Europium ion doped borosilicate / germanate red fluorescent material as well as preparation method and application thereof
By using Eu3+-doped Ba2InBM2O9 (M=Si, Ge) fluorescent material, the stability and cost issues of existing red fluorescent materials have been solved, realizing a red light material with high color purity, narrow band red light emission and long lifespan, which is suitable for high-performance LED devices.
Patent Information
- Application Number
- CN202510823809.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-19
- Publication Date
- 2025-10-31
AI Technical Summary
Existing red fluorescent materials suffer from problems such as high raw material costs, poor thermal stability, easy moisture absorption, complex synthesis processes, or humidity sensitivity, making it difficult to meet the application requirements of high-performance full-spectrum LED devices.
Using Eu3+-doped Ba2InBM2O9 (M=Si, Ge) fluorescent material, and utilizing a silicate/germanate structure as the matrix, a red fluorescent material with good chemical stability, low cost, and narrow-band emission was synthesized by high-temperature solid-state method. Eu3+ preferentially replaces In3+ without changing the crystal structure of the matrix material.
It achieves high color purity, narrow-band red light emission, significantly enhanced luminous intensity, and millisecond-level fluorescence lifetime, making it suitable for high-performance red LED devices. It also exhibits good thermal and chemical stability, making it suitable for both red and deep red LED devices.
Smart Images

Figure CN120865910A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of rare earth luminescent materials, specifically to a europium ion-doped borosilicate / borogermanate red fluorescent material, which has advantages such as high color purity, narrow-band emission, and high thermal stability, and is suitable for solid-state lighting, display devices, and fluorescent probes. Background Technology
[0002] Rare earth ion-doped fluorescent materials, as a core component of solid-state lighting and display technologies, have undergone decades of development and have formed a Ce-based... 3+ Eu 2+ / Eu 3+ Mn 4+ A system dominated by activated ions. Among them, Eu... 3+ As a typical rare earth activated ion, it relies on its 5 D0→ 9 F j The high-purity red light produced during the transition makes Eu... 3+ Doped phosphors are widely used in high color rendering index LED devices and full-color displays. Currently, the most widely used red phosphors include sulfides (such as Y₂O₂S:Eu). 3+ ), nitrides (such as CaAlSiN3:Eu) 2+ ) and fluorides (such as K2SiF6:Mn 4+ These materials, such as sulfide materials, have their own advantages, but also many limitations: sulfide materials have high raw material costs, poor thermal stability, and are prone to moisture absorption, leading to device lifespan degradation; nitride materials have complex synthesis processes and high synthesis temperatures; and fluorides are sensitive to humidity and have demanding synthesis processes. Therefore, developing novel red fluorescent materials with strong chemical stability, good thermal stability, high color purity, and low preparation cost has become a research hotspot in the field of fluorescent materials.
[0003] Silicates, germanates, and other oxyacid salts have become widely studied novel matrix materials due to their rich structural tunability, good thermal stability, environmentally friendly properties, and inexpensive raw materials. 3+ The combination with silicate and germanate matrices provides a new approach for the development of low-cost, high-stability red fluorescent materials. The layered, chain-like, or three-dimensional network structures formed by [SiO4] / [GeO4] tetrahedra in silicate and germanate matrices can modulate the Eu... 3+ Local coordination environment, enhancing Eu 3+ of 5 D0→ 7 F j Electric dipole transitions improve red light luminescence efficiency. Currently, although some research has begun to focus on the luminescence properties of such materials, in Eu... 3+There are still many challenges in optimizing doping concentration, controlling the spectrum, and regulating thermal stability. There is an urgent need to develop a new type of red fluorescent material with high red light emission intensity, long lifetime, high color purity and suitable for ultraviolet light excitation, as well as its controllable preparation method, to meet the application requirements of the next generation of high-performance full-spectrum LED devices. Summary of the Invention
[0004] In view of this, the present invention provides an Eu 3+ Doped Ba₂InBM₂O₉ (M = Si, Ge) red fluorescent material utilizes its stable silicate / germanate structure as a matrix, through Eu... 3+ Doping enables efficient narrowband red light emission. Under 395nm ultraviolet light excitation, this fluorescent material exhibits typical red light emission with an emission peak at 616nm and deep red light emission with an emission peak at 707nm. It also has good thermal and chemical stability, making it suitable for red light-emitting devices and deep red LED devices.
[0005] The first aspect of this invention aims to provide a europium ion-doped borosilicate / germanate red fluorescent material with the chemical formula: Ba2InBM2O9:xEu 3+ Where M is Si or Ge, and x is Eu 3+ Molar doping concentration, ranging from 1 to 15 mol%.
[0006] More preferably, x takes values of 1%, 3%, 5%, 7%, 9%, 11%, 13%, and 15%.
[0007] In some specific embodiments of the present invention, the molecular formula of the fluorescent material is: Ba2InBGe2O9:1mol%Eu 3+ Ba2InBGe2O9:3mol%Eu 3+ Ba2InBGe2O9:5mol%Eu 3+ Ba2InBGe2O9:7mol%Eu 3+ Ba2InBGe2O9:9mol%Eu 3+ Ba2InBGe2O9:11mol%Eu 3+ Ba2InBGe2O9:13mol%Eu 3+ Ba2InBGe2O9:15mol%Eu 3+ Ba2InBSi2O9: 1mol%Eu 3+ Ba2InBSi2O9:3mol%Eu 3+ Ba2InBSi2O9:5mol%Eu 3+ Ba2InBSi2O9:7mol%Eu 3+Ba2InBSi2O9:9mol%Eu 3+ Ba2InBSi2O9:11mol%Eu 3+ Ba2InBSi2O9:13mol%Eu 3+ Ba2InBSi2O9:15mol%Eu 3+ .
[0008] The Eu provided by this invention 3+ The doped Ba₂InBM₂O₉ fluorescent material, based on a silicon / germanate structure, is synthesized using a high-temperature solid-state method and possesses advantages such as good chemical stability, low cost, narrow-band emission, and strong luminescence. When excited at 395 nm, the fluorescent material emits red / deep red light with center wavelengths of 616 nm and 707 nm. The full width at half maximum (FWHM) of the 616 nm main peak is only 10.83 nm, and that of the 707 nm main peak is only 4.76 nm, exhibiting typical narrow-band red light emission characteristics.
[0009] A second aspect of this invention provides a method for preparing europium ion-doped borosilicate / germanate red fluorescent materials, the method comprising:
[0010] Raw materials were weighed according to the molar ratio of each element in the general chemical formula Ba:In:B:Si / Ge:Eu=2:(1–x):1:2:x; among them, barium-containing compounds, indium-containing compounds, boron-containing compounds, silicon / germanium-containing compounds and europium-containing compounds were uniformly mixed and thoroughly ground according to the stoichiometric ratio, placed in a muffle furnace, pre-calcined at low temperature to remove moisture and gas from the raw materials, and then calcined at high temperature. During the process, the materials were taken out and ground multiple times to finally obtain europium ion-doped borosilicate / germanium salt red fluorescent material.
[0011] Preferably, the barium-containing compound is at least one of barium oxide, barium hydroxide, or a barium salt; more preferably, the barium salt includes at least one of barium carbonate, barium chloride, barium nitrate, barium bicarbonate, barium sulfate, and barium oxalate.
[0012] Preferably, the indium-containing compound is at least one of indium oxide, indium hydroxide, or an indium salt; more preferably, the indium salt includes at least one of indium nitrate, indium chloride, indium sulfate, and indium acetate.
[0013] Preferably, the boron-containing compound is at least one of boron oxide, boron hydroxide, or borates; more preferably, the borates include at least one of boric acid, sodium metaborate, sodium tetraborate, and zinc borate.
[0014] Preferably, the silicon-containing compound is at least one of silicon oxide or a silicon salt; more preferably, the silicon salt includes at least one of silicon chloride and silicon bromide.
[0015] Preferably, the germanium-containing compound is at least one of germanium oxide, germanium hydroxide, or a germanium salt; more preferably, the germanium salt includes at least one of germanium dioxide, germanium chloride, germanium nitrate, and germanium acetate.
[0016] Preferably, the europium-containing compound is at least one of europium oxide, europium hydroxide, or a europium salt; more preferably, the europium salt includes at least one of europium nitrate, europium chloride, europium sulfate, europium acetate, europium carbonate, and europium oxalate.
[0017] Preferably, the apparatus for multiple grinding is an agate mortar and pestle.
[0018] Preferably, the preheating temperature is 200 to 500°C; including but not limited to 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, or a range of the above values as the lower or upper limit.
[0019] Preferably, the pre-burning time is 0.5h to 24d, including but not limited to 0.5h, 1h, 6h, 12h, 24h, 1d, 7d, 14d or 24d, or a range with the above values as the lower or upper limit.
[0020] Preferably, the calcination temperature is 800-1400℃, including but not limited to 800℃, 900℃, 1000℃, 1050℃, 1100℃, 1050℃, 1200℃, 1300℃, and 1400℃; more preferably, it is 1000-1200℃, or a range with the above values as the lower or upper limit.
[0021] Preferably, the calcination time is 0.5h to 30d; including but not limited to 0.5h, 1h, 6h, 12h, 24h, 1d, 7d, 14d or 30d, or a range with the above values as the lower or upper limit.
[0022] The entire preparation process of this invention can be completed in an air atmosphere without the need for a protective gas, making it suitable for industrial scale-up production.
[0023] Preferably, the apparatus for both pre-firing and calcining is a platinum crucible.
[0024] Europium ion-doped borosilicate / germanate red fluorescent material obtained by the method described in this invention, Eu 3+ Prioritize replacing In 3+ Since the ionic radii of the two are similar (the difference is only 1.07%, which meets the substitution condition), doping does not change the crystal structure of the matrix material and has good chemical stability. At the same time, substitution doping can avoid structural defects caused by lattice mismatch.
[0025] The europium ion-doped borosilicate / germanate red fluorescent material obtained by the method described in this invention exhibits excellent optical properties. After doping, the red light emission (616 nm) and deep red light emission (707 nm) are significantly enhanced. The excitation spectrum shows a sharp peak shape, with a full width at half maximum (FWHM) of only 9.09 nm for the 395 nm main peak, indicating high color purity. The main peaks (616 nm and 707 nm) in the emission spectrum have narrow band characteristics, with color purity >90%.
[0026] The europium ion-doped borosilicate / germanate red fluorescent material obtained by the method described in this invention exhibits tunable luminescence behavior, which can be achieved by controlling the Eu ion doping behavior. 3+ The doping concentration can be adjusted to control the emission intensity of red light (616nm) and deep red light (707nm);
[0027] The europium ion-doped borosilicate / germanate red fluorescent material obtained by the method described in this invention can effectively address the fluorescence quenching problem, with the highest luminescence intensity reaching its peak at 9 mol%.
[0028] The europium ion-doped borosilicate / germanate red fluorescent material obtained by the method described in this invention achieves a fluorescence lifetime in the millisecond range. 3+ When the doping concentration is 9 mol%, the fluorescence lifetime of Ba2InBGe2O9 is 1.67 ms and that of Ba2InBSi2O9 is 2.11 ms; these meet the slow decay requirements of lighting devices and are beneficial for improving luminous efficiency and device stability.
[0029] The europium ion-doped borosilicate / germanate red fluorescent material obtained by the method described in this invention uses inexpensive and readily available raw materials, has a controllable process, and is environmentally friendly; the synthesis process is clear and stable, and does not require high pressure or hazardous chemical atmosphere.
[0030] The europium ion-doped borosilicate / germanate obtained by the method of this invention has good application prospects as a high-color-purity red luminescent material in optoelectronic fields such as white LED devices, backlights and full-color displays, laser lighting, plant lighting or fluorescent probes. Attached Figure Description
[0031] Figure 1 The red fluorescent material BIBMO:xEu prepared in this invention 3+ XRD patterns of (x = 1–15 mol%);
[0032] Figure 2 The red fluorescent material BIBMO:xEu prepared in this invention 3+ Emission spectra of (x = 1–15 mol%) under 395 nm excitation and excitation spectra under 616 nm emission;
[0033] Figure 3The red fluorescent material BIBMO:xEu prepared in this invention 3+ Color coordinate diagram of (x = 1–15 mol%);
[0034] Figure 4 The red fluorescent material BIBMO prepared for this invention: 9 mol% Eu 3+ The fluorescence decay curve and calculated fluorescence lifetime;
[0035] Figure 5 The red fluorescent material BIBMO prepared for this invention: 15 mol% Eu 3+ SEM images and distribution maps of each element. Detailed Implementation
[0036] The present invention will now be described in detail with reference to the accompanying drawings and embodiments, but is not limited to the embodiments described herein. Any improvements and variations made based on the present invention are within the scope of protection of the present invention.
[0037] Example 1:
[0038] This embodiment provides two high-color-purity, narrow-band red fluorescent materials, and the specific preparation methods are as follows:
[0039] BaCO3, In2O3, H3BO3, SiO2 / GeO2, and Eu2O3 raw materials with a molar ratio of 4:0.99:2:4:0.01 were placed in an agate mortar, mixed evenly, and ground for about 10 minutes. The mixture was then placed in a platinum crucible and pre-calcined at 400°C for 6 hours. The pre-calcined sample was then removed, ground and mixed again, and placed in a platinum crucible for further calcination at 1200°C for 6 hours. The sample was then cooled to room temperature with the furnace.
[0040] The obtained sintered body is ground into powder to obtain a product with the chemical composition Ba2InBSi2O9:1mol%Eu. 3+ Ba2InBGe2O9:1mol%Eu 3+ Red fluorescent material.
[0041] Example 2:
[0042] This embodiment provides two high-color-purity, narrow-band red fluorescent materials, and the specific preparation methods are as follows:
[0043] BaCO3, In2O3, H3BO3, SiO2 / GeO2, and Eu2O3 raw materials with a molar ratio of 4:0.97:2:4:0.03 were placed in an agate mortar, mixed evenly, and ground for about 10 minutes. The mixture was then placed in a platinum crucible and pre-calcined at 400°C for 6 hours. The pre-calcined sample was then removed, ground and mixed again, and placed in a platinum crucible for further calcination at 1200°C for 12 hours. The sample was then cooled to room temperature in the furnace.
[0044] The sintered body is ground into powder to obtain a product with the chemical composition Ba2InBSi2O9:3mol%Eu. 3+ Ba2InBGe2O9:3mol%Eu 3+ Red fluorescent material.
[0045] Example 3:
[0046] This embodiment provides two high-color-purity, narrow-band red fluorescent materials, and the specific preparation methods are as follows:
[0047] BaCO3, In2O3, H3BO3, SiO2 / GeO2, and Eu2O3 raw materials with a molar ratio of 4:0.95:2:4:0.05 were placed in an agate mortar, mixed evenly, and ground for about 10 minutes. The mixture was then placed in a platinum crucible and pre-calcined at 400°C for 6 hours. The pre-calcined sample was then removed, ground and mixed again, and placed in a platinum crucible for further calcination at 1200°C for 6 hours. The sample was then cooled to room temperature in the furnace.
[0048] The sintered body is ground into powder to obtain a product with the chemical composition Ba2InBSi2O9:5mol%Eu. 3+ Ba2InBGe2O9:5mol%Eu 3+ Red fluorescent material.
[0049] Example 4:
[0050] This embodiment provides two high-color-purity, narrow-band red fluorescent materials, and the specific preparation methods are as follows:
[0051] BaCO3, In2O3, H3BO3, SiO2 / GeO2, and Eu2O3 raw materials with a molar ratio of 4:0.93:2:4:0.07 were placed in an agate mortar, mixed evenly, and ground for about 10 minutes. The mixture was then placed in a platinum crucible and pre-calcined at 400°C for 12 hours. The pre-calcined sample was then removed, ground and mixed again, and placed in a platinum crucible for further calcination at 1200°C for 12 hours. The sample was then cooled to room temperature with the furnace.
[0052] The sintered body is ground into powder to obtain a product with the chemical composition Ba2InBSi2O9:7mol%Eu. 3+ Ba2InBGe2O9:7mol%Eu 3+ Red fluorescent material.
[0053] Example 5:
[0054] This embodiment provides two high-color-purity, narrow-band red fluorescent materials, and the specific preparation methods are as follows:
[0055] BaCO3, In2O3, H3BO3, SiO2 / GeO2, and Eu2O3 raw materials with a molar ratio of 4:0.91:2:4:0.09 were placed in an agate mortar, mixed evenly, and ground for about 10 minutes. The mixture was then placed in a platinum crucible and pre-fired at 400°C for 6 hours. The pre-fired sample was then removed, ground and mixed again, and placed in a platinum crucible. It was then calcined at 1200°C for 12 hours and cooled to room temperature with the furnace.
[0056] The sintered body is ground into powder to obtain a product with the chemical composition Ba2InBSi2O9:9mol%Eu. 3+ Ba2InBGe2O9:9mol%Eu 3+ Red fluorescent material.
[0057] Example 6:
[0058] This embodiment provides two high-color-purity, narrow-band red fluorescent materials, and the specific preparation methods are as follows:
[0059] BaCO3, In2O3, H3BO3, SiO2 / GeO2, and Eu2O3 raw materials with a molar ratio of 4:0.89:2:4:0.11 were placed in an agate mortar, mixed evenly, and ground for about 10 minutes. The mixture was then placed in a platinum crucible and pre-calcined at 400°C for 12 hours. The pre-calcined sample was then removed, ground and mixed again, and placed in a platinum crucible for further calcination at 1200°C for 12 hours. The sample was then cooled to room temperature with the furnace.
[0060] The sintered body is ground into powder to obtain a product with the chemical composition Ba2InBSi2O9:11mol%Eu. 3+ Ba2InBGe2O9:11mol%Eu 3+ Red fluorescent material.
[0061] Example 7:
[0062] This embodiment provides two high-color-purity, narrow-band red fluorescent materials, and the specific preparation methods are as follows:
[0063] BaCO3, In2O3, H3BO3, SiO2 / GeO2, and Eu2O3 raw materials with a molar ratio of 4:0.87:2:4:0.13 were placed in an agate mortar, mixed evenly, and ground for about 10 minutes. The mixture was then placed in a platinum crucible and pre-calcined at 400°C for 12 hours. The pre-calcined sample was then removed, ground and mixed again, and placed in a platinum crucible for further calcination at 1200°C for 12 hours. The sample was then cooled to room temperature with the furnace.
[0064] The sintered body is ground into powder to obtain a product with the chemical composition Ba2InBSi2O9:13mol%Eu.3+ Ba2InBGe2O9:13mol%Eu 3+ Red fluorescent material.
[0065] Example 8:
[0066] This embodiment provides two high-color-purity, narrow-band red fluorescent materials, and the specific preparation methods are as follows:
[0067] BaCO3, In2O3, H3BO3, SiO2 / GeO2, and Eu2O3 raw materials with a molar ratio of 4:0.85:2:4:0.15 were placed in an agate mortar, mixed evenly, and ground for about 10 minutes. The mixture was then placed in a platinum crucible and pre-calcined at 400°C for 6 hours. The pre-calcined sample was then removed, ground and mixed again, and placed in a platinum crucible for further calcination at 1200°C for 12 hours. The sample was then cooled to room temperature with the furnace.
[0068] The sintered body is ground into powder to obtain a product with the chemical composition Ba2InBSi2O9:15mol%Eu. 3+ Ba2InBGe2O9:15mol%Eu 3+ Red fluorescent material.
[0069] Example 9:
[0070] The only difference between this embodiment and Example 1 is that the barium source compound is barium oxide; all other conditions and parameters are exactly the same as in Example 1.
[0071] Example 10:
[0072] The only difference between this embodiment and Example 1 is that the barium source compound is barium hydroxide; all other conditions and parameters are exactly the same as in Example 1.
[0073] Example 11:
[0074] The only difference between this embodiment and Example 1 is that the barium source compound is barium chloride; all other conditions and parameters are exactly the same as in Example 1.
[0075] Example 12:
[0076] The only difference between this embodiment and Example 1 is that the barium source compound is barium nitrate; all other conditions and parameters are exactly the same as in Example 1.
[0077] Example 13:
[0078] The only difference between this embodiment and Example 1 is that the barium source compound is barium bicarbonate; all other conditions and parameters are exactly the same as in Example 1.
[0079] Example 14:
[0080] The only difference between this embodiment and Example 1 is that the barium source compound is barium sulfate; all other conditions and parameters are exactly the same as in Example 1.
[0081] Example 15:
[0082] The only difference between this embodiment and Example 1 is that the indium source compound is indium hydroxide; all other conditions and parameters are exactly the same as in Example 1.
[0083] Example 16:
[0084] The only difference between this embodiment and Example 1 is that the indium source compound is indium nitrate; all other conditions and parameters are exactly the same as in Example 1.
[0085] Example 17:
[0086] The only difference between this embodiment and Example 1 is that the indium source compound is indium chloride; all other conditions and parameters are exactly the same as in Example 1.
[0087] Example 18:
[0088] The only difference between this embodiment and Example 1 is that the indium source compound is indium sulfate; all other conditions and parameters are exactly the same as in Example 1.
[0089] Example 19:
[0090] The only difference between this embodiment and Example 1 is that the indium source compound is indium acetate; all other conditions and parameters are exactly the same as in Example 1.
[0091] Example 20:
[0092] The only difference between this embodiment and Example 1 is that the boron source compound is boron oxide; all other conditions and parameters are exactly the same as in Example 1.
[0093] Example 21:
[0094] The only difference between this embodiment and Example 1 is that the boron source compound is boron hydroxide; all other conditions and parameters are exactly the same as in Example 1.
[0095] Example 22:
[0096] The only difference between this embodiment and Example 1 is that the boron source compound is sodium metaborate; all other conditions and parameters are exactly the same as in Example 1.
[0097] Example 23:
[0098] The only difference between this embodiment and Embodiment 1 is that the silicon source compound is silicon chloride; all other conditions and parameters are exactly the same as in Embodiment 1.
[0099] Example 24:
[0100] The only difference between this embodiment and Embodiment 1 is that the silicon source compound is silicon bromide; all other conditions and parameters are exactly the same as in Embodiment 1.
[0101] Example 25:
[0102] The only difference between this embodiment and Embodiment 1 is that the germanium source compound is germanium hydroxide; all other conditions and parameters are exactly the same as in Embodiment 1.
[0103] Example 26:
[0104] The only difference between this embodiment and Embodiment 1 is that the germanium source compound is germanium chloride; all other conditions and parameters are exactly the same as in Embodiment 1.
[0105] Example 26:
[0106] The only difference between this embodiment and Example 1 is that the germanium source compound is germanium nitrate; all other conditions and parameters are exactly the same as in Example 1.
[0107] Example 27:
[0108] The only difference between this embodiment and Embodiment 1 is that the germanium source compound is germanium acetate; all other conditions and parameters are exactly the same as in Embodiment 1.
[0109] Example 28:
[0110] The only difference between this embodiment and Example 1 is that the europium source compound is europium hydroxide; all other conditions and parameters are exactly the same as in Example 1.
[0111] Example 29:
[0112] The only difference between this embodiment and Example 1 is that the europium source compound is europium nitrate; all other conditions and parameters are exactly the same as in Example 1.
[0113] Example 30:
[0114] The only difference between this embodiment and Example 1 is that the europium source compound is europium chloride; all other conditions and parameters are exactly the same as in Example 1.
[0115] Example 31:
[0116] The only difference between this embodiment and Example 1 is that the europium source compound is europium nitrate; all other conditions and parameters are exactly the same as in Example 1.
[0117] Example 32:
[0118] The only difference between this embodiment and Example 1 is that the europium source compound is europium sulfate; all other conditions and parameters are exactly the same as in Example 1.
[0119] Example 33:
[0120] The only difference between this embodiment and Example 1 is that the europium source compound is europium acetate; all other conditions and parameters are exactly the same as in Example 1.
[0121] Example 34:
[0122] The only difference between this embodiment and Embodiment 1 is that the europium source compound is europium carbonate; all other conditions and parameters are exactly the same as in Embodiment 1.
[0123] Performance testing:
[0124] Take the narrowband red fluorescent material Ba2InBGe2O9 prepared in Examples 1-8: 1 mol% Eu 3+ Ba2InBGe2O9:3mol%Eu 3+ Ba2InBGe2O9:5mol%Eu 3+ Ba2InBGe2O9:7mol%Eu 3+ Ba2InBGe2O9:9mol%Eu 3+ Ba2InBGe2O9:11mol%Eu 3+ Ba2InBGe2O9:13mol%Eu 3+ Ba2InBGe2O9:15mol%Eu 3+ Ba2InBSi2O9: 1mol%Eu 3+ Ba2InBSi2O9:3mol%Eu 3+ Ba2InBSi2O9:5mol%Eu 3+ Ba2InBSi2O9:7mol%Eu 3+ Ba2InBSi2O9:9mol%Eu 3+ Ba2InBSi2O9:11mol%Eu 3+ Ba2InBSi2O9:13mol%Eu 3+ Ba2InBSi2O9:15mol%Eu 3+ The powder was subjected to X-ray diffraction testing, and the test results are as follows: Figure 1 As shown, Eu 3+ The doping of Eu has almost no effect on the phase purity of the Ba2InBM2O9 host material. Therefore, it can be inferred that Eu 3+ It almost completely enters the main lattice of Ba2InBM2O9.
[0125] Take the narrowband red fluorescent material Ba2InBGe2O9 prepared in Examples 1-8: 1 mol% Eu 3+ Ba2InBGe2O9:3mol%Eu 3+ Ba2InBGe2O9:5mol%Eu 3+ Ba2InBGe2O9:7mol%Eu 3+ Ba2InBGe2O9:9mol%Eu 3+ Ba2InBGe2O9:11mol%Eu 3+ Ba2InBGe2O9:13mol%Eu 3+ Ba2InBGe2O9:15mol%Eu 3+ Ba2InBSi2O9: 1mol%Eu 3+ Ba2InBSi2O9:3mol%Eu 3+ Ba2InBSi2O9:5mol%Eu 3+ Ba2InBSi2O9:7mol%Eu 3+ Ba2InBSi2O9:9mol%Eu 3+ Ba2InBSi2O9:11mol%Eu 3+ Ba2InBSi2O9:13mol%Eu 3+ Ba2InBSi2O9:15mol%Eu 3+ Powder luminescence properties study, such as Figure 2 As shown, by Figure 2 It can be seen that BIBGO and BIBSO phosphor materials exhibit typical narrow-band emission characteristics, possessing: excellent excitation-emission matching; tunable red and deep red light output; high color purity and narrow spectral width; and extremely low excitation-emission overlap. They are highly suitable for high-performance red LED devices, backlights, and full-color display systems.
[0126] Take the narrowband red fluorescent material Ba2InBGe2O9 prepared in Examples 1-8: 1 mol% Eu 3+ Ba2InBGe2O9:3mol%Eu 3+ Ba2InBGe2O9:5mol%Eu 3+ Ba2InBGe2O9:7mol%Eu 3+ Ba2InBGe2O9:9mol%Eu 3+ Ba2InBGe2O9:11mol%Eu 3+ Ba2InBGe2O9:13mol%Eu 3+Ba2InBGe2O9:15mol%Eu 3+ Ba2InBSi2O9: 1mol%Eu 3+ Ba2InBSi2O9:3mol%Eu 3+ Ba2InBSi2O9:5mol%Eu 3+ Ba2InBSi2O9:7mol%Eu 3+ Ba2InBSi2O9:9mol%Eu 3+ Ba2InBSi2O9:11mol%Eu 3+ Ba2InBSi2O9:13mol%Eu 3+ Ba2InBSi2O9:15mol%Eu 3+ The powder was used to test the color purity and fluorescence lifetime of fluorescent materials, such as... Figure 3 and Figure 4 As shown, by Figure 3 and Figure 4 It can be seen that this series of Eu 3+ Doped fluorescent materials possess: extremely high red light purity (>90%); reasonable fluorescence lifetime (reaching the millisecond level); suitable for use as high color purity red light emitting materials, and have good application prospects in optoelectronic fields such as white LEDs, displays, and lasers.
[0127] Take the narrowband red fluorescent material Ba2InBGe2O9 prepared in Examples 1-8: 1 mol% Eu 3+ Ba2InBGe2O9:3mol%Eu 3+ Ba2InBGe2O9:5mol%Eu 3+ Ba2InBGe2O9:7mol%Eu 3+ Ba2InBGe2O9:9mol%Eu 3+ Ba2InBGe2O9:11mol%Eu 3+ Ba2InBGe2O9:13mol%Eu 3+ Ba2InBGe2O9:15mol%Eu 3+ Ba2InBSi2O9: 1mol%Eu 3+ Ba2InBSi2O9:3mol%Eu 3+ Ba2InBSi2O9:5mol%Eu 3+ Ba2InBSi2O9:7mol%Eu 3+ Ba2InBSi2O9:9mol%Eu 3+ Ba2InBSi2O9:11mol%Eu 3+Ba2InBSi2O9:13mol%Eu 3+ Ba2InBSi2O9:15mol%Eu 3+ The powder was subjected to SEM-EDS testing, such as... Figure 5 The results showed that the prepared Eu 3+ Doped BIBGO and BIBSO fluorescent materials exhibit good particle morphology; high purity and no impurities; Eu 3+ The dopant elements are evenly distributed. This provides structural assurance in terms of morphology and composition for its excellent optical properties, and further verifies the controllability and effectiveness of the material synthesis process.
[0128] The above embodiments are merely illustrative of the method and basic concept of the present invention. Based on the above embodiments, the pre-calcination conditions in the preparation method of the present invention can be selected within the range of temperature 200–500℃ and holding time 0.5h–24d, while the continued calcination conditions can be selected within the range of temperature 800–1400℃ and holding time 0.5h–30d, with the same effect as the above embodiments. It should be emphasized that those skilled in the art can make various optimizations and adjustments without departing from the basic spirit of the present invention, and these modifications and improvements should also be considered as the content protected by the present invention.
Claims
1. A europium ion-doped borosilicate / germanate red fluorescent material, characterized in that, The general chemical formula of the fluorescent material is Ba2InBM2O9:xEu 3+ Where: B is boron; M is silicon or germanium; x is Eu3. + The mole fraction satisfies 1%mol≤x≤15%mol.
2. The method for preparing europium ion-doped borosilicate / germanate red fluorescent material according to claim 1, characterized in that, Includes the following steps: (1) Weigh the raw materials according to the stoichiometric ratio Ba:In:B:M:Eu=2:(1–x):1:2:x. The raw materials include barium source compounds, indium source compounds, boron source compounds, silicon source or germanium source compounds and europium source compounds. After mixing and grinding evenly, a raw material mixture is formed. (2) The mixture obtained in step (1) is pre-calcined at a temperature of 200-500℃ for 0.5h-24d to remove volatile impurities, and then ground again to obtain the intermediate product. (3) The intermediate product is sintered at high temperature in air atmosphere at 800-1400℃ for 0.5h-30d, and then ground after cooling to obtain the target phosphor.
3. The preparation method according to claim 2, characterized in that: The calcination process is carried out in an air atmosphere or a weak oxidizing atmosphere, without the need for a reducing protective atmosphere.
4. The preparation method according to claim 2, characterized in that: The barium source compound is selected from one or more of the following: oxides, hydroxides, sulfates, carbonates, nitrates, oxalates, citrates, or acetates containing the element Ba. The indium source compound is selected from one or more of oxides, hydroxides, chlorides, sulfates, nitrates or acetates containing the element In; The boron source compound is selected from one or more of boron oxide, boron hydroxide, boric acid, sodium metaborate, sodium tetraborate, and zinc borate; The silicon source compound is selected from one or more of silicon oxide, silicic acid, silicon chloride, and silicon bromide; The germanium source compound is selected from one of germanium oxide, germanium hydroxide, germanium dioxide, germanium chloride, germanium nitrate, and germanium acetate. The europium source compound is selected from one or more of the following: oxides, hydroxides, chlorides, sulfates, nitrates, carbonates, oxalates, or acetates containing the element Eu.
5. The preparation method according to claim 2, characterized in that: The preheating temperature is 200℃, 250℃, 300℃, 350℃, 400℃, 450℃ or 500℃, and the heat preservation time is 0.5h, 1h, 6h, 12h, 24h, 1d, 7d, 14d or 24d.
6. The preparation method according to claim 2, characterized in that: The calcination temperature is 800℃, 900℃, 1000℃, 1050℃, 1100℃, 1150℃, 1200℃, 1300℃ or 1400℃, and the heat preservation time is 0.5h, 1h, 6h, 12h, 24h, 1d, 7d, 14d or 30d.
7. The use of the europium ion-doped borosilicate / germanate red fluorescent material according to claim 1, characterized in that: This material is used in white LED packaging, red backlight displays, laser lighting, plant lighting, or fluorescent marking.