Intelligent preparation method of high-strength high-toughness corrosion-resistant green aluminum frame
Through the design of microalloy compositions and the full-process automation process, the problems of low reuse rate of recycled aluminum, high energy consumption, large carbon emissions and high surface scratches are solved, and the preparation of high-strength, high toughness, corrosion-resistant green aluminum frames is realized, which improves production efficiency and performance stability.
Patent Information
- Application Number
- CN202510697064.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-28
- Publication Date
- 2025-07-29
AI Technical Summary
In the prior art, the recycled aluminum has low reuse rate, high energy consumption, large carbon emissions, high surface scratch rate and unstable mechanical properties, and the traditional process flow is discontinuous, resulting in low production efficiency.
The microalloy composition design and full-process automation process are adopted, including controlling alloy composition, homogenization treatment, extrusion treatment, aging treatment and oxidation closed-loop treatment. The impurity phase is suppressed through Cr-Ti microalloyation, and the Fe tolerance is improved, and intelligent equipment is used for parameter control and automated operations.
The reuse rate of recycled aluminum is improved to more than 60%, energy consumption is reduced by 24.4%, carbon emissions are reduced by 30%, surface defect rate is reduced to 0.8%, mechanical performance pass rate is improved to 97%, and production cycle is shortened by 30%.
Smart Images

Figure CN120384212A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for the intelligent preparation of high-strength, high-toughness, corrosion-resistant and green aluminum frames, belonging to the technical field of alloy material preparation. Background Art
[0002] In the current market, the recycling of recycled aluminum faces double constraints of composition and process. The global photovoltaic modules are about to enter a peak retirement period. Data from the China Photovoltaic Industry Association shows that after 2030, the waste volume of photovoltaic modules in China will reach 14 million tons, of which the proportion of aluminum alloy frames is about 20% (about 280,000 tons / year). The traditional 6005 alloy frame strictly restricts the impurity content (Fe≤0.15%, Cr≤0.1%), but the median content of Cr, Mn, and Zn in building profiles and waste frame scraps reaches 0.18%, 0.25%, and 0.22% respectively, all exceeding the standard;
[0003] Cr and Mn are prone to form coarse compounds, significantly reducing the formability and corrosion resistance of the alloy; excessive Zn greatly increases the risk of stress corrosion. The combined action of these impurity elements with Fe and Cu results in the recycling rate of recycled aluminum in the 6005 alloy system being less than 35%. A large amount of waste is forced to be downgraded. In addition, the energy consumption of the traditional melting and casting process is as high as 1200 kWh / ton, about 30% higher than the international advanced level; the melting loss rate of recycled aluminum is ≥8%. The large use of primary aluminum ingots leads to a carbon emission intensity far exceeding the international average level;
[0004] The traditional "extrusion - framing - aging - oxidation" process has three major defects: a large amount of manual intervention: the surface scratch rate of the profiles reaches 5% - 8% due to framing and transportation, the floor area of the material frame is large and the utilization rate of the aging furnace is less than 60%; rough parameter control: the aging temperature deviation is ±10°C, the size uniformity of the precipitated phase is poor, the dispersion of the salt spray corrosion resistance duration reaches ±200 hours, and the qualified rate of the mechanical properties of the finished product is only 88%; the process is not continuous: the extrusion and oxidation links are separated, the interval time is long, the production is not compact and continuous, affecting the production efficiency;
[0005] Technical Bottlenecks:
[0006] Low recycling rate of recycled aluminum: Impurity elements result in a recycling rate of recycled aluminum in the traditional process of less than 35%, and a large amount of waste is downgraded; high energy consumption and carbon emissions: The energy consumption of the traditional melting and casting process is 1200 kWh / ton (30% higher than the international advanced level), and the melting loss rate is ≥8%; defects of manual intervention: the surface scratch rate of the traditional process is 5% - 8%, the utilization rate of the aging furnace is less than 60%, and the qualified rate of the mechanical properties is only 88%. Breakthrough points of the present invention: By Cr - Ti microalloying to inhibit impurity phases, the Fe tolerance is increased to 0.25%, and the recycling rate of recycled aluminum breaks through 60%; full-process automation makes the parameter fluctuation ≤±2%, and the surface defect rate is reduced to 0.8%. Summary of the Invention
[0007] The technical problem to be solved by the present invention is to overcome the defects of the existing technology and, in response to the dual needs of high-value utilization of recycled aluminum in the non-ferrous metal industry and high-end photovoltaic equipment, provide an intelligent preparation method for high-strength, high-toughness, corrosion-resistant green aluminum frame, which can improve the mechanical properties stability of aluminum alloy and increase the yield of finished products.
[0008] In order to solve the above technical problems, the technical solution of the present invention is: an intelligent preparation method of a high-strength, high-toughness, corrosion-resistant green aluminum frame, comprising the following steps:
[0009] S1. Melting and casting: According to the mass percentage, the alloy composition is controlled as follows: Si: 0.70%-0.80%, Fe: less than 0.25%, Cu: less than 0.15%, Mn: less than 0.15%, Mg: 0.60%-0.70%, Cr: less than 0.15%, Ti: 0.02%-0.06%, Zn: less than 0.05%, and the balance is Al;
[0010] After mixing and melting the above materials, casting into round ingots;
[0011] S2. Homogenization treatment: Place the round ingot in a multi-stage homogenization furnace, heat it to 300°C at 5°C / min, keep it at 560±10°C for 8 hours, eliminate segregation by pre-cooling and air cooling, and then return it to room temperature;
[0012] S3. Extrusion treatment: The homogeneous ingot is extruded into aluminum material in an extrusion furnace (the upper machine temperature is 460-480℃, and the extrusion speed is ≥15m / min);
[0013] S4, sand blasting: sand particle size 50-80μm, pressure 0.3-0.5MPa;
[0014] S5, automatic loading: the positioning accuracy of the robotic arm is ±0.5mm, realizing contactless loading;
[0015] S6. Aging treatment: In a tunnel-type continuous aging furnace, pass through a 190±2℃ zone at a speed of 3-5m / min and keep warm for 240-270min;
[0016] S7, closed-loop oxidation treatment: an 8-28 μm oxide film is formed in the automatic oxidation tank (voltage 18-22 V, temperature 20 ± 1 ° C).
[0017] Furthermore, Si is preferably 0.76%, Mg is preferably 0.67%, and Ti is preferably 0.04%. Cr and Fe form a FeCrAl composite phase, the solidification range is 720-680°C, and the intergranular corrosion current density is reduced by 42%.
[0018] Furthermore, the hydrogen content of the aluminum liquid after smelting is controlled to H2≤0.17cm 3 / 100g, the control accuracy of argon flow rate is ±0.1 L / min, and the error of hydrogen content predicted by AI algorithm is ≤ ±0.02 cm 3 / 100g.
[0019] Furthermore, the aging furnace adopts a far-infrared temperature control module and a PID algorithm, the standard deviation of furnace temperature is ≤ 2°C, and the response time is ≤ 10 seconds / °C.
[0020] After adopting the above technical solutions, the present invention has the following beneficial effects:
[0021] 1. In the present invention, the microalloying composition system: the main strengthening phase: Mg / Si ≈ 1:1 (Si 0.73% - 0.78%, Mg 0.65% - 0.70%), forming a uniform Mg2Si strengthening phase, and the yield strength is increased to 288 MPa (traditional 265 MPa, +8.7%);
[0022] Impurity compatibility technology: Fe ≤ 0.25% (traditional ≤ 0.15%), adding 0.05% Cr to form an orthorhombic FeCrAl composite phase (lattice constant a = 0.882 nm, and the intergranular corrosion current density is reduced by 42%), and adding 0.04% Ti to refine the grain size to ≤ 20 μm (traditional 50 μm).
[0023] 2. In the present invention, intelligent process control:
[0024] Melting stage: The AI algorithm is linked with a hydrogen detector (sampling frequency ≥ 50 Hz), the control accuracy of argon flow rate is ±0.1 L / min, and the hydrogen content is controlled to 0.17 cm 3 / 100g (industry standard 0.2 cm 3 / 100g);
[0025] Aging stage: The tunnel-type continuous aging furnace is equipped with 12 groups of far-infrared temperature control modules, which compensate the temperature in real time based on the PID algorithm, the standard deviation in the furnace is ≤ 2°C, and the uniformity of the precipitated phase is increased by 35%.
[0026] 3. In the present invention, the green manufacturing process, the recycling rate of recycled aluminum is ≥ 60%, the unit energy consumption is reduced to 1020 kWh / ton (a reduction of 24.4%), and the carbon emission is only 1 / 8 of that of primary aluminum. Brief Description of the Drawings
[0027] Figure 1 It is a table of the preferred values of the alloy composition for an intelligent preparation method of a high-strength, high-toughness, corrosion-resistant green aluminum frame according to the present invention;
[0028] Figure 2 It is a table of the extrusion process parameters for an intelligent preparation method of a high-strength, high-toughness, corrosion-resistant green aluminum frame according to the present invention. Detailed Description of the Invention
[0029] In order to make the contents of the present invention more clearly understood, the present invention is further described in detail below based on specific embodiments in conjunction with the accompanying drawings.
[0030] like Figure 1-2 As shown, a method for intelligently preparing a high-strength, high-toughness, and corrosion-resistant green aluminum frame includes the following steps:
[0031] S1. Melting and casting: According to the mass percentage, the alloy composition is controlled as follows: Si: 0.70%-0.80%, Fe: less than 0.25%, Cu: less than 0.15%, Mn: less than 0.15%, Mg: 0.60%-0.70%, Cr: less than 0.15%, Ti: 0.02%-0.06%, Zn: less than 0.05%, and the balance is Al;
[0032] After mixing and melting the above materials, casting into round ingots;
[0033] S2. Homogenization treatment: Place the round ingot in a multi-stage homogenization furnace, heat it to 300°C at 5°C / min, keep it at 560±10°C for 8 hours, eliminate segregation by pre-cooling and air cooling, and then return it to room temperature;
[0034] S3. Extrusion treatment: The homogeneous ingot is extruded into aluminum material in an extrusion furnace (the upper machine temperature is 460-480℃, and the extrusion speed is ≥15m / min);
[0035] S4, sand blasting: sand particle size 50-80μm, pressure 0.3-0.5MPa;
[0036] S5, automatic loading: the positioning accuracy of the robotic arm is ±0.5mm, realizing contactless loading;
[0037] S6. Aging treatment: In a tunnel-type continuous aging furnace, pass through a 190±2℃ zone at a speed of 3-5m / min and keep warm for 240-270min;
[0038] S7, closed-loop oxidation treatment: an 8-28 μm oxide film is formed in the automatic oxidation tank (voltage 18-22 V, temperature 20 ± 1 ° C).
[0039] In this embodiment, the main strengthening phase is: Si 0.73%-0.78%, Mg 0.65%-0.70% (Mg / Si is strictly controlled to be approximately equal to 1:1 to form a uniformly distributed Mg2Si strengthening phase);
[0040] Impurity Compatibility System: Fe ≤ 0.25% (breaking through the traditional internal control limit of 0.15%), Cu ≤ 0.15%, by adding 0.05% Cr (forming FeCrAl composite phase, the intergranular corrosion tendency is reduced by 40%) and 0.02% - 0.06% Ti (the grain size is refined from 50μm to 20μm, and the grain boundary strength is increased by 25%);
[0041] Raw Material Ratio: The recycling rate of waste frame materials ≥ 60%, combined with Al-Ti master alloy (the comprehensive performance is optimal when Ti = 0.04%), realizing the high-quality utilization of recycled aluminum resources.
[0042] Specifically, Si is preferably 0.76%, Mg is preferably 0.67%, Ti is preferably 0.04%, Cr forms FeCrAl composite phase with Fe, the solidification range is 720 - 680°C, and the intergranular corrosion current density is reduced by 42%.
[0043] Specifically, the hydrogen content in the molten aluminum after melting is controlled to be H2 ≤ 0.17cm 3 / 100g, the control accuracy of argon flow rate is ±0.1L / min, and the error of hydrogen content predicted by AI algorithm is ≤ ±0.02cm 3 / 100g.
[0044] Specifically, the aging furnace adopts a far-infrared temperature control module and PID algorithm, the standard deviation of furnace temperature ≤ 2°C, and the response time ≤ 10 seconds / °C.
[0045] In this embodiment, a 2000-ton extruder is equipped with a 4-hole die, the extrusion speed is 15 - 20m / min, and the temperature is measured in real time by an infrared thermometer (measurement accuracy ±1 degree Celsius, sampling frequency 200Hz), and the optimal extrusion temperature and speed ratio are adjusted in real time to ensure the collaborative accuracy of profile shape and dimensional accuracy of ±0.1mm;
[0046] In this embodiment, a "rotary degassing in furnace + dual-rotor on-line degassing" combined device is adopted, and through the AI neural network algorithm, it is linked with a ZR-2000 hydrogen detector (measurement accuracy ±0.01cm 3 / 100g), and the argon flow rate is adjusted in real time (control accuracy ±0.1L / min) to ensure that the hydrogen content in the melt ≤ 0.17cm 3 / 100g (lower than the industry standard of 0.2cm 3 / 100g);
[0047] Melt Purification: Double-stage ceramic filtration (10μm + 5μm) in series with deep bed filtration, the slag removal rate ≥ 99%, and the cleanliness of the filtered melt reaches ISO 4406:1999 grade 16 / 14 / 12.
[0048] In this embodiment, through the microalloying composition design of elements such as copper, chromium, manganese, and zinc (the Fe tolerance is increased to 0.25%, the recycled aluminum reuse rate is ≥60%, and the Cr / Ti composite inhibits impurity phases) and the innovation of the full-process automation process (parameter fluctuation ≤±2%), the limitations of traditional 6005 alloy are broken through. Technical achievements: Performance breakthrough: yield strength ≥280 MPa, salt spray corrosion resistance ≥1000 hours, grain refinement to 20 μm, and the intergranular corrosion tendency is reduced by 40%; Green manufacturing: unit energy consumption is reduced by 15%, carbon emissions are reduced by 30%, and high-value recycling of recycled aluminum is achieved; Intelligent production: the finished product qualification rate is increased from 88% to 97%, the production cycle is shortened by 30%, and the surface defect rate ≤1%. This technology provides a "low-carbon + intelligent" solution for the recycling of photovoltaic retired components and high-end aluminum alloy manufacturing, leading the technological upgrade of the industry.
[0049] In the above specific embodiments, the technical problems solved, technical solutions, and beneficial effects of the present invention have been further described in detail. It should be understood that the above are only specific embodiments of the present invention and are not used to limit the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An intelligent preparation method for a high-strength, high-toughness, corrosion-resistant and green aluminum frame, characterized in that, The following steps are involved: S1. Melting and casting: According to the mass percentage, the alloy composition is controlled as follows: Si: 0.70%-0.80%, Fe: less than 0.25%, Cu: less than 0.15%, Mn: less than 0.15%, Mg: 0.60%-0.70%, Cr: less than 0.15%, Ti: 0.02%-0.06%, Zn: less than 0.05%, and the balance is Al; After mixing and melting the above materials, casting into round ingots; S2. Homogenization treatment: Place the round ingot in a multi-stage homogenization furnace, heat it to 300°C at 5°C / min, keep it at 560±10°C for 8 hours, eliminate segregation by pre-cooling and air cooling, and then return it to room temperature; S3. Extrusion treatment: The homogeneous ingot is extruded into aluminum material in an extrusion furnace (the upper machine temperature is 460-480℃, and the extrusion speed is ≥15m / min); S4, sand blasting: sand particle size 50-80μm, pressure 0.3-0.5MPa; S5, automatic loading: the positioning accuracy of the robotic arm is ±0.5mm, realizing contactless loading; S6. Aging treatment: In a tunnel-type continuous aging furnace, pass through a 190±2℃ zone at a speed of 3-5m / min and keep warm for 240-270min; S7, closed-loop oxidation treatment: an 8-28μm oxide film is formed in the automatic oxidation tank (voltage 18-22V, temperature 20±1℃).
2. The intelligent preparation method of a high-strength, high-toughness, corrosion-resistant green aluminum frame according to claim 1 is characterized by: The preferred content of Si is 0.76%, the preferred content of Mg is 0.67%, and the preferred content of Ti is 0.04%. Cr and Fe form a FeCrAl composite phase. The solidification range is 720-680°C, and the intergranular corrosion current density is reduced by 42%.
3. The intelligent preparation method of a high-strength, high-toughness, corrosion-resistant green aluminum frame according to claim 1 is characterized by: After smelting, the hydrogen content of the aluminum liquid is controlled to H2≤0.17 cm³ / 100g, the argon flow control accuracy is ±0.1L / min, and the AI algorithm predicts the hydrogen content error ≤±0.02cm³ / 100g.
4. The intelligent preparation method of a high-strength, high-toughness, corrosion-resistant green aluminum frame according to claim 1 is characterized by: The aging furnace uses a far-infrared temperature control module and PID algorithm, with a furnace temperature standard deviation of ≤2°C and a response time of ≤10 seconds / °C.
Citation Information
Cited By
Recycled aluminum alloy profile precision extrusion process based on stepped temperature control melt rheological characteristics
CN122252478A