Flame retardant for shaving board as well as preparation method and application of flame retardant
Through the combination of boron-based flame retardant, melamine cyanurate and nano-alumina, the thermal stability and mechanical properties of particle board flame retardant are solved, and the coordinated improvement of flame retardant effect and mechanical properties are achieved, meeting the technical standards and safety requirements of particle board.
Patent Information
- Application Number
- CN202510492971.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-18
- Publication Date
- 2025-07-22
AI Technical Summary
The flame retardants of the existing particle board have problems such as poor thermal stability, easy precipitation, and poor compatibility with the matrix, resulting in a decrease in mechanical properties. The existing composite flame retardants have not significantly improved the mechanical properties of the plate while improving the flame retardant effect.
The combination of boron-based flame retardant, melamine cyanurate and nano-alumina is adopted to achieve synergistic complementarity of the flame retardant mechanism by controlling the dosage of the three. MCA uses non-combustible gases, and boron-based flame retardant and nano-alumina form a glass-like or dense oxide layer on the surface of the material, blocking the transfer of heat and oxygen, enhancing the strength of the carbon layer, reducing melt droplets, and improving safety.
The flame retardant effect and mechanical properties of particle board are improved, the static curve strength can reach 85.69MPa, the elastic modulus reaches 9739MPa, the internal bonding strength reaches 0.75MPa, and the 24-h water absorption thickness expansion rate is 11.4%, meeting the technical standards of directional particle board, and the combustion level reaches B1(C).
Smart Images

Figure BDA0005366101910000111 
Figure BDA0005366101910000121 
Figure BDA0005366101910000122
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of flame retardant materials, and particularly relates to a flame retardant for particleboard, a preparation method thereof and an application thereof. Background Art
[0002] Disclosing the information of this background art section is only intended to increase the understanding of the overall background of the present invention, and is not necessarily regarded as an admission or an implication in any form that this information constitutes the prior art already known to those of ordinary skill in the art.
[0003] Particleboard is a board made of wood or other lignocellulosic materials. It is prepared by applying an adhesive and pressing raw materials such as wood into a board shape under high temperature and high pressure, and has the characteristics of environmental protection, heat insulation, sound insulation, insulation, etc. At present, it is widely used in the fields of furniture, decoration and decoration, etc. The raw material of particleboard is wood with flammability, and there are great fire safety hazards during use. Therefore, it is of great significance to develop a particleboard with certain flame retardant properties.
[0004] Nitrogen-phosphorus flame retardants are the most commonly used flame retardants in the field of particleboard, but they have disadvantages such as poor thermal stability, easy precipitation during the drying process of particles, loss of flame retardant effect, poor compatibility with the matrix, and easy reduction of the mechanical properties of the board, which limit their application in particleboard. Boron-based flame retardants (such as zinc borate) form a glassy coating to isolate oxygen and heat when heated. Zinc borate is usually used in combination with other flame retardants to obtain excellent flame retardant and smoke suppression effects. For example, a flame retardant prepared by compounding zinc borate with melamine cyanurate, aluminum hydroxide and xylene phosphate, the synergistic effect of multiple flame retardants improves the flame retardant effect of the board, but the improvement effect of the mechanical properties of the board is not obvious (the elastic modulus is less than 3000 MPa, the static bending strength is less than 25 MPa, etc.). Therefore, it is of great significance to develop a flame retardant with certain flame retardant properties and improve the mechanical properties of the board. Summary of the Invention
[0005] In order to solve the deficiencies of the prior art, the purpose of the present invention is to provide a flame retardant for particleboard, a preparation method thereof and an application thereof. The flame retardant for particleboard provided by the present invention improves the flame retardant effect and greatly improves the mechanical properties of the particleboard through the compounding of boron-based flame retardants, melamine cyanurate (MCA) and nano-aluminum oxide.
[0006] In order to achieve the above purpose, the technical solution of the present invention is as follows:
[0007] In the first aspect of the present invention, there is provided a flame retardant for particleboard, which comprises, by weight: 1-5 parts of boron-based flame retardant, 1-5 parts of melamine cyanurate, and 0.5-1.5 parts of nano-aluminum oxide.
[0008] In some embodiments of the present invention, the boron-based flame retardant includes at least one of borax, boric acid, zinc borate, and borate.
[0009] The borate includes at least one of barium metaborate, ammonium fluoroborate, sodium metaborate, ammonium pentaborate, ammonium metaborate, and ammonium pentaborate.
[0010] In some embodiments of the present invention, the boron-based flame retardant is composed of borax and boric acid, and the mass ratio of borax to boric acid is (0.9 - 1.1):(0.9 - 1.1).
[0011] In some embodiments of the present invention, the flame retardant for particleboard, by weight, includes: 4 - 5 parts of boron-based flame retardant, 4 - 5 parts of melamine cyanurate, and 0.5 - 1.5 parts of nano-aluminum oxide.
[0012] In some embodiments of the present invention, the flame retardant for particleboard, by weight, includes: 4.5 parts of boron-based flame retardant, 4.5 parts of melamine cyanurate, and 45 parts of nano-aluminum oxide;
[0013] The boron-based flame retardant is obtained by mixing borax and boric acid in a mass ratio of (0.9 - 1.1):(0.9 - 1.1).
[0014] In some embodiments of the present invention, the flame retardant for particleboard further includes water.
[0015] In the second aspect of the present invention, there is provided a method for preparing the above-mentioned flame retardant for particleboard, which is obtained by mixing the boron-based flame retardant, melamine cyanurate, and nano-aluminum oxide in proportion.
[0016] In the third aspect of the present invention, there is provided an application of the above-mentioned flame retardant for particleboard in particleboard.
[0017] In the fourth aspect of the present invention, there is provided a particleboard, including particles and a flame retardant, and the flame retardant is the above-mentioned flame retardant for particleboard.
[0018] In some embodiments of the present invention, the dosage of the flame retardant for particleboard is 5 - 10% of the total mass of the particles.
[0019] In the fifth aspect of the present invention, there is provided a method for preparing the above-mentioned particleboard, including:
[0020] Preparing a melamine cyanurate emulsion and an aqueous nano-aluminum oxide solution respectively, adding the boron-based flame retardant to the melamine cyanurate emulsion, and then adding the aqueous nano-aluminum oxide solution, and mixing evenly to obtain a mixed solution;
[0021] Spray the mixed solution onto the wood chips, and then dry, size, orientedly lay, and hot-press the wood chips to obtain a particleboard.
[0022] In some embodiments of the present invention, when spraying the mixed solution onto the wood chips, the drug loading amount is 5-15 wt%.
[0023] In some embodiments of the present invention, the drying is to dry to a moisture content of 1-8%.
[0024] In some embodiments of the present invention, in the sizing, the sizing amount is 1-5%.
[0025] In some embodiments of the present invention, the orientedly laying is to perform three-layer longitudinal and transverse oriented laying on the sized wood chips, and the laying thickness ratio of the surface layer of the lower slab, the core layer of the slab, and the surface layer of the upper slab is 1-5:1-5:1-5, preferably 3:4:3.
[0026] In some embodiments of the present invention, the hot pressing is to first perform pre-pressing, and then perform staged hot pressing after raising the core layer temperature and the surface layer temperature.
[0027] In some embodiments of the present invention, the pre-pressing pressure is 1.5-2.0 N / mm 2 .
[0028] In some embodiments of the present invention, both the core layer temperature and the surface layer temperature are raised to 90-110 °C.
[0029] In some embodiments of the present invention, the staged hot pressing is to perform hot pressing treatments at pressures of 1.8-2.4 N / mm 2 , 1.0-1.5 N / mm 2 and 0.5-1.0 N / mm 2 respectively, and the hot pressing temperature is 170-250 °C.
[0030] The beneficial effects of the present invention are:
[0031] The present invention provides a flame retardant for particleboard, which is obtained by compounding a boron-based flame retardant, melamine cyanurate, and nano-aluminum oxide. For the flame retardant for particleboard provided by the present invention, the boron-based flame retardant, MCA, and nano-aluminum oxide cooperate synergistically, greatly improving the mechanical properties of the particleboard while enhancing the flame retardancy. Specifically, by controlling the dosages of the three, the synergistic complementarity of the flame retardant mechanism is achieved. MCA decomposes and releases non-combustible gases to dilute combustible gases, and the boron-based flame retardant and nano-aluminum oxide form a glassy or dense oxide layer on the material surface, blocking the transfer of heat and oxygen. When the three are used in combination, multi-dimensional flame retardancy of gas-phase flame retardancy and condensed-phase flame retardancy is achieved, greatly improving the flame retardant and smoke suppression effects. Moreover, the boron-based compound inhibits smoke generation, and nano-aluminum oxide enhances the strength of the carbon layer, reduces melt dripping, and improves safety. The synergistic effect among the three can reduce the dosages of each flame retardant, lower the cost, and mitigate the negative impact on the mechanical properties of the particleboard, and even offset the weakening of the mechanical properties of the particleboard by the flame retardant.
[0032] The flame retardant for particleboard provided by the present invention also has the advantages of low toxicity and environmental friendliness, and has a wide range of raw material sources and a simple preparation method, being suitable for industrial production.
[0033] The particleboard prepared by using the flame retardant for particleboard provided by the present invention has excellent mechanical properties and flame retardant and smoke suppression properties. The modulus of rupture can reach 85.69 MPa, the modulus of elasticity can reach 9739 MPa; the internal bond strength can reach 0.75 MPa, and the 24-hour water absorption thickness swelling rate is 11.4%, meeting the technical standards of oriented strand board (OSB / 2 type), and the combustion level reaches B1(C). Specific embodiments
[0034] Aiming at the problems existing in the flame retardants in the prior art, such as affecting the mechanical strength of the oriented structural board, the 24-hour water absorption thickness swelling rate, and being easily precipitated during the particle drying process, resulting in low flame retardant and smoke suppression properties of the board, the present invention provides a nitrogen-phosphorus-aluminum-based flame retardant, its preparation method and application.
[0035] In a first typical embodiment of the present invention, a flame retardant for particleboard is provided, which includes, by weight: 1-5 parts of a boron-based flame retardant, 1-5 parts of melamine cyanurate, and 0.5-1.5 parts of nano-aluminum oxide.
[0036] MCA decomposes and releases non-combustible gases to dilute combustible gases, and the boron-based flame retardant and nano-aluminum oxide form a glassy or dense oxide layer on the material surface, blocking the transfer of heat and oxygen. When the three are used in combination, multi-dimensional flame retardancy of gas-phase flame retardancy and condensed-phase flame retardancy is achieved, greatly improving the flame retardant and smoke suppression effects. Moreover, the boron-based compound inhibits smoke generation, and nano-aluminum oxide enhances the strength of the carbon layer, reduces melt dripping, and improves safety.
[0037] Moreover, the nano-effect of nano-aluminum oxide can improve the hardness and wear resistance of the particleboard, offset the weakening of the mechanical properties of the particleboard by other flame retardants, and improve the comprehensive performance of the particleboard.
[0038] The present invention has found through research that if the dosages of the boron-based flame retardant, melamine cyanurate, and nano-aluminum oxide are not within the above ranges, excellent flame retardant effects cannot be achieved, the improvement of the mechanical properties and flame retardant and smoke suppression properties of the particleboard cannot be realized, and the 24-hour water absorption thickness swelling rate cannot be reduced.
[0039] In some embodiments of this embodiment, the boron-based flame retardant includes at least one of borax, boric acid, zinc borate, and borate;
[0040] The borate includes but is not limited to at least one of barium metaborate, ammonium fluoroborate, sodium metaborate, ammonium pentaborate, ammonium metaborate, and ammonium pentaborate.
[0041] The boron-based flame retardants used in the present invention are all commonly used flame retardants in the field of flame retardants and can be obtained by purchase.
[0042] In some embodiments of this embodiment, the boron-based flame retardant is composed of borax and boric acid, and the mass ratio of borax to boric acid is (0.9-1.1):(0.9-1.1).
[0043] The present invention uses borax (Na2B4O7·10H2O) and boric acid (H3BO3) to form a boron-based flame retardant. Boric acid is weakly acidic and borax is weakly basic. After the two are compounded, they can adjust the pH value of the flame retardant system, reduce the interference of the flame retardant system on the curing process of the adhesive, and improve the bonding strength of the particleboard. Moreover, boric acid dehydrates to form a B2O3 glass layer at high temperature (condensed-phase flame retardancy), borax decomposes to produce Na2O and B2O3, further promoting the densification of the carbon layer, and at the same time releasing crystal water to absorb heat (gas-phase flame retardancy). At the same time, borax and boric acid have the functions of anti-corrosion and insect prevention for wood raw materials, and can extend the service life of the particleboard.
[0044] In some embodiments of this embodiment, the flame retardant for particleboard, by weight, includes: 4-5 parts of boron-based flame retardant, 4-5 parts of melamine cyanurate, and 0.5-1.5 parts of nano-aluminum oxide. Among them, the dosage of the boron-based flame retardant can be 4.0 parts, 4.1 parts, 4.2 parts, 4.3 parts, 4.4 parts, 4.5 parts, 4.6 parts, 4.7 parts, 4.8 parts, 4.9 parts, or 5.0 parts, etc., and the dosage of the melamine cyanurate can be 4.0 parts, 4.1 parts, 4.2 parts, 4.3 parts, 4.4 parts, 4.5 parts, 4.6 parts, 4.7 parts, 4.8 parts, 4.9 parts, or 5.0 parts, etc.
[0045] In some examples of this embodiment, the flame retardant for particleboard includes, by weight: 4.5 parts of boron flame retardant, 4.5 parts of melamine cyanurate, and 45 parts of nano-alumina;
[0046] The boron flame retardant is obtained by mixing borax and boric acid in a mass ratio of (0.9-1.1):(0.9-1.1).
[0047] A second typical embodiment of the present invention provides a method for preparing the flame retardant for particleboard, which is obtained by mixing a boron flame retardant, melamine cyanurate and nano-alumina in proportion.
[0048] A third typical embodiment of the present invention provides a use of the above-mentioned flame retardant for particle board in particle board.
[0049] The particleboard uses the flame retardant as a flame retardant to prepare the particleboard, which can increase the drug loading of large pieces of wood particles, reduce smoke release, and has good stability, and the flame retardant does not precipitate during the preparation process.
[0050] A fourth typical embodiment of the present invention provides a particle board, comprising particles and a flame retardant, wherein the flame retardant is the above-mentioned flame retardant for particle board.
[0051] In some examples of this embodiment, the amount of the flame retardant for particleboard is 5-10% of the total mass of the particles.
[0052] A fifth typical embodiment of the present invention provides a method for preparing the particleboard, comprising:
[0053] Prepare melamine cyanurate emulsion and nano-alumina aqueous solution respectively, add boron flame retardant to the melamine cyanurate emulsion, then add nano-alumina aqueous solution, mix well, and obtain a mixed solution;
[0054] The mixed solution is sprayed on wood chips, and then the wood chips are dried, glued, oriented and hot-pressed to obtain particleboard.
[0055] In some examples of this embodiment, the melamine cyanurate emulsion is an emulsion formed by mixing melamine cyanurate with water, and its concentration is 10-20wt%, specifically 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%, etc., preferably 14-16wt%.
[0056] The aqueous nano-aluminum oxide solution is obtained by adding nano-aluminum oxide into water, and its concentration is 10-30 wt%, specifically, it can be 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt% or 30 wt% etc., and preferably 18-22 wt%.
[0057] In some embodiments of this embodiment, the mixed solution is sprayed on the wood chips so that the drug loading amount is 5-15 wt%.
[0058] It should be noted that the term "drug loading amount" refers to the mass of the flame retardant for particleboard loaded on the wood chips. For example, the total mass of the wood chips is 100 g, and the drug loading amount is 10 wt%, that is, the mass of the flame retardant loaded on the wood chips is 10% of the total mass of the wood chips, that is, 10 g.
[0059] In some embodiments of this embodiment, the drying is carried out until the moisture content is 1-8%. Specifically, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7% or 8% etc., and preferably 3-5%.
[0060] It should be noted that the term "moisture content" refers to the ratio of the weight of the water contained in the wood chips per unit mass to the dry weight of the wood chips, expressed as a mass percentage. The moisture content is an important factor affecting the stability of particleboard. Too high or too low moisture content will affect the dimensional stability and mechanical properties of the board. The present invention limits the moisture content to 1-5%, and within this range, the dimensional stability and mechanical properties of the obtained particleboard can be guaranteed.
[0061] In some embodiments of this embodiment, in the sizing, the sizing amount is 1-5%, specifically, it can be 1%, 2%, 3%, 4% or 5% etc.
[0062] It should be noted that the term "adhesive application amount" refers to the percentage of the absolute dry mass of the adhesive added to the absolute dry mass of the wood chips during the process of mixing the wood chips with the adhesive. For example, when the adhesive application amount is 5%, it means that the absolute dry mass of the adhesive used is 5% of the absolute dry mass of the wood chips. In the production of particleboard, determining an appropriate adhesive application amount is the key to ensuring product quality and cost control. Excessive adhesive application amount will cause the glue to overflow, which not only affects the appearance quality of the oriented strand board, but may also lead to difficulties in subsequent processing; and excessive adhesive application may result in uneven distribution of the glue inside the board, causing a decline in certain physical properties of the particleboard (such as internal bond strength, water resistance, etc.), and also causing unevenness on the board surface during the pressing process. While too little adhesive application amount will lead to insufficient bonding strength of the board, a decline in the board quality, and may also affect the waterproof and moisture-proof properties of the board, resulting in it being prone to moisture absorption and deformation in a humid environment. The present invention defines the adhesive application amount as 1-5%, and the performance of the obtained oriented strand board is very excellent within this range.
[0063] The present invention does not make any requirements on the type of adhesive used in the adhesive application process, and adhesives commonly used in the art, such as MDI adhesive, can be selected.
[0064] In some embodiments of this embodiment, the oriented paving is to perform three-layer vertical and horizontal oriented paving on the glued wood chips, and the paving thickness ratio of the surface layer of the lower board blank, the core layer of the board blank, and the surface layer of the upper board blank is 1-5:1-5:1-5, preferably 3:4:3;
[0065] In some embodiments of this embodiment, the hot pressing is to first perform pre-pressing, and then perform staged hot pressing after raising the core layer temperature and the surface layer temperature.
[0066] In some embodiments of this embodiment, the pre-pressing pressure is 1.5-2.0 N / mm 2 , specifically it can be 1.5 N / mm 2 , 1.6 N / mm 2 , 1.7 N / mm 2 , 1.8 N / mm 2 , 1.9 N / mm 2 or 2.0 N / mm 2 etc. Through the pre-pressing treatment, the wood chips are initially bonded at room temperature to form a certain shape and density, so that it is easier to achieve an ideal forming effect during the hot pressing process in terms of thickness, reduce defects, improve the physical properties and appearance quality of the board; it can reduce the air content in the raw materials, and it is not easy to generate bubbles during the forming process, improve the quality of the oriented strand board, and is conducive to shortening the overall hot pressing cycle.
[0067] In some embodiments of this embodiment, both the core layer temperature and the surface layer temperature are increased to 90 - 110 °C, specifically, it can be 90 °C, 91 °C, 92 °C, 93 °C, 94 °C, 95 °C, 96 °C, 97 °C, 98 °C, 99 °C, 100 °C, 101 °C, 102 °C, 103 °C, 104 °C, 105 °C, 106 °C, 107 °C, 108 °C, 109 °C or 110 °C, etc., and preferably 95 - 105 °C.
[0068] To improve the hot pressing effect, the core layer temperature and the surface layer temperature need to be consistent. The present invention does not require the method for increasing the core layer temperature and the surface layer temperature, as long as the temperature can be increased to the set temperature. For example, a microwave preheating device can be used to increase the core layer temperature, and a hot steam preheating device can be used to increase the surface layer temperature.
[0069] In some embodiments of this embodiment, the staged hot pressing is carried out under pressures of 1.8 - 2.4 N / mm 2 , 1.0 - 1.5 N / mm 2 and 0.5 - 1.0 N / mm 2 respectively for hot pressing treatment, and the hot pressing temperature is 170 - 250 °C
[0070] Among them, for the three-stage hot pressing, the pressures in the high-pressure area, the medium-pressure area and the low-pressure area are preferably 2.0 N / mm 2 , 1.2 N / mm 2 and 0.8 N / mm 2 .
[0071] Among them, the hot pressing temperature is 170 - 250 °C. This temperature is a general temperature and can be selected according to the actual pressing plate temperature, such as 225 °C, 200 °C or 185.5 °C, etc.
[0072] In some embodiments of this embodiment, after the hot pressing is completed, the preparation method further includes processing steps such as cutting, cooling, board inspection and sanding, etc., and the particleboard is obtained after packaging.
[0073] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with specific embodiments.
[0074] For all the raw materials involved in the following examples and comparative examples, there is no special limitation on their sources, and they can all be purchased from the market or prepared by conventional technical means well-known to those skilled in the art.
[0075] Examples 1 - 7
[0076] A flame retardant for particleboard, in parts by mass, its raw material composition is shown in Table 1.
[0077] Comparative Examples 1 - 12
[0078] A flame retardant, by mass parts, its raw material composition is shown in Table 1.
[0079] Table 1 Formulations of the flame retardants in the examples and comparative examples
[0080]
[0081]
[0082] Comparative Example 13 - 21
[0083] A flame retardant, by mass parts, its raw material composition is shown in Table 2.
[0084] Table 2 Formulations of the flame retardants in Comparative Example 13 - 21
[0085]
[0086]
[0087] Experimental Example 1
[0088] A particleboard, its preparation method includes the following steps:
[0089] The raw material is fast-growing poplar (radiata pine), the adhesive used is MDI adhesive, the designed density of the board is 0.65 g / cm 3 、and the thickness is 9 mm of oriented strand board, the flame retardant for the particleboard prepared in Example 1 of the flame retardant.
[0090] First, mix melamine cyanurate in the flame retardant for the particleboard prepared in Example 1 with water to obtain an emulsion with a concentration of 15 wt%, add borax and boric acid to the emulsion; mix nano-aluminum oxide with water to obtain a solution with a concentration of 20 wt%. Mix the two solutions to obtain a mixed solution for standby.
[0091] Secondly, debark the poplar with a diameter of 20 - 40 cm on a debarking machine, and carry out ultra-large particle cutting by a veneer lathe. The particle size is 120 - 150 mm in length, 20 - 50 mm in width, and 0.3 - 0.6 mm in thickness.
[0092] The cut particles are transported to a rotary flame retardant adding device by a conveyor belt. The flame retardant (i.e., the mixed solution) is evenly sprayed on the surface of the particles through a high-pressure nozzle, and the addition amount is 8 wt%. Subsequently, it enters a drum-type drying cylinder for flue gas drying at 200 °C, and the moisture content of the dried flame-retardant particles is 3 - 5%.
[0093] The dried flame-retardant particles enter a drum-type glue mixer for sizing. The sizing amount of large particles is 3%, and 1 wt% of paraffin emulsion as a waterproofing agent is added.
[0094] The sized particles are laid in three layers with longitudinal and transverse orientation through three diamond roller laying heads, and the laying thickness ratio of the surface layer of the lower slab, the core layer of the slab, and the surface layer of the upper slab is 3:4:3.
[0095] The laid slab enters the pre-pressing stage, and the pre-pressing pressure is 1.7 N / mm 2 , and the pre-pressing time is 10 s - 30 s.
[0096] The pre-pressed slab enters the microwave preheating device, and after microwave preheating, the core layer temperature rises to 100 °C. After the core layer is preheated, the slab enters the hot steam preheating device, and after hot steam preheating, the surface layer temperature rises to 100 °C.
[0097] After hot steam preheating, the slab enters the hot pressing stage, and the pressures in the high-pressure zone, the medium-pressure zone, and the low-pressure zone are 2.0 N / mm 2 , 1.2 N / mm 2 and 0.8 N / mm 2 respectively; the platen temperatures in the press temperature control zones are 225 °C, 200 °C, and 185 °C respectively.
[0098] After the board is taken out, it is cut, cooled, inspected for the board, and sanded, and then packaged to obtain the oriented strand board.
[0099] Experimental Example 2 - 28
[0100] A particleboard, the difference in its preparation method from Experimental Example 1 is that the flame retardants are replaced with the flame retardants provided in Examples 2 - 7 and Comparative Examples 1 - 21 respectively, and the remaining steps are exactly the same as those in Experimental Example 1.
[0101] The physical properties (GB / T 41715 - 2022) and flame retardant properties (GB / T 2406.2 - 2009, GB / T 20284 - 2006, GB / T 8626 - 2007) of the oriented strand boards obtained in Experimental Examples 1 - 28 are shown in Tables 3 and 4 for the test results.
[0102] Table 3 Physical properties of the oriented strand boards obtained in the experimental examples
[0103]
[0104] Table 4 Flame retardant properties of the oriented strand boards obtained in the experimental examples
[0105] Experimental Example Oxygen Index (%) Experimental Example Oxygen Index (%) 1 44.5 15 37.5 2 42.5 16 38.1 3 42.9 17 37.5 4 42.5 18 32.5 5 42.9 19 33.9 6 42.9 20 31.9 7 42.9 21 21.6 8 39.9 22 39.5 9 39.5 23 38.1 10 38.1 24 37.5 11 36.7 25 37.9 12 36.1 26 38.1 13 35.9 27 37.5 14 36.5 28 36.9
[0106] As can be seen from Tables 3 and 4, the final density of the oriented strand board prepared in Example 1 of the present invention is 0.66 g / cm 3, its modulus of rupture is 96.8 MPa, modulus of elasticity is 10071 MPa, internal bond strength is 1.15 MPa, and the thickness swelling rate after 24-hour water absorption is 10.8%, meeting the technical standards of oriented strand board (OSB / 2 type), and its combustion rating reaches B1 (C).
[0107] It can be seen from the data comparison of Experimental Example 1 and Experimental Examples 8, 9, 10, and 11 that the nitrogen-phosphorus-aluminum-based flame retardant obtained by compounding the boron-based flame retardant, melamine cyanurate, and nano-aluminum oxide provided by the present invention can synergistically improve the flame retardant effect only under specific ratios, and reduce the influence of the addition of the nitrogen-phosphorus-based flame retardant on the mechanical properties of the board.
[0108] It can be seen from the data comparison of Experimental Example 1 and Experimental Examples 12 - 29 that the boron-based flame retardant, melamine cyanurate, and nano-aluminum oxide adopted by the present invention have a synergistic effect in improving the flame retardant and smoke suppression performance of the board and improving the mechanical properties of the board.
[0109] The above are only the preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention can have various changes and modifications. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included within the protection scope of the present invention.
Claims
1. A flame retardant for particleboard, characterized in that, By weight parts, it includes: 1-5 parts of boron-based flame retardant, 1-5 parts of melamine cyanurate, and 0.5-1.5 parts of nano-aluminum oxide.
2. The flame retardant for particleboard according to claim 1, wherein The boron-based flame retardant includes at least one of borax, boric acid, zinc borate, and borate. The borate includes at least one of barium metaborate, ammonium fluoroborate, sodium metaborate, ammonium pentaborate, ammonium metaborate, and ammonium pentaborate.
3. The flame retardant for particleboard according to claim 2, wherein, The boron-based flame retardant is composed of borax and boric acid, and the mass ratio of borax to boric acid is (0.9-1.1):(0.9-1.1).
4. The flame retardant for particle board according to claim 1, characterized in that, The flame retardant for particleboard, by weight parts, includes: 4-5 parts of boron-based flame retardant, 4-5 parts of melamine cyanurate, and 0.5-1.5 parts of nano-aluminum oxide.
5. The flame retardant for particle board according to claim 1, characterized in that, The flame retardant for particleboard, by weight parts, includes: 4.5 parts of boron-based flame retardant, 4.5 parts of melamine cyanurate, and 45 parts of nano-aluminum oxide; The boron-based flame retardant is obtained by mixing borax and boric acid in a mass ratio of (0.9-1.1):(0.9-1.1).
6. The flame retardant for particleboard according to any one of claims 1-5, characterized in that, It also includes water.
7. A preparation method of the flame retardant for particleboard according to claim 1, characterized in that, Mix the boron-based flame retardant, melamine cyanurate, and nano-aluminum oxide in proportion and remember.
8. Application of the flame retardant for particleboard according to any one of claims 1-6 in particleboard.
9. A particleboard, characterized in that, It includes particles and a flame retardant, and the flame retardant is the flame retardant for particleboard according to any one of claims 1-6; Preferably, the dosage of the flame retardant for particleboard is 5-10% of the total mass of the particles.
10. A method for preparing the particle board according to claim 9, characterized in that, It includes: Prepare a melamine cyanurate emulsion and a nano-aluminum oxide aqueous solution respectively. After adding the boron-based flame retardant to the melamine cyanurate emulsion, then add the nano-aluminum oxide aqueous solution and mix evenly to obtain a mixed solution; Spray the mixed solution onto the particles, and then dry, size, orientedly lay, and hot press the particles to obtain a particleboard; Preferably, spray the mixed solution onto the particles so that the drug loading amount is 5-15 wt%. Preferably, the drying is to dry to a moisture content of 1-8%. Preferably, in the sizing, the sizing amount is 1-5%. Preferably, the oriented laying is to perform three-layer longitudinal and transverse oriented laying on the sized particles, and the laying thickness ratio of the lower board blank surface layer, the board blank core layer, and the upper board blank surface layer is 1-5:1-5:1-5, preferably 3:4:3; Preferably, the hot pressing is to first perform pre-pressing, and then perform staged hot pressing after raising the core layer temperature and the surface layer temperature; Preferably, the preloading pressure is 1.5 - 2.0 N / mm 2 ; Preferably, both the core layer temperature and the surface layer temperature are raised to 90-110 °C; Preferably, the staged hot pressing is carried out under pressures of 1.8 - 2.4 N / mm 2 , 1.0 - 1.5 N / mm 2 and 0.5 - 1.0 N / mm 2 respectively, and the hot pressing temperature is 170 - 250 °C.