Multifunctional electronic product screen protection film and preparation method thereof

By adopting a multi-layer structural design in the screen protector of electronic products, combined with the modified base film, gradient density elastic buffer layer and self-healing layer, the shortcomings of the existing protective film in terms of scratch resistance, bonding and explosion-proof screen performance are solved. , achieving higher protection effect and user experience.

CN119502517APending Publication Date: 2025-02-25东莞市鸿富瀚科技有限公司

Patent Information

Application Number
CN202411628023.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-14
Publication Date
2025-02-25

AI Technical Summary

Technical Problem

The existing electronic product screen protectors have shortcomings in scratch resistance, fitting performance and explosion-proof screen performance, which is difficult to effectively protect the screen, affecting service life and user experience.

Method used

The multi-layer structural design is adopted, including a modified base film, a gradient density elastic buffer layer and a self-healing layer, and the overall performance of the protective film is improved through the combination of these layers. The modified base film provides base strength, the elastic buffer layer enhances the explosion-proof screen performance, and the self-healing layer achieves scratch resistance and self-healing functions.

Benefits of technology

It significantly improves the scratch resistance, self-repair ability, explosion-proof screen performance, fit and anti-static properties of the protective film, extends the service life of the screen and improves the user experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119502517A_ABST
    Figure CN119502517A_ABST
Patent Text Reader

Abstract

The invention discloses a multifunctional electronic product screen protective film and a preparation method thereof. The protective film comprises a modified base film and a multifunctional composite layer compounded on the surface of the modified base film, the multifunctional composite layer comprises an elastic buffer layer and a self-repairing layer which are sequentially arranged from inside to outside; wherein the elastic buffer layer is an elastic buffer layer with gradient density; the elastic buffer layer comprises the following components in parts by weight: 100 parts of a thermoplastic polyurethane elastomer, 15-25 parts of hollow glass microspheres, 10-15 parts of polyethylene glycol and 3-6 parts of an isocyanate cross-linking agent; the self-repairing layer comprises the following components in parts by weight: 100 parts of a dynamic reversible covalent bond polymer, 30-40 parts of phase change material microcapsules, 10-15 parts of nano cellulose, 5-8 parts of a near-infrared photosensitive initiator and 2-4 parts of an antioxidant. Compared with the prior art, the protective film provided by the invention has excellent scratch self-repairing performance, good adhesion and high anti-explosion screen performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic product protective films, and in particular to a multifunctional electronic product screen protective film and a preparation method thereof. Background Art

[0002] With the increasing popularity and widespread use of electronic products, people have placed higher demands on screen protection. The screens of electronic products such as mobile phones and tablets are susceptible to damage from daily use, such as scratches, abrasions, and cracks, which seriously affect the device's lifespan and user experience. To protect the screens of electronic products, a variety of screen protector products have emerged on the market.

[0003] While existing screen protectors can protect electronic device screens to a certain extent, they still have many shortcomings. First, many screen protectors lack scratch resistance. Despite claiming high scratch resistance, they are still prone to scratches in actual use. These scratches not only affect the appearance but also reduce the visibility and touch sensitivity of the screen. More importantly, these scratches are often unable to repair themselves and are permanent once they appear, seriously affecting the user's viewing experience.

[0004] Secondly, the adhesion of existing screen protectors needs to be improved. Many screen protectors have poor ductility or elasticity, making it difficult to achieve a perfect fit with electronic product screens. This can lead to problems such as bubbles, warping, and detachment between the screen and the film, which not only affects the appearance but also reduces the protective effect. If the protective film warps or detaches, dust and moisture can enter the gap between the film and the screen, further exacerbating damage.

[0005] Furthermore, existing screen protectors lack the necessary protection against explosions. When electronic products are accidentally dropped or impacted, standard screen protectors are unable to effectively absorb and disperse the force, causing the screen to crack, break, or suffer other serious damage. This not only results in financial losses for users but can also pose safety risks, especially for large electronic products like tablets.

[0006] Therefore, there is an urgent need to develop a multifunctional electronic product screen protective film that can effectively solve the shortcomings of existing products in terms of scratch resistance, adhesion and explosion-proof screen performance. Summary of the Invention

[0007] The main purpose of the present invention is to provide a multifunctional electronic product screen protective film and a preparation method thereof in response to the deficiencies of the existing technology. The protective film has excellent scratch self-repairing performance, good adhesion and high explosion-proof screen performance.

[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] A multifunctional electronic product screen protective film, comprising a modified base film and a multifunctional composite layer composited on the surface of the modified base film; the multifunctional composite layer comprises an elastic buffer layer and a self-repairing layer arranged in sequence from the inside out;

[0010] The elastic buffer layer has a gradient density, wherein the density is lower on the side close to the base film and higher on the side away from the base film, and the density gradient satisfies the following relationship:

[0011] ρ(x)=ρ0+kx n ;

[0012] Where ρ(x) is the density at a distance x from the base film (g / cm 3 );ρ0 is the minimum density near the basement membrane, and the value range of ρ0 is 0.8-1.0g / cm 3 ; k is the density gradient coefficient, and the value range of k is 0.005-0.015g / cm 3 μm -n ; x is the distance from the basement membrane (μm); n is the gradient index, and the value range of n is 1.2-1.8;

[0013] The elastic buffer layer comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer (TPU), 15-25 parts of hollow glass microspheres, 10-15 parts of polyethylene glycol (PEG), and 3-6 parts of isocyanate crosslinking agent;

[0014] The self-repairing layer comprises the following components in parts by weight: 100 parts of a dynamically reversible covalent bond polymer, 30-40 parts of a phase change material microcapsule, 10-15 parts of nanocellulose, 5-8 parts of a near-infrared photosensitive initiator, and 2-4 parts of an antioxidant.

[0015] Preferably, the modified base film comprises the following components by weight: 100 parts polyethylene terephthalate (PET), 3-7 parts graphene, 2-5 parts ionic liquid antistatic agent, and 1-3 parts benzotriazole UV absorber. PET provides base strength and transparency, graphene enhances mechanical strength and thermal conductivity, the ionic liquid antistatic agent prevents static electricity accumulation, and the UV absorber protects the product from UV damage; this combination improves the overall performance of the base film.

[0016] Preferably, the ionic liquid antistatic agent is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. This ionic liquid has excellent thermal stability and conductivity, maintaining its antistatic effect over a wide temperature range without affecting the transparency of the base film. Its unique ionic structure enables rapid charge transfer at the molecular level, effectively preventing static electricity accumulation. Its excellent thermal stability ensures a sustained effect in various operating environments.

[0017] Preferably, the phase change material microcapsule comprises a core material and a shell material coated on the surface of the core material, the core material is a mixture of octadecanoic acid and hexadecanoic acid, and the shell material is polymethyl methacrylate;

[0018] The preparation method of the phase change material microcapsules comprises the following steps: a) mixing octadecanoic acid and hexadecanoic acid in a mass ratio of 3:1, and heating to 80° C. to completely fuse them; b) dissolving methyl methacrylate, azobisisobutyronitrile (AIBN) and 1,6-hexanediol dimethacrylate in deionized water, and adding a small amount of sodium lauryl sulfate as an emulsifier; c) slowly adding the mixture in step a) to the solution in step b), and emulsifying at high speed shearing at 80° C. for 30 minutes; d) heating the emulsion to 85° C. under nitrogen protection, and reacting for 4 hours; and e) cooling to room temperature, filtering, washing with water, and drying to obtain the phase change material microcapsules.

[0019] When damaged by scratches or other factors, the phase change material microcapsules rupture, releasing the phase change material. These materials, in the process of absorbing or releasing latent heat, provide additional energy and increased mobility to the surrounding polymer chains, thereby promoting the self-healing process. The microcapsules prepared by this method have good encapsulation efficiency and thermal stability, and can provide stable phase change latent heat during the self-healing process, enhancing the self-healing effect.

[0020] Preferably, the hollow glass microspheres in the elastic buffer layer have an average particle size of 20-50 μm and a wall thickness of 0.5-2 μm.

[0021] Preferably, the nanocellulose in the self-repairing layer has a length of 100-500 nm and a diameter of 5-20 nm.

[0022] Preferably, the thickness of the elastic buffer layer is 150-250 μm, and the thickness of the self-repairing layer is 20-40 μm.

[0023] Preferably, the near-infrared photoinitiator in the self-repairing layer is a manganese-based metal porphyrin complex.

[0024] Preferably, the self-healing layer further comprises 5-10 parts by weight of polydopamine and 2-6 parts by weight of fluorinated graphene. Polydopamine has excellent adhesion and self-healing properties, and the catechol groups on its molecular chain can form reversible hydrogen bonds and coordination bonds. These dynamic bonds can be quickly rebuilt after being damaged by external forces, further enhancing the repair ability and adhesion strength of the self-healing layer; fluorinated graphene is used to provide hydrophobic and anti-fingerprint properties.

[0025] Preferably, the surface of the self-repairing layer is coated with a 1-3 μm thick fluorosilane-modified silica nanoparticle coating;

[0026] The preparation method of the fluorosilane-modified silica nanoparticle coating is as follows: a) dispersing 1 weight part of nano-silica powder in 50 weight parts of anhydrous ethanol, ultrasonically treating for 15 minutes to obtain a suspension; adding 0.5 weight parts of 1H,1H,2H,2H-perfluorooctyltriethoxysilane (PFOTES) to the above suspension, and continuing ultrasonic treatment for 10 minutes; adding 0.5 mL of deionized water, stirring at room temperature for 2 hours to obtain a coating solution; b) immersing the surface of the self-repairing layer in the coating solution by a dip coating method, with an immersion and pulling speed of 2 mm / s; air drying at room temperature for 5 minutes; and heat treating at 80°C for 30 minutes; c) controlling the final coating thickness within the range of 1-3 μm by adjusting the coating solution concentration and the number of dip coatings, wherein the coating solution concentration is 1-3wt% and the number of dip coatings is 1-3 times.

[0027] The fluorosilane-modified silica nanoparticle coating provides excellent hydrophobic and antifouling properties. The low surface energy of fluorosilane combined with the microscopic roughness of the silica nanoparticles creates a superhydrophobic surface, effectively preventing the adhesion of water, oil, and other stains. As a result, the fluorosilane-modified silica nanoparticle coating prepared by this method exhibits superhydrophobic and antifouling properties, with a contact angle greater than 150° and a sliding angle less than 5°, effectively preventing the adhesion of fingerprints and stains.

[0028] Preferably, the self-repairing layer contains 1-3 parts by weight of upconversion luminescent nanoparticles NaYF4:Yb,Er. These nanoparticles can convert near-infrared light into visible light, providing additional energy during the self-repairing process, accelerating the repair reaction, and also serving as an anti-counterfeiting mark.

[0029] Preferably, a conductive layer with a thickness of 2-6 μm is provided between the modified base film and the elastic buffer layer, and the conductive layer is composed of poly 3,4-ethylenedioxythiophene (PEDOT), polystyrene sulfonate (PSS) and silver nanowires in a mass ratio of (50-58): (40-48): (0.5-2). This conductive layer not only enhances the antistatic properties of the protective film, but also enables the protective film to have a capacitive touch function and is compatible with the touch system of the electronic device. Among them, PEDOT and PSS provide basic conductivity, while the silver nanowire network greatly improves the conductive efficiency, allowing the protective film to be seamlessly integrated with the device touch system.

[0030] In addition, the present invention also provides a method for preparing the multifunctional electronic product screen protective film, comprising the following steps:

[0031] 1) Preparing a modified base film: mixing PET, graphene, an ionic liquid antistatic agent, and a benzotriazole ultraviolet absorber, and extruding the mixture through a twin-screw extruder at 260-280° C. at a line speed of 5-8 m / min to prepare a modified base film;

[0032] 2) preparing an elastic buffer layer: mixing TPU, hollow glass microspheres, PEG, and an isocyanate crosslinker, and preparing an elastic buffer layer with a gradient density by solution casting;

[0033] 3) Preparation of self-repairing layer:

[0034] a) Synthesis of a dynamically reversible covalently bonded polymer: 4,4'-diaminoazobenzene and maleic anhydride are reacted in N,N-dimethylformamide (DMF) at 60-70°C for 4-6 hours to obtain a prepolymer containing a Diels-Alder addition product;

[0035] b) mixing the prepolymer with phase change material microcapsules, nanocellulose, near-infrared photoinitiator and antioxidant, and stirring at 80-90° C. under nitrogen protection;

[0036] c) coating the mixture on a release film treated with silicone oil to a thickness of 20-40 μm, and vacuum drying at 80-100° C. for 2-4 hours to obtain a self-healing layer;

[0037] 4) Compounding the elastic buffer layer on the surface of the modified base film by roller pressing at a pressure of 0.5-1.0 MPa and a temperature of 60-80°C;

[0038] 5) Transferring the self-healing layer to the surface of the elastic buffer layer by hot pressing, with a pressure of 1.0-1.5 MPa, a temperature of 100-120°C, and a holding time of 30-60 seconds;

[0039] 6) Annealing at 80-100° C. for 2-4 hours to prepare a multifunctional electronic product screen protective film.

[0040] Compared with the prior art, the present invention has at least the following beneficial effects:

[0041] 1) The present invention adopts a multi-layer structure design of a modified base film, an elastic buffer layer and a self-repairing layer. This multi-layer structure design enables the protective film to provide all-round screen protection while maintaining lightness and thinness; the modified base film provides basic strength and stability, the elastic buffer layer enhances the explosion-proof screen performance, and the self-repairing layer provides scratch resistance and self-repairing functions, together realizing the multifunctionality of the protective film.

[0042] 2) The elastic buffer layer of the present invention adopts a unique gradient density design, with lower density on the side close to the base film and higher density on the side away from the base film. This gradient density design significantly improves the explosion-proof performance of the protective film. When impacted by external forces, the lower-density side can effectively absorb and disperse energy, while the higher-density side provides sufficient strength to protect the screen. This structure can also improve the fit between the protective film and the device screen and reduce the generation of bubbles. The elastic buffer layer is composed of TPU, hollow glass microspheres, PEG, and isocyanate crosslinkers. TPU provides good elasticity and toughness, hollow glass microspheres enhance the buffering effect and reduce weight, PEG improves the flexibility of the material, and the isocyanate crosslinker enhances the stability of the overall structure. This combination ensures both the elasticity of the buffer layer and sufficient strength and durability.

[0043] 3) The self-repairing layer of the present invention comprises a dynamically reversible covalent bond polymer, a phase change material microcapsule, nanocellulose, a near-infrared photosensitive initiator and an antioxidant; wherein, the dynamically reversible covalent bond polymer provides self-repairing ability, and the phase change material microcapsule can release the phase change material when scratched, providing additional energy and fluidity for the self-repair process, thereby promoting the self-repair process; the nanocellulose enhances the strength and toughness of the material, the near-infrared photosensitive initiator enables the self-repair process to be carried out under natural light, and the antioxidant extends the life of the material; the self-repairing layer achieves excellent scratch resistance and self-repairing ability. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 Schematic diagram of the three-dimensional structure of a protective film in one embodiment of the present invention;

[0045] Figure 2 is a schematic diagram of the cross-sectional structure of a protective film in one embodiment of the present invention;

[0046] Figure 3 is a schematic diagram of the three-dimensional structure of a protective film in another embodiment of the present invention;

[0047] Figure 4 Schematic diagram of the cross-sectional structure of a protective film in another embodiment of the present invention.

[0048] In the figure: 1. Modified base film; 2. Elastic buffer layer; 3. Self-healing layer; 4. Fluorosilane-modified silica nanoparticle coating. DETAILED DESCRIPTION

[0049] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0050] Please see the attached Figures 1-2 According to the first aspect of the present application, a multifunctional electronic product screen protective film is provided, comprising a modified base film 1 and a multifunctional composite layer composited on the surface of the modified base film 1; the multifunctional composite layer comprises an elastic buffer layer 2 and a self-repairing layer 3 arranged sequentially from the inside out;

[0051] The elastic buffer layer 2 is an elastic buffer layer 2 with a gradient density, wherein the density is lower on the side close to the base film and higher on the side away from the base film, and the density gradient satisfies the following relationship:

[0052] ρ(x)=ρ0+kx n ;

[0053] Where ρ(x) is the density at a distance x from the base film (g / cm 3 );ρ0 is the minimum density near the basement membrane, and the value range of ρ0 is 0.8-1.0g / cm 3 ; k is the density gradient coefficient, and the value range of k is 0.005-0.015g / cm 3 μm -n ; x is the distance from the basement membrane (μm); n is the gradient index, and the value range of n is 1.2-1.8;

[0054] The elastic buffer layer 2 comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer (TPU), 15-25 parts of hollow glass microspheres, 10-15 parts of polyethylene glycol (PEG), and 3-6 parts of isocyanate crosslinking agent;

[0055] The self-repairing layer 3 comprises the following components in parts by weight: 100 parts of a dynamically reversible covalent bond polymer, 30-40 parts of phase change material microcapsules, 10-15 parts of nanocellulose, 5-8 parts of a near-infrared photosensitive initiator, and 2-4 parts of an antioxidant.

[0056] In one embodiment of the present invention, the modified base film 1 comprises the following components by weight: 100 parts polyethylene terephthalate (PET), 3-7 parts graphene, 2-5 parts ionic liquid antistatic agent, and 1-3 parts benzotriazole UV absorber. The PET provides base strength and transparency, the graphene enhances mechanical strength and thermal conductivity, the ionic liquid antistatic agent prevents static electricity accumulation, and the UV absorber protects the product from UV damage. This combination improves the overall performance of the base film.

[0057] In one embodiment of the present application, the ionic liquid antistatic agent is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. This ionic liquid has excellent thermal stability and conductivity, maintaining its antistatic effect over a wide temperature range without affecting the transparency of the base film. Its unique ionic structure enables rapid charge transfer at the molecular level, effectively preventing static electricity accumulation. Its excellent thermal stability ensures a sustained effect in various operating environments.

[0058] In one embodiment of the present application, the phase change material microcapsule includes a core material and a shell material coated on the surface of the core material, the core material is a mixture of octadecanoic acid and hexadecanoic acid, and the shell material is polymethyl methacrylate;

[0059] The preparation method of the phase change material microcapsule is as follows:

[0060] a) mixing octadecanoic acid and hexadecanoic acid in a mass ratio of 3:1 and heating to 80° C. to completely blend;

[0061] b) dissolving methyl methacrylate, azobisisobutyronitrile (AIBN) and 1,6-hexanediol dimethacrylate in deionized water, and adding a small amount of sodium lauryl sulfate as an emulsifier;

[0062] c) slowly adding the mixture from step a) to the solution from step b), and emulsifying under high shearing conditions at 80° C. for 30 minutes;

[0063] d) Under nitrogen protection, the emulsion was heated to 85° C. and reacted for 4 hours;

[0064] e) cooling to room temperature, filtering, washing with water, and drying to obtain phase change material microcapsules.

[0065] When damaged by scratches or other factors, the phase change material microcapsules rupture, releasing the phase change material. These materials, in the process of absorbing or releasing latent heat, provide additional energy and increased mobility to the surrounding polymer chains, thereby promoting the self-healing process. The microcapsules prepared by this method have good encapsulation efficiency and thermal stability, and can provide stable phase change latent heat during the self-healing process, enhancing the self-healing effect.

[0066] In one embodiment of the present application, the average particle size of the hollow glass microspheres in the elastic buffer layer 2 is 20-50 μm, for example, 20 μm, 30 μm, 40 μm or 50 μm; the wall thickness is 0.5-2 μm, for example, 0.5 μm, 1 μm, 1.5 μm or 2 μm.

[0067] In one embodiment of the present application, the nanocellulose in the self-healing layer 3 has a length of 100-500 nm, for example, 100 nm, 200 nm, 300 nm, 400 nm or 500 nm; and a diameter of 5-20 nm, for example, 5 nm, 10 nm, 15 nm or 20 nm.

[0068] In one embodiment of the present application, the thickness of the elastic buffer layer 2 is 150-250 μm, for example, it can be 150 μm, 180 μm, 200 μm, 230 μm or 250 μm; the thickness of the self-repairing layer 3 is 20-40 μm, for example, it can be 20 μm, 30 μm or 40 μm.

[0069] In one embodiment of the present application, the near-infrared photoinitiator in the self-repairing layer 3 is a manganese-based metal porphyrin complex, and the antioxidant is 2,6-di-tert-butyl-4-methylphenol (BHT).

[0070] In one embodiment of the present application, the self-healing layer 3 further comprises 5-10 parts by weight of polydopamine and 2-6 parts by weight of fluorinated graphene. Polydopamine has excellent adhesion and self-healing properties, and the catechol groups on its molecular chain can form reversible hydrogen bonds and coordination bonds. These dynamic bonds can be quickly rebuilt after being damaged by external forces, further enhancing the repair ability and adhesion strength of the self-healing layer 3. The fluorinated graphene is used to provide hydrophobic and anti-fingerprint properties.

[0071] In one embodiment according to the present application, Figures 3-4 As shown, the surface of the self-repairing layer 3 is coated with a 1-3 μm thick fluorosilane modified silica nanoparticle coating 4;

[0072] The preparation method of the fluorosilane-modified silica nanoparticle coating 4 is as follows:

[0073] a) dispersing 1 part by weight of nano-silica powder in 50 parts by weight of anhydrous ethanol and ultrasonically treating for 15 minutes to prepare a suspension; adding 0.5 parts by weight of 1H,1H,2H,2H-perfluorooctyltriethoxysilane (PFOTES) to the suspension and ultrasonically treating for 10 minutes; adding 0.5 mL of deionized water and stirring at room temperature for 2 hours to obtain a coating solution;

[0074] b) immersing the surface of the self-repairing layer 3 into the coating solution using a dip coating method at an immersion and pulling speed of 2 mm / s; air-drying at room temperature for 5 minutes; and heat treating at 80° C. for 30 minutes;

[0075] c) controlling the final coating thickness within the range of 1-3 μm by adjusting the coating solution concentration and the number of dipping times, wherein the coating solution concentration is 1-3 wt % and the number of dipping times is 1-3 times.

[0076] The fluorosilane-modified silica nanoparticle coating 4 provides excellent hydrophobic and antifouling properties. The low surface energy of fluorosilane combined with the microscopic roughness of the silica nanoparticles creates a superhydrophobic surface, effectively preventing the adhesion of water, oil, and other stains. As a result, the fluorosilane-modified silica nanoparticle coating 4 prepared by this method exhibits superhydrophobic and antifouling properties, with a contact angle greater than 150° and a sliding angle less than 5°, effectively preventing the adhesion of fingerprints and stains.

[0077] In one embodiment of the present application, 1-3 parts by weight of upconversion luminescent nanoparticles NaYF4:Yb,Er are added to the self-repairing layer 3. These nanoparticles can convert near-infrared light into visible light, providing additional energy during the self-repair process, accelerating the repair reaction, and also serving as an anti-counterfeiting mark.

[0078] In one embodiment of the present application, a conductive layer with a thickness of 2-6 μm is provided between the modified base film 1 and the elastic buffer layer 2. The conductive layer is composed of poly 3,4-ethylenedioxythiophene (PEDOT), polystyrene sulfonate (PSS) and silver nanowires in a mass ratio of (50-58): (40-48): (0.5-2). This conductive layer not only enhances the antistatic properties of the protective film, but also enables the protective film to have a capacitive touch function, which is compatible with the touch system of the electronic device. Among them, PEDOT and PSS provide basic conductivity, while the silver nanowire network greatly improves the conductive efficiency, allowing the protective film to be seamlessly integrated with the device touch system.

[0079] In one embodiment of the present application, both side surfaces of the protective film are respectively covered with PET release films. Before covering the screen of the electronic product, the release films on both sides need to be torn off respectively.

[0080] According to the second aspect of the present application, the present application also provides a method for preparing the above-mentioned multifunctional electronic product screen protective film, comprising the following steps:

[0081] 1) Preparing a modified base film 1: mixing PET, graphene, an ionic liquid antistatic agent, and a benzotriazole ultraviolet absorber, and extruding the mixture through a twin-screw extruder at 260-280° C. at a line speed of 5-8 m / min to prepare a modified base film 1;

[0082] 2) preparing the elastic buffer layer 2: mixing TPU, hollow glass microspheres, PEG and isocyanate crosslinking agent, and preparing the elastic buffer layer 2 with gradient density by solution casting;

[0083] 3) Preparation of self-repairing layer 3:

[0084] a) Synthesis of a dynamically reversible covalently bonded polymer: 4,4'-diaminoazobenzene and maleic anhydride are reacted in N,N-dimethylformamide (DMF) at 60-70°C for 4-6 hours to obtain a prepolymer containing a Diels-Alder addition product;

[0085] b) mixing the prepolymer with phase change material microcapsules, nanocellulose, near-infrared photoinitiator and antioxidant, and stirring at 80-90° C. under nitrogen protection;

[0086] c) coating the mixture on a release film treated with silicone oil to a thickness of 20-40 μm, and vacuum drying at 80-100° C. for 2-4 hours to obtain a self-repairing layer 3;

[0087] 4) The elastic buffer layer 2 is laminated on the surface of the modified base film 1 by a roller pressing method at a pressure of 0.5-1.0 MPa and a temperature of 60-80° C.;

[0088] 5) Transfer the self-repairing layer 3 to the surface of the elastic buffer layer 2 by hot pressing, with a pressure of 1.0-1.5 MPa, a temperature of 100-120°C, and a holding time of 30-60 seconds;

[0089] 6) Annealing at 80-100° C. for 2-4 hours to prepare a multifunctional electronic product screen protective film.

[0090] The following embodiments of the present invention are described in detail. The following embodiments are illustrative and are intended only to explain the present invention and are not to be construed as limiting the present invention. All reagents and instruments used without manufacturer's indication are commercially available conventional products.

[0091] Example 1

[0092] 1) Preparation of modified base film 1

[0093] 100 parts by weight of PET, 5 parts by weight of graphene, 3 parts by weight of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide and 2 parts by weight of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole were mixed and extruded through a twin-screw extruder at 270° C. with a linear speed of 6 m / min to obtain a modified base film 1.

[0094] 2) Preparation of elastic buffer layer 2

[0095] 100 parts by weight of TPU, 20 parts by weight of hollow glass microspheres with an average particle size of 35 μm and a wall thickness of 1 μm, 12 parts by weight of PEG (molecular weight 4000) and 4 parts by weight of hexamethylene diisocyanate were mixed to prepare an elastic buffer layer 2 with a gradient density by solution casting. The minimum density ρ0 near the base film was 0.9 g / cm 3, the density gradient coefficient k is 0.01 g / cm 3 μm -n , the gradient index n is 1.5. The thickness of the elastic buffer layer 2 is 200 μm.

[0096] 3) Preparation of self-repairing layer 3

[0097] a) Synthesis of a dynamically reversible covalently bonded polymer: 4,4'-diaminoazobenzene and maleic anhydride were reacted in a molar ratio of 1:2 in DMF at 65°C for 5 hours to obtain a prepolymer containing a Diels-Alder addition product.

[0098] b) 100 parts by weight of the above prepolymer was mixed with 35 parts by weight of phase change material microcapsules, 12 parts by weight of nanocellulose (length 300 nm, diameter 10 nm), 6 parts by weight of manganese-based metalloporphyrin complex and 3 parts by weight of antioxidant (BHT), and stirred at 85° C. under nitrogen protection.

[0099] c) The mixture was coated on a release film treated with silicone oil to a thickness of 30 μm, and vacuum dried at 90° C. for 3 hours to obtain a self-repairing layer 3.

[0100] 4) Assembly of multi-layer structures

[0101] a) The elastic buffer layer 2 is compounded on the surface of the modified base film 1 by a roller pressing method at a pressure of 0.8 MPa and a temperature of 70°C.

[0102] b) The self-repairing layer 3 is transferred to the surface of the elastic buffer layer 2 by hot pressing, with a pressure of 1.2 MPa, a temperature of 110° C., and a holding time of 45 seconds.

[0103] c) annealing the film at 90° C. for 3 hours to prepare a multifunctional electronic product screen protective film.

[0104] Example 2

[0105] Based on Example 1, the following improvements were made to the self-repairing layer 3: 7 parts by weight of polydopamine and 4 parts by weight of fluorinated graphene were additionally added to the self-repairing layer 3. Other steps and parameters remained unchanged.

[0106] Example 3

[0107] Based on Example 2, the following improvement is made: a 2 μm thick fluorosilane-modified silica nanoparticle coating 4 is coated on the surface of the self-repairing layer 3 .

[0108] The specific steps are as follows:

[0109] a) 1 part by weight of nano-silicon dioxide powder (particle size 15-25 nm) was dispersed in 50 parts by weight of anhydrous ethanol and ultrasonicated for 15 minutes to prepare a suspension.

[0110] b) adding 0.5 parts by weight of 1H,1H,2H,2H-perfluorooctyltriethoxysilane (PFOTES) to the above suspension, and continuing ultrasonic treatment for 10 minutes.

[0111] c) Add 0.5 mL of deionized water and stir at room temperature for 2 hours to obtain a coating solution.

[0112] d) The surface of the self-repairing layer 3 is immersed in the coating solution using a dip coating method, with an immersion and pulling speed of 2 mm / s.

[0113] e) Air-dry at room temperature for 5 minutes, and then heat-treat at 80°C for 30 minutes.

[0114] f) Repeat steps d) and e) once more to achieve a coating thickness of 2 μm.

[0115] The other steps and parameters remain unchanged.

[0116] Example 4

[0117] Based on Example 2, the following improvement was made: 2 parts by weight of up-conversion luminescent nanoparticles NaYF4:Yb,Er were added to the self-repairing layer 3 .

[0118] The specific steps are as follows:

[0119] a) 2 parts by weight of NaYF4:Yb,Er nanoparticles (average particle size 50 nm) were dispersed in 10 parts by weight of anhydrous ethanol and ultrasonically treated for 30 minutes.

[0120] b) Slowly add the dispersion into the mixture of the self-repairing layer 3 in Example 2, and stir evenly at 85° C. for 30 minutes under nitrogen protection.

[0121] c) Coating and drying were carried out according to step c) of Example 2.

[0122] The other steps and parameters remain unchanged.

[0123] Example 5

[0124] Combining the improvements of Example 3 and Example 4, that is, on the basis of Example 2, a fluorosilane-modified silica nanoparticle coating 4 and upconversion luminescent nanoparticles NaYF4:Yb,Er are added simultaneously.

[0125] The specific steps are as follows:

[0126] According to the method of Example 4, upconversion luminescent nanoparticles NaYF4:Yb,Er are added to the self-repairing layer 3.

[0127] After the self-repairing layer 3 is prepared, a fluorosilane-modified silica nanoparticle coating 4 is coated on its surface according to the method of Example 3.

[0128] The other steps and parameters remain unchanged.

[0129] Comparative Example 1

[0130] A traditional single-layer PET protective film with a thickness of 200μm is used.

[0131] Comparative Example 2

[0132] A double-layer composite protective film is used, including a 200μm thick PET base film and a 30μm thick ordinary TPU self-repairing layer.

[0133] The following performance tests were performed on the protective films of the embodiment and the comparative example, and the test results are shown in Table 1.

[0134] 1) Scratch resistance test: Use a pencil hardness tester to test and record the maximum pencil hardness that does not leave obvious scratches on the film surface.

[0135] 2) Self-healing performance test: A 10 cm long scratch was made on the film surface using a 2H pencil with a 500 g load, and the time required for the scratch to automatically heal was observed at room temperature.

[0136] 3) Explosion-proof screen performance test: Use a falling ball impact tester to record the maximum falling ball height that will not cause the protective film to rupture (steel ball diameter 25.4mm, weight 66g).

[0137] 4) Fit test: Use the bubble counting method to count the number of visible bubbles in an area of ​​10 cm × 10 cm.

[0138] 5) Antistatic performance test: Use a surface resistance tester to measure the surface resistance.

[0139] 6) Optical performance test: The total light transmittance was measured using a spectrophotometer.

[0140] 7) Hydrophobicity test: The contact angle of water droplets on the membrane surface was measured using a contact angle meter.

[0141] 8) Self-cleaning performance test: Sprinkle dust evenly on the membrane surface, tilt it at 45 degrees, spray water with a spray bottle, and record the number of water droplets required to completely remove the dust.

[0142] Table 1

[0143]

[0144] The above experimental test results are analyzed as follows:

[0145] 1. Analyze the test results of each embodiment and comparative example:

[0146] a) Scratch resistance: The pencil hardness of Examples 1-5 is significantly higher than that of Comparative Examples 1 and 2, indicating that the multilayer structure design and functional coating of the present invention significantly improve the scratch resistance of the protective film.

[0147] b) Self-repair performance: Examples 1-5 all exhibited excellent self-repair capabilities, with Examples 4 and 5 having the shortest self-repair times. In contrast, Comparative Example 1 had no self-repair capability, and Comparative Example 2 had a longer self-repair time.

[0148] c) Explosion-proof screen performance: The explosion-proof screen performance of Examples 1-5 far exceeds that of Comparative Examples 1 and 2, which is mainly attributed to the unique gradient density elastic buffer layer design of the present invention; among them, Example 5 performs the best.

[0149] d) Conformity: The conformability of Examples 1-5 is significantly better than that of Comparative Examples 1 and 2. In particular, there are almost no visible bubbles in Examples 3 and 5, which is due to the multi-layer structure and gradient density design.

[0150] e) Antistatic performance: The surface resistance of Examples 1-5 is significantly lower than that of Comparative Examples 1 and 2, indicating that the protective film of the present invention has better antistatic performance.

[0151] f) Optical properties: Although the total light transmittance of Examples 1-5 is slightly lower than that of Comparative Examples 1 and 2, the difference is very small and will not significantly affect the actual use effect.

[0152] g) Hydrophobicity: The water contact angles of Examples 3 and 5 exceeded 150°, reaching the super-hydrophobic standard, which was mainly due to the effect of the fluorosilane-modified silica nanoparticle coating.

[0153] h) Self-cleaning performance: Examples 3 and 5 showed excellent self-cleaning performance, requiring only 2-3 drops of water to completely remove surface dust, which was far superior to other samples.

[0154] 2. Analyze the test results between the various embodiments:

[0155] a) Compared with Example 1, Example 2 has improvements in various properties, especially scratch resistance and self-repairing properties, which is attributed to the addition of polydopamine and fluorinated graphene.

[0156] b) Example 3 adds a fluorosilane-modified silica nanoparticle coating to Example 2, which significantly improves the scratch resistance, hydrophobicity and self-cleaning performance, but has little effect on other properties.

[0157] c) Example 4 adds upconversion luminescent nanoparticles on the basis of Example 2, which mainly improves the self-repair performance and shortens the self-repair time.

[0158] d) Example 5 combines the advantages of Examples 3 and 4, and reaches the best or near-optimal level in all performance aspects, especially in terms of scratch resistance, self-repairing performance, explosion-proof screen performance, hydrophobicity and self-cleaning performance.

[0159] In summary, the multifunctional electronic product screen protector of the present invention significantly outperforms conventional protective films in terms of scratch resistance, self-repairing ability, explosion-proof performance, conformability, antistatic properties, hydrophobicity, and self-cleaning properties. Through gradual optimization and the addition of functional components, the overall performance of the protective film has been further enhanced.

[0160] Among them, Example 5 performed the best, reaching optimal levels in almost all test items. It combines the superhydrophobic and self-cleaning properties of the fluorosilane-modified silica nanoparticle coating with the enhanced self-healing ability of the upconversion luminescent nanoparticles, while maintaining excellent explosion-proof shield performance and conformability.

[0161] Although there is a slight sacrifice in optical performance, this slight reduction in light transmittance is acceptable considering the significant improvement in other properties. Overall, the present invention provides a comprehensive and feature-rich screen protector solution for electronic products, which is expected to bring a significant improvement in user experience in practical applications.

[0162] Throughout this specification, references to terms such as "one embodiment," "example," or "specific example" indicate that the specific features, structures, materials, or characteristics described in conjunction with that embodiment or example are included in at least one embodiment or example of the present invention. In this specification, schematic representations of these terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.

[0163] The preferred embodiments of the present invention disclosed above are intended only to help illustrate the present invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the present invention to the specific embodiments described. Obviously, many modifications and variations are possible based on the content of this specification. These embodiments are selected and described in detail in this specification to better explain the principles and practical applications of the present invention, thereby enabling those skilled in the art to better understand and utilize the present invention. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A multifunctional electronic product screen protective film, characterized in that: It comprises a modified base film and a multifunctional composite layer composited on the surface of the modified base film; the multifunctional composite layer comprises an elastic buffer layer and a self-repairing layer arranged in sequence from the inside to the outside; The elastic buffer layer is an elastic buffer layer with gradient density, wherein the density is lower on the side close to the base film and higher on the side away from the base film, and the density gradient satisfies the following relationship: ρ(x)=ρ0+kx n ; Where ρ(x) is the density at a distance x from the base film (g / cm 3 );ρ0 is the minimum density near the basement membrane, and the value range of ρ0 is 0.8-1.0g / cm 3 ; k is the density gradient coefficient, and the value range of k is 0.005-0.015g / cm 3 μm -n ; x is the distance from the basement membrane (μm); n is the gradient index, and the value range of n is 1.2-1.8; The elastic buffer layer comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer, 15-25 parts of hollow glass microspheres, 10-15 parts of polyethylene glycol, and 3-6 parts of isocyanate crosslinking agent; The self-repairing layer comprises the following components in parts by weight: 100 parts of a dynamically reversible covalent bond polymer, 30-40 parts of a phase change material microcapsule, 10-15 parts of nanocellulose, 5-8 parts of a near-infrared photosensitive initiator, and 2-4 parts of an antioxidant.

2. The multifunctional electronic product screen protective film according to claim 1, characterized in that: The modified base film comprises the following components in parts by weight: 100 parts of polyethylene terephthalate, 3-7 parts of graphene, 2-5 parts of ionic liquid antistatic agent, and 1-3 parts of benzotriazole ultraviolet absorber.

3. The multifunctional electronic product screen protective film according to claim 1, characterized in that: The phase change material microcapsule comprises a core material and a shell material coated on the surface of the core material, wherein the core material is a mixture of octadecanoic acid and hexadecanoic acid, and the shell material is polymethyl methacrylate; The preparation method of the phase change material microcapsule is as follows: a) octadecanoic acid and hexadecanoic acid are mixed in a mass ratio of 3:1, and heated to 80°C to completely fuse them; b) methyl methacrylate, azobisisobutyronitrile and 1,6-hexanediol dimethacrylate are dissolved in deionized water, and a small amount of sodium dodecyl sulfate is added as an emulsifier; c) the mixture in step a) is slowly added to the solution in step b), and high-speed shear emulsification is performed at 80°C for 30 minutes; d) under nitrogen protection, the emulsion is heated to 85°C and reacted for 4 hours; e) cooled to room temperature, filtered, washed with water, and dried to obtain phase change material microcapsules.

4. The multifunctional electronic product screen protective film according to claim 1, characterized in that: The hollow glass microspheres in the elastic buffer layer have an average particle size of 20-50 μm and a wall thickness of 0.5-2 μm.

5. The multifunctional electronic product screen protective film according to claim 1, characterized in that: The nanocellulose in the self-repairing layer has a length of 100-500 nm and a diameter of 5-20 nm.

6. The multifunctional electronic product screen protective film according to claim 1, characterized in that: The thickness of the elastic buffer layer is 150-250 μm, and the thickness of the self-repairing layer is 20-40 μm.

7. The multifunctional electronic product screen protective film according to claim 1, characterized in that: The near-infrared photosensitive initiator in the self-repairing layer is a manganese-based metal porphyrin complex.

8. The multifunctional electronic product screen protective film according to claim 1, characterized in that: The self-repairing layer further comprises 5-10 parts by weight of polydopamine and 2-6 parts by weight of fluorinated graphene.

9. The multifunctional electronic product screen protective film according to claim 1, characterized in that: The surface of the self-repairing layer is coated with a 1-3 μm thick fluorosilane-modified silica nanoparticle coating; The preparation method of the fluorosilane-modified silica nanoparticle coating is as follows: a) dispersing 1 weight part of nano silica powder in 50 weight parts of anhydrous ethanol, ultrasonically treating for 15 minutes to obtain a suspension; adding 0.5 weight part of 1H,1H,2H,2H-perfluorooctyltriethoxysilane to the suspension, and continuing ultrasonic treatment for 10 minutes; adding 0.5 mL of deionized water, stirring at room temperature for 2 hours to obtain a coating solution; b) using a dip coating method to immerse the surface of the self-repairing layer in the coating solution, with an immersion and pulling speed of 2 mm / s; air drying at room temperature for 5 minutes; and heat treating at 80°C for 30 minutes; c) controlling the final coating thickness within the range of 1-3 μm by adjusting the coating solution concentration and the number of dip coatings, wherein the coating solution concentration is 1-3wt% and the number of dip coatings is 1-3 times.

10. A method for preparing a multifunctional electronic product screen protective film according to any one of claims 1 to 9, characterized in that: The following steps are involved: 1) preparing a modified base film: mixing polyethylene terephthalate, graphene, an ionic liquid antistatic agent and a benzotriazole ultraviolet absorber, and extruding through a twin-screw extruder at 260-280° C. at a line speed of 5-8 m / min to obtain a modified base film; 2) preparing an elastic buffer layer: mixing a thermoplastic polyurethane elastomer, hollow glass microspheres, polyethylene glycol and an isocyanate crosslinking agent, and preparing an elastic buffer layer with a gradient density by a solution casting method; 3) Preparation of self-repairing layer: a) Synthesis of a dynamically reversible covalent bond polymer: reacting 4,4'-diaminoazobenzene with maleic anhydride in N,N-dimethylformamide at 60-70°C for 4-6 hours to obtain a prepolymer containing a Diels-Alder addition product; b) mixing the prepolymer with phase change material microcapsules, nanocellulose, near-infrared photoinitiator and antioxidant, and stirring at 80-90° C. under nitrogen protection; c) coating the mixture on a release film treated with silicone oil to a thickness of 20-40 μm, and vacuum drying at 80-100° C. for 2-4 hours to obtain a self-healing layer; 4) The elastic buffer layer is compounded on the surface of the modified base film by a roller pressing method at a pressure of 0.5-1.0 MPa and a temperature of 60-80°C; 5) The self-healing layer is transferred to the surface of the elastic buffer layer by hot pressing, with a pressure of 1.0-1.5 MPa, a temperature of 100-120°C, and a holding time of 30-60 seconds; 6) Annealing at 80-100° C. for 2-4 hours to prepare a multifunctional electronic product screen protective film.

Citation Information

Patent Citations

  • Fluorosilicone material for super-hydrophobic coating and its preparation method and use method

    CN103224719A

  • Low-temperature phase-change energy storage microcapsule and preparation method thereof

    CN104650816A

  • Surface superhydrophobic TPU (thermoplastic polyurethane) film and preparation method thereof

    CN108034228A

  • Bamboo fiber gradient density foaming cushion packaging material

    CN111019194A

  • Expansion flow type electronic product protective sleeve / shell

    CN111166031A

Cited By

  • Self-repairing TPU color changing film and preparation process thereof

    CN120116506A

  • A self-repairing TPU color-changing film and its preparation process

    CN120116506B

  • Multi-layer composite shielding PVC wire harness adhesive tape and preparation method thereof

    CN120519097A

  • Anti-fingerprint coating as well as preparation method and application thereof

    CN121182344A