650 221 863 339 156 236

[0128] 6) Dilute the purified acid with water (the mass ratio of purified acid to water is 1:1), and add ammonia dropwise to the diluted purified acid until the pH value is 4.0-4.5, with the addition time being 60 min; then, react at 70℃ for 40 min, filter, dry and granulate the filter cake to obtain fire-fighting grade monoammonium phosphate product. The mother liquor obtained from filtration is reused to dilute the purified acid or to prepare the calcium carbonate slurry in step a). The indicators of the fire-fighting grade monoammonium phosphate product are shown in Table 5.

[0129] Table 5. Specifications of fire-fighting grade monoammonium phosphate products

[0130] <![CDATA[NH4H2PO4 / wt%]]> Moisture / wt% <![CDATA[Bulk density / (g / cm 3 )]]> Moisture absorption rate / % Example 1 95.9 0.91 0.82 2.5 Example 2 95.5 0.91 0.78 2.5 Example 3 95.7 0.89 0.71 2.2 Example 4 94.9 0.89 0.73 2.4 Example 5 94.4 0.86 0.71 3.1 Fire-grade monoammonium phosphate quality standards ≥90.0 ≤1.0 ≥0.65 ≤4.0

[0131] Example 6

[0132] The difference from Example 3 is as follows:

[0133] Replace isopropanol with n-butanol in step 2). In step 2), after primary solvent purification, the phosphorus yield is 88.24%; in step 4), after secondary precipitation purification, the Mg yield is... 2+ The removal rate was 84.3%, SO4 2- The removal rate was 85.5%.

[0134] Example 7

[0135] The difference from Example 3 is as follows:

[0136] Replace isopropanol with ethanol in step 2). In step 2), after primary solvent purification, the phosphorus yield is 82.2%; in step 4), after secondary precipitation purification, the Mg yield is... 2+ The removal rate was 95.5% for SO4. 2- The removal rate was 96.8%.

[0137] Example 8

[0138] The difference from Example 3 is as follows:

[0139] Replace isopropanol with methanol in step 2). In step 2), phosphorus recovery is 92.2% after primary solvent purification; in step 4), Mg recovery is 92.2% after secondary precipitation purification. 2+ The removal rate was 92.8%, SO4 2- The removal rate was 92.5%.

[0140] Example 9

[0141] The difference from Example 3 is as follows:

[0142] Replace the ammonia in step 6) with ammonium carbonate.

[0143] Example 10

[0144] The difference from Example 3 is as follows:

[0145] Replace the ammonia in step 6) with ammonium bicarbonate.

[0146] Example 11

[0147] The difference from Example 4 is as follows:

[0148] In step 2), isopropanol was replaced with dimethyl ether. In step 2), after primary solvent purification, the phosphorus yield was 78.2%; in step 4), after secondary precipitation purification, Mg... 2+ The removal rate was 92.7%, SO4 2- The removal rate was 95.5%.

[0149] Example 12

[0150] The difference from Example 4 is as follows:

[0151] Replace isopropanol with acetone in step 2). In step 2), after primary solvent purification, the phosphorus yield is 88.5%; in step 4), after secondary precipitation purification, the Mg yield is... 2+ The removal rate was 94.3%, SO42- 2- The removal rate was 96.9%.

[0152] Comparative Example 1

[0153] The difference from Example 4 is as follows:

[0154] Replace barium fluoride in step 4) with calcium fluoride. In step 4), Mg is purified through secondary precipitation. 2+ The removal rate was 33.1%, SO4 2- The removal rate was 45%.

[0155] Comparative Example 2

[0156] The difference from Example 4 is as follows:

[0157] If the ammonia in step 6) is replaced with ammonium sulfate, ammonium nitrate or ammonium chloride, monoammonium phosphate cannot be produced.

[0158] The specifications of the monoammonium phosphate products obtained in Examples 6-12 and Comparative Examples 1-4 are shown in Table 6.

[0159] Table 6. Indicators of Monoammonium Phosphate Products

[0160] NH4H2PO4 / wt% Moisture / wt% <![CDATA[Bulk density / (g / cm 3 )]]> Moisture absorption rate / % Example 6 89.9 1.00 0.86 3.9 Example 7 94.5 0.89 0.77 2.5 Example 8 91.4 0.78 0.80 3.1 Example 9 93.7 0.95 0.88 3.6 Example 10 93.9 0.91 0.84 3.6 Example 11 91.4 0.79 0.76 3.0 Example 12 92.6 0.76 0.73 3.1 Comparative Example 1 84.9 1.32 0.89 4.5 Fire-grade monoammonium phosphate quality standards ≥90.0 ≤1.0 ≥0.65 ≤4.0

[0161] The descriptions of the above embodiments are merely illustrative of the methods and core ideas of the present invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing monoammonium phosphate using residual raffinate, comprising the following steps: S1) Mix the residual acid with concentrated sulfuric acid, concentrate the mixture, and then separate the solid and liquid phases to obtain the concentrated solution. S2) A solvent is added dropwise to the concentrate for primary solvent purification; the solvent includes at least one of isopropanol, n-butanol, ethanol, methanol, dimethyl ether, and acetone; the volume ratio of the solvent to the concentrate is 1~3.5:1; the time for adding the solvent dropwise is controlled at 30~90 min; the temperature for primary solvent purification is 55~65℃. S3) The light and heavy mixed phase obtained by the purification of the primary solvent is allowed to stand and separate into two phases: the upper layer is the acid-containing solvent phase and the lower layer is the impurity-containing heavy phase. S4) The acid-containing solvent phase is mixed with barium fluoride to carry out the reaction, and F is released from the dissociation of barium fluoride. - and Ba 2+ Remove Mg from the acid-containing solvent phase 2+ and SO4 2- After solid-liquid separation, a secondary purified acidic solvent and purified residue are obtained; S5) Vacuum distill the acidic solvent in the secondary purification process to recover the solvent. The resulting regenerated solvent is returned to the primary solvent purification process for recycling. The residue in the distillation kettle is the purified acid. S6) The purified acid is diluted and then mixed with an ammonia-containing alkaline substance to carry out a neutralization reaction. After the reaction, the mixture is filtered, the filter cake is dried and granulated to obtain fire-fighting grade monoammonium phosphate product. The ammonia-containing alkaline substances include ammonia water, ammonia gas, ammonium carbonate, or ammonium bicarbonate.

2. The method according to claim 1, characterized in that, In step S1), concentrated sulfuric acid and residual raffinate are mixed according to SO4. 2- Mix with P2O5 at a mass ratio of 4.2~30:

100.

3. The method according to claim 1, characterized in that, In step S1), the concentration method includes vacuum concentration, atmospheric pressure concentration, or one-stage single-effect atmospheric pressure concentration followed by one-stage double-effect vacuum concentration. The vacuum degree of the vacuum concentration is 80~90 kPa; after concentration, the mass concentration of P2O5 in the solution is 23%~54%.

4. The method according to claim 1, characterized in that, In step S2), the time for primary solvent purification after adding solvent is 10~90 min.

5. The method according to claim 1, characterized in that, In step S3), the pH value of the acid-containing solvent phase is 0.8~1.

2.

6. The method according to claim 1, characterized in that, In step S3), after obtaining the impurity-containing heavy phase, the process further includes: Superphosphate is prepared using a heavy phase containing impurities, calcium carbonate, and phosphogypsum; the phosphogypsum includes the precipitated phosphogypsum obtained in step S1). The P2O5 in the impure heavy phase and the Ca in calcium carbonate 2+ The mass ratio is 4.8~5.2:1; the mass ratio of phosphogypsum to P2O5 in the impurity heavy phase is 18~22:

100.

7. The method according to claim 1, characterized in that, In step S4), the Mg in the acid-containing solvent phase 2+ and the F in the barium fluoride - The molar ratio is 1:

2.

8. The method according to claim 1, characterized in that, In step S4), mixing the acid-containing solvent phase with barium fluoride includes: Barium fluoride is added dropwise to the acid-containing solvent phase; the dropwise addition time is 30-120 min. The reaction temperature is 55~65℃; the reaction time after mixing is 10~60 min.

9. The method according to claim 1, characterized in that, In step S5), the temperature of the vacuum distillation is 60~80℃ and the vacuum degree is 80~90 KPa.

10. The method according to claim 1, characterized in that, In step S6), the dilution is achieved by adding water; the mass ratio of the purified acid to water is 0.8~1.2:0.8~1.

2. When the ammonia-containing alkaline substance is ammonia water, mixing with the ammonia-containing alkaline substance includes: Ammonia water is added dropwise to the diluted purified acid until the pH value reaches 4.0-4.5; the dropwise addition time is 30-90 minutes. The neutralization reaction temperature is 65~80℃; after mixing with ammonia-containing alkaline substances, the neutralization reaction time is 30~60min.

Citation Information

Patent Citations

  • Method for purifying raffinate acid

    CN101704518B

  • Method for preparing MAP and water-soluble fertilizer thereof by utilizing reextraction residual acid