Preparation method of composite metal foil

The one-step method of continuous chemical and electroplating with surface pre-treatment for composite metal foils addresses production inefficiencies and costs by enhancing bonding and uniformity, offering a cost-effective and efficient process for composite metal foil production.

CN120311260AActive Publication Date: 2025-07-15JIANGMEN DEZATE HIGH-TECH CO LTD

Patent Information

Application Number
CN202510346625.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-24
Publication Date
2025-07-15
Estimated Expiration
2045-03-24

AI Technical Summary

Technical Problem

The existing composite metal foil preparation process has problems such as low production efficiency, high cost, poor binding force and complex process. Especially in the full-dry process, magnetron sputtering and vacuum evaporation technology are complex and may lead to base film perforation at high temperatures. Traditional electroplating methods cannot directly plating copper on polymer materials.

Method used

A one-step process combining continuous electrochemical plating and electroplating is used to form micro pits by surface pretreating the film of polymer material, and a metal layer is deposited in the micro pits by electrochemical plating and electrochemical deposition to form composite metal foils.

Benefits of technology

It realizes efficient and low-cost composite metal foil preparation, with strong bonding force of the metal layer, smooth surface, and high production efficiency, and is suitable for current collectors of new energy battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120311260A_ABST
    Figure CN120311260A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a composite metal foil. The method comprises the following steps: preparing a high polymer material into a continuous film; carrying out surface pretreatment on the continuous film; carrying out chemical plating on the pretreated film to form a metal conductive layer; and after the metal conductive layer is formed, electrochemically depositing a metal layer to obtain the composite metal foil. According to the composite metal foil prepared according to the technical scheme, the plating layer is high in binding force, more uniform and high in conductivity; the preparation method is simple to operate, short in technological process, low in production cost and high in production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of composite metal materials, and particularly relates to a method for preparing a composite metal foil. Background Art

[0002] A composite metal foil is a composite material with a "metal - polymer material - metal" sandwich structure. The most common composite metal foils are composite copper foils and composite aluminum foils, which are currently widely used as current collectors for new energy batteries.

[0003] As an organic component, the surface binding force between the polymer film and the metal is very weak, and the metal cannot be directly electroplated on the surface. Therefore, most traditional preparation processes adopt a two / three-step method. In the two-step method, a layer of metal is first deposited on the film surface by magnetron sputtering to increase the binding force between the film and the metal, and then the metal layer is deposited by electroplating in water. The three-step method, based on the two-step method, adds a vacuum evaporation process between magnetron sputtering and electroplating in water to accelerate the deposition of the metal layer by evaporation. However, when copper is deposited on the base film by the magnetron sputtering process, under high speed and high temperature conditions, particles may splash and melt through the base film, resulting in perforations; moreover, the magnetron sputtering and vacuum evaporation technologies are relatively complex, and new processes such as transfer welding need to be added, increasing equipment investment and production costs and reducing production efficiency.

[0004] Currently, the two / three-step production process of composite copper foils has problems such as low yield and insufficient binding force between layers. In addition, the two / three-step production process is complex and requires multiple production steps, reducing production efficiency. Relatively speaking, the one-step method has a short process, high production efficiency, and can improve the production yield and coating uniformity of products, so it has attracted much attention. According to whether the process contacts water, the one-step method can be divided into a fully wet method (such as electroless plating) and a fully dry method (such as magnetron sputtering, vacuum evaporation).

[0005] For the fully dry method, magnetron sputtering may reduce the physical properties of the composite copper foil during continuous sputtering, and the cost is relatively high. In addition, it is difficult to achieve a thickness of 1 μm by vacuum evaporation, with low efficiency, poor surface flatness of the copper foil, high energy consumption, and high production costs. Moreover, due to the strong corrosion resistance of polymer materials such as PET, PP, and PI, the traditional ABS electroplating method cannot be directly used to electroplate a copper layer. By depositing a conductive metal layer by chemical plating and then electroplating, the defect of non-conductivity of polymer materials can be solved.

[0006] Plastic electroplating, also known as wet electroplating or aqueous solution electroplating, is a technique that deposits a metal layer on the surface of non-metal substrates such as plastics through an electrochemical method. It usually requires pre-treatment on the plastic surface (such as roughening, sensitization, activation, electroless nickel plating, etc.) to enhance the adhesion between the metal coating and the plastic substrate. Plastic electroplating coats the plastic surface with metal, endows it with metallic properties, and fully integrates the characteristics of plastics and metals. Plastic electroplated products are applied in industries such as electronics, automotive, and household items. Currently, the most widely used plastics for electroplating in the market are ABS (terpolymer of acrylonitrile (A)-butadiene (B)-styrene (S)) or PC / ABS alloy materials. There is a lack of a preparation method for continuously producing composite metal foils in one step, with high production efficiency, high coating adhesion, smooth metal layer surface, low cost, and low energy consumption. Summary of the Invention

[0007] In view of the deficiencies of the prior art and to solve at least one problem in the prior art, the present invention provides a method for preparing a composite metal foil. This method uses a polymer material as the substrate, combines continuous electroless plating and continuous electroplating under dynamic conditions, and electroplates the composite metal foil in one step. The operation is simple, the production cost is low, the coating adhesion is high, the process flow is short, and the production efficiency is high.

[0008] Specifically, the present invention is realized through the following method:

[0009] On the one hand, the present invention provides a method for preparing a composite metal foil, including:

[0010] Making the polymer material into a continuous film;

[0011] Performing surface pre-treatment on the continuous film;

[0012] Performing electroless plating on the pre-treated film to form a metal conductive layer;

[0013] Then performing electrochemical deposition of a metal layer to obtain a composite metal foil.

[0014] In the present invention, the film contains two or more components, and at least one of them can be etched.

[0015] Furthermore, the content of the etched film component is less than 30 wt%; preferably, the content of the etched film component is less than 20 wt%; preferably, the content is 5 - 30 wt%. In some embodiments, if the content of the etched film component is too high, it will cause film perforation problems during the roughening process, and if it is too low, it will lead to a decrease in the adhesion between the film and the metal. Among them, the perforation problem during the roughening process mainly affects the strength of the composite metal foil and the flatness of the surface of the composite copper foil, resulting in poor phenomena such as perforation of the composite metal foil and affecting the yield of the composite metal foil.

[0016] Further, the polymer materials used to prepare the continuous film include, but are not limited to, polypropylene (PP), polyethylene (PE), polyethylene terephthalate (PET), polyamide (PA), polyphenylene sulfide (PPS), polysulfone (PPSU), polyimide (PI), polyvinylidene fluoride (PVDF), polylactic acid (PLA), polycaprolactone (PCL), polystyrene (PS), polymethyl methacrylate (PMMA), acrylonitrile - butadiene - styrene terpolymer (ABS), thermoplastic elastomers (TPU, TPE, etc.), and two or more of their derivatives, cross - linked products and copolymers.

[0017] Further, for the method of forming a film from the polymer material, first, the etchable component is blended with the target polymer material. The blending process can be achieved by methods such as using a mixer, single - screw, double - screw or multi - screw for blending, or by melt blending in a polymerization kettle. Preferably, the blending process is melt blending in a polymerization kettle.

[0018] Further, process conditions such as the melting temperature, stirring speed, blending and stirring time of the polymer material can be selected according to the type of polymer material actually used.

[0019] Further, by selecting a suitable blending process and raw material ratio, the etchable component is uniformly dispersed in the main polymer, which is beneficial for subsequent etching to form uniform pits. However, the present invention is not limited to the case where the etchable component is uniformly distributed. Other suitable dispersion cases, such as sea - island structure, interpenetrating network, etc. are also within the scope of the present invention.

[0020] Further, the composite material obtained after blending is formed into a sheet through melting, screw extrusion, casting and film - casting processes; then the obtained sheet is formed into a composite film through a biaxial stretching process.

[0021] Further, the thickness of the continuous film made of the polymer material is 1 - 15 μm; preferably, the thickness of the film is 2 - 14 μm, 3 - 13 μm, 4 - 12 μm, 5 - 11 μm, 6 - 10 μm, 7 - 9 μm; more preferably, the thickness of the film is 2 - 6 μm.

[0022] Since these polymer materials and the films prepared from them are organic substances themselves, their bonding force with metals is very weak, and a metal layer cannot be directly electroplated on the surface. In the prior art, a metal layer is usually deposited on the polymer surface by vapor deposition before subsequent electroplating can be carried out. On the one hand, in the vapor deposition method, the adhesion between the coating and the polymer material layer is weak, and since the deposition requires the metal to be vaporized at a high temperature, it is easy to damage the polymer material and generate internal stress during the production process. In this application, the surface of the film is pretreated. The pretreatment process is carried out at room temperature. An etching solution in a solution state is used to etch the polymer surface, making the polymer surface present micro-pits, and then metal atoms are deposited in the micro-pits by electroless plating, avoiding the damage to the polymer material caused by high temperature and avoiding the use of expensive vapor deposition instruments. The pretreatment process includes roughening, sensitization, activation, electroless nickel plating, etc. Among them, roughening refers to treating the substrate with solutions such as strong acids (such as chromic acid, sulfuric acid), strong bases, and strong oxidants, making the surface of the substrate in a microscopically rough state, increasing the contact surface between the coating and the substrate, forming a large number of hydrophilic groups on the surface of the substrate, and changing the substrate from a hydrophobic body to a hydrophilic body. The surface of the substrate after roughening is negatively charged and easily adsorbs Sn 2+ , Ag + , etc., enabling sensitization, activation, and electroless plating to proceed smoothly.

[0023] Furthermore, before the surface pretreatment of the continuous film, steps such as degreasing, cleaning, and drying are also included. Among them, solutions such as alkalis, acids, and organic solvents can be used for degreasing. The degreasing methods include immersion brushing, ultrasonic cleaning, or spraying, and degreasing can also be carried out by heating.

[0024] Furthermore, the surface pretreatment of the continuous film described in the present invention is an etching treatment, and the etching treatment can be carried out by chemical etching with acids, alkalis, or reactive gases, or by etching with plasma.

[0025] Even further, the surface pretreatment of the continuous film is to immerse the film in the etching solution to form micro-pits on the surface of the film.

[0026] Further, the etching solution includes acids (such as chromic acid, hydrochloric acid, sulfuric acid, or nitric acid), bases (such as sodium hydroxide or potassium hydroxide), salt solutions (such as potassium permanganate), organic solvents (such as chloroform, carbon tetrachloride, dichloromethane, trichloroethane, or acetone), etc. In the present invention, the etching solution is not limited to a single etching solution component, and the etching solution can also be a mixed solution containing two or more components, such as a mixed acid of chromic acid and hydrochloric acid. In this application, when the etching solution is an acid or a base, on the one hand, the destructive effect of the acid or base on the polymer chain is utilized to partially etch the etchable components, and on the other hand, the oxidation effect of the acid or base is utilized to generate hydrophilic polar groups on the polymer surface, thereby enhancing the binding with the coating. When an organic solvent is used as the etching solution, the principle of like dissolves like is utilized to dissolve the etchable components in the solution, thereby leaving micro-pits on the film surface.

[0027] Further, the etching treatment forms micro-pits with a diameter less than 0.5 μm on the film surface; preferably, the diameter of the micro-pits is less than 0.3 μm.

[0028] In the present invention, the diameter of the micro-pits is related to the residence time of the film in the etching solution and the concentration of the etching solution. This application preferably selects the above-mentioned diameter of the micro-pits. The diameter in this range is conducive to the deposition of metal atoms on the surface and inside of the micro-pits, thereby enhancing the binding force of the metal film, but the invention is not limited to the above diameter range.

[0029] In the present invention, the etchable component is blended with the target polymer material to form a film. The etchable component in the continuous film is removed by etching, and the target polymer is retained, so that pits are formed on the surface of the polymer film, increasing the specific surface area. During the subsequent electroless plating process, metal atoms are deposited in the pits, effectively enhancing the binding force between the film and the plated metal. Among them, since the etchable component is uniformly distributed in the film, the etchable component is distributed on both sides of the film. During the surface pretreatment process, since the entire film is immersed in the solution, micro-pits are formed on the surfaces of both sides of the film, so metal atoms can be deposited on both sides of the film simultaneously during the subsequent electroless plating and electroplating.

[0030] Further, before the electroless plating of the film after surface pretreatment, it also includes conventional steps of the prior art such as reduction, activation, and peptization.

[0031] Further, the film after surface pretreatment is subjected to electroless plating to form a metal conductive layer. The electroless plating means that in the electroless plating stage, by adding a catalyst to the electroless plating solution, metal ions are reduced to atoms and then deposited on the film surface. In this way, the binding force between the metal atoms and the film is enhanced, and the polymer film is not damaged.

[0032] Preferably, the material of the metal conductive layer is selected from one or more of copper, gold, silver, aluminum, nickel, titanium, aluminum, chromium, zinc, cadmium, lead, platinum, iron, cobalt, manganese, antimony, bismuth, gallium, indium, thallium, palladium, rhenium, rhodium, osmium, iridium, niobium, tungsten; more preferably, selected from one or more of nickel, copper, gold, silver, aluminum.

[0033] Furthermore, the thickness of the metal conductive layer formed by electroless plating is 10 - 500 nm. Preferably, the thickness is 20 - 100 nm (i.e., 0.02 - 0.1 μm).

[0034] Furthermore, an electrochemical deposition metal layer is carried out on the film after electroless plating treatment to obtain a composite metal foil. The electrochemical deposition metal layer means using the film as the cathode and an electrolytic metal foil or metal plate as the anode, and depositing a dense metal layer on the film surface by electrochemical action.

[0035] Preferably, the material of the metal layer is selected from one or more of copper, gold, silver, aluminum, nickel, titanium, aluminum, chromium, zinc, cadmium, lead, platinum, iron, cobalt, manganese, antimony, bismuth, gallium, indium, thallium, palladium, rhenium, rhodium, osmium, iridium, niobium, tungsten; more preferably, selected from one or more of nickel, copper, gold, silver, aluminum.

[0036] Furthermore, during the electrochemical deposition process, continuous electroplating is carried out until the thickness of the metal layer is greater than 0.5 μm.

[0037] In the present invention, the metal layer deposited by electrochemistry can be plated with one or more than one metal according to actual needs to form one or more than one metal layer. Therefore, according to the metal to be electroplated and the number of metal layers, the electrochemical deposition process can continue electroplating until the metal layer reaches the required thickness. Therefore, the present invention is not limited to the above - mentioned electroplated metal layer thickness range.

[0038] Preferably, during the electroplating process, a conductive film is used as the cathode and a metal (such as titanium, gold, silver, copper, etc.) is used as the anode, and electroplating is carried out in an electrolyte solution. More preferably, during the electroplating process, the film is used as the cathode and a solid copper plate is used as the anode, and electroplating is carried out in a copper sulfate electrolyte solution.

[0039] By controlling the metal ion concentration, current density, and additive concentration in the electrolyte solution, the metal layer is thickened to the specified thickness.

[0040] Furthermore, the electroplated film is subjected to passivation and drying treatments to make the final product have excellent antioxidant properties.

[0041] Furthermore, the composite metal foil described in the present invention is a continuous body, and subsequent different specifications can be prepared by cutting according to actual needs.

[0042] On the one hand, the present invention also provides a composite metal foil obtained by the above - mentioned preparation method.

[0043] On the other hand, the present invention also provides an application of the composite metal foil prepared by the above preparation method in the preparation of new energy batteries.

[0044] Advantages of the present invention:

[0045] In the prior art, the final product can only be prepared by a two-step method (magnetron sputtering + electroplating) or a three-step method (magnetron sputtering + vacuum evaporation + electroplating), which has problems such as cumbersome process, low production efficiency, high cost, poor bonding strength between metal layers, and poor uniformity of metallic copper.

[0046] The present invention provides a preparation method of a composite metal foil. This method performs surface pretreatment, electroless plating, and electrochemically depositing a metal layer on the thin film, and there is no need to interrupt or replace the fixture during the process, realizing one-step continuous production from the thin film to the composite metal foil.

[0047] The method of the present invention first prepares a continuous thin film containing two or more polymer materials, etches at least one of the components therein, thereby forming micro-pits on the surface of the thin film, enhancing the bonding force between the thin film and the plated metal through the formed micro-pits, and then laminating conductive metal through subsequent electroless plating and electroplating.

[0048] The preparation method of the composite metal foil provided by the present invention is simple in operation, low in production cost, short in process flow, and high in production efficiency; the obtained composite metal foil has strong coating adhesion, good uniformity, and strong conductivity. Description of the Drawings

[0049] The following further describes the present invention with reference to the drawings and embodiments, wherein:

[0050] Figure 1 It is a schematic structural diagram of the composite metal foil prepared in Example 6 of the present invention.

[0051] Figure 2 It is the composite metal foil prepared in Example 6 of the present invention.

[0052] Figure 3 It is a scanning electron microscope image of the surface-pretreated thin film in Example 8 of the present invention.

[0053] Figure 4 It is a scanning electron microscope image of the surface-pretreated thin film in Comparative Example 3 of the present invention.

[0054] Figure 5 It is a process flow chart of the continuous electroplating of the composite metal foil of the present invention. Detailed Embodiments

[0055] The following details the embodiments of the present invention. The embodiments described below are exemplary and are only used to explain the present invention and should not be construed as a limitation to the present invention.

[0056] Among them, unless otherwise specified, the materials can all be obtained through commercial channels, and unless otherwise specified, the methods are all conventional methods.

[0057] Example 1

[0058] The polymer material 1 is PP M09, and the manufacturer is Maoming Branch of China Petroleum & Chemical Corporation.

[0059] Example 2

[0060] Polymer material 2: 75wt% of PP M09 and 25wt% of TPU material are blended and modified to prepare polymer material 2. The blending and modification can be achieved by blending methods such as internal mixer, single-screw, double-screw or multi-screw, or can also be achieved by melt blending in a polymerization kettle. It is preferably achieved by melt blending in a polymerization kettle to achieve uniform dispersion. The blending temperature does not exceed 280 °C, the blending duration does not exceed 24 h, and the stirring speed is not less than 100 revolutions / min.

[0061] Example 3

[0062] Polymer material 3: 95wt% of PET and 5wt% of TPE material are blended and modified to prepare polymer material 2. The blending and modification can be achieved by blending methods such as internal mixer, single-screw, double-screw or multi-screw, or can also be achieved by melt blending in a polymerization kettle. It is preferably achieved by melt blending in a polymerization kettle to achieve uniform dispersion. The blending temperature does not exceed 300 °C, the blending duration does not exceed 24 h, and the stirring speed is not less than 100 revolutions / min.

[0063] Example 4

[0064] Polymer material 4: 75wt% of PET, 5wt% of TPU and 20wt% of TPE material are blended and modified to prepare polymer material 2. The blending and modification can be achieved by blending methods such as internal mixer, single-screw, double-screw or multi-screw, or can also be achieved by melt blending in a polymerization kettle. It is preferably achieved by melt blending in a polymerization kettle to achieve uniform dispersion. The blending temperature does not exceed 300 °C, the blending duration does not exceed 24 h, and the stirring speed is not less than 100 revolutions / min.

[0065] Example 5

[0066] Polymer material 5: 65% of PET and 35% of TPE material are blended and modified to prepare polymer material 5. The blending and modification can be achieved by blending methods such as internal mixer, single-screw, double-screw or multi-screw, or can also be achieved by melt blending in a polymerization kettle. It is preferably achieved by melt blending in a polymerization kettle to achieve uniform dispersion. The blending temperature does not exceed 300 °C, the blending duration does not exceed 24 h, and the stirring speed is not less than 100 revolutions / min.

[0067] Example 6

[0068] The polymer material 2 was made into a continuous film with a thickness of 6 μm. The specific operation was as follows: The uniformly mixed composite material was formed into a sheet with a certain thickness and width through melting, screw extrusion, casting, and sheet casting processes. The sheet was finally formed into a composite continuous film through a biaxial stretching process.

[0069] The above-mentioned film was continuously electroplated using a continuous electroplating device.

[0070] First, the polymer film was hung up so that it could be connected to the power supply to form a closed circuit, enabling the electroplating to proceed smoothly.

[0071] Then, the film was sent into a roughening tank and continuously immersed in an etching solution to form micro-pits on the film surface. The average diameter of the micro-pits was 0.12 μm. The roughening solution in the roughening tank was a high-chromic acid type roughening solution, containing 400 g / L chromic anhydride and 400 g / L sulfuric acid, and was treated at 70 °C for 12 min.

[0072] The roughened film was sent into a reduction tank for reduction treatment, and then placed in a cleaning tank and rinsed with clean water after treatment. The reduction solution was an aqueous solution of 1 g / L sodium borohydride, carried out at room temperature for 10 min. After the reduction treatment, it was placed in a cleaning tank and rinsed with clean water.

[0073] After the reduction treatment, the film was sent into an activation tank for activation treatment, and then placed in a cleaning tank and rinsed with clean water after treatment. The activation solution in the activation tank was a Pd-Sn activation solution, specifically containing 250 mL / L hydrochloric acid, 2 - 8 g / L stannous chloride, and 15 ppm palladium, at a temperature of 35 °C and an activation time of 4 min.

[0074] After the activation treatment, the film was sent into a peptizing tank for peptizing treatment, and then placed in a cleaning tank and rinsed with clean water after treatment. The peptizing solution in the peptizing tank was 80 g / L hydrochloric acid, at a temperature of 35 °C and a time of 8 min.

[0075] Next, the above-treated film was electrolessly plated with copper to form a 0.06-μm-thick copper metal. The electroless copper plating solution included: 16 g / L copper sulfate, 14 g / L sodium potassium tartrate, 14.5 g / L sodium hydroxide, 15 mL / L formaldehyde, 2 mg / L 2,2′-bipyridine, 19.5 g / L EDTA, 2 mg / L potassium ferrocyanide, 2 mg / L methanol, with a pH of 12.5, a temperature of 35 °C, and a time of 7 min.

[0076] The above-treated thin film is electrochemically deposited with metallic copper until the thickness reaches 1.2 μm, thus obtaining a composite copper foil. In electroplating, the thin film serves as the cathode and the copper foil serves as the anode. The composition of the electroplating solution includes 200 g / L of copper sulfate, 35 g / L of sulfuric acid, and 100 mL / L of hydrochloric acid. The time is 45 min and the temperature is 25 °C.

[0077] The above thin film forms a composite metal foil with a certain thickness of the metal layer through the hydroelectroplating process, and the obtained electroplated copper layer is dense, smooth, and flat.

[0078] After electroplating, the thin film is washed with water in a water washing tank filled with water, then passivated in a passivation tank, and then washed again in a water washing tank filled with water. The thin film is dried by a dryer at 60 °C for 30 min. The passivation temperature is room temperature, the passivation solution is an aqueous solution containing 3 g / L of benzotriazole, the running speed of the film is 30 m / h, and the passivation time is 20 min.

[0079] After completing all steps, the thin film is unhooked.

[0080] Example 7

[0081] The preparation method of the composite metal foil is the same as that of Example 6, except that:

[0082] The above-treated thin film is electroless plated to form a 0.06-μm-thick metallic silver.

[0083] The composition and process conditions of electroless silver plating are: 5 g / L of silver nitrate, 5 g / L of EDTA, 50 mL / L of ethanol, 2 mL / L of OP-10, 5 mL / L of formaldehyde, carried out at room temperature, and the time is 30 min.

[0084] Example 8

[0085] The preparation method of the composite metal foil is the same as that of Example 6, except that:

[0086] The polymer material 3 is made into a continuous thin film with a thickness of 6 μm;

[0087] Example 9

[0088] The preparation method of the composite metal foil is the same as that of Example 6, except that:

[0089] The polymer material 4 is made into a continuous thin film with a thickness of 6 μm;

[0090] Example 10

[0091] The preparation method of the composite metal foil is the same as that of Example 6, except that:

[0092] The polymer material 4 is made into a continuous thin film with a thickness of 4 μm;

[0093] The polymer thin film is continuously immersed in the etching solution to form micropits on the surface of the polymer base film, and the average diameter of the micropits is 0.19 μm;

[0094] The above-treated thin film is electroless plated to form a 0.10-μm-thick metallic copper;

[0095] The above-treated thin film is electrochemically deposited with metallic copper until the thickness reaches 1.5 μm, and the composite copper foil is obtained.

[0096] Example 11

[0097] The preparation method of the composite metal foil is the same as that of Example 6, except that:

[0098] Acetone is used as the etching solution in the roughening stage.

[0099] Comparative Example 1

[0100] The preparation method of the composite metal foil is the same as that of Example 6, except that:

[0101] The polymer material 1 is made into a 6-μm-thick continuous thin film;

[0102] Comparative Example 2

[0103] A commercially available two-step method-prepared composite copper foil is used, with a PET thickness of 6 μm and a copper layer thickness of 1 μm.

[0104] Comparative Example 3

[0105] The preparation method of the composite metal foil is the same as that of Example 8, except that:

[0106] The polymer material 5 is made into a 6-μm-thick continuous thin film.

[0107] Test Example 1

[0108] Test method for the peel strength of the composite metal foil:

[0109] (1) Cut the composite copper foil material into 100 mm × 50 mm; (2) Lay the composite copper sample flat on the stainless steel substrate and gently press it with a leather mallet to ensure close contact between the sample and the stainless steel substrate; (3) Put it into the peel strength tester, set the test speed at 2 mm / min, and conduct the peel strength test. The peel strength tester will automatically record the maximum peel strength N between the sample and the metal substrate, repeat the test 5 times, and take the average value; (4) Calculate the adhesion: According to the recorded maximum peel strength and the sample size, calculate the adhesion of the sample according to the following formula.

[0110] Adhesion (N / cm) = Maximum peel strength (N) / Sample contact area (cm)

[0111] Test Example 2

[0112] Tensile strength and elongation at break of the thin film: After roughening the thin film, the tensile strength and elongation at break were measured according to the measurement method related to tensile strength and elongation at break in 7.1 of the standard GB / T 29847—2013 "Test Methods for Copper Foil for Printed Circuit Boards", and the test speed was 5 mm / min.

[0113] Test Example 3

[0114] Resistance: After electroplating the composite copper foil, the mass resistivity was measured with reference to the relevant method in GB / T 2036.

[0115] The test results are shown in Table 1. It can be seen from Table 1 that compared with the composite metal foils of Comparative Examples 1-3, the composite metal foils (Examples 6-10) prepared by the method provided by the present invention significantly improve the bonding strength between the thin film and the plated metal; this is because when only one matrix component is used (Comparative Example 1), it is difficult to control the micropore size formed by etching, and thus it is difficult to control the bonding between the metal layer and the thin film. Therefore, the bonding strength between the metal and the thin film is low; in the prior art, since the metal layer is directly deposited on the surface of the thin film (Comparative Example 2), the bonding strength between the metal and the thin film is low, and internal stress easily exists in the thin film. Therefore, the measured bonding strength between the metal and the thin film is also weak; when the etchable component is greater than 30 wt% (Comparative Example 3), due to the increase in the etched component, perforations appear in the thin film, affecting the deposition flatness of the metal layer and the strength of the matrix, resulting in a poor bonding strength between the thin film and the metal layer.

[0116] From the mechanical test results, it can also be seen that by controlling the content of the etchable component in the present application, the continuity of the matrix thin film is ensured, and thus the mechanical strength of the obtained composite metal foil is also relatively high, especially compared with Comparative Example 3 where perforations are formed. This shows that only surface-treating the thin film to ensure the continuity of the matrix is beneficial to enhancing the mechanical properties of the composite metal foil.

[0117] The resistance test results show that the conductive performance of the composite metal foil prepared in the present application is comparable to that of the composite foil prepared by the two-step method in the prior art, indicating that the composite metal foil of the present application can be used as a current collector for new energy batteries.

[0118] Table 1: Test Results of Examples and Comparative Examples

[0119]

[0120]

[0121] 4. Scanning Electron Microscope Test

[0122] The surface-pretreated thin films of Example 8 and Comparative Example 3 were characterized for their microscopic morphological features using a scanning electron microscope SEM. The test results are as followsFigure 3 and Figure 4 As shown in Figure 3 , it can be clearly seen that micro-pits are evenly etched on the surface of the film pretreated in Example 8, which is beneficial to the deposition of metal atoms in the electroless plating stage; while in Comparative Example 3 ( Figure 4 ), since the etched component is greater than 30%, the surface of the film is over-etched and even perforated. Due to the over-etching of the surface, it is difficult to deposit a complete and continuous metal layer under the same electroless plating conditions, which in turn affects the deposition of metal on the film surface in the electroplating stage, making it difficult to prepare a composite metal foil with good adhesion between the metal and the film.

[0123] The above has described the embodiments of the present invention in detail. The present invention is not limited to the above embodiments. Within the knowledge scope of those of ordinary skill in the art to which the present invention pertains, various changes can be made without departing from the gist of the present invention. In addition, without conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other.

Claims

1. A method for preparing a composite metal foil, characterized in that, It includes the following steps: Manufacture a polymer material into a continuous film; Perform surface pretreatment on the continuous film; Perform electroless plating on the pretreated film to form a metal conductive layer; Perform electrochemical deposition of a metal layer on the film after electroless plating to obtain a composite metal foil.

2. The method according to claim 1, characterized in that, The film contains two or more components, at least one of which can be etched.

3. The method according to claim 2, wherein The content of the etched film component is less than 30 wt%.

4. The method according to claim 1, wherein The surface pretreatment refers to immersing the film in a solution and using the etching components in the solution to etch at least one component of the film to form micro-pits on the film.

5. The method according to claim 4, wherein The diameter of the micro-pits is less than 0.5 μm.

6. The method according to claim 1, characterized in that The thickness of the film is 1-15 μm.

7. The method according to claim 1, characterized in that, The electroless plating refers to adding a catalyst to the solution during the electroless plating stage to reduce metal ions to atoms and then deposit them on the film surface; the metal is selected from one or more of nickel, copper, gold, silver, and aluminum.

8. The method according to claim 1, characterized in that The electrochemical deposition of the metal layer refers to using the film as the cathode and a metal plate as the anode to deposit a dense metal layer on the film surface by electrochemical action, and the metal is selected from one or more of nickel, copper, gold, silver, and aluminum.

9. A composite metal foil prepared by the preparation method according to any one of claims 1-8.

10. Use of the composite metal foil according to claim 9 in the preparation of new energy batteries.

Citation Information

Patent Citations

  • Preparation method of composite current collector

    CN114551896A

  • Preparation method of negative electrode composite current collector and product prepared by preparation method

    CN114678534A

  • Preparation method of composite current collector and product thereof

    CN116145121A

  • Composite current collector and preparation method and application thereof

    CN116207270A

  • Porous mesh polymer film carrier copper foil and preparation method thereof

    CN117239140A

Cited By

  • Positive electrode current collector, preparation method thereof and battery comprising positive electrode current collector

    CN120967291A