Composite catalyst for hydrogen production by steam reforming of bio-oil light component, and preparation method and application thereof
The nickel-magnesium-aluminum composite cobalt catalyst was prepared by co-precipitation method and impregnation method, which solved the problems of high energy consumption and degradation of catalyst performance during the hydrogen reforming of light components of bio-oil, and achieved the effect of low energy consumption, long-term stability and high-purity hydrogen production.
Patent Information
- Application Number
- CN202510219083.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-02-26
- Publication Date
- 2025-06-10
AI Technical Summary
The prior art has problems such as high energy consumption, degradation of catalyst performance and low hydrogen selectivity in the steam reforming and hydrogen production process of light components of bio-oil. Especially under high temperature conditions, the catalyst is prone to carbon accumulation and the reaction product is not conducive to the extraction of high-purity hydrogen.
A nickel-magnesium-aluminum composite cobalt catalyst was prepared by a combination of coprecipitation method and impregnation method. The thermal stability and chemical stability of the catalyst were improved by impregnating the active metal cobalt, and a mesoporous structure was formed to improve the catalytic activity and stability.
It has achieved low energy consumption, long-lasting and stable catalytic performance, and high-purity hydrogen production. The catalyst maintains a conversion rate of 80%-90% within a reaction time of more than 50 hours, the H2 yield remains above 60%, and the H2 gas concentration produced remains above 40%.
Smart Images

Figure CN120115153A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steam reforming hydrogen production, and in particular to a composite catalyst for steam reforming hydrogen production of light components of bio-oil, and a preparation method and application thereof. Background Art
[0002] Pyrolysis and gasification of biomass to generate renewable fuels and chemicals is one of the ways to achieve sustainable energy development in the future. Despite significant technological advances in recent decades, the utilization of biomass pyrolysis products, bio-oil, remains challenging. Bio-oil can be further utilized by processing. The water-soluble part of bio-oil is a bio-oil derivative, which is mainly an aqueous solution composed of acetic acid, aromatics and phenolic compounds. The light components of bio-oil contain acetic acid, propionic acid, phenol, m-cresol and other components, which require a catalyst with strong adaptability. Therefore, a catalyst regulation method with multiple strategies is crucial. The use of light components of bio-oil to produce hydrogen can not only convert low calorific value products into high calorific value products and reduce dependence on fossil fuels, but also can be used as a way to treat pyrolysis waste liquid products to promote sustainable energy development.
[0003] At present, light components of biomass can be continuously used to produce hydrogen through steam reforming. Compared with the autothermal steam reforming process (introducing oxygen or air to participate in the reaction), the conditions of direct steam reforming are relatively harsh, and the catalyst is more likely to deposit carbon during the reaction. It is more of the catalytic effect of acetic acid molecules on the catalyst. Autothermal steam reforming will generate a large amount of carbon-containing gas to participate in the reaction with the participation of oxygen. It is a multi-component complex catalytic reaction, and there is a greater safety risk in practical application. Therefore, in the steam reforming reaction, the reaction system and the generated products are relatively simple, and there is no need to consider issues such as system thermal management and further reaction optimization.
[0004] Steam reforming of light components of bio-oil requires catalytic active sites with excellent CC and CH bond breaking ability, and also avoids rapid deactivation caused by coke deposition. Precious metals have high catalytic activity, but are limited by high prices and are difficult to promote in industrial applications. In contrast, transition metals have the potential to become a potential substitute for precious metals with their excellent catalytic properties. For steam reforming of multi-carbon organic compounds or aromatic compounds, transition metal catalysts face challenges in thermal stability, chemical stability and durability. Patent Publication No. CN111644176A discloses a biomass tar steam reforming catalyst, a catalyst with coal gangue lime carrier loaded with Ni and metal additives (Mo, Co, Ce, Mn, Fe). Although it is cheap, its catalytic reforming temperature is too high, and the energy consumption generated in the process is large. As the reaction time increases, its catalyst performance gradually decreases. Patent publication number CN110639606A discloses a catalyst for steam reforming of biomass pyrolysis tar, which is a HZSM-5 zeolite-loaded Ni, Mg, and Ce metal catalyst. Under the reforming conditions of 700°C, space velocity 6000mL / (g·h), and S / C=3, the tar carbon conversion rate is as high as 97%, and the CO ratio is as high as 23%, which is not conducive to further extraction of high-purity hydrogen.
[0005] Patent Publication No. CN116902916A discloses a catalyst for water-phase reforming of biomass alcohol derivatives to produce hydrogen, which is a nickel-magnesium-aluminum hydrotalcite catalyst. It is used in combination with an alkaline solution in water-phase reforming and has good hydrogen selectivity, but its catalytic effect is poor when simply applied to the field of steam reforming, the degree of methanation is high, and the conversion rate is low. Patent Grant No. CN109225249B discloses a nickel-manganese-aluminum composite oxide catalyst suitable for hydrogen production by autothermal reforming of acetic acid, which realizes reforming hydrogen production by optimizing the specific surface area and redox properties of the catalyst, and introduces oxygen during the reaction process to further improve the ability of anti-carbon deposition and stability, but the reaction at high temperature (600-800°C) greatly increases energy consumption, and the reaction gas product may be doped with incompletely reacted oxygen at high gas space velocity. At present, Ni-based catalysts used for steam reforming have the disadvantages of easy carbon deposition deactivation and low hydrogen selectivity during application.
[0006] To this end, the present invention develops a catalyst for efficient hydrogen production by steam reforming of light components of biomass, which is suitable for low energy consumption, long-lasting and stable catalytic performance, and production of high-purity hydrogen, as well as a preparation method and application thereof. Summary of the invention
[0007] The present invention provides a composite catalyst for hydrogen production by steam reforming of light components of bio-oil, and a preparation method and application thereof, the purpose of which is to achieve full utilization of light components of bio-oil and improve the energy utilization efficiency of biomass pyrolysis.
[0008] In order to achieve the above-mentioned purpose, an embodiment of the present invention provides a composite catalyst for steam reforming of light components of bio-oil to produce hydrogen, and a preparation method and application thereof. The preparation method mainly adopts a combination of co-precipitation and impregnation methods, and improves the problems of easy sintering and oxidation of active metals caused by the co-precipitation method by impregnating active metal cobalt. A small amount of metal cobalt can be evenly distributed on the surface of spinel, and the formed metal oxide greatly reduces the deactivation degree of the active sites of the spinel itself. At the same time, the stability of the spinel structure of the catalyst before and after the reaction is guaranteed.
[0009] The embodiment of the present invention provides a method for preparing a nickel-magnesium-aluminum composite cobalt catalyst for steam reforming of light components of bio-oil to produce hydrogen, comprising the following steps:
[0010] S1. Weigh nickel salt, aluminum salt, magnesium salt and organic chelating agent according to mass ratio and dissolve them in deionized water, stir them thoroughly to prepare solution A; weigh carbonate and alkali according to mass ratio and dissolve them in deionized water, stir them thoroughly to prepare solution B; dissolve alkali in deionized water, stir them thoroughly to prepare solution C;
[0011] S2. The solutions A and B were slowly dripped into the solution C, and the mixture was stirred in an oil bath until a precipitate was formed. The suspension was filtered, rinsed with deionized water and dried, and ground to obtain a carrier precursor.
[0012] S3. The carrier precursor is placed in a high temperature furnace and calcined to obtain a nickel-magnesium-aluminum composite spinel carrier;
[0013] S4. The cobalt salt solution is impregnated and loaded on a nickel-magnesium-aluminum composite spinel carrier, stirred and dried;
[0014] S5. Placed under high temperature reducing atmosphere for reduction to obtain a composite catalyst;
[0015] The composite catalyst is applied to the fixed bed reaction device in the process of steam reforming hydrogen production from light components of bio-oil, and the stability reaction time is more than 50 hours, and the conversion rate is maintained at 80%-90%. 2 The yield was maintained above 60%, and the H 2 The gas concentration was kept above 40%.
[0016] Preferably, in step S1, the nickel salt is at least one of nickel nitrate, nickel nitrite, nickel acetate, nickel sulfate, nickel sulfite, nickel carbonate, nickel chloride, and nickel sulfide; but it is not limited to the above forms, and it can also be other organic acid salts; the magnesium salt is at least one of magnesium nitrate, magnesium nitrite, magnesium acetate, magnesium sulfate, magnesium sulfite, magnesium carbonate, magnesium chloride, and magnesium sulfide; but it is not limited to the above forms, and it can also be other organic acid salts; the aluminum salt is at least one of aluminum nitrate, aluminum nitrite, aluminum acetate, aluminum sulfate, aluminum sulfite, aluminum carbonate, aluminum chloride, and aluminum sulfide; but it is not limited to the above forms, and it can also be other organic acid salts; the organic chelating agent is at least one of citric acid, oxalic acid, urea, malic acid, and glycine; m(C) / m(M)=0.01-10; the carbonate is at least one of sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate; the alkali is at least one of potassium hydroxide, sodium hydroxide, and ammonia water, and the addition amount is 2-15g; OH - With Al 3+ The molar ratio of CO is 4 to 8. 3 2- With Al 3+ The molar ratio of Ni is 0.2 to 5. 2+ With Mg 2+ The molar ratio is 0.1 to 10; m(Ni 2+ and Mg 2+ ):m(Al 3+ )=0.4~0.6.
[0017] Preferably, in step S2, the solution has a pH value of 8 to 14, a stirring temperature of 40 to 90° C., a stirring time of 6 to 18 hours, and is rinsed with deionized water until the pH value is 7 to 8. The drying temperature is 50 to 90° C., and the drying time is 6 to 18 hours.
[0018] Preferably, in step S3, the calcination is carried out under ventilation, still air, nitrogen or argon atmosphere conditions, the calcination temperature is 400-600° C., the calcination time is 2-6 hours, and the heating rate is 10° C. / min.
[0019] Preferably, in step S4, the cobalt salt is at least one of cobalt nitrate, cobalt nitrite, cobalt acetate, cobalt sulfate, cobalt sulfite, cobalt carbonate, cobalt chloride, and cobalt sulfide; but is not limited to the above forms, and can also be other organic acid salts; the cobalt loading is 0-20%, and is not zero.
[0020] Preferably, in step S4, 0-100 wt.% methanol or ethanol aqueous solution is used for impregnation, the stirring time is 12-24 hours, the drying temperature is 50-100° C., and the drying time is 6-18 hours.
[0021] Preferably, in step S5, the reducing atmosphere is at least one of hydrogen, ammonia, carbon monoxide and methane; the reducing temperature is 300-800°C, the reducing time is 1-3h, and the heating rate is 10°C / min.
[0022] Based on a general inventive concept, an embodiment of the present invention provides a composite catalyst prepared by the above-mentioned preparation method.
[0023] Preferably, the composite catalyst has multiple mesoporous structures.
[0024] The embodiments of the present invention also provide a composite catalyst prepared by the above preparation method or the use of the above composite catalyst in hydrogen production by steam reforming of light components of bio-oil.
[0025] Preferably, the application comprises the following specific steps:
[0026] (1) adding a certain amount of deionized water to the biomass light component or its model compound, and stirring and mixing the mixture to obtain a reactant solution, wherein S / C is 1-9 (S / C is the ratio of the number of moles of water molecules to the number of moles of carbon atoms of the organic compound);
[0027] (2) Filling the catalyst into the middle of the fixed bed reactor and fixing the catalyst with quartz wool;
[0028] (3) Before heating the reaction, use carrier gas (nitrogen) to purge the catalyst bed for 10 minutes;
[0029] (4) continuously introducing carrier gas into the catalyst bed to increase the temperature of the fixed bed reactor and adjust the injection rate of the injection pump to carry out the reaction;
[0030] More preferably, the amount of catalyst used is 0.1 to 1 g.
[0031] More preferably, the carrier gas flow rate is 10-100 ml / min, the injection flow rate is 0.1-0.3 ml / min, the heating rate is 5-10° C. / min, the reaction temperature is 350-600° C., and the constant temperature is maintained for 10-50 hours.
[0032] Reaction mechanism
[0033] The present invention modifies the spinel carrier by adjusting the Ni / Mg ratio. The formed new carrier not only changes in acidity and alkalinity, but also increases the number of oxygen vacancy defects, promotes the large-scale dissociation of water vapor on the catalyst surface, thereby improving the catalyst activity and stability. On the other hand, under the addition of the impregnation method, the incorporation of Co introduces CoO x species, and with the spinel support modification, there is a strong interaction, which can achieve Co and CoO xThe efficient redox between the two promotes the efficient conversion of coke gasification and CO, effectively reduces the catalytic deactivation of Ni active metal and CO selectivity, and indirectly improves hydrogen selectivity. The appropriate amount of Mg incorporation can increase the acid sites of the catalyst and increase the number of strong acid sites. A large reduction in the Ni content will greatly reduce the overall acid sites. Although the acid sites of the 5Co / Ni0.2-Mg0.8-Al catalyst are concentrated in the strong acid region, the number is too small, which is not conducive to the catalytic activity in AcOH steam reforming. 2+ / Mg 2+ =1 5Co / Ni0.5-Mg0.5-Al catalyst has good acid site distribution characteristics, thus showing strong ability to break CC and CH bonds. The addition of Mg increases the total number of oxygen vacancies, and as the Ni / Mg ratio decreases, the proportion of oxygen vacancies gradually increases. In the reaction, water molecules can be continuously activated to promote coke gasification.
[0034] At the same time, under the reaction conditions of medium and low temperature 550℃, the yield of 2.43 mol / mol was continuously obtained in the acetic acid steam reforming experiment for up to 50 hours with a loading amount of 0.2g catalyst. AcOH The present invention optimizes the anti-coking and high-efficiency conversion performance of the catalyst system from two aspects, namely, the carrier and the auxiliary metal, greatly improves the stability of the catalyst, and ensures the continuous output of a gas product with high hydrogen selectivity.
[0035] A hydrogen membrane separation device can be further connected to the exhaust port of the reaction gas product to separate 98% high-purity hydrogen. At the same time, the separated gas by-products are introduced into an alkaline potassium hydroxide solution, and carbon dioxide can be captured and utilized by adding calcium oxide and filtering and calcining. Nitrogen can also be collected and compressed to achieve recycling of the reaction carrier gas.
[0036] The above scheme of the present invention has the following beneficial effects:
[0037] 1. The spinel carrier prepared by the present invention has high mechanical strength and heat resistance stability. The nickel-magnesium composite spinel catalyst is modified by introducing cobalt metal by impregnation method. The active metal nickel and cobalt have strong interaction, which improves the anti-sintering performance of nickel, and also changes the gas selectivity and improves the hydrogen yield.
[0038] 2. The specific surface area of the catalyst prepared by the present invention is as high as 218.9m 2 / g, the specific surface area of spinel prepared by traditional methods is increased by 50%, which can efficiently convert reactants; low-loaded cobalt metal efficiently promotes reactants to participate in the reaction and enhances the coke gasification effect.
[0039] 3. The catalytic reaction device of the present invention adopts a fixed bed and the catalyst filling amount is 0.2g. When the reactant is a 35.7wt% acetic acid solution, the carrier gas flow rate is 35ml / min, the liquid inlet flow rate is 0.15ml / min, and the reaction temperature is maintained at 550°C. In the stability experimental test lasting up to 50h, the catalyst exhibits excellent anti-coking performance, the carbon deposition rate is 0.308mg / h, and in terms of catalytic performance, after 50h of reaction, the conversion rate still remains at the initial conversion rate level; when the reactant is a mixed solution of 1wt% phenol and 9wt% acetic acid, the carrier gas flow rate is 35ml / min, the liquid inlet flow rate is 0.15ml / min, and the reaction temperature is maintained at 550°C. In the stability experimental test lasting up to 50h, the catalyst exhibits excellent hydrogen and carbon dioxide selectivity. After 50h of reaction, the reaction effect does not change much. Combined with hydrogen membrane separation equipment and carbon dioxide capture technology, hydrogen purification and carrier gas recycling can be achieved.
[0040] 4. The catalyst prepared by the present invention can be applied to the bio-oil light component steam reforming hydrogen production reaction system, and has a good catalytic effect of high hydrogen yield, low carbon deposition rate and high stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1 is the XRD diagram of the catalysts of Examples 1-3 of the present invention and Comparative Example 1;
[0043] Figure 2 is the NH of the catalysts of Examples 1-3 and Comparative Example 1 of the present invention. 3 -TPD graph.
[0044] Figure 3 It is the BET adsorption-desorption isotherm curve and pore size distribution curve of the catalyst of Examples 1-3 of the present invention and Comparative Example 1;
[0045] Figure 4 It is the XPS energy spectrum diagram of the catalysts of Examples 1-3 of the present invention and Comparative Example 1.
[0046] Figure 5It is the stability reaction test result of Examples 1-3 of the present invention and Comparative Example 1, wherein the catalyst is a reaction effect diagram under the stability test experiment with the conditions of 0.2g catalyst loaded on the catalyst bed, reaction temperature of 550°C, S / C=3 (carbon number molar ratio of water to acetic acid), carrier gas flow rate of 35ml / min, and liquid inlet flow rate of 0.15ml / min.
[0047] Figure 6 It is the XRD diagram of the catalysts of Examples 1-3 of the present invention and Comparative Example 1 after the stability test experiment.
[0048] Figure 7 It is the TG-DTG graph of the catalysts of Examples 1-3 of the present invention and Comparative Example 1 after the stability test experiment.
[0049] Figure 8 It is a reaction effect diagram of steam reforming of wood vinegar model compound in Example 2 of the present invention.
[0050] Fig. 9 It is the reaction test result of Example 2 of the present invention and Comparative Example 2, wherein the catalyst is a reaction effect diagram under the reaction test experiment conditions of 0.2g catalyst loaded on the catalyst bed, 550°C reaction temperature, S / C=3 (carbon number molar ratio of water to acetic acid), 35ml / min carrier gas flow rate, and 0.15ml / min liquid inlet flow rate. DETAILED DESCRIPTION
[0051] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.
[0052] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0053] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0054] The following “m(C) / m(M)” has a specific meaning: C represents the carbon content in the organic chelating agent, and M refers to the three metal contents of nickel, magnesium and aluminum.
[0055] In view of the existing problems, an embodiment of the present invention provides a method for preparing a composite catalyst for steam reforming of light components of bio-oil to produce hydrogen, comprising the following steps:
[0056] S1. Weigh nickel salt, aluminum salt, magnesium salt and organic chelating agent according to mass ratio and dissolve them in deionized water, stir them thoroughly to prepare solution A; weigh carbonate and alkali according to mass ratio and dissolve them in deionized water, stir them thoroughly to prepare solution B; dissolve alkali in deionized water, stir them thoroughly to prepare solution C;
[0057] S2. The solutions A and B were slowly dripped into the solution C, and the mixture was stirred in an oil bath until a precipitate was formed. The suspension was filtered, rinsed with deionized water and dried, and ground to obtain a carrier precursor.
[0058] S3. The carrier precursor is placed in a high temperature furnace and calcined to obtain a nickel-magnesium-aluminum composite spinel carrier;
[0059] S4. The cobalt salt solution is impregnated and loaded on a nickel-magnesium-aluminum composite spinel carrier, stirred and dried;
[0060] S5. Placed under high temperature reducing atmosphere for reduction to obtain a composite catalyst;
[0061] The composite catalyst is applied to the fixed bed reaction device in the process of steam reforming hydrogen production from light components of bio-oil, and the stability reaction time is more than 50 hours, and the conversion rate is maintained at 80%-90%. 2 The yield was maintained above 60%, and the H 2 The gas concentration was kept above 40%.
[0062] Preferably, in step S1, the nickel salt is at least one of nickel nitrate, nickel nitrite, nickel acetate, nickel sulfate, nickel sulfite, nickel carbonate, nickel chloride, and nickel sulfide; but it is not limited to the above forms, and it can also be other organic acid salts; the magnesium salt is at least one of magnesium nitrate, magnesium nitrite, magnesium acetate, magnesium sulfate, magnesium sulfite, magnesium carbonate, magnesium chloride, and magnesium sulfide; but it is not limited to the above forms, and it can also be other organic acid salts; the aluminum salt is at least one of aluminum nitrate, aluminum nitrite, aluminum acetate, aluminum sulfate, aluminum sulfite, aluminum carbonate, aluminum chloride, and aluminum sulfide; but it is not limited to the above forms, and it can also be other organic acid salts; the organic chelating agent is at least one of citric acid, oxalic acid, urea, malic acid, and glycine; m(C) / m(M)=0.01-10; the carbonate is at least one of sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate; the alkali is at least one of potassium hydroxide, sodium hydroxide, and ammonia water, and the addition amount is 2-15g; OH - With Al 3+ The molar ratio of CO is 4 to 8. 3 2- With Al 3+ The molar ratio of Ni is 0.2 to 5. 2+ With Mg 2+ The molar ratio is 0.1 to 10; m(Ni 2+ and Mg 2+):m(Al 3+ )=0.4~0.6.
[0063] Preferably, in step S2, the solution has a pH value of 8 to 14, a stirring temperature of 40 to 90° C., a stirring time of 6 to 18 hours, and is rinsed with deionized water until the pH value is 7 to 8. The drying temperature is 50 to 90° C., and the drying time is 6 to 18 hours.
[0064] Preferably, in step S3, the calcination is carried out under ventilation, still air, nitrogen or argon atmosphere conditions, the calcination temperature is 400-600° C., the calcination time is 2-6 hours, and the heating rate is 10° C. / min.
[0065] Preferably, in step S4, the cobalt salt is at least one of cobalt nitrate, cobalt nitrite, cobalt acetate, cobalt sulfate, cobalt sulfite, cobalt carbonate, cobalt chloride, and cobalt sulfide; but is not limited to the above forms, and can also be other organic acid salts; the cobalt loading is 0-20%, and is not zero.
[0066] Preferably, in step S4, 0-100 wt.% methanol or ethanol aqueous solution is used for impregnation, the stirring time is 12-24 hours, the drying temperature is 50-100° C., and the drying time is 6-18 hours.
[0067] Preferably, in step S5, the reducing atmosphere is at least one of hydrogen, ammonia, carbon monoxide and methane; the reducing temperature is 300-800°C, the reducing time is 1-3h, and the heating rate is 10°C / min.
[0068] Based on a general inventive concept, an embodiment of the present invention provides a composite catalyst prepared by the above-mentioned preparation method.
[0069] Preferably, the composite catalyst has multiple mesoporous structures.
[0070] The embodiments of the present invention also provide a composite catalyst prepared by the above preparation method or the use of the above composite catalyst in hydrogen production by steam reforming of light components of bio-oil.
[0071] Preferably, the application comprises the following specific steps:
[0072] (1) adding a certain amount of deionized water to the biomass light component or its model compound, and stirring and mixing the mixture to obtain a reactant solution, wherein S / C is 1-9 (S / C is the ratio of the number of moles of water molecules to the number of moles of carbon atoms of the organic compound);
[0073] (2) Filling the catalyst into the middle of the fixed bed reactor and fixing the catalyst with quartz wool;
[0074] (3) Before heating the reaction, use carrier gas (nitrogen) to purge the catalyst bed for 10 minutes;
[0075] (4) continuously introducing carrier gas into the catalyst bed to increase the temperature of the fixed bed reactor and adjust the injection rate of the injection pump to carry out the reaction;
[0076] More preferably, the amount of catalyst used is 0.1 to 1 g.
[0077] More preferably, the carrier gas flow rate is 10-100 ml / min, the injection flow rate is 0.1-0.3 ml / min, the heating rate is 5-10° C. / min, the reaction temperature is 350-600° C., and the constant temperature is maintained for 10-50 hours.
[0078] The following is a detailed description through specific embodiments.
[0079] Example 1
[0080] A method for preparing a composite catalyst for steam reforming of light components of bio-oil to produce hydrogen comprises the following steps:
[0081] S1. 4.75g Ni(NO 3 ) 2 6H 2 O, 1.03 g Mg(NO 3 ) 2 6H 2 O, 15gAl(NO 3 ) 3 9H 2 O, 5.76g citric acid C 6 H 8 O 7 Dissolve in 50 ml of deionized water to obtain metal ion salt solution A; weigh 1.59 g Na 2 CO 3 , 5g NaOH was dissolved in 50ml deionized water to prepare anionic solution B; 5.5g NaOH was dissolved in 50ml deionized water to prepare alkaline solution C (OH - / Al 3+ =6.3, CO 3 2- / Al 3+ =0.375);
[0082] S2. Solution A and solution B are added dropwise to solution C together, and stirred continuously to form a preliminary suspension. During the process, the dripping speed of solution A and solution B needs to be controlled to be slow and uniform. After the dropwise addition is completed, the suspension is transferred to an oil bath at a temperature of 80°C and stirred for 12 hours. The precipitate is then filtered with deionized water and repeatedly washed until neutral. The precipitate is placed in a 65°C air drying oven for drying, and then ground into powder after drying;
[0083] S3. Place in a muffle furnace and calcine for 4 hours at 600℃;
[0084] S4. Weigh 1 g of the calcined catalyst support into a crucible and dissolve 0.25 g of Co(NO 3 ) 2 6H 2 O, drip an equal volume into a crucible containing 1 g of the carrier, stir for 12 h, and then put it into a forced air drying oven at 80 °C to dry;
[0085] S5. Place in an atmosphere containing hydrogen and reduce at 600°C for 2h to obtain a composite catalyst in which the molar ratio of Ni and Mg to Al is 1 / 2, the molar ratio of Ni to Mg is 4, and the Co content is 5wt%, recorded as 5Co / Ni0.8-Mg0.2-Al.
[0086] The application of the composite catalyst in hydrogen production by steam reforming of acetic acid comprises the following steps:
[0087] (1) A certain amount of deionized water was added to acetic acid, a light component of bio-oil, to prepare a 35.7 wt % mixed solution with S / C=3.
[0088] (2) The catalyst filling amount is 0.2 g and is fixed with quartz wool.
[0089] (3) Use nitrogen to purge the bed for 10 minutes, then keep the nitrogen flow rate at 35 ml / min, raise the reactor temperature to 550°C at a rate of 10°C / min, and inject the reactant solution at a rate of 0.15 ml / min for constant temperature reaction (stop the reaction when the reaction time reaches 50 hours, and stop it if the reaction bed is blocked in the middle).
[0090] (4) Use a flow meter to monitor the gas flow rate at the outlet. At the same time, collect the gas product every 1 hour, and use a gas chromatograph to analyze the product gas concentration, and finally organize the analysis data.
[0091] Example 2
[0092] A method for preparing a composite catalyst for steam reforming of light components of bio-oil to produce hydrogen comprises the following steps:
[0093] S1. 2.97gNi(NO 3 ) 2 6H 2 O, 2.56 g Mg (NO 3 ) 2 6H 2 O, 15gAl(NO 3 ) 3 9H 2O, 5.76g citric acid C 6 H 8 O 7 Dissolve in 50 ml of deionized water to obtain metal ion salt solution A; weigh 1.59 g Na 2 CO 3 , 5g NaOH was dissolved in 50ml deionized water to prepare anionic solution B; 5.5g NaOH was dissolved in 50ml deionized water to prepare alkaline solution C (OH - / Al 3+ =6.3, CO 3 2- / Al 3+ =0.375);
[0094] S2. Solution A and solution B are added dropwise to solution C together, and stirred continuously to form a preliminary suspension. During the process, the dripping speed of solution A and solution B needs to be controlled to be slow and uniform. After the dropwise addition is completed, the suspension is transferred to an oil bath at a temperature of 80°C and stirred for 12 hours. The precipitate is then filtered with deionized water and repeatedly washed until neutral. The precipitate is placed in a 65°C air drying oven for drying, and then ground into powder after drying;
[0095] S3. Place in a muffle furnace and calcine for 4 hours at 600℃;
[0096] S4. Weigh 1 g of the calcined catalyst support into a crucible and dissolve 0.25 g of Co(NO 3 ) 2 6H 2 O, drip an equal volume into a crucible containing 1 g of the carrier, stir for 12 h, and then put it into a forced air drying oven at 80 °C to dry;
[0097] S5. Place in an atmosphere containing hydrogen and reduce at 600°C for 2h to obtain a composite catalyst in which the molar ratio of Ni and Mg to Al is 1 / 2, the molar ratio of Ni to Mg is 1, and the Co content is 5wt%, recorded as 5Co / Ni0.5-Mg0.5-Al.
[0098] The application of the composite catalyst in hydrogen production by steam reforming of acetic acid comprises the following steps:
[0099] (1) A certain amount of deionized water was added to acetic acid, a light component of bio-oil, to prepare a 35.7 wt % mixed solution with S / C=3.
[0100] (2) The catalyst filling amount is 0.2 g and is fixed with quartz wool.
[0101] (3) Use nitrogen to purge the bed for 10 minutes, then keep the nitrogen flow rate at 35 ml / min, raise the reactor temperature to 550°C at a rate of 10°C / min, and inject the reactant solution at a rate of 0.15 ml / min for constant temperature reaction (stop the reaction when the reaction time reaches 50 hours, and stop it if the reaction bed is blocked in the middle).
[0102] (4) Use a flow meter to monitor the gas flow rate at the outlet. At the same time, collect the gas product every 1 hour, and use a gas chromatograph to analyze the product gas concentration, and finally organize the analysis data.
[0103] Example 3
[0104] A method for preparing a composite catalyst for steam reforming of light components of bio-oil to produce hydrogen comprises the following steps:
[0105] S1. 1.19g Ni(NO 3 ) 2 6H 2 O, 4.1gMg(NO 3 ) 2 6H 2 O, 15gAl(NO 3 ) 3 9H 2 O, 5.76g citric acid C 6 H 8 O 7 Dissolve in 50 ml of deionized water to obtain metal ion salt solution A; weigh 1.59 g Na 2 CO 3 , 5g NaOH was dissolved in 50ml deionized water to prepare anionic solution B; 5.5g NaOH was dissolved in 50ml deionized water to prepare alkaline solution C (OH - / Al 3+ =6.3, CO 3 2- / Al 3+ =0.375);
[0106] S2. Solution A and solution B are added dropwise to solution C together, and stirred continuously to form a preliminary suspension. During the process, the dripping speed of solution A and solution B needs to be controlled to be slow and uniform. After the dropwise addition is completed, the suspension is transferred to an oil bath at a temperature of 80°C and stirred for 12 hours. The precipitate is then filtered with deionized water and repeatedly washed until neutral. The precipitate is placed in a 65°C air drying oven for drying, and then ground into powder after drying;
[0107] S3. Place in a muffle furnace and calcine for 4 hours at 600℃;
[0108] S4. Weigh 1 g of the calcined catalyst support into a crucible and dissolve 0.25 g of Co(NO 3 ) 2 6H 2 O, drip an equal volume into a crucible containing 1 g of the carrier, stir for 12 h, and then put it into a forced air drying oven at 80 °C to dry;
[0109] S5. Place in an atmosphere containing hydrogen and reduce at 600°C for 2h to obtain a composite catalyst in which the molar ratio of Ni and Mg to Al is 1 / 2, the molar ratio of Ni to Mg is 1 / 4, and the Co content is 5wt%, recorded as 5Co / Ni0.2-Mg0.8-Al.
[0110] The application of the composite catalyst in hydrogen production by steam reforming of acetic acid comprises the following steps:
[0111] (1) A certain amount of deionized water was added to acetic acid, a light component of bio-oil, to prepare a 35.7 wt % mixed solution with S / C=3.
[0112] (2) The catalyst filling amount is 0.2 g and is fixed with quartz wool.
[0113] (3) Use nitrogen to purge the bed for 10 minutes, then keep the nitrogen flow rate at 35 ml / min, raise the reactor temperature to 550°C at a rate of 10°C / min, and inject the reactant solution at a rate of 0.15 ml / min for constant temperature reaction (stop the reaction when the reaction time reaches 50 hours, and stop it if the reaction bed is blocked in the middle).
[0114] (4) Use a flow meter to monitor the gas flow rate at the outlet. At the same time, collect the gas product every 1 hour, and use a gas chromatograph to analyze the product gas concentration, and finally organize the analysis data.
[0115] Example 4
[0116] A method for preparing a composite catalyst for steam reforming of light components of bio-oil to produce hydrogen comprises the following steps:
[0117] S1. 2.97gNi(NO 3 ) 2 6H 2 O, 2.56 g Mg (NO 3 ) 2 6H 2 O, 15gAl(NO 3 ) 3 9H 2 O, 5.76g citric acid C 6 H 8 O7 Dissolve in 50 ml of deionized water to obtain metal ion salt solution A; weigh 1.59 g Na 2 CO 3 , 5g NaOH was dissolved in 50ml deionized water to prepare anionic solution B; 5.5g NaOH was dissolved in 50ml deionized water to prepare alkaline solution C (OH - / Al 3+ =6.3, CO 3 2- / Al 3+ =0.375);
[0118] S2. Solution A and solution B are added dropwise to solution C together, and stirred continuously to form a preliminary suspension. During the process, the dripping speed of solution A and solution B needs to be controlled to be slow and uniform. After the dropwise addition is completed, the suspension is transferred to an oil bath at a temperature of 80°C and stirred for 12 hours. The precipitate is then filtered with deionized water and repeatedly washed until neutral. The precipitate is placed in a 65°C air drying oven for drying, and then ground into powder after drying;
[0119] S3. Place in a muffle furnace and calcine for 4 hours at 600℃;
[0120] S4. Weigh 1 g of the calcined catalyst support into a crucible and dissolve 0.25 g of Co(NO 3 ) 2 6H 2 O, drip an equal volume into a crucible containing 1 g of the carrier, stir for 12 h, and then put it into a forced air drying oven at 80 °C to dry;
[0121] S5. Place in an atmosphere containing hydrogen and reduce at 600°C for 2h to obtain a composite catalyst in which the molar ratio of Ni and Mg to Al is 1 / 2, the molar ratio of Ni to Mg is 1, and the Co content is 5wt%, recorded as 5Co / Ni0.5-Mg0.5-Al.
[0122] The application of the composite catalyst in hydrogen production by steam reforming of acetic acid comprises the following steps:
[0123] (1) Adding acetic acid and phenol, light components of bio-oil, to a certain amount of deionized water to prepare a mixed solution of 1 wt % phenol and 9 wt % acetic acid.
[0124] (2) The catalyst filling amount is 0.2 g and is fixed with quartz wool.
[0125] (3) Use nitrogen to purge the bed for 10 minutes, then keep the nitrogen flow rate at 35 ml / min, raise the reactor temperature to 550°C at a rate of 10°C / min, and inject the reactant solution at a rate of 0.15 ml / min for constant temperature reaction (stop the reaction when the reaction time reaches 50 hours, and stop it if the reaction bed is blocked in the middle).
[0126] (4) Use a flow meter to monitor the gas flow rate at the outlet. At the same time, collect the gas product every 1 hour, and use a gas chromatograph to analyze the product gas concentration, and finally organize the analysis data.
[0127] Comparative Example 1
[0128] A method for preparing a composite cobalt catalyst for hydrogen production by steam reforming of light components of bio-oil, characterized in that it comprises the following steps:
[0129] S1. 5.94gNi(NO 3 ) 2 6H 2 O, 15gAl(NO 3 ) 3 9H 2 O, 5.76g citric acid C 6 H 8 O 7 Dissolve in 50 ml of deionized water to obtain metal ion salt solution A; weigh 1.59 g Na 2 CO 3 , 5g NaOH was dissolved in 50ml deionized water to prepare anionic solution B; 5.5g NaOH was dissolved in 50ml deionized water to prepare alkaline solution C (OH - / Al 3+ =6.3, CO 3 2- / Al 3+ =0.375);
[0130] S2. Solution A and solution B are added dropwise to solution C together, and stirred continuously to form a preliminary suspension. During the process, the dripping speed of solution A and solution B needs to be controlled to be slow and uniform. After the dropwise addition is completed, the suspension is transferred to an oil bath at a temperature of 80°C and stirred for 12 hours. The precipitate is then filtered with deionized water and repeatedly washed until neutral. The precipitate is placed in a 65°C air drying oven for drying, and then ground into powder after drying;
[0131] S3. Place in a muffle furnace and calcine for 4 hours at 600℃;
[0132] S4. Weigh 1 g of the calcined catalyst support into a crucible and dissolve 0.25 g of Co(NO3 ) 2 6H 2 O, drip an equal volume into a crucible containing 1 g of the carrier, stir for 12 h, and then put it into a forced air drying oven at 80 °C to dry;
[0133] S5. Place it in an atmosphere containing hydrogen and reduce it at 600°C for 2h to obtain a composite cobalt catalyst in which the molar ratio of Ni to Al is 1 / 2 and the Co content is 5wt%, recorded as 5Co / Ni1-Mg0-Al.
[0134] The application of the composite cobalt catalyst in hydrogen production by steam reforming of acetic acid comprises the following steps:
[0135] (1) A certain amount of deionized water was added to acetic acid, a light component of bio-oil, to prepare a 35.7 wt % mixed solution with S / C=3.
[0136] (2) The catalyst filling amount is 0.2 g and is fixed with quartz wool.
[0137] (3) Use nitrogen to purge the bed for 10 minutes, then keep the nitrogen flow rate at 35 ml / min, raise the reactor temperature to 550°C at a rate of 10°C / min, and inject the reactant solution at a rate of 0.15 ml / min for constant temperature reaction (stop the reaction when the reaction time reaches 50 hours, and stop it if the reaction bed is blocked in the middle).
[0138] (4) Use a flow meter to monitor the gas flow rate at the outlet. At the same time, collect the gas product every 1 hour, and use a gas chromatograph to analyze the product gas concentration, and finally organize the analysis data.
[0139] Comparative Example 2
[0140] A method for preparing a nickel-magnesium-aluminum catalyst for steam reforming of light components of bio-oil to produce hydrogen comprises the following steps:
[0141] S1. 2.97gNi(NO 3 ) 2 6H 2 O, 2.56 g Mg(NO 3 ) 2 6H 2 O, 15gAl(NO 3 ) 3 9H 2 O, 5.76g citric acid C 6 H 8 O 7 Dissolve in 50 ml of deionized water to obtain metal ion salt solution A; weigh 1.59 g Na 2 CO3 , 5g NaOH was dissolved in 50ml deionized water to prepare anionic solution B; 5.5g NaOH was dissolved in 50ml deionized water to prepare alkaline solution C (OH - / Al 3+ =6.3, CO 3 2- / Al 3+ =0.375);
[0142] S2. Solution A and solution B are added dropwise to solution C together, and stirred continuously to form a preliminary suspension. During the process, the dripping speed of solution A and solution B needs to be controlled to be slow and uniform. After the dropwise addition is completed, the suspension is transferred to an oil bath at a temperature of 80°C and stirred for 12 hours. The precipitate is then filtered with deionized water and repeatedly washed until neutral. The precipitate is placed in a 65°C air drying oven for drying, and then ground into powder after drying;
[0143] S3. Place in a muffle furnace and calcine for 4 hours at 600℃;
[0144] S4. Place in an atmosphere containing hydrogen and reduce at 600°C for 2h to obtain an unloaded metal catalyst, which is recorded as Ni0.5-Mg0.5-Al.
[0145] The application of the nickel-magnesium-aluminum catalyst in hydrogen production by steam reforming of acetic acid comprises the following steps:
[0146] (1) A certain amount of deionized water was added to acetic acid, a light component of bio-oil, to prepare a 35.7 wt % mixed solution with S / C=3.
[0147] (2) The catalyst filling amount is 0.2 g and is fixed with quartz wool.
[0148] (3) The bed was purged with nitrogen for 10 min, and then the nitrogen flow rate was kept constant at 35 ml / min. The reactor temperature was raised to 550 °C at a rate of 10 °C / min, and the reactant solution was injected at a rate of 0.15 ml / min for constant temperature reaction.
[0149] (4) Use a flow meter to monitor the gas flow rate at the outlet. At the same time, collect the gas product every 1 hour, and use a gas chromatograph to analyze the product gas concentration, and finally organize the analysis data.
[0150] The above embodiments and comparative examples data and effects are discussed:
[0151] Examples 1-3 and Comparative Examples 1-2 of the present invention investigate the effects of changes in the structure and species of the catalyst on the reaction effect.
[0152] (one) Figure 1and Figure 2 It shows that the physical phases of Examples 1-3 and Comparative Example 1 are composed of spinel and nickel-cobalt metal and have different chemical properties, wherein the catalyst phase spinel carrier in Comparative Example 1 is mainly a nickel-aluminum spinel carrier, and the catalysts in Examples 1-3 contain a carrier of mixed nickel-aluminum spinel and magnesium-aluminum spinel. The four catalysts have good crystallinity, and it can be seen from the overall integrated area that Example 2 has more acidic sites.
[0153] (two) Figure 3 and Figure 4 The specific surface area, pore size and XPS of Examples 1-3 and Comparative Example 1 are shown. The four catalysts show an H1 type hysteresis loop. It can be seen that the addition of Mg and the change of the Ni / Mg molar ratio have a certain effect on the surface structure of the catalyst. As the Ni / Mg molar ratio decreases, the average pore size of the catalyst in Example 3 reaches a maximum value of 12.4 nm, while the specific surface area of the catalyst in Example 2 reaches a maximum value of 218.9 m 2 / g, and the change of Ni / Mg ratio leads to different oxygen vacancies and changes in the amount of active metals in the catalysts.
[0154] (three) Figure 5 The effects of Examples 1-3 and Comparative Example 1 on the stability test reaction of acetic acid, a light component of bio-oil, are shown. In terms of reaction conditions, the high concentration of reactants and the long contact time pose a great challenge to the high efficiency of the reaction. The formula for selectivity and acetic acid conversion is as follows:
[0155]
[0156]
[0157] Obviously, Examples 2 and 3 show a stable reaction effect of up to 50 hours, and the product gas components are mainly hydrogen and carbon dioxide with a large proportion, and carbon monoxide and methane with a small proportion. The acetic acid conversion rate in Example 2 is stably maintained at a level of 80-90%.
[0158] (Four) Figure 6 The phase composition of the spent catalyst after the stability test experiment of Examples 1-3 and Comparative Example 1 is shown. After the stability test experiment, the spinel structure is still maintained, in which MgAl 2 O 4 It can stabilize the nanoparticles and well inhibit the aggregation and sintering of metal Ni. In the presence of Co metal, the spinel species peak still exists, and no NiO or other species peaks related to nickel metal oxides are detected. Ni metal is dominant relative to the oxidized form because the covered Co is more easily oxidized to form CoO. CoO and Co synergistically adsorb bridge acetate, which reacts rapidly with water vapor to form COx and H 2 The addition of Co enhances the water gas conversion activity, resulting in low CO selectivity and high H 2 Selective.
[0159] (five) Figure 7 The carbon deposition of waste catalysts after the stability test experiments of Examples 1-3 and Comparative Example 1 is shown, among which the carbon deposition rate of Example 3 is the lowest, and the carbon deposition rate of Example 2 is close to that of Example 3, and the reaction effect is relatively the best. The carbon deposition can be eliminated by introducing air at a high temperature of 600°C, and there is potential in the ability to regenerate the catalyst.
[0160] (six) Figure 8 The steam reforming effect of the wood vinegar model compound (1wt% phenol + 9wt% acetic acid) was demonstrated (catalyst: 5Co / Ni0.5-Mg0.5-Al). At 550°C, the hydrogen selectivity was maintained at a fairly good level. Due to excessive water vapor, the conversion rate fluctuated around 61%. At the same time, the methane selectivity was extremely low at around 0.08% (not shown in the figure due to its low proportion), and the CO selectivity was around 4%, which was conducive to carbon capture and hydrogen purification and utilization.
[0161] (seven) Fig. 9 The gas selectivity and reactant conversion effect of Example 2 and Comparative Example 2 in the reaction of acetic acid, a light component of bio-oil, are demonstrated.
[0162] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a composite catalyst for hydrogen production by steam reforming of light components of bio-oil, characterized in that: The steps include: S1. Weigh nickel salt, aluminum salt, magnesium salt and organic chelating agent according to mass ratio and dissolve them in deionized water, stir them thoroughly to prepare solution A; weigh carbonate and alkali according to mass ratio and dissolve them in deionized water, stir them thoroughly to prepare solution B; dissolve alkali in deionized water, stir them thoroughly to prepare solution C; S2. The solutions A and B were slowly dripped into the solution C, and the mixture was stirred in an oil bath until a precipitate was formed. The suspension was filtered, rinsed with deionized water and dried, and ground to obtain a carrier precursor; S3. The carrier precursor is placed in a high temperature furnace and calcined to obtain a nickel-magnesium-aluminum composite spinel carrier; S4. The cobalt salt solution is impregnated and loaded on a nickel-magnesium-aluminum composite spinel support, stirred and dried; S5. Placed under high temperature reducing atmosphere for reduction to obtain the composite catalyst; The composite catalyst is applied to the fixed bed reaction device in the process of steam reforming hydrogen production from light components of bio-oil, and the stable reaction time is more than 50 hours, the conversion rate is maintained at 80%-90%, the H2 yield is maintained at more than 60%, and the output H2 gas concentration is maintained at more than 40%.
2. The preparation method according to claim 1, characterized in that: In step S1, the nickel salt is at least one of nickel nitrate, nickel nitrite, nickel acetate, nickel sulfate, nickel sulfite, nickel carbonate, nickel chloride, and nickel sulfide; the magnesium salt is at least one of magnesium nitrate, magnesium nitrite, magnesium acetate, magnesium sulfate, magnesium sulfite, magnesium carbonate, magnesium chloride, and magnesium sulfide; the aluminum salt is at least one of aluminum nitrate, aluminum nitrite, aluminum acetate, aluminum sulfate, aluminum sulfite, aluminum carbonate, aluminum chloride, and aluminum sulfide; the organic chelating agent is at least one of citric acid, oxalic acid, urea, malic acid, and glycine; m(C) / m(M)=0.01-10; the carbonate is at least one of sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate; the alkali is at least one of potassium hydroxide, sodium hydroxide, and ammonia water, and the addition amount is 2-15g; OH - With Al 3+ The molar ratio of CO3 is 4 to 8. 2- With Al 3+ The molar ratio of Ni is 0.2 to 5. 2+ With Mg 2+ The molar ratio is 0.1-10; m(Ni 2+ and Mg 2+ ):m(Al 3+ )=0.4~0.
6.
3. The preparation method according to claim 1, characterized in that: In step S2, the solution has a pH value of 8 to 14, a stirring temperature of 40 to 90° C., a stirring time of 6 to 18 hours, and is rinsed with deionized water until the pH value is 7 to 8. The drying temperature is 50 to 90° C., and the drying time is 6 to 18 hours.
4. The preparation method according to claim 1, characterized in that: In step S3, the calcination is carried out under ventilation, still air, nitrogen or argon atmosphere conditions, the calcination temperature is 400-600° C., the calcination time is 2-6 hours, and the heating rate is 10° C. / min.
5. The preparation method according to claim 1, characterized in that: In step S4, the cobalt salt is at least one of cobalt nitrate, cobalt nitrite, cobalt acetate, cobalt sulfate, cobalt sulfite, cobalt carbonate, cobalt chloride, and cobalt sulfide, and the cobalt loading is 0-20% and is not zero.
6. The preparation method according to claim 1, characterized in that: In step S4, 0-100 wt.% methanol or ethanol aqueous solution is used for impregnation, the stirring time is 12-24 hours, the drying temperature is 50-100° C., and the drying time is 6-18 hours.
7. The preparation method according to claim 1, characterized in that: In step S5, the reducing atmosphere is at least one of hydrogen, ammonia, carbon monoxide, and methane; the reducing temperature is 300 to 800° C., the reducing time is 1 to 3 hours, and the heating rate is 10° C. / min.
8. The composite catalyst obtained by the preparation method according to any one of claims 1 to 7.
9. The composite catalyst according to claim 8, characterized in that The composite catalyst has multiple mesoporous structures.
10. Use of the composite catalyst prepared by the preparation method according to any one of claims 1 to 7 or the composite catalyst according to claim 8 or 9 in steam reforming of light components of bio-oil to produce hydrogen.
Citation Information
Patent Citations
A nickel-manganese-aluminum composite oxide catalyst for hydrogen production from acetic acid autothermal reforming
CN109225249B
Preparation method of catalyst for biomass pyrolysis tar steam reforming
CN110639606A
Biomass tar steam reforming catalyst and preparation method thereof
CN111644176A
Method for hydrogen production by promoting water-phase reforming of recyclable biomass alcohol derivatives through alkali liquor
CN116902916A
Cited By
Ni-based glycerol steam reforming catalyst and preparation method thereof
CN120550811A