Multi-functional group synergistic reverse osmosis membrane and preparation method thereof

By introducing sulfonic acid groups and sulfite groups into the reverse osmosis membrane, utilizing aqueous phase additives and surface chemical reactions, a multi-functional group synergistic reverse osmosis membrane is constructed, which solves the trade-off problem between water permeability and desalination rate of traditional reverse osmosis membranes and achieves the effects of high water permeability flux and high desalination rate.

CN120618272APending Publication Date: 2025-09-12SHANDONG JINYU MEMBRANE TECH DEV CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202511001824.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-21
Publication Date
2025-09-12

AI Technical Summary

Technical Problem

There is a trade-off between the water permeability and desalination rate of existing reverse osmosis membranes, making it difficult to increase them simultaneously.

Method used

By introducing sulfonic acid groups and sulfite groups, utilizing aqueous phase additives and surface chemical reactions, a multi-functional group synergistic reverse osmosis membrane is constructed to increase water transfer channels, improve hydrophilicity, and enhance the cross-linking degree of the polyamide network through diazo coupling reaction.

Benefits of technology

It significantly improves the water permeation flux and desalination rate of the reverse osmosis membrane, solves the flux-desalination rate trade-off contradiction of traditional reverse osmosis membranes, and achieves efficient water molecule transfer and ion retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120618272A_ABST
    Figure CN120618272A_ABST
Patent Text Reader

Abstract

The invention discloses a polyfunctional group synergistic reverse osmosis membrane and a preparation method thereof, and relates to the technical field of new materials and membrane separation. The polysulfone porous base membrane is sequentially soaked in a water phase monomer solution and an oil phase monomer solution, the polyamide reverse osmosis membrane is prepared through interfacial polymerization, sulfonic acid groups are introduced in the process, and water transfer channels are increased; soaking in an aminobenzene sulfonic acid aqueous solution, and introducing a benzenesulfonic acid group to improve the hydrophilicity of the reverse osmosis membrane; then treating with a sodium nitrite aqueous solution, and carrying out diazotization coupling reaction on the surface, so as to improve the crosslinking degree of the polyamide separation functional layer. The reverse osmosis membrane is cleaned by using a sodium sulfite aqueous solution, and an unreacted diazo group is replaced by a sulfurous acid group, so that the surface stability of the reverse osmosis membrane is improved. The preparation method provided by the invention is easy to control and simple in process, and the reverse osmosis membrane obtained by the preparation method has a synergistic effect of polyfunctional groups, so that the desalination rate and the water permeation flux of the reverse osmosis membrane are both improved, and the reverse osmosis membrane can be applied to the fields of purified water preparation, industrial sewage and wastewater deep treatment, seawater desalination and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new materials and membrane separation, and in particular to a multi-functional group synergistic reverse osmosis membrane and a preparation method thereof. Background Art

[0002] With the rapid development of modern society, the demand for water resources is increasing, and water shortage has become a major challenge facing the world. Membrane water treatment technologies, including microfiltration, ultrafiltration, nanofiltration, and reverse osmosis, are widely used due to their advantages such as simple operation, low operating costs, and strong separation capabilities. Microfiltration and ultrafiltration can remove suspended matter and large molecules from water, while nanofiltration can remove divalent ions and organic matter with a molecular weight greater than 200. Reverse osmosis membranes are the most delicate water treatment membranes, allowing only water molecules to pass through and almost completely intercepting inorganic salts in the water. Reverse osmosis membranes are used to produce pure water from surface water, purify, desalinate, and recycle industrial wastewater and sewage, and desalinate seawater to produce water for civil and industrial use.

[0003] Reverse osmosis is a pressure-driven membrane separation process. When the pressure applied to the feed solution exceeds the osmotic pressure of the solution, the solvent water passes through the reverse osmosis membrane in the opposite direction of natural osmosis, resulting in pure water on the low-pressure side. Since the 1960s, research has been underway on reverse osmosis membranes with ultrathin separation layers, with polyamide reverse osmosis membranes emerging as the highest-performing membrane material. Reverse osmosis membranes consist of a separation layer, typically an aromatic polyamide, and a porous support layer, a non-woven fabric-coated polysulfone ultrafiltration membrane. Polyamide reverse osmosis membrane sheets are rolled into various reverse osmosis membrane modules and are widely used in a wide range of applications, including industrial wastewater treatment, brackish water desalination, and high-purity water production.

[0004] There are many explanations for the mass transfer mechanism of reverse osmosis membranes, mainly the preferential adsorption-capillary flow mechanism and the solute diffusion model. The preferential adsorption-capillary flow theory originates from the Gibbs adsorption equation and states that when the feed liquid contacts the reverse osmosis membrane, the membrane surface has the property of adsorbing water molecules and repelling salt ions. Pure water adsorbed on the membrane surface preferentially permeates, achieving desalination. The solute-diffusion model is the most widely accepted description of the transport mechanism of water and salt in reverse osmosis membranes. The active layer of the reverse osmosis membrane is a "dense" polymer phase in which water molecules "dissolve" into the membrane and then diffuse through the membrane along its concentration gradient. The permeability of water depends on the "solubility" of water molecules within the membrane and the diffusivity of water molecules within the membrane.

[0005] Interfacial polymerization is the most widely used process for preparing reverse osmosis membranes for industrial large-scale production. During interfacial polymerization, the immiscible oil and water phases dissolve aqueous phase monomers and oil phase monomers, respectively. A restricted monomer diffusion and reaction interface layer is formed at the oil-water liquid-liquid interface, and the two-phase monomers polymerize on the surface of the support to form a polyamide separation functional layer. Interfacial polymerization is simple to operate and easy to produce on an industrial large scale, but various factors during the preparation process can affect the morphological structure, pore size, porosity, surface roughness, and surface chemical properties of the reverse osmosis membrane. Therefore, the polyamide reverse osmosis membranes produced using this method typically have a thicker separation layer and greater transmembrane resistance for water molecules, resulting in lower water permeability and lower salt rejection rates.

[0006] To develop high-performance reverse osmosis (RO) membranes, researchers are focusing on modifying the intrinsic structure of the polyamide separation layer, attempting to further enhance the membrane's water permeation flux while maintaining high desalination performance. The permeation flux of RO membranes is closely related to the surface morphology, thickness, hydrophilicity, surface charge, and water content of the separation layer. The higher the hydrophilicity and surface area of ​​the RO membrane separation layer, the smaller the bulk thickness, and the lower the transmembrane resistance of water molecules, leading to higher water permeation. Therefore, researchers have designed and manipulated the RO membrane's separation layer from multiple perspectives. By reducing the thickness of the separation layer, increasing the degree of wrinkling, manipulating the pore size distribution, adding additional water channels, and forming a loose pore structure, they have achieved not only high retention performance but also high water permeation performance by overcoming the trade-off effect of traditional polyamide membranes. The implementation of a single strategy has limited impact on RO membrane performance. However, the synergistic application of two or more strategies in the construction and regulation of the functional separation layer is expected to further enhance RO membrane performance. Summary of the Invention

[0007] The present invention aims to provide a multi-functional synergistic reverse osmosis membrane and a preparation method thereof. By using aqueous phase additives and surface chemical reaction methods, the performance of the reverse osmosis membrane is improved through the synergy of multiple functional groups. The preparation method introduces sulfonic acid groups into the main body of the reverse osmosis membrane separation functional layer to provide more water transfer channels. Benzenesulfonic acid groups and sulfite groups are introduced onto the surface of the reverse osmosis membrane to improve the hydrophilicity of the reverse osmosis membrane. Furthermore, the salt rejection rate of the reverse osmosis membrane is improved through a diazotization coupling reaction. The multifunctional synergistic reverse osmosis membrane has a high salt rejection rate and a high water permeation flux, and can be used in the fields of pure water preparation, deep treatment of industrial sewage and wastewater, and seawater desalination.

[0008] Based on the above purpose, the present invention discloses a method for preparing a multi-functional group synergistic reverse osmosis membrane, comprising the following steps:

[0009] Step (1) Preparation of aqueous and oily phase monomer solutions: preparing an aqueous phase monomer solution containing m-phenylenediamine and diaminobenzenesulfonic acid as an aqueous phase additive, and preparing an oily phase monomer solution of trimesoyl chloride;

[0010] Step (2) interfacial polymerization membrane formation: soaking the polysulfone porous base membrane in the aqueous monomer solution and the oily monomer solution in sequence to generate a polyamide separation functional layer, and heat-treating the polyamide to increase the cross-linking degree to prepare a nascent reverse osmosis membrane; diaminobenzenesulfonic acid participates in the interfacial polymerization reaction to introduce sulfonate groups, thereby increasing the water transfer channels of the polyamide separation functional layer;

[0011] Step (3) hydrophilic surface modification of the nascent reverse osmosis membrane: soaking the nascent reverse osmosis membrane in an aqueous solution of aminobenzenesulfonic acid, causing a surface chemical reaction between the acyl chloride groups remaining on the membrane surface and the amino groups of aminobenzenesulfonic acid, thereby introducing benzenesulfonic acid groups and improving the hydrophilicity of the reverse osmosis membrane;

[0012] Step (4) diazo optimization treatment: soaking the primary reverse osmosis membrane treated in step (3) in a low-concentration sodium nitrite aqueous solution to cause a diazo coupling reaction, thereby improving the desalination rate of the reverse osmosis membrane; using a high-concentration sodium sulfite aqueous solution to clean the reverse osmosis membrane, allowing the sulfite group to replace the residual diazo group, thereby improving the stability and hydrophilicity of the reverse osmosis membrane surface; obtaining a multi-functional group-coordinated reverse osmosis membrane, and then soaking it in a protective liquid and heat-treating it to obtain a dry reverse osmosis membrane.

[0013] Preferably, in step (1), the mass fraction concentration of phenylenediamine in the aqueous monomer solution is 1-5%, the aqueous phase additive is diaminobenzenesulfonic acid, and the mass fraction concentration is 0.1-1%; camphorsulfonic acid and triethylamine buffer solution are used to adjust the pH value of the aqueous monomer solution to 9-10.

[0014] Preferably, the solvent of the oil phase monomer solution in step (1) is any one of n-hexane, n-heptane, and isoparaffin; and the mass fraction concentration of trimesoyl chloride in the oil phase monomer solution is 0.1-0.5%.

[0015] Preferably, the preparation of the polysulfone porous base membrane in step (2) comprises the following steps:

[0016] a. dissolving polysulfone in a dimethylformamide solution, wherein the mass fraction concentration of polysulfone in the solution is 18%, and preparing a polysulfone casting solution after the polysulfone is completely dissolved and degassed;

[0017] b. Coat the polysulfone casting solution on the non-woven fabric to convert it into a polysulfone porous base membrane.

[0018] Preferably, in step (2), the polysulfone porous base membrane is immersed in the aqueous monomer solution for 1-10 minutes, and immersed in the oily monomer solution for 1-10 minutes;

[0019] The heat treatment temperature is 50-90° C., and the heat treatment time is 1-10 minutes to obtain a nascent reverse osmosis membrane.

[0020] Preferably, in step (3), the mass fraction concentration of aminobenzenesulfonic acid in the aminobenzenesulfonic acid aqueous solution is 1-5%, and the soaking time is 5-10 minutes.

[0021] Preferably, the mass fraction concentration of sodium nitrite in the sodium nitrite aqueous solution in step (4) is 0.1-1%, and the pH value of the sodium nitrite aqueous solution is adjusted to 2-4 using hydrochloric acid; the reverse osmosis membrane is soaked for 5-10 minutes;

[0022] The mass fraction concentration of sodium sulfite in the sodium sulfite aqueous solution is 2-5%.

[0023] Preferably, in step (4), the protective liquid is a glycerol protective liquid, the mass fraction concentration of glycerol in the protective liquid is 5-20%, the heat treatment temperature is 70-90°C, and the time is 5-10 minutes. Glycerol prevents membrane pore shrinkage and maintains the performance of the reverse osmosis membrane.

[0024] The present invention also provides a multi-functional group synergistic reverse osmosis membrane prepared by the above preparation method.

[0025] Preferably, the surface of the reverse osmosis membrane contains benzenesulfonic acid groups and sulfite groups, and the main body of the separation functional layer of the reverse osmosis membrane contains sulfonic acid groups.

[0026] Therefore, the present invention adopts the above-mentioned multi-functional group synergistic reverse osmosis membrane and its preparation method, which has the following beneficial effects:

[0027] 1. The present invention introduces sulfonic acid groups into the polyamide separation layer through the aqueous phase additive diaminobenzenesulfonic acid to construct an efficient water molecule transfer channel, significantly improve the hydrophilicity, and make the water permeation flux greater than 5L / m 2 ·h·bar. Simultaneously, the diazo coupling reaction triggered by sodium nitrite treatment forms a high density of azo bonds on the membrane surface, significantly enhancing the crosslinking of the polyamide network and boosting the salt rejection rate to >99.0%. The synergistic effect of the sulfonic acid groups and azo bonds ensures both high flux and enhanced ion retention, resolving the "flux-rejection" trade-off inherent in traditional reverse osmosis membranes.

[0028] 2. This invention utilizes the reactivity of residual acyl chloride groups in the nascent membrane to introduce benzenesulfonic acid groups via surface grafting with aminobenzenesulfonic acid. Combined with the sulfite groups generated by sodium sulfite replacing the diazo groups, a stable hydrophilic protective layer is formed on the membrane surface. This design implements a triple stabilization mechanism: ① The disulfonic acid groups continuously maintain a super-hydrophilic surface (contact angle <30°), delaying organic contamination; ② The sulfite groups eliminate the photothermal-sensitive diazo groups, increasing the chemical tolerance range; and ③ The diazo cross-linked network inhibits polyamide swelling, ensuring long-term salt rejection stability, thereby increasing the service life of the reverse osmosis membrane.

[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the SEM image of the reverse osmosis membrane prepared in Example 1. DETAILED DESCRIPTION

[0031] Unless otherwise defined, technical or scientific terms used in the present invention shall have the same meaning as commonly understood by one of ordinary skill in the art to which the present invention belongs.

[0032] Furthermore, it should be understood that although this specification describes the embodiments, not every embodiment includes only one independent technical solution. This description is for clarity only. Those skilled in the art should consider the specification as a whole. The technical solutions in the various embodiments may also be appropriately combined to form other embodiments that are understandable to those skilled in the art. These other embodiments are also encompassed within the scope of protection of the present invention.

[0033] The present invention discloses a method for preparing a multifunctional synergistic reverse osmosis membrane, which is implemented through aqueous phase additives and surface chemical reactions. A polysulfone casting solution is coated on a non-woven fabric, and a polysulfone porous base membrane is prepared by phase inversion. The base membrane is then immersed in an aqueous monomer solution of m-phenylenediamine and diaminobenzenesulfonic acid and an oil-phase monomer solution of trimesoyl chloride for interfacial polymerization. The aqueous phase additive diaminobenzenesulfonic acid participates in the interfacial polymerization, introducing sulfonic acid groups into the main body of the reverse osmosis membrane separation functional layer, thereby increasing water transfer channels. After heat treatment, a nascent reverse osmosis membrane is obtained.

[0034] The nascent reverse osmosis membrane is soaked in an aqueous solution of aminobenzenesulfonic acid. The residual acyl chloride groups on the membrane surface react with the amino groups of aminobenzenesulfonic acid, introducing benzenesulfonic acid groups through a surface chemical reaction. The membrane is then treated with an aqueous sodium nitrite solution, which causes a diazotization coupling reaction on the membrane surface, increasing the crosslinking degree of the polyamide layer and thus the membrane's salt rejection rate. The membrane is then cleaned with an aqueous sodium sulfite solution. The sulfite groups replace the unreacted diazo groups, introducing sulfite groups onto the membrane surface and improving its surface stability and hydrophilicity. Finally, the membrane is soaked in an aqueous glycerol solution as a protective solution and dried to obtain a dry, multi-functional, synergistic reverse osmosis membrane.

[0035] The structural design of the separation layer body and surface of the reverse osmosis membrane improves the desalination rate and water permeation flux of reverse osmosis through the synergistic effect of multiple functional groups.

[0036] The specific steps include:

[0037] Step 1: prepare an aqueous monomer solution of m-phenylenediamine and diaminobenzenesulfonic acid, and prepare an oily monomer solution of trimesoyl chloride.

[0038] The aqueous monomer solution contains 1-5% m-phenylenediamine by mass, and the aqueous additive diaminobenzenesulfonic acid by mass is 0.1-1%. The pH of the aqueous monomer solution is adjusted to 9-10 using a buffer solution of camphorsulfonic acid and triethylamine. The oil-phase monomer solvent can be n-hexane, n-heptane, or an isoparaffin. The mass fraction of trimesoyl chloride in the oil-phase solution is 0.1-0.5%.

[0039] Step 2: The polysulfone porous base membrane is sequentially immersed in the aqueous monomer solution and the oily monomer solution to generate an interfacial polymerization reaction, thereby forming a polyamide separation functional layer. After heat treatment, the crosslinking degree of the polyamide is further increased to obtain a nascent reverse osmosis membrane.

[0040] The polysulfone porous base membrane is prepared by dissolving polysulfone in dimethylformamide, wherein the mass fraction of polysulfone is 18%, stirring to completely dissolve it to prepare a polysulfone casting solution, degassing the casting solution, coating it on a non-woven fabric, and immersing it in water for phase conversion to prepare a polysulfone porous base membrane.

[0041] In the above process, the polysulfone-based membrane is immersed in the aqueous monomer solution for 1-10 minutes and in the oil-phase monomer solution for 1-10 minutes. Interfacial polymerization occurs between the aqueous monomer m-phenylenediamine and the oil-phase monomer trimesoyl chloride, forming a polyamide separation functional layer. Heat treatment is then performed in an oven at 50-90°C for 1-10 minutes to further promote the polyamide crosslinking reaction and increase density, resulting in a nascent reverse osmosis membrane.

[0042] In the above process, the amino group of the aqueous phase additive diaminobenzenesulfonic acid participates in the interfacial polymerization reaction, introduces sulfonate groups into the main body of the reverse osmosis membrane separation functional layer, forms more water channels, and improves the permeation flux of the reverse osmosis membrane.

[0043] Step 3: Soak the nascent reverse osmosis membrane in an aqueous solution of aminobenzenesulfonic acid. The residual acyl chloride groups on the membrane surface react with the amino groups of the aminobenzenesulfonic acid, introducing benzenesulfonic acid groups and increasing the hydrophilicity and water permeation flux of the reverse osmosis membrane. The concentration of aminobenzenesulfonic acid in the aqueous solution is 1-5% by mass, and the soaking time is 5-10 minutes.

[0044] Step 4: The reverse osmosis membrane is immersed in a sodium nitrite aqueous solution. The nitrite oxidizes the amino groups on the membrane surface, causing a diazotization reaction. The diazo groups further undergo a coupling reaction with the amino groups, thereby increasing the cross-linking density of the polyamide and improving the salt rejection rate of the reverse osmosis membrane. The reverse osmosis membrane is then washed with a sodium sulfite aqueous solution. The sulfite groups replace the residual diazo groups on the reverse osmosis membrane.

[0045] The mass fraction concentration of sodium nitrite in the aqueous solution is 0.1-1%, and the pH of the solution is adjusted to 2-4 using hydrochloric acid. The reverse osmosis membrane is soaked for 5-10 minutes. Sodium sulfite is then used for cleaning, with the mass fraction concentration of sodium sulfite in the aqueous solution being 2-5%. Sulfite groups replace residual azo groups on the surface of the reverse osmosis membrane, improving the stability and hydrophilicity of the reverse osmosis membrane.

[0046] Step 5: Soak the reverse osmosis membrane in a protective solution of glycerol aqueous solution and dry it to obtain a dry multi-functional synergistic reverse osmosis membrane. The mass fraction of glycerol in the aqueous solution is 5-20%, and the soaking time is 5-10 minutes. The membrane is then dried in an oven at a heat treatment temperature of 70-90°C for 5-10 minutes to obtain a dry reverse osmosis membrane. The glycerol prevents membrane pore shrinkage and maintains the performance of the reverse osmosis membrane.

[0047] The technical solution of the present invention is further described below with reference to the accompanying drawings and embodiments.

[0048] Unless otherwise defined, technical or scientific terms used in the present invention shall have the same meaning as commonly understood by one of ordinary skill in the art to which the present invention belongs.

[0049] Furthermore, it should be understood that although this specification describes the embodiments, not every embodiment includes only one independent technical solution. This description is for clarity only. Those skilled in the art should consider the specification as a whole. The technical solutions in the various embodiments may also be appropriately combined to form other embodiments that are understandable to those skilled in the art. These other embodiments are also encompassed within the scope of protection of the present invention.

[0050] Example 1

[0051] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, comprising the following steps:

[0052] Step 1: Prepare an aqueous solution of m-phenylenediamine monomers with a mass fraction of 2%. Add diaminobenzenesulfonic acid (DBSA) as an aqueous additive until the mass fraction of DBSA reaches 0.1%. Adjust the pH of the aqueous solution to 9.5 using a pH buffered solution of 2% camphorsulfonic acid and 1% triethylamine.

[0053] An oil phase monomer solution was prepared, wherein the solvent was n-heptane, and trimesoyl chloride was added thereto to a concentration of 0.2% by mass to obtain an oil phase monomer solution.

[0054] Step 2: dissolving polysulfone in a dimethylformamide solution to make the mass fraction concentration of polysulfone in the solution 18%, and preparing a polysulfone casting solution after the polysulfone is completely dissolved and degassed; coating the polysulfone casting solution on a non-woven fabric to convert the phase into a polysulfone porous base membrane.

[0055] The polysulfone porous base membrane was sequentially immersed in the aqueous monomer solution for 2 minutes and the oily monomer solution for 2 minutes to cause interfacial polymerization reaction, and then heat-treated in an oven at 60° C. for 5 minutes to obtain a nascent reverse osmosis membrane.

[0056] Step 3. Soak the nascent reverse osmosis membrane in an aqueous solution of aminobenzenesulfonic acid with a mass fraction concentration of 1% for 5 minutes to allow the residual acyl chloride groups and amino groups on the membrane surface to react. After rinsing with clean water, soak it in an aqueous solution of nitrous acid with a pH value of 2 and a mass fraction concentration of 0.2%. The amino groups on the surface of the reverse osmosis membrane undergo a diazotization reaction, and further a coupling reaction occurs to increase the cross-linking degree of the polyamide. The soaking time is 5 minutes. After the soaking is completed, rinse with water, and then soak it in an aqueous solution of sodium sulfite to replace the residual diazo groups with sulfite groups. The mass fraction concentration of sodium sulfite in the aqueous solution is 1%.

[0057] Finally, the membrane was immersed in a glycerol aqueous solution and dried to obtain a dry reverse osmosis membrane. The glycerol concentration in the aqueous solution was 10%. The membrane was then heat-treated in an oven at 80°C for 10 minutes to prepare a dry reverse osmosis membrane.

[0058] The SEM image of the reverse osmosis membrane prepared in this example is as follows: Figure 1 As shown in the figure, it can be seen that the morphology of the reverse osmosis membrane is an irregular convex surface structure of a typical interfacial polymerization polyamide membrane. The high surface roughness can increase the specific surface area and water permeation flux of the reverse osmosis membrane.

[0059] Example 2

[0060] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of diaminobenzenesulfonic acid as an aqueous phase additive is 0.2%.

[0061] Example 3

[0062] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of diaminobenzenesulfonic acid as an aqueous phase additive is 0.25%.

[0063] Example 4

[0064] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of diaminobenzenesulfonic acid as an aqueous phase additive is 0.3%.

[0065] Example 5

[0066] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of m-phenylenediamine in the aqueous solution is 1.5%.

[0067] Example 6

[0068] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of m-phenylenediamine in the aqueous solution is 2.5%.

[0069] Example 7

[0070] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of m-phenylenediamine in the aqueous solution is 3%.

[0071] Example 8

[0072] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as those in Example 1, except that the mass fraction concentration of trimesoyl chloride in the oil phase solution is 0.15%.

[0073] Example 9

[0074] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of trimesoyl chloride in the oil phase solution is 0.25%.

[0075] Example 10

[0076] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the solvent of the oil phase monomer solution is n-hexane.

[0077] Example 11

[0078] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the solvent of the oil phase monomer solution is isoparaffin.

[0079] Example 12

[0080] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction of aminobenzenesulfonic acid in the aqueous solution is 1.5%.

[0081] Example 13

[0082] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which is the same as the steps in Example 1, except that the mass fraction concentration of aminobenzenesulfonic acid in the aqueous solution is 2%.

[0083] Example 14

[0084] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of sodium nitrite in the aqueous solution is 0.1%.

[0085] Example 15

[0086] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of sodium nitrite in the aqueous solution is 0.3%.

[0087] Example 16

[0088] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of sodium sulfite in the aqueous solution is 1%.

[0089] Example 17

[0090] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of sodium sulfite in the aqueous solution is 3%.

[0091] Example 18

[0092] This embodiment provides a method for preparing a multi-functional group synergistic reverse osmosis membrane, which has the same steps as Example 1, except that the mass fraction concentration of glycerol in the aqueous solution is 15%.

[0093] Test Case

[0094] The reverse osmosis membrane prepared in Examples 1-18 was installed in a cross-flow test device. The reverse osmosis membrane was first flushed with pure water for 0.5 h, then replaced with a 0.1% sodium chloride aqueous solution. The operating pressure was adjusted to 8 bar, and the water permeation flux and salt rejection rate of the reverse osmosis membrane were tested. The water permeation flux of the reverse osmosis membrane was calculated using formula (1):

[0095]

[0096] In formula (1): J is water flux, L / (m 2 hbar); V is the water permeation volume, L; A is the membrane surface area, m 2 ; Δt is the running time, h; P is the operating pressure, bar.

[0097] The sodium chloride concentration in the raw material solution was measured using a conductivity meter. The rejection rate of the reverse osmosis membrane was calculated using formula (2):

[0098]

[0099] In formula (2): R is the sodium chloride retention rate, %; C p is the sodium chloride concentration of the diafiltrate; C f is the sodium chloride concentration of the raw material solution.

[0100] The water permeation flux and sodium chloride rejection of the reverse osmosis membranes prepared in Examples 1-18 are shown in Table 1:

[0101] Table 1 Reverse osmosis membrane test results of Examples 1-18

[0102]

[0103]

[0104] Therefore, the present invention provides a multi-group synergistic reverse osmosis membrane and a preparation method thereof. The preparation method is easy to control and the process is simple. The reverse osmosis membrane obtained by the preparation method has a synergistic effect of multiple functional groups, which improves its desalination rate and water permeation flux. It can be used in the fields of pure water preparation, deep treatment of industrial sewage and wastewater, and seawater desalination.

[0105] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific implementation method of the present invention and does not limit the scope of protection of the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a multi-functional group synergistic reverse osmosis membrane, characterized in that: The following steps are involved: Step (1) Preparation of aqueous and oily phase monomer solutions: preparing an aqueous monomer solution containing m-phenylenediamine and an aqueous phase additive, and preparing an oily phase monomer solution of trimesoyl chloride; Step (2) interfacial polymerization membrane preparation: soaking the polysulfone porous base membrane in the aqueous monomer solution and the oily monomer solution in sequence to generate a polyamide separation functional layer, and heat-treating the polyamide to increase the cross-linking degree to prepare a nascent reverse osmosis membrane; Step (3) hydrophilic surface modification of the nascent reverse osmosis membrane: soaking the nascent reverse osmosis membrane in an aqueous solution of aminobenzenesulfonic acid to introduce benzenesulfonic acid groups; Step (4) diazo optimization treatment: The nascent reverse osmosis membrane treated in step (3) is immersed in a low-concentration sodium nitrite aqueous solution for treatment. After the diazo coupling reaction occurs, the reverse osmosis membrane is cleaned with a high-concentration sodium sulfite aqueous solution to replace the residual diazo groups with the sulfite groups, thereby obtaining a multi-functional group-coordinated reverse osmosis membrane. The membrane is then immersed in a protective liquid and subjected to heat treatment to obtain a dry reverse osmosis membrane.

2. The method for preparing a multi-functional group synergistic reverse osmosis membrane according to claim 1, characterized in that: In step (1), the mass fraction concentration of phenylenediamine in the aqueous monomer solution is 1-5%, the aqueous phase additive is diaminobenzenesulfonic acid, and the mass fraction concentration is 0.1-1%; camphorsulfonic acid and triethylamine buffer solution are used to adjust the pH value of the aqueous monomer solution to 9-10.

3. The method for preparing a multi-functional group synergistic reverse osmosis membrane according to claim 1, characterized in that: The solvent of the oil phase monomer solution in step (1) is any one of n-hexane, n-heptane and isoparaffin; the mass fraction concentration of trimesoyl chloride in the oil phase monomer solution is 0.1-0.5%.

4. The method for preparing a multi-functional group synergistic reverse osmosis membrane according to claim 1, characterized in that: The preparation of the polysulfone porous base membrane in step (2) comprises the following steps: a. dissolving polysulfone in a dimethylformamide solution, wherein the mass fraction concentration of polysulfone in the solution is 18%, and preparing a polysulfone casting solution after the polysulfone is completely dissolved and degassed; b. Coat the polysulfone casting solution on the non-woven fabric to convert it into a polysulfone porous base membrane.

5. The method for preparing a multi-functional group synergistic reverse osmosis membrane according to claim 1, characterized in that: In step (2), the polysulfone porous base membrane is immersed in the aqueous monomer solution for 1-10 minutes and in the oily monomer solution for 1-10 minutes; The heat treatment temperature is 50-90° C., and the heat treatment time is 1-10 minutes to obtain a nascent reverse osmosis membrane.

6. The method for preparing a multi-functional group synergistic reverse osmosis membrane according to claim 1, characterized in that: In step (3), the mass fraction concentration of aminobenzenesulfonic acid in the aminobenzenesulfonic acid aqueous solution is 1-5%, and the soaking time is 5-10 minutes.

7. The method for preparing a multi-functional group synergistic reverse osmosis membrane according to claim 1, characterized in that: In step (4), the mass fraction concentration of sodium nitrite in the sodium nitrite aqueous solution is 0.1-1%, and the pH value of the sodium nitrite aqueous solution is adjusted to 2-4 using hydrochloric acid; the reverse osmosis membrane is soaked for 5-10 minutes; The mass fraction concentration of sodium sulfite in the sodium sulfite aqueous solution is 2-5%.

8. The method for preparing a multi-functional group synergistic reverse osmosis membrane according to claim 1, characterized in that: In step (4), the protective liquid is a glycerol protective liquid, the mass fraction concentration of glycerol in the protective liquid is 5-20%, the heat treatment temperature is 70-90° C., and the time is 5-10 minutes.

9. A multi-functional group synergistic reverse osmosis membrane, characterized in that: The preparation method is described in any one of claims 1 to 8.

10. The multi-functional group synergistic reverse osmosis membrane according to claim 9, characterized in that: The surface of the reverse osmosis membrane contains benzenesulfonic acid groups and sulfite groups, and the main body of the separation functional layer of the reverse osmosis membrane contains sulfonic acid groups.

Citation Information

Cited By

  • Super-anti-pollution thin-layer composite polymer film for treating electroplating wastewater and preparation method of super-anti-pollution thin-layer composite polymer film

    CN121891954A