Preparation method of modified catalyst and application of modified catalyst in methanol regeneration in methane conversion
By synergistically designing nitrogen-doped zinc oxide catalysts, hydrogen bond traps were constructed to suppress CH bond breaking, solving the problem of excessive CO2 generation during the photo-oxidation of methane to methanol. This achieved highly selective production of methanol and formaldehyde, improving the catalyst's activation performance and conversion rate.
Patent Information
- Application Number
- CN202511279139.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-09
- Publication Date
- 2025-10-17
- Estimated Expiration
- 2045-09-09
AI Technical Summary
Existing catalysts for the photo-oxidation of methane to methanol lack precise control over the reaction pathway, resulting in almost zero methanol production and high CO2 selectivity, which seriously pollutes the environment and causes economic losses. Existing control strategies have failed to fundamentally solve the balance between methane activation and methanol stability in the catalytic process.
By synergistically designing nitrogen-doped zinc oxide (N-ZnO) catalysts, hydrogen bond traps are constructed to preferentially capture electrons, suppress CH bond breaking, and maintain the activation performance of the catalyst. NH bonds are used as traps to suppress methane peroxidation and improve the selectivity of methanol and formaldehyde formation.
It achieves near 100% production of methanol and formaldehyde, significantly reduces CO2 generation, improves methane conversion rate and catalyst activation performance, and resolves the economic and environmental contradiction in the photocatalytic oxidation of methane to methanol.
Smart Images

Figure CN120790203A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of catalyst preparation, in particular to a modified catalyst preparation method and its application in regenerating methanol in methane conversion. BACKGROUND
[0002] Methane selective oxidation to methanol is a major challenge in the field of energy and chemical industry. Although photocatalytic technology can activate methane under mild conditions, existing catalysts (such as ZnO, TiO2) lack precise control over the reaction path, resulting in the target product being easily over-oxidized to CO2. The traditional ZnO catalyst has a CO2 selectivity as high as 67% in the CH4 photo-oxidation process, while the methanol product is almost zero. The fundamental reason is that: (1) the active sites on the catalyst surface (such as Zn-O) have insufficient stability for the intermediate CH3OH*, leading to continuous dehydrogenation; (2) the photo-generated holes directly attack the C-H bond, resulting in an uncontrollable reaction path. This will lead to a large amount of carbon loss (more than 50% in most systems), seriously polluting the environment, causing huge economic losses, and exacerbating the greenhouse effect. The root cause of this problem lies in the thermodynamic properties of the reaction: the extremely strong C-H bond in the methane molecule (bond energy as high as 435 kJ / mol) requires a high-activity catalyst site to activate, but these active sites often further oxidize the product methanol (C-H bond energy 402 kJ / mol) to CO2 during the catalytic process. In response to this challenge, researchers have proposed various control strategies, but each method has obvious limitations. From the perspective of thermodynamics, increasing the reaction pressure can inhibit the generation of CO2, but additional energy is required for gas compression, which increases overall energy consumption. In terms of kinetic control, reducing the reaction temperature can effectively inhibit over-oxidation, but it also significantly reduces the reaction rate, resulting in a significant decrease in production efficiency. The time control strategy avoids further oxidation of methanol by shortening the reaction time, but this method artificially sets an upper limit on the yield, making it difficult to achieve the high yield required for industrial production. In addition, the use of membrane reactors and other spatial restriction methods can separate the product in time, but the complex device design and high equipment investment bring new economic burdens. These control methods are essentially compromises and trade-offs in reaction conditions, and do not fundamentally solve the core contradiction in the catalytic process: the balance between the high-activity oxygen species required for methane activation and the stability of methanol. The existence of this key scientific problem has seriously restricted the practical application and industrialization process of methane photocatalytic oxidation to methanol technology.
[0003] The strategy of only focusing on inhibiting over-oxidation by traditional methods cannot solve the inherent thermodynamic limitations, which prompts an innovative catalyst design strategy: by constructing hydrogen bond traps (such as N-H bonds) to preferentially capture electrons and inhibit C-H bond breaking, and also ensuring the activation performance of the material. The present application is a synergistic design of nitrogen-doped zinc oxide (N-ZnO): on the one hand, the substrate material ZnO is used to ensure the activation performance of the catalyst, and on the other hand, the over-oxidation of methane is inhibited to reduce the generation of CO2. SUMMARY
[0004] In view of the deficiencies of the prior art, the purpose of the present application is to provide a preparation method of a modified catalyst and its application in regenerating methanol in methane conversion. In view of the problems existing in the prior art of methane photocatalytic conversion process, the selectivity of high-value chemicals in methane conversion is low, the present application realizes the generation of more than 95% of high-value chemicals by inhibiting the continuous dehydrogenation of methane, and a method for preparing high-performance photocatalytic materials is prepared. In the process of catalyzing methane conversion, the nitrogen-doped catalytic material is designed as a trap by constructing a chemical bond with a bond energy less than the "C-H" bond, which preferentially breaks to inhibit the breaking of the "C-H" bond of methane to realize the generation of nearly 100% of methanol and formaldehyde. In addition, the nitrogen doping successfully improves the activation performance of the base material and increases the methane conversion rate. This technology successfully modifies the catalytic performance of the base material and can be widely used in natural gas conversion, solar fuel preparation and other clean energy fields.
[0005] To achieve the above purpose, the present application provides the following technical solutions: The preparation method of the nitrogen-doped modified catalyst comprises the following preparation steps: S1. Mix 36-40 parts of zinc nitrate, 22-25 parts of urea, 1-3 parts of mesoporous regulator and 300-350 parts of deionized water by mass fraction, and stir at a speed of 550-600 r / min under the condition of water bath at 68-70℃ for 10-15 min; S2. Age the mixed solution obtained in step S1 at 68-70℃ for 2-3h, and after centrifugal separation, wash the solid to neutral with deionized water, then wash with anhydrous ethanol for 3-4 times, dry for 10-12h to obtain a precursor powder; S3. Ball mill mix the precursor powder, 3-4 parts of urea and 1-3 parts of loading modifier for 20-30 min, calcine in a muffle furnace under air atmosphere, grind through a 200 mesh sieve after natural cooling to obtain a nitrogen-doped modified catalyst; The preparation of the mesoporous regulator comprises the following steps: S11. Add 0.5-1 parts of cetyltrimethylammonium bromide and 0.5-1 parts of P123 to 20-25 parts of deionized water by mass fraction, and stir at a speed of 350-400 r / min under the condition of water bath at 60-65℃ for 15-20 min; S12. Add 0.2-0.4 parts of 1,3,5-trimethylbenzene and 0.5-0.8 parts of a stabilizing agent to the solution obtained in step S11 and continue stirring for 10-13 min; S13. The mixed solution obtained in step S12 is allowed to stand at 55-60° C. for 3-4 hours, centrifuged to obtain a solid, washed with ethanol 3-4 times, and freeze-dried in vacuum to obtain a mesoporous modulator.
[0006] Preferably, the preparation of the loaded modifier comprises the following steps: S31. In parts by mass, 0.1-0.3 parts of chloroplatinic acid were dissolved in 15-20 parts of anhydrous ethanol and stirred in a water bath at 38-40 ° C for 8-10 min to obtain a solution A; S32. 2-3 parts of hexamethylenetetramine and 4-6 parts of ammonium borate were added to 15-20 parts of anhydrous ethanol and ultrasonically dispersed at a frequency of 40 kHz for 15-20 min to obtain a solution B; S33. Add solution B to solution A at a rate of 1-2 ml / min at 58-60°C, then heat to 70-75°C, stir at 350-400 r / min for 1-2 h, centrifuge and separate the precipitate, wash with anhydrous ethanol 3-4 times, and vacuum dry at 78-80°C to obtain the loaded modifier.
[0007] Preferably, the preparation of the stability enhancer comprises the following steps: S121. In parts by mass, 0.2-0.3 parts of graphene oxide were added to 4-6 parts of anhydrous ethanol and ultrasonically dispersed for 20-30 min to obtain a preliminary mixed solution; S122. To the preliminary mixture were added 0.2-0.3 parts of tetraethyl silicate, 0.1-0.2 parts of boric acid, 0.05-0.1 parts of polyethylene glycol, and stirred at 350-400 r / min in a water bath at 58-60 ° C for 10-15 min to obtain a secondary mixed solution; S123. Add 0.1-0.2 parts by mass of 50% hydrochloric acid dropwise to the mixed solution of the second step, react for 1-2 hours, and then age at 35-40°C for 5-6 hours. Then, vacuum dry at 65-70°C for 10-12 hours. Grind and pass through a 200-mesh sieve to obtain a stabilizing enhancer.
[0008] Preferably, the calcination in step S3 is performed by heating the temperature to 300° C. at a heating rate of 5° C. / min and then keeping the temperature for 1 hour.
[0009] Preferably, the drying temperature in step S2 is 78-80°C.
[0010] Preferably, the vacuum freeze-drying temperature in step S13 is -50 to -40°C.
[0011] Preferably, the stirring speed in step S31 is 300-350 r / min.
[0012] Preferably, the frequency of ultrasonic dispersion in step S121 is 40 kHz.
[0013] Application of a modified catalyst in the regeneration of methanol in methane conversion.
[0014] Compared with the prior art, the application has the beneficial effects that: 1. The application is directed to the field of photocatalytic methane to high-value chemicals, solves the problem of methane peroxidation to generate carbon dioxide, proposes a method of inhibiting methane peroxidation by constructing chemical bonds, and provides a new method for solving the problem of methane peroxidation. At the same time, the activation performance of the base material is optimized, the activation performance of the original catalyst is improved, the yield and selectivity of methanol are improved, and the directional generation of methanol is promoted.
[0015] 2. The application improves the photo-generated carrier separation efficiency of the nitrogen-doped modified catalyst by loading a modifier, inhibits methane peroxidation, forms a deep synergy of electron-hole separation and reaction microenvironment regulation with a mesoporous regulator, improves the thermal stability of the catalyst, inhibits C-H bond rupture, blocks the over-oxidation path from the root, and solves the economic and environmental contradictions of photocatalytic methane to methanol. BRIEF DESCRIPTION OF DRAWINGS
[0016] Figure 1 The preparation process flow chart of the modified catalyst of the application is shown in the figure; Figure 2 The XRD spectrum of the nitrogen-doped modified catalyst obtained from Example 1 and Comparative Examples 1-3 of the application is shown in the figure; Figure 3 The TEM image of the nitrogen-doped modified catalyst obtained from Comparative Example 1 of the application is shown in the figure; Figure 4 The TEM image of the nitrogen-doped modified catalyst obtained from Example 1 of the application is shown in the figure; Figure 5 The EPR spectrum of the nitrogen-doped modified catalyst obtained from Comparative Example 1 of the application is shown in the figure; Figure 6 The EPR spectrum of the nitrogen-doped modified catalyst obtained from Example 1 of the application is shown in the figure; Figure 7 The bar chart of the CH3OH yield of the nitrogen-doped modified catalyst obtained from Example 1 and Comparative Examples 1-3 of the application changing with time is shown in the figure; Figure 8 The bar chart of the CO2 yield of the nitrogen-doped modified catalyst obtained from Example 1 and Comparative Examples 1-3 of the application changing with time is shown in the figure; Figure 9The CO production of the nitrogen-doped modified catalyst obtained in Example 1 and Comparative Examples 1-3 of the present application is plotted against time; Figure 10 The total amount of products at 40 min of the nitrogen-doped modified catalyst obtained in Example 1 and Comparative Example 1 of the present application is plotted for comparison; Figure 11 The product proportion of the nitrogen-doped modified catalyst obtained in Example 1 and Comparative Example 1 of the present application is plotted; Figure 12 The in-situ infrared spectrum of the nitrogen-doped modified catalyst obtained in Example 1 of the present application is plotted; Figure 13 The in-situ infrared spectrum of the nitrogen-doped modified catalyst obtained in Comparative Example 1 of the present application is plotted. DETAILED DESCRIPTION
[0017] The present application will be described in detail below with reference to the embodiments thereof, it is apparent that the described embodiments are only a part of the embodiments of the present application, but not all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by a person of ordinary skill in the art without creative labor fall within the scope of protection of the present application.
[0018] Please refer to Figures 1-13 The present application provides a technical solution: In order to solve the problem of photocatalytic methane peroxidation, the present application proposes a nitrogen-doped modified catalyst for photocatalytic preparation of methanol from methane under mild conditions without additional oxidants. Through synergistic effect, not only the activation performance of the base material is improved to promote the activation of methane, but also a chemical bond that preferentially breaks the "C-H" bond is constructed as a trap to inhibit the continuous dehydrogenation of methane, on the one hand, to achieve nearly 100% generation of high-value chemicals methanol and formaldehyde, and on the other hand, to inhibit the generation of CO2. The modified agent is loaded in the form of trace platinum nanoparticles on the boron nitride carrier, which does not enter the ZnO crystal lattice after calcination, ensuring that the main phase of the catalyst is still N-ZnO, and the increase of ZnO oxygen vacancies during nitrogen doping further enhances the activation performance of the catalyst, efficiently converts methane (methanol selectivity > 78%) in the same time, which is 2.1 times higher than that of the un-doped ZnO, and successfully modifies the nitrogen-doped modified catalyst. On the other hand, the formaldehyde generated by the nitrogen-doped modified catalyst during the catalysis process combines with protons (H*) to regenerate methanol, while the formaldehyde generated by ZnO during the catalysis process is further dehydrogenated to CO2.
[0019] Example 1 Preparation method of the modified catalyst: Before preparing the nitrogen-doped modified catalyst, the preparation of the stability enhancer, mesoporous regulator and loading modifier is carried out: The preparation of the stability enhancer includes the following steps: S121. 0.2 g of graphene oxide was added to 4 ml of anhydrous ethanol and ultrasonically dispersed at a frequency of 40 kHz for 20 min to obtain a preliminary mixed solution; S122. To the preliminary mixture, 0.2 g of tetraethyl silicate, 0.1 g of boric acid, and 0.05 g of polyethylene glycol were added and stirred at 350 rpm in a 58°C water bath for 10 min to obtain a secondary mixture. S123. 0.1 ml of 50% hydrochloric acid was added dropwise to the mixture in the second step. After reacting for 1 hour, the mixture was allowed to stand at 35°C for 5 hours, and then dried under vacuum at 65°C for 10 hours. The mixture was ground and passed through a 200-mesh sieve to obtain a stabilizing enhancer. The preparation of the mesoporous modulator includes the following steps: S11. Add 0.5 g of hexadecyltrimethylammonium bromide and 0.5 g of P123 to 20 ml of deionized water and stir at 350 rpm in a 60°C water bath for 15 min. S12. To the solution obtained in step S11, 0.2 g of 1,3,5-trimethylbenzene and 0.5 g of a stabilizing agent were added and stirring was continued for 10 min; S13. The mixed solution obtained in step S12 was allowed to stand at 55°C for 3 hours, centrifuged to obtain a solid, washed three times with ethanol, and freeze-dried in a vacuum (-50°C) to obtain a mesoporous modulator; The preparation of the loaded modifier comprises the following steps: S31. Dissolve 0.1 g of chloroplatinic acid in 15 ml of anhydrous ethanol and stir at 300 rpm in a 38°C water bath for 8 min to obtain solution A. S32. 2 g of hexamethylenetetramine and 4 g of ammonium borate were added to 15 ml of anhydrous ethanol and ultrasonically dispersed at a frequency of 40 kHz for 15 min to obtain solution B; S33. Solution A was added to solution B at 58°C at a rate of 1 ml / min, then heated to 70°C and stirred at 350 r / min for 1 h. The precipitate was separated by centrifugation, washed three times with anhydrous ethanol, and dried in vacuo at 78°C to obtain the loaded modifier. S1. 36 g zinc nitrate, 22 g urea, 1 g mesoporous modifier, and 300 g deionized water were mixed and stirred at 550 rpm in a 68 ° C water bath for 10 min. S2. The mixture obtained in step S1 was aged at 68 ° C for 2 h, centrifuged and the solid was washed with deionized water until neutral, then washed three times with anhydrous ethanol, and dried at 78 ° C for 10 h to obtain a precursor powder; S3. The precursor powder, 3 g of urea and 1 g of the supported modifier were ball-milled for 20 min, calcined in a muffle furnace under air atmosphere (heated to 300°C at a heating rate of 5°C / min and kept for 1 h), and ground through a 200 mesh screen after natural cooling to obtain the nitrogen-doped modified catalyst. The doping amount of nitrogen in this example was about 0.5, and this example was further named as 0.5N-ZnO and N-ZnO.
[0020] Example 2 Preparation method of the modified catalyst: Before preparing the nitrogen-doped modified catalyst, the preparation of the stability enhancer, the mesopore regulator and the supported modifier was performed: The preparation of the stability enhancer included the following steps: S121. 0.3 g of graphene oxide was added to 6 ml of anhydrous ethanol, and ultrasonic dispersion was performed at a frequency of 40 kHz for 30 min to obtain a primary mixed solution; S122. 0.3 g of tetraethyl orthosilicate, 0.2 g of boric acid and 0.1 g of polyethylene glycol were added to the primary mixed solution, and stirring was performed at a speed of 400 r / min under the condition of a water bath at 60°C for 15 min to obtain a secondary mixed solution; S123. 0.2 ml of 50% hydrochloric acid was added dropwise to the secondary mixed solution, and reaction was performed for 2 h. After that, the solution was left to stand at 40°C for aging for 6 h, and then vacuum drying was performed at 70°C for 12 h. After grinding, the stability enhancer was obtained by passing through a 200 mesh screen; The preparation of the mesopore regulator included the following steps: S11. 1 g of cetyltrimethylammonium bromide and 1 g of P123 were added to 25 ml of deionized water, and stirring was performed at a speed of 400 r / min under the condition of a water bath at 65°C for 20 min; S12. 0.4 g of mesitylene and 0.8 g of the stability enhancer were added to the solution obtained in step S11, and stirring was continued for 13 min; S13. The mixed solution obtained in step S12 was left to stand at 60°C for aging for 4 h, and centrifugation was performed to obtain a solid. The solid was washed with ethanol for 4 times, and vacuum freeze-drying was performed at -40°C to obtain the mesopore regulator; The preparation of the supported modifier included the following steps: S31. 0.3 g of chloroplatinic acid was dissolved in 20 ml of anhydrous ethanol, and stirring was performed at a speed of 350 r / min under the condition of a water bath at 40°C for 10 min to obtain solution A; S32. 3 g of hexamethylenetetramine and 6 g of ammonium borate were added to 20 ml of anhydrous ethanol, and ultrasonic dispersion was performed at a frequency of 40 kHz for 20 min to obtain solution B; S33. Solution A was added to solution B at 60℃ with a dropping speed of 2ml / min, and then the temperature was increased to 75℃, and stirred at 400r / min for 2h. The precipitate was separated by centrifugation, washed with anhydrous ethanol for 4 times, and dried at 80℃ under vacuum to obtain the modified catalyst loaded with the modifier; S1. 40g of zinc nitrate, 25g of urea, 3g of mesoporous regulator were mixed with 350g of deionized water, and stirred at 600r / min for 15min under the condition of 70℃ water bath; S2. The mixed solution obtained in step S1 was aged at 70℃ for 3h, and then the solid was washed with deionized water until neutral, and then washed with anhydrous ethanol for 4 times, and dried at 80℃ for 12h to obtain the precursor powder; S3. The precursor powder, 4g of urea and 3g of the loaded modifier were ball-milled for 30min, and then calcined in a muffle furnace under air atmosphere (heated to 300℃ at a heating rate of 5℃ / min, and then kept for 1h), and then ground through a 200 mesh sieve to obtain the nitrogen-doped modified catalyst.
[0021] Example 3 Preparation method of the modified catalyst: Before preparing the nitrogen-doped modified catalyst, the preparation of the stability enhancer, mesoporous regulator and loaded modifier was carried out: The preparation of the stability enhancer includes the following steps: S121. 0.22g of graphene oxide was added to 5ml of anhydrous ethanol, and ultrasonically dispersed at a frequency of 40kHz for 22min to obtain a preliminary mixed solution; S122. 0.22g of tetraethyl orthosilicate, 0.12g of boric acid and 0.06g of polyethylene glycol were added to the preliminary mixed solution, and stirred at 370r / min for 11min under the condition of 59℃ water bath to obtain a secondary mixed solution; S123. 0.12ml of 50% hydrochloric acid was added dropwise to the secondary mixed solution, and reacted for 1.5h, and then aged at 36℃ for 5.5h, and then dried at 66℃ under vacuum for 11h, and then ground through a 200 mesh sieve to obtain the stability enhancer; The preparation of the mesoporous regulator includes the following steps: S11. 0.6g of cetyltrimethylammonium bromide and 0.6g of P123 were added to 21ml of deionized water, and stirred at 370r / min for 16min under the condition of 61℃ water bath; S12. 0.3g of mesitylene and 0.6g of the stability enhancer were added to the solution obtained in step S11, and continued to stir for 11min; S13. The mixed solution obtained in step S12 is aged at 56°C for 3.5 h, and then centrifuged to obtain a solid, which is washed with ethanol for 3 times and vacuum freeze-dried (-42°C) to obtain the mesoporous regulator; The preparation of the support modifier comprises the following steps: S31. 0.2 g of chloroplatinic acid is dissolved in 16 ml of anhydrous ethanol, and stirred at a speed of 320 r / min for 9 min under the condition of a 39°C water bath to obtain solution A; S32. 2.2 g of hexamethylenetetramine and 5 g of ammonium borate are added to 16 ml of anhydrous ethanol, and ultrasonically dispersed at a frequency of 40 kHz for 16 min to obtain solution B; S33. Solution A is added to solution B at a dropping speed of 1 ml / min under the condition of 59°C, and then the temperature is increased to 71°C, and stirred at a speed of 370 r / min for 1 h, and then centrifuged to separate the precipitate, which is washed with anhydrous ethanol for 3 times and dried under the condition of 79°C to obtain the support modifier; S1. 37 g of zinc nitrate, 23 g of urea, 2 g of mesoporous regulator and 320 g of deionized water are mixed, and stirred at a speed of 570 r / min for 11 min under the condition of a 69°C water bath; S2. The mixed solution obtained in step S1 is aged at 69°C for 2.5 h, and then centrifuged to separate the solid, which is washed with deionized water until neutral, and then washed with anhydrous ethanol for 3 times and dried at 79°C for 11 h to obtain the precursor powder; S3. The precursor powder, 3.2 g of urea and 2.2 g of the support modifier are ball-mixed for 22 min, and then calcined in a muffle furnace under the condition of air atmosphere (heated to 300°C at a heating speed of 5°C / min and then kept for 1 h), and then ground through a 200-mesh sieve to obtain the nitrogen-doped modified catalyst.
[0022] Example 4 The preparation method of the modified catalyst comprises the following steps: Before the preparation of the nitrogen-doped modified catalyst, the preparation of the stability enhancer, the mesoporous regulator and the support modifier is carried out: The preparation of the stability enhancer comprises the following steps: S121. 0.28 g of graphene oxide is added to 5.5 ml of anhydrous ethanol, and ultrasonically dispersed at a frequency of 40 kHz for 28 min to obtain a preliminary mixed solution; S122. 0.28 g of tetraethyl orthosilicate, 0.18 g of boric acid and 0.07 g of polyethylene glycol are added to the preliminary mixed solution, and stirred at a speed of 380 r / min for 14 min under the condition of a 59°C water bath to obtain a secondary mixed solution; S123.0.16ml 50% hydrochloric acid was added dropwise into the mixture, and the reaction was allowed to proceed for 1.5h, and then the mixture was aged at 38℃ for 5.5h, and then vacuum dried at 68℃ for 11.5h. After grinding, the mixture was passed through a 200 mesh sieve to obtain the stability enhancer; The preparation of the mesopore regulator comprises the following steps: S11.0.8g hexadecyl trimethyl ammonium bromide and 0.8g P123 were added into 24ml deionized water, and the mixture was stirred at 380r / min for 18min under the condition of a water bath at 64℃; S12.0.35g 1,3,5-trimethylbenzene and 0.7g stability enhancer were added into the solution obtained in step S11, and the mixture was continuously stirred for 12min; S13. The mixture obtained in step S12 was aged at 58℃ for 3.5h, and then centrifuged to obtain a solid, which was washed with ethanol for 4 times and vacuum freeze-dried (-48℃) to obtain the mesopore regulator; The preparation of the supported modifier comprises the following steps: S31.0.25g chloroplatinic acid was dissolved in 18ml anhydrous ethanol, and the solution was stirred at 340r / min for 9min under the condition of a water bath at 39℃ to obtain solution A; S32.2.8g hexamethylenetetramine and 5.8g ammonium borate were added into 17ml anhydrous ethanol, and the mixture was ultrasonically dispersed at a frequency of 40kHz for 17min to obtain solution B; S33.Solution A was added into solution B at a dropping speed of 2ml / min under the condition of 59℃, and then the temperature was increased to 74℃, and the mixture was stirred at 380r / min for 1.5h. The precipitate was separated by centrifugation, washed with anhydrous ethanol for 4 times, and dried at 79℃ to obtain the supported modifier; S1.39g zinc nitrate, 24g urea, 2.5g mesopore regulator and 340g deionized water were mixed, and the mixture was stirred at 580r / min for 14min under the condition of a water bath at 69℃; S2. The mixture obtained in step S1 was aged at 69℃ for 2.5h, and then the solid was washed with deionized water until neutral, and then washed with anhydrous ethanol for 4 times, and dried at 79℃ for 11.5h to obtain a precursor powder; S3. The precursor powder, 3.8g urea and 2.5g supported modifier were ball-milled for 27min, and then calcined in a muffle furnace under air atmosphere (heated to 300℃ at a heating speed of 5℃ / min, and then kept at 300℃ for 1h), and then ground to pass through a 200 mesh sieve to obtain a nitrogen-doped modified catalyst.
[0023] Comparative Example 1 Comparative Example 1 differs from Example 1 in that urea is not added in this comparative example, and the remaining steps are exactly the same in Comparative Example 1 and Example 1, and this comparative example is further named ZnO.
[0024] Comparative Example 2 Comparative Example 2 differs from Example 1 in that the nitrogen doping amount in this comparative example is controlled to be 0.1, that is, the amount of urea added in step S1 is 3.8 g. The remaining steps are exactly the same in Comparative Example 2 and Example 1, and this comparative example is further named 0.1N-ZnO.
[0025] Comparative Example 3 Comparative Example 3 differs from Example 1 in that the nitrogen doping amount in this comparative example is controlled to be 0.9, that is, the amount of urea added in step S1 is 34.2 g. The remaining steps are exactly the same in Comparative Example 3 and Example 1, and this comparative example is further named 0.9N-ZnO.
[0026] Performance testing: Attachment Figure 2 The XRD patterns of the nitrogen-doped modified catalysts obtained in Example 1 and Comparative Examples 1-3 of the present invention are shown in FIG. Figure 2 It can be seen that no impurity phase is generated in Example 1, indicating that the addition of urea, loading modifier, and mesopore control agent in the present invention does not destroy the ZnO crystal framework. Figures 3-4 The TEM images of the nitrogen-doped modified catalysts obtained in Comparative Example 1 and Example 1 of the present invention are shown respectively. As can be seen from the figure, Comparative Example 1 presents a uniform nanorod structure with a smooth surface. The surface of the nanorods in Example 1 is roughened, with holes or defective structures, which directly proves that oxygen vacancies increase. Figures 5-6 The EPR spectra of the nitrogen-doped modified catalysts obtained in Comparative Example 1 and Example 1 of the present invention are shown. Comparative Example 1 shows only a weak ∙OH signal (g = 2.003), indicating limited oxidation capacity of photogenerated holes. In Example 1, the ∙OH signal intensity is significantly enhanced, demonstrating that nitrogen doping enhances the separation efficiency of photogenerated carriers and promotes ∙OH generation.
[0027] The nitrogen-doped modified catalysts prepared in Example 1 and Comparative Examples 1-3 were used to achieve 100% selective production of high-value chemicals from photocatalytic methane conversion. This process was carried out in a 400 mL glass reactor (PQ-256, Beijing Perfect Light Technology Co., Ltd., Beijing, China) with a quartz window for light irradiation. A 300 W xenon lamp (full spectrum light, 600 mW cm -2A CEL-HXF300 (CEAULIGHT Technology Co., Ltd., Beijing, China) was used as the light source. The reaction system temperature was controlled at 60 ± 1°C using a cooling water bath. First, 5 g of the nitrogen-doped modified catalyst was dispersed in 20 mL of deionized water and added to the reactor cell. The reactor was sealed and purged with nitrogen-oxygen gas for 10 minutes. Subsequently, 5 mL of CH₄ (99.99%) was injected into the reactor along with the light irradiation. As the reaction proceeded, methane was continuously converted into methanol, formaldehyde, and carbon dioxide. After 40 minutes, the carbon dioxide yield reached its lowest point, and the products methanol and formaldehyde accounted for over 92% of the system.
[0028] Attachment Figure 7 The following is a bar graph showing the change in CH3OH yield over time for the nitrogen-doped modified catalysts obtained in Example 1 of the present invention and Comparative Examples 1-3. The methanol yield in Comparative Example 1 is close to 0 μmol, while the performance of Example 1 is the best, indicating that the modified catalyst of the present invention has the best methanol yield, and the optimal nitrogen doping ratio is 0.5. Figure 8 The following is a bar graph showing the CO2 production over time for the nitrogen-doped modified catalysts obtained in Example 1 and Comparative Examples 1-3 of the present invention. The CO2 production in Comparative Example 1 was as high as 14 μmol, while that in Example 1 was only 1.8 μmol (a decrease of 87%), confirming that the "hydrogen bond trap" effectively blocks the continuous dehydrogenation pathway. Figure 9 The following is a bar graph showing the CO production of the nitrogen-doped modified catalysts obtained in Example 1 of the present invention and Comparative Examples 1-3 over time. In Comparative Example 1, CO is continuously generated, while in Example 1, CO production approaches 0, indicating that the modified catalyst of the present invention almost completely inhibits the partial oxidation side reaction. Figure 10 This is a comparison chart of the total amount of products of the nitrogen-doped modified catalyst obtained in Example 1 of the present invention and Comparative Examples 1-3 in 40 minutes. Methanol accounts for the highest proportion of the total product in Example 1, and the total amount of CO2 and CO is less than 2 μmol. The methanol selectivity of Example 1 is increased from 0% in Comparative Example 1 to >78%, and the CO2 selectivity is reduced from 67% to <10%. Figure 11 This figure shows the product percentages of the nitrogen-doped modified catalysts obtained in Example 1 and Comparative Example 1. In Comparative Example 1, CO₂ dominates (85%), with methanol absent. In Example 1, methanol and formaldehyde account for 92%, with CO₂ accounting for only 8%, achieving targeted conversion of high-value chemicals. This compares to the traditional metal oxide catalyst ZnO, which produces significant amounts of carbon dioxide (over 85%) and zero methanol production. In contrast, the present invention significantly increases methanol production and achieves near-100% selectivity for methanol and formaldehyde.
[0029] Attachment Figures 12-13In-situ FTIR spectra of the nitrogen-doped modified catalysts obtained from Example 1 and Comparative Example 1 of the present application, respectively. It can be observed that ZnO and N-ZnO exhibit significantly different intermediate evolution behaviors during the photocatalytic oxidation of methane. For ZnO, the signal enhancement of CH2*and CO2species at 1471 cm -1 and 1583 cm -1 , respectively, indicates that methane undergoes a continuous dehydrogenation and peroxidation process on the surface of ZnO, eventually generating CO2. However, the FTIR spectra of N-ZnO have different intermediates: OH*at 1645 cm -1 , CH3*at 1071 cm -1 , and CH3O*at 956 cm -1 . Nitrogen doping not only promotes the adsorption and dissociation of water molecules OH*, but also effectively regulates the activation and selective conversion of methane by stabilizing CH3*and CH3O*intermediates. In addition, CH2O*add H*to regenerate methanol.
[0030] Although embodiments of the present application have been shown and described, it is to be understood that various modifications, substitutions, replacements and variations can be made to these embodiments without departing from the principles and spirit of the present application, and the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a modified catalyst, characterized in that: The method comprises the following preparation steps: S1. In parts by mass, 36-40 parts of zinc nitrate, 22-25 parts of urea, 1-3 parts of a mesoporous modifier and 300-350 parts of deionized water were mixed and stirred at a speed of 550-600 r / min for 10-15 min in a water bath at 68-70 ° C; S2. The mixture obtained in step S1 was aged at 68-70 ° C for 2-3h, centrifuged and the solid was washed with deionized water until neutral, then washed 3-4 times with anhydrous ethanol, and dried for 10-12h to obtain a precursor powder; S3 The precursor powder, 3-4 parts of urea and 1-3 parts of the loading modifier were ball-milled for 20-30min, calcined in an air atmosphere in a muffle furnace, and then ground through a 200 mesh sieve after natural cooling to obtain a nitrogen-doped modified catalyst; The preparation of the mesoporous modulator comprises the following steps: S11. In parts by mass, 0.5-1 parts of hexadecyltrimethylammonium bromide and 0.5-1 parts of P123 were added to 20-25 parts of deionized water and stirred at 350-400r / min in a water bath at 60-65°C for 15-20min; S12. Add 0.2-0.4 parts of 1,3,5-trimethylbenzene and 0.5-0.8 parts of a stabilizing agent to the solution obtained in step S11 and continue stirring for 10-13 min; S13. The mixed solution obtained in step S12 is allowed to stand at 55-60° C. for 3-4 hours, centrifuged to obtain a solid, washed with ethanol 3-4 times, and freeze-dried in vacuum to obtain a mesoporous modulator.
2. The method for preparing a modified catalyst according to claim 1, wherein: The preparation of the loaded modifier comprises the following steps: S31. In parts by mass, 0.1-0.3 parts of chloroplatinic acid were dissolved in 15-20 parts of anhydrous ethanol and stirred in a water bath at 38-40 ° C for 8-10 min to obtain a solution A; S32. 2-3 parts of hexamethylenetetramine and 4-6 parts of ammonium borate were added to 15-20 parts of anhydrous ethanol and ultrasonically dispersed at a frequency of 40 kHz for 15-20 min to obtain a solution B; S33. Add solution B to solution A at a rate of 1-2 ml / min at 58-60°C, then heat to 70-75°C, stir at 350-400 r / min for 1-2 h, centrifuge and separate the precipitate, wash with anhydrous ethanol 3-4 times, and vacuum dry at 78-80°C to obtain the loaded modifier.
3. The method for preparing a modified catalyst according to claim 1, wherein: The preparation of the stability enhancer comprises the following steps: S121. In parts by mass, 0.2-0.3 parts of graphene oxide were added to 4-6 parts of anhydrous ethanol and ultrasonically dispersed for 20-30 min to obtain a preliminary mixed solution; S122. To the preliminary mixture were added 0.2-0.3 parts of tetraethyl silicate, 0.1-0.2 parts of boric acid, 0.05-0.1 parts of polyethylene glycol, and stirred at 350-400 r / min in a water bath at 58-60 ° C for 10-15 min to obtain a secondary mixed solution; S123. Add 0.1-0.2 parts by mass of 50% hydrochloric acid dropwise to the mixed solution of the second step, react for 1-2 hours, and then age at 35-40°C for 5-6 hours. Then, vacuum dry at 65-70°C for 10-12 hours. Grind and pass through a 200-mesh sieve to obtain a stabilizing enhancer.
4. The method for preparing a modified catalyst according to claim 1, wherein: The calcination in step S3 is carried out by heating the temperature to 300° C. at a heating rate of 5° C. / min and then keeping the temperature for 1 hour.
5. The method for preparing a modified catalyst according to claim 1, wherein: The drying temperature in step S2 is 78-80°C.
6. The method for preparing a modified catalyst according to claim 1, wherein: The temperature of vacuum freeze drying in step S13 is -50 to -40°C.
7. The method for preparing a modified catalyst according to claim 2, wherein: The stirring speed in step S31 is 300-350 r / min.
8. The method for preparing a modified catalyst according to claim 3, wherein: The frequency of ultrasonic dispersion in step S121 is 40 kHz.
9. Use of a modified catalyst prepared according to the preparation method according to any one of claims 1 to 8 in methanol regeneration in methane conversion.
Citation Information
Patent Citations
Preparation method of Zn-Zr bi-metal dimer catalyst
CN108786875A
Supported zinc oxide catalyst as well as preparation method and application thereof
CN114618469A
Preparation method of monatomic copper-based catalyst and application of monatomic copper-based catalyst in photocatalytic methane oxidation
CN116440924A
Nitrogen-doped catalyst for oxidative coupling reaction of methane, manufacturing method of nitrogen-doped catalyst for oxidative coupling reaction of methane thereby, and method for oxidative coupling reaction of methane using the same
US20220161249A1
Cited By
Preparation method of quantum dot homogeneous photocatalytic material and application of quantum dot homogeneous photocatalytic material in preparation of methanol by photocatalysis of methane
CN121372520A
Preparation method of metal-nonmetal b-site synergistic catalytic material and application thereof in methane conversion
CN122499820A