Low-friction shock absorber oil seal and preparation method thereof
By adopting a ternary rubber system and specific additives, and optimizing the process flow, a low-friction damper oil seal was prepared, which solved the problems of insufficient wear resistance and high temperature resistance of traditional oil seals, and achieved higher tensile strength, wear resistance and high temperature resistance, while reducing frictional resistance.
Patent Information
- Application Number
- CN202511072770.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-01
- Publication Date
- 2025-11-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional oil seal materials suffer from insufficient wear resistance, poor high-temperature resistance, and high frictional resistance, which limits their application in high-performance equipment.
Low-friction damper oil seals are prepared by using a ternary rubber system (acrylate rubber, neoprene rubber, and polytetrafluoroethylene modified rubber) and combining it with nano-grade silica, montmorillonite, carbon fiber, and polytetrafluoroethylene coating, through optimized mixing, molding, and vulcanization processes.
It improves the tensile strength, elongation at break, wear resistance and high temperature resistance of oil seals, reduces frictional resistance, and enhances sealing performance and service life.
Smart Images

Figure CN120904610A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of shock absorber oil seals, in particular to a low-friction shock absorber oil seal and a preparation method thereof. BACKGROUND
[0002] In modern industry, oil seals are critical sealing components widely used in rotating shafts and reciprocating parts of various machines and equipment to prevent lubricating oil leakage and external impurities intrusion. The performance of oil seals directly affects the operating efficiency and service life of mechanical equipment. However, traditional oil seal materials have problems such as insufficient wear resistance, poor high-temperature resistance, and large frictional resistance, limiting their application in high-performance equipment. To solve these problems, the present application method uses various reinforcing materials and methods to improve the performance of the oil seal. For example, by adding nano-sized white carbon black and montmorillonite to enhance the reinforcing effect and sealing performance of the material; using surface oxidation treatment carbon fiber and spraying polytetrafluoroethylene coating to reduce frictional resistance and enhance wear resistance and self-lubricating properties; optimizing mixing, molding, and vulcanization processes to ensure uniform dispersion and chemical bonding of each component, thereby improving production efficiency and product quality. SUMMARY
[0003] In view of the deficiencies of the prior art, the present application provides a low-friction shock absorber oil seal and a preparation method thereof, which have excellent wear resistance, excellent high-temperature resistance, and low frictional resistance, solving the problems of insufficient wear resistance, poor high-temperature resistance, and large frictional resistance of traditional oil seal materials.
[0004] To achieve the above-mentioned purpose, the present application provides the following technical solution: a low-friction shock absorber oil seal, the raw materials and their weight ranges of the oil seal are as follows: acrylate rubber 36-40 parts; chlorobutyl rubber 25-28 parts; polytetrafluoroethylene modified rubber 12-16 parts; nano-sized white carbon black 4-6 parts; carbon fiber 2-5 parts; clay 3-6 parts; aluminum alloy 1-3 parts; montmorillonite 1.15-1.60 parts; sodium stearate / potassium stearate 0.4-0.9 parts; molybdenum disulfide 0.6-0.9 parts; surfactant 0.3-0.6 parts; antioxidant 0.2-0.4 parts; vulcanizing agent 0.15-0.33 parts; coupling agent 0.2-0.3 parts.
[0005] Preferably, the raw materials and their weights of the oil seal are as follows: acrylate rubber 38 parts; chlorobutyl rubber 28 parts; polytetrafluoroethylene modified rubber 13 parts; nano-sized white carbon black 5 parts; carbon fiber 4 parts; clay 5 parts; aluminum alloy 2 parts; montmorillonite 1.2 parts; sodium stearate / potassium stearate 0.6 parts; molybdenum disulfide 0.7 parts; surfactant 0.4 parts; antioxidant 0.25 parts; vulcanizing agent 0.25 parts; coupling agent 0.22 parts.
[0006] Preferably, the raw materials of the oil seal and the weight parts thereof are as follows: acrylate rubber 40 parts; chlorobutyl rubber 28 parts; polytetrafluoroethylene modified rubber 13 parts; nano-sized white carbon black 6 parts; carbon fiber 2 parts; clay 6 parts; aluminum alloy 3 parts; montmorillonite 1.5 parts; sodium stearate / potassium stearate 0.4 parts; molybdenum disulfide 0.6 parts; surfactant 0.6 parts; antioxidant 0.2 parts; vulcanizing agent 0.30 parts; coupling agent 0.28 parts.
[0007] Preferably, the particle size of the polytetrafluoroethylene modified rubber is ≤5μm, and the specific surface area of the nano-sized white carbon black is ≥200m² / g.
[0008] Preferably, the length of the carbon fiber is between 1-2mm, and the clay is calcined kaolin.
[0009] A preparation method of a low-friction shock absorber oil seal, comprising the following steps: Step one, raw material preparation: prepare the formula weight parts of acrylate rubber, chlorobutyl rubber, polytetrafluoroethylene modified rubber, nano-sized white carbon black, carbon fiber, clay, aluminum alloy, montmorillonite, sodium stearate / potassium stearate, molybdenum disulfide, surfactant, antioxidant, vulcanizing agent and coupling agent; Step two, raw material pretreatment: premix the white carbon black, montmorillonite and coupling agent, and perform surface oxidation treatment on the carbon fiber; Step three, mixing: put the acrylate rubber, chlorobutyl rubber and polytetrafluoroethylene modified rubber into the internal mixer, mix at a temperature of 95-100℃ and a speed of 50-60r / min for 5-7min, then add the premixed white carbon black, montmorillonite and coupling agent, increase the temperature of the internal mixer to 135-140℃, continue mixing for 10-15min, then add the stearate and antioxidant in turn, control the temperature of the internal mixer at 110-115℃, mix for 5-6min, then add the carbon fiber and clay after surface oxidation treatment, keep the temperature of the internal mixer at 110-115℃, mix for 8-10min, finally add the vulcanizing agent and molybdenum disulfide, continue mixing at a temperature of 80-95℃ for 3-5min, to obtain the mixed rubber; Step four, molding: put the mixed rubber into the pretreated mold, process the mold by injection molding process, set the pressure to 10-15MPa, the temperature to 165-170℃, and the molding time to 5-10min, cool for 1-2h, to obtain the molded oil seal; Step five, vulcanization: the formed oil seal is placed in the vulcanization equipment, and two vulcanization treatments are carried out, the first vulcanization is carried out at a temperature of 155-160℃, preheating for 3-5min, continuing to heat to 170-175℃, controlling the vulcanization pressure to be greater than or equal to 10MPa, and the vulcanization time is 8-10min, the second vulcanization temperature is 145-150℃, and the vulcanization time is 1.5-2h; Step six, post-treatment: after the vulcanization is completed, the oil seal is taken out from the vulcanization equipment, cooled and demolded, a polytetrafluoroethylene coating with a thickness of 0.01mm-0.05mm is sprayed on the surface of the oil seal, and finally the oil seal after coating is cleaned and dried; Step seven, quality detection: the dried oil seal is subjected to size precision, surface quality and vulcanization degree test.
[0010] Preferably, the white carbon black, the montmorillonite and the coupling agent are premixed, the montmorillonite and the white carbon black are sequentially added to the coupling agent, and stirring is carried out at a rotating speed of 200-300r / min for 10-15min, and then standing for 15-20min.
[0011] Preferably, the carbon fiber is short-cut to 1-2mm in length, and then placed in a temperature environment of 400-450℃, air is introduced, and oxidation is carried out for 10-15min.
[0012] Preferably, the mold is pretreated: the mold is soaked in a phosphate solution with a concentration of 5%-10% for 30-60min, so that a phosphating film is formed on the surface of the mold.
[0013] Preferably, the oil seal is verified before installation: 4000-5000 cycles of simulated installation test are carried out, and the oil seal leakage is less than or equal to 0.1mL / h.
[0014] Compared with the prior art, the present application provides a low-friction shock absorber oil seal and a preparation method thereof, which has the following beneficial effects: 1、The present application realizes the synergistic reinforcement of the rubber material by adopting a ternary rubber system (acrylate rubber, chlorobutyl rubber and polytetrafluoroethylene modified rubber), wherein the chlorobutyl rubber can improve the elasticity and rigidity of the material, and the polytetrafluoroethylene modified rubber enhances the wear resistance and high temperature resistance, thereby improving the tensile strength, elongation at break, wear resistance and high temperature resistance of the oil seal.
[0015] 2、The present application further optimizes the reinforcement and sealing performance of the material by using and pretreating the nanoscale white carbon black and the montmorillonite, wherein the high specific surface area and reinforcement effect of the nanoscale white carbon black are better than the lamellar structure of graphite, which can enhance the crosslinking density and wear resistance of the rubber, and the addition of the montmorillonite can improve the barrier property of the material, thereby reducing the influence of oil swelling on the performance of the oil seal.
[0016] 3、The present application can further reduce the frictional resistance between the oil seal lip and the shaft, enhance the wear resistance and self-lubricating property by surface oxidation treatment of carbon fiber and spraying of polytetrafluoroethylene coating, the surface oxidation treated carbon fiber can be tightly combined with rubber molecules to improve the material strength and rigidity, and the polytetrafluoroethylene coating can provide additional lubrication effect, thereby further optimizing the dynamic performance of the oil seal.
[0017] 4、The present application can ensure uniform dispersion and chemical bonding of components, improve production efficiency and product quality by optimizing mixing, molding and vulcanization process, and eliminate residual stress by twice vulcanization treatment to improve the size stability and service life of the oil seal, and the pretreatment of the mold and strict control of the vulcanization condition can further improve the vulcanization quality and ensure the reliability of the product. BRIEF DESCRIPTION OF DRAWINGS
[0018] Figure 1 Preparation flow chart of the present application. DETAILED DESCRIPTION
[0019] The technical solutions in the embodiments of the present application will be clearly and completely described below with reference to the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative labor fall within the scope of protection of the present application.
[0020] Please refer to Figure 1 A low-friction shock absorber oil seal, raw materials and weight parts of the oil seal are as follows: acrylate rubber 36-40 parts; chlorobutyl rubber 25-28 parts; polytetrafluoroethylene (polytetrafluoroethylene) modified rubber 12-16 parts; nano-sized white carbon black 4-6 parts; carbon fiber 2-5 parts; clay 3-6 parts; aluminum alloy 1-3 parts; montmorillonite 1.15-1.60 parts; sodium stearate / potassium stearate 0.4-0.9 parts; molybdenum disulfide 0.6-0.9 parts; surfactant 0.3-0.6 parts; antioxidant 0.2-0.4 parts; vulcanizing agent 0.15-0.33 parts; coupling agent 0.2-0.3 parts.
[0021] Specifically, the particle size of the polytetrafluoroethylene modified rubber is ≤5 μm, and the specific surface area of the nano-sized white carbon black is ≥200 m² / g.
[0022] The advantages are that the synergistic reinforcement of the rubber material is realized by adopting a ternary rubber system (acrylate rubber, chlorobutyl rubber and polytetrafluoroethylene modified rubber), the chlorobutyl rubber can improve the elasticity and rigidity of the material, and the polytetrafluoroethylene modified rubber enhances the wear resistance and high temperature resistance, thereby improving the tensile strength, elongation at break, wear resistance and high temperature resistance of the oil seal.
[0023] Specifically, the length of the carbon fiber is between 1-2mm, and the clay is calcined kaolin.
[0024] Specifically, a preparation method of a low-friction shock absorber oil seal comprises the following steps: Step one, raw material preparation: prepare the formula weight parts of acrylate rubber, chlorobutyl rubber, polytetrafluoroethylene modified rubber, nano white carbon black, carbon fiber, clay, aluminum alloy, montmorillonite, sodium / potassium stearate, molybdenum disulfide, surfactant, antioxidant, vulcanizing agent and coupling agent; Step two, raw material pretreatment: premix white carbon black, montmorillonite and coupling agent, and perform surface oxidation treatment on carbon fiber; Step three, mixing: put acrylate rubber, chlorobutyl rubber and polytetrafluoroethylene modified rubber into a mixer, mix at a temperature of 95-100℃ and a speed of 50-60r / min for 5-7min to preliminarily mix the three kinds of rubber uniformly to form a plastic mixture, then add the premixed white carbon black, montmorillonite and coupling agent, increase the mixer temperature to 135-140℃, and continue mixing for 10-15min; at this time, due to the increase in temperature, the activity of the coupling agent is enhanced, which can better promote the uniform dispersion of the white carbon black and montmorillonite in the rubber matrix and produce chemical bonding with the rubber molecules, thereby improving the strength, wear resistance and barrier property of the rubber; then add sodium / potassium stearate and antioxidant in sequence, control the mixer temperature at 110-115℃, and mix for 5-6min; the sodium / potassium stearate can reduce the friction between rubber molecules and improve the flowability of the rubber compound, which is beneficial to subsequent processing and molding; the antioxidant is uniformly dispersed in the rubber compound to provide antioxidant protection for the rubber during subsequent processing and use; then add the surface-oxidized carbon fiber and clay, and keep the mixer temperature at 110-115℃, and mix for 8-10min; at this time, due to the active groups on the surface of the carbon fiber, it can be tightly combined with the rubber molecules, which helps to enhance the strength and rigidity of the rubber; and the clay is used as a filler and is uniformly dispersed in the rubber matrix, which helps to further improve the processing property of the rubber compound and reduce the cost; finally, add the vulcanizing agent and molybdenum disulfide, and continue mixing at a temperature of 80-95℃ for 3-5min to obtain the mixed rubber compound; the vulcanizing agent is uniformly distributed in the rubber compound to prepare for the subsequent vulcanization reaction, and the molybdenum disulfide is uniformly dispersed in the rubber matrix as a solid lubricant to further reduce the friction coefficient of the rubber compound; after the mixing is completed, the rubber compound is taken out for quality detection to ensure that the performance meets the requirements; Step four, molding: put the mixed rubber compound into a pretreated mold, process the mold by injection molding, set the pressure to 10-15MPa, the temperature to 165-170℃, and the molding time to 5-10min, and cool for 1-2h to obtain the molded oil seal; Step five, vulcanization: after molding, the oil seal is placed in the vulcanization equipment for two times of vulcanization treatment, the first vulcanization is at a temperature of 155-160 DEG C, preheating for 3-5 min, continuing to heat to 170-175 DEG C, controlling the vulcanization pressure to be greater than or equal to 10 MPa, the pressure can make the rubber molecules arrange more closely, help to improve the density and strength of the rubber, reduce the internal voids and defects, at the same time, the appropriate pressure is also beneficial to the better contact of the rubber and the heating medium in the vulcanization equipment, the heat transfer is more uniform, further improves the vulcanization quality, the vulcanization time is 8-10 min, the temperature accuracy is ± 1 DEG C, and the T90 time measured by the vulcanization instrument is used to control the vulcanization time, so as to ensure the vulcanization quality, the second vulcanization temperature is 145-150 DEG C, and the vulcanization time is 1.5-2 h, the main purpose of the second vulcanization is to eliminate residual stress, in the first vulcanization process, the residual stress is generated in the oil seal due to temperature change and chemical reaction factors, the lower temperature and longer time can make the rubber molecular chain relax and rearrange under the relatively mild conditions, effectively eliminate the residual stress, improve the size stability and service life of the oil seal, the second vulcanization can further improve the physical and mechanical properties of the oil seal, improve the size stability and sealing reliability; Step six, post-processing: after vulcanization, the oil seal is taken out from the vulcanization equipment, cooled and demolded, after demolding, the oil seal is inspected in appearance, the products with surface defects are removed, a polytetrafluoroethylene coating with a thickness of 0.01 mm-0.05 mm is sprayed on the surface of the oil seal, the PTFE coating has good self-lubricating property and chemical stability, can effectively reduce the friction resistance between the oil seal lip and the shaft, improve the wear resistance and service life of the oil seal, further reduce the friction coefficient, finally, the oil seal after coating is cleaned and dried to remove surface impurities and moisture; The advantages are that: through the surface oxidation treatment of carbon fiber and the spraying of polytetrafluoroethylene coating, not only the friction resistance between the oil seal lip and the shaft can be further reduced, but also the wear resistance and self-lubricating property can be improved, the surface oxidation treated carbon fiber can be closely combined with the rubber molecules to improve the material strength and rigidity, and the polytetrafluoroethylene coating can provide additional lubricating effect, so as to further optimize the dynamic performance of the oil seal.
[0025] Step seven, quality detection: the dried oil seal is tested in size accuracy, surface quality and vulcanization degree.
[0026] The advantages are that: through the optimization of mixing, molding and vulcanization process, the uniform dispersion and chemical bonding of each component can be ensured, the production efficiency and product quality are improved, and through two times of vulcanization treatment, the residual stress can be eliminated, the size stability and service life of the oil seal are improved, at the same time, the pretreatment of the mold and the strict control of the vulcanization conditions are helpful to further improve the vulcanization quality and ensure the reliability of the product.
[0027] Specifically, the white carbon black, the montmorillonite and the coupling agent are premixed, the montmorillonite and the white carbon black are sequentially added into the coupling agent, and stirring is carried out at a rotating speed of 200-300 r / min for 10-15 min, and then standing for 15-20 min.
[0028] The advantage is that the reinforcing and sealing performance of the material can be further optimized by using and pretreating the nanoscale white carbon black and the montmorillonite, wherein the high specific surface area and reinforcing effect of the nanoscale white carbon black are superior to the lamellar structure of graphite, which can enhance the crosslinking density and wear resistance of the rubber, and the addition of the montmorillonite can improve the barrier performance of the material, thereby reducing the influence of oil swelling on the oil seal performance.
[0029] Specifically, the carbon fiber is short-cut to 1-2 mm in length, and then placed in a temperature environment of 400-450°C, air is introduced, and oxidation is carried out for 10-15 min.
[0030] Specifically, the mold is pretreated by immersing the mold in a phosphate solution with a concentration of 5%-10% for 30-60 min to form a phosphating film on the surface of the mold.
[0031] Specifically, the oil seal is verified before installation: simulate the installation test for 4000-5000 cycles, and the oil seal leakage is ≤0.1 mL / h. Embodiment
[0032] Specifically, the raw materials of the oil seal and the weight parts thereof are as follows: acrylate rubber 38 parts; chlorobutyl rubber 28 parts; polytetrafluoroethylene modified rubber 13 parts; nanoscale white carbon black 5 parts; carbon fiber 4 parts; clay 5 parts; aluminum alloy 2 parts; montmorillonite 1.2 parts; sodium stearate / potassium stearate 0.6 parts; molybdenum disulfide 0.7 parts; surfactant 0.4 parts; antioxidant 0.25 parts; vulcanizing agent 0.25 parts; coupling agent 0.22 parts.
[0033] Comparative Example 1 Specifically, the raw materials of the oil seal and the weight parts thereof are as follows: acrylate rubber 70 parts; nanoscale white carbon black 5 parts; carbon fiber 4 parts; clay 5 parts; aluminum alloy 2 parts; montmorillonite 1.2 parts; sodium stearate / potassium stearate 0.6 parts; molybdenum disulfide 0.7 parts; surfactant 0.4 parts; antioxidant 0.25 parts; vulcanizing agent 0.25 parts; coupling agent 0.22 parts. Embodiment
[0034] Specifically, the raw materials of the oil seal and the weight parts thereof are as follows: acrylate rubber 40 parts; chlorobutyl rubber 28 parts; polytetrafluoroethylene modified rubber 13 parts; nanoscale white carbon black 6 parts; carbon fiber 2 parts; clay 6 parts; aluminum alloy 3 parts; montmorillonite 1.5 parts; sodium stearate / potassium stearate 0.4 parts; molybdenum disulfide 0.6 parts; surfactant 0.6 parts; antioxidant 0.2 parts; vulcanizing agent 0.30 parts; coupling agent 0.28 parts.
[0035] Comparative Example 2 Specifically, the raw materials of the oil seal and their weight parts are as follows: acrylic ester rubber 40 parts; chlorobutyl rubber 28 parts; polytetrafluoroethylene modified rubber 13 parts; graphite 6 parts; carbon fiber 2 parts; clay 6 parts; aluminum alloy 3 parts; sodium stearate / potassium stearate 0.4 parts; molybdenum disulfide 0.6 parts; surfactant 0.6 parts; antioxidant 0.2 parts; vulcanizing agent 0.30 parts; coupling agent 0.28 parts. Example
[0036] The raw materials of the oil seal and their weight parts are as follows: acrylic ester rubber 37 parts; chlorobutyl rubber 26 parts; polytetrafluoroethylene (polytetrafluoroethylene) modified rubber 12 parts; nanoscale white carbon black 4 parts; carbon fiber 2-5 parts; clay 5 parts; aluminum alloy 2 parts; montmorillonite 1.46 parts; sodium stearate / potassium stearate 0.5 parts; molybdenum disulfide 0.75 parts; surfactant 0.45 parts; antioxidant 0.25 parts; vulcanizing agent 0.26 parts; coupling agent 0.28 parts.
[0037] Comparative Example 3 The raw materials of the oil seal and their weight parts are as follows: acrylic ester rubber 37 parts; chlorobutyl rubber 26 parts; polytetrafluoroethylene (polytetrafluoroethylene) modified rubber 12 parts; nanoscale white carbon black 4 parts; carbon fiber 2-5 parts; clay 5 parts; aluminum alloy 2 parts; montmorillonite 1.46 parts; sodium stearate / potassium stearate 0.5 parts; surfactant 0.45 parts; vulcanizing agent 0.26 parts; coupling agent 0.28 parts.
[0038] The above examples and comparative examples are made into oil seals according to the method of the present application, and are tested, and the test data are as follows in Table 1: Table 1 Test item Example 1 Example 2 Comparative Example 1 Comparative Example 2 Example 3 Comparative Example 3 Tensile strength (MPa) 15.3 16.1 14.8 15.0 15.5 15.2 Elongation at break (%) 230 245 220 235 238 233 Compression set (%) 12 10 15 13 11 12 Hardness (Shore A) 75 78 72 74 76 73 Wear resistance (g / 1000r) 0.08 0.07 0.10 0.09 0.08 0.09 Oil resistance (24h, %) 98 99 95 96 98 97 High temperature resistance (150℃, 24h, %) 90 92 85 88 91 89 Cold resistance (-30℃, 24h, %) 85 88 80 83 87 84 Density (g / cm³) 1.25 1.23 1.30 1.28 1.26 1.27 Vulcanization time (min) 25 23 28 26 24 27 According to the above examples and comparative examples, the following information is obtained: Example 1 and Comparative Example 1: Example 1 uses a ternary rubber system (acrylic ester + chlorobutyl + polytetrafluoroethylene modified), while Comparative Example 1 only uses acrylic ester rubber. Comparative Example 1 actually contains montmorillonite (listed in the formula), but its effect is limited due to the single rubber system. The performance comparison is shown in Table 2: Table 2 Test index Example 1 Comparative Example 1 Difference reason Tensile strength 15.3 14.8 Synergistic reinforcement of the ternary rubber, neoprene improves rigidity, and polytetrafluoroethylene modified rubber enhances wear resistance. Elongation at break 230% 220% The elasticity contribution of neoprene is better than that of a single acrylate system. Compression set 12% 15% The high resilience of polytetrafluoroethylene modified rubber reduces permanent deformation. Wear resistance 0.08g 0.10g The wear resistance of polytetrafluoroethylene dominates, and the comparative example lacks this component. High temperature resistance 90% 85% The high temperature resistance of polytetrafluoroethylene modified rubber is significantly better than that of acrylate rubber. Density 1.25 1.30 Comparative Example 1 has high rubber content (70 parts of acrylate), resulting in increased density. From Table 2, it is obtained that the ternary rubber system helps to improve the comprehensive performance, thereby verifying the synergistic effect of chlorobutyl rubber (oil resistance) and polytetrafluoroethylene modified rubber (wear resistance, temperature resistance).
[0039] Example 2 and Comparative Example 2: Example 2 uses nanoscale white carbon black (6 parts), and Comparative Example 2 replaces it with graphite (6 parts). Comparative Example 2 does not add montmorillonite. The performance comparison is shown in Table 3: Table 3 Test index Example 2 Comparative Example 2 Difference reason Tensile strength 16.1 15.0 The nanoscale reinforcing effect of white carbon black is better than the lamellar structure of graphite. Compression set 10% 13% White carbon black enhances crosslinking density, reducing permanent deformation; graphite lubricity causes the material to easily flow and deform. Wear resistance 0.07g 0.09g The high reinforcing property of white carbon black improves wear resistance, and although graphite is lubricating, it sacrifices material strength. Oil resistance 99% 96% Montmorillonite (1.5 parts in Example 2) improves barrier properties and reduces oil swelling. Density 1.23 1.28 The density of graphite (2.2 g / cm³) is higher than that of white carbon black (1.9-2.1 g / cm³), resulting in a higher density in the comparative example From Table 3, it can be seen that the nano white carbon black is superior to graphite in reinforcement and sealing, and the addition of montmorillonite further optimizes the barrier properties.
[0040] Example 3 and Comparative Example 3: Comparative Example 3 lacks molybdenum disulfide (lubricant) and antioxidant, and its performance is compared in Table 4: Table 4 Test index Example 3 Comparative Example 3 Difference reason Wear resistance 0.08g 0.09g The solid lubricating effect of molybdenum disulfide reduces friction and wear. High temperature resistance 91% 89% Antioxidants delay high temperature oxidative degradation, and Comparative Example 3 ages faster. Cold resistance 87% 84% Antioxidants inhibit low temperature embrittlement and improve material toughness at low temperature. Vulcanization time 24 min 27 min Molybdenum disulfide may promote the formation of a sulfurized network, shortening the vulcanization time. From Table 4, it can be seen that the absence of molybdenum disulfide and antioxidant directly leads to a decrease in friction performance, aging resistance and vulcanization efficiency.
[0041] Summary: Through the comparative analysis of examples and comparative examples, it is summarized that the low-friction shock-absorbing oil seal prepared by the present application has many beneficial effects. By using a ternary rubber system (acrylate rubber, chloroprene rubber and polytetrafluoroethylene modified rubber) compared with a single acrylate rubber system, the tensile strength, elongation at break, wear resistance and high temperature resistance of the oil seal can be improved, and there is a synergistic effect between different rubber components. Among them, chloroprene rubber provides rigidity and oil resistance, and polytetrafluoroethylene modified rubber enhances wear resistance and high temperature resistance. The use of nano-sized white carbon black as a reinforcing agent can not only increase the crosslinking density of the material, reduce the compression permanent set, but also improve the wear resistance and barrier properties, ultimately showing advantages in reinforcement and sealing. The introduction of montmorillonite can further enhance the barrier properties of the oil seal, thereby effectively reducing oil swelling and improving oil resistance. Molybdenum disulfide as a solid lubricant can reduce friction and wear, promote the formation of a vulcanized network, shorten the vulcanization time, and thus optimize the vulcanization efficiency. The presence of an antioxidant can effectively delay the oxidative degradation process at high temperatures, improve the aging resistance and low temperature toughness of the oil seal. In summary, by optimizing the raw materials and their ratio, combined with specific pretreatment, mixing, molding, vulcanization and post-treatment processes, the low-friction shock-absorbing oil seal with excellent comprehensive performance can be successfully prepared, thereby reducing the friction coefficient of the oil seal, improving the wear resistance, enhancing the temperature resistance and cold resistance, and improving the processing performance.
[0042] Although embodiments of the present application have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made therein without departing from the principles and spirit of the application, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A low-friction shock absorber oil seal characterized by, The raw materials of the oil seal and their weight parts are as follows: acrylic ester rubber 36-40 parts; chlorobutyl rubber 25-28 parts; polytetrafluoroethylene modified rubber 12-16 parts; nano-grade white carbon black 4-6 parts; carbon fiber 2-5 parts; clay 3-6 parts; aluminum alloy 1-3 parts; montmorillonite 1.15-1.60 parts; sodium stearate / potassium stearate 0.4-0.9 parts; molybdenum disulfide 0.6-0.9 parts; surfactant 0.3-0.6 parts; antioxidant 0.2-0.4 parts; vulcanizing agent 0.15-0.33 parts; coupling agent 0.2-0.3 parts.
2. A low-friction shock absorber oil seal according to claim 1, characterized in that: The raw materials of the oil seal and their weight parts are as follows: acrylic ester rubber 38 parts; chlorobutyl rubber 28 parts; polytetrafluoroethylene modified rubber 13 parts; nano-grade white carbon black 5 parts; carbon fiber 4 parts; clay 5 parts; aluminum alloy 2 parts; montmorillonite 1.2 parts; sodium stearate / potassium stearate 0.6 parts; molybdenum disulfide 0.7 parts; surfactant 0.4 parts; antioxidant 0.25 parts; vulcanizing agent 0.25 parts; coupling agent 0.22 parts. The raw materials of the oil seal and their weight parts are as follows: acrylic ester rubber 40 parts; chlorobutyl rubber 28 parts; polytetrafluoroethylene modified rubber 13 parts; nano-grade white carbon black 6 parts; carbon fiber 2 parts; clay 6 parts; aluminum alloy 3 parts; montmorillonite 1.5 parts; sodium stearate / potassium stearate 0.4 parts; molybdenum disulfide 0.6 parts; surfactant 0.6 parts; antioxidant 0.2 parts; vulcanizing agent 0.30 parts; coupling agent 0.28 parts.
3. A low-friction shock absorber oil seal according to claim 1, characterized in that: The particle size of the polytetrafluoroethylene modified rubber is ≤5 μm, and the specific surface area of the nano-grade white carbon black is ≥200 m² / g.
4. A low-friction shock absorber oil seal according to claim 1, wherein The length of the carbon fiber is between 1-2 mm, and the clay is calcined kaolin.
5. A low-friction shock absorber oil seal according to claim 1, wherein The method comprises the following steps:
6. A method of preparing a low-friction shock absorber oil seal, characterized by, Step one, raw material preparation: prepare the formula weight parts of acrylic ester rubber, chlorobutyl rubber, polytetrafluoroethylene modified rubber, nano-grade white carbon black, carbon fiber, clay, aluminum alloy, montmorillonite, sodium stearate / potassium stearate, molybdenum disulfide, surfactant, antioxidant, vulcanizing agent and coupling agent; Step two, raw material pretreatment: premix the white carbon black, montmorillonite and coupling agent, and perform surface oxidation treatment on the carbon fiber; Step three, mixing: put the acrylic ester rubber, chlorobutyl rubber and polytetrafluoroethylene modified rubber into a mixing mill, mix at a temperature of 95-100 ℃ and a speed of 50-60 r / min for 5-7 min, then add the premixed white carbon black, montmorillonite and coupling agent, increase the temperature of the mixing mill to 135-140 ℃, and continue mixing for 10-15 min, then add the stearate and antioxidant in sequence, control the temperature of the mixing mill at 110-115 ℃, mix for 5-6 min, then add the carbon fiber and clay subjected to surface oxidation treatment, keep the temperature of the mixing mill at 110-115 ℃, mix for 8-10 min, and finally add the vulcanizing agent and molybdenum disulfide, continue mixing at a temperature of 80-95 ℃ for 3-5 min, to obtain the mixed rubber compound; Step four, molding: the mixing of the rubber material into the mold after pretreatment, using injection molding process for the mold, the pressure is set to 10-15MPa, temperature is set to 165-170℃, molding time is set between 5-10min, cooling 1-2h, get the molding of the oil seal; Step five, vulcanization: the oil seal after molding placed in the vulcanization equipment, two vulcanization treatment, the first vulcanization at 155-160℃, preheating 3-5min, continue to heat to 170-175℃, control the pressure of vulcanization ≥10MPa, vulcanization time is 8-10min, the second vulcanization temperature is 145-150℃, vulcanization time is 1.5-2h; Step six, post-processing: after vulcanization, the oil seal from the vulcanization equipment, cooling and demolding, in its surface spraying thickness of 0.01mm-0.05mm of polytetrafluoroethylene coating, finally the oil seal after coating cleaning and drying treatment; Step seven, quality detection: the drying treatment of the oil seal for size accuracy, surface quality and vulcanization degree test.
7. A method of making a low-friction shock absorber oil seal according to claim 6, characterized in that: The white carbon black, montmorillonite and coupling agent for pre-mixed, in order to montmorillonite and white carbon black into the coupling agent, and in the speed of 200-300r / min stirring 10-15min, then stand 15-20min.
8. The method of claim 6, wherein: The carbon fiber will be short cut to 1-2mm, then placed in the temperature environment of 400-450℃, into the air, oxidation 10-15min.
9. The method of claim 6, wherein: The mold pretreatment: the mold into the concentration of 5%-10% of phosphate solution for 30-60min, so that its surface form a layer of phosphating film.