Method for preparing sludge and biomass blended and solidified fuel particles based on ultrasonic synergy
The sludge-biomass blended solid fuel pellets prepared by ultrasonic synergistic process solve the problems of low fuel utilization rate and high energy consumption of sludge molding in biomass boilers, and achieve efficient and low-cost fuel preparation and low NOx emissions.
Patent Information
- Application Number
- CN202511114763.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-11
- Publication Date
- 2025-11-07
- Estimated Expiration
- 2045-08-11
AI Technical Summary
Existing biomass boiler fuels suffer from problems such as low fuel utilization, easy coking during combustion, high energy consumption for separate sludge pelleting, low mechanical strength of pellets, high cost and pollution due to the need to add a large amount of binder for traditional mixed pelleting, and excessive NOx emissions during combustion.
An ultrasonic-assisted method for preparing solidified fuel pellets by blending sludge and biomass was developed. Using a composite additive of Ca(OH)2, sodium lignosulfonate, and Fe2(SO4)3, the process involved gradient drying, low-temperature carbonization, ultrasonic pore expansion, and low-temperature pressing to produce high-efficiency, low-cost solidified fuel pellets.
It reduces the amount of binder used, improves production efficiency, reduces energy consumption, increases the calorific value and mechanical strength of fuel, reduces NOx emissions, and achieves low-cost and high-efficiency combustion.
Smart Images

Figure CN120904943A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of solid waste processing, in particular to a sludge and biomass blending solidification fuel particle preparation method based on ultrasonic cooperation. BACKGROUND
[0002] With the acceleration of global energy transformation and the rigid constraints of the "double carbon" target, biomass boilers have become a new type of equipment for carbon reduction and are widely used.
[0003] Biomass boilers have the advantages of higher fuel utilization rate and low carbon emission, which meet the current low-carbon control target. In the current energy utilization technology field, biomass boilers, as equipment for heating or power generation using biomass energy, are usually composed of a combustion chamber, a heat exchange system, and a flue gas purification system.
[0004] However, biomass fuel (such as tree trunks, wood chips) is rich in alkali metals such as K and Na, and the dust generated by combustion has strong adhesion. Single sludge incineration also has poor furnace temperature stability (±40℃) due to fluctuation of sludge moisture content (45%-65%), and the high-temperature zone shifts, reducing the dioxin decomposition rate to 88% (theoretically required >99%), and consuming 0.25 tons of standard coal to treat 1 ton of sludge (moisture content 60%), while the recovered heat energy is only 0.18 tons of standard coal equivalent, resulting in a negative net energy gain.
[0005] However, the existing biomass processing technology has the following problems: 1. High energy consumption for sludge alone (moisture content >80%), low mechanical strength of particles (compressive strength <500N); 2. Limited heat value of single biomass fuel (14-16MJ / kg), and easy coking during combustion; 3. Traditional mixing and granulation requires adding more than 20% binder, increasing cost and causing secondary pollution.
[0006] 4. High-temperature drying (>300℃) leads to decomposition of organic matter, resulting in a heat value loss of ≥15%, and the prepared particles emit NOx exceeding 150mg / m³ during combustion. SUMMARY
[0007] The present application relates to the technical field of solid waste processing, in particular to a sludge and biomass blending solidification fuel particle preparation method based on ultrasonic cooperation.
[0008] The technical solution of the present application is: The preparation method of sludge and biomass blended solidified fuel particles based on ultrasonic cooperation comprises 30-40wt% of dewatered sludge, 60-70wt% of biomass and 0.5-3.5wt% of composite additives; the dewatered sludge is prepared by dewatering sludge including at least municipal sludge, papermaking sludge and printing and dyeing sludge, and the water content of the dewatered sludge is ≤60%; the biomass includes at least forest and farm biomass including tree trunk, tree bark, furniture scrap and wood chips, and the particle size of the biomass is 0.5-2mm; the composite additives are Ca(OH)2, sodium lignosulfonate and Fe2(SO4)3; the mass ratio of Ca(OH)2:sodium lignosulfonate:Fe2(SO4)3 is 2:1:0.5.
[0009] The preparation method of sludge and biomass blended solidified fuel particles based on ultrasonic cooperation as mentioned above comprises the following steps: S1, biomass raw material pretreatment: the biomass is crushed to obtain biomass particles with a particle size of 0.5-2mm; S2, sludge gradient drying: the sludge is subjected to gradient drying by a hot air circulation system, and is subjected to stepwise dewatering at 75-115℃ to obtain dewatered sludge; the water content of the dewatered sludge is ≤60%; S3, carbonization ultrasonic reaming: the dewatered sludge is carbonized at 180℃ in a fluidized bed for 20-30min, and 40kHz / 5kW ultrasonic is applied synchronously; S4, additive injection; S5, ultrasonic blending modification: the dewatered sludge and the biomass particles are blended by double screw extrusion with 200-400W ultrasonic oscillation to obtain a blend; S6, low-temperature pressing forming: the blend is subjected to pressing forming by a ring mold forming machine at 70-90℃ in a mold with a pressure of 15-25MPa; S7, low-temperature curing: the product particles are obtained by curing at 40-50℃ in a ventilated environment for 20-28h; S8, product packaging.
[0010] In the preparation method of sludge and biomass blended solidified fuel particles based on ultrasonic cooperation as mentioned above, the sludge gradient drying in S2 has the following specific content: S2.1, free water removal: the sludge is subjected to free water removal in a phase change dewatering zone, the dewatering temperature is 75-85℃, and the dewatering time is 40-50min; S2.2, bound water removal: the sludge is subjected to bound water removal in a bound water removal zone, the dewatering temperature is 105-115℃, and the dewatering time is 15-25min.
[0011] In the preparation method of sludge and biomass blended solidified fuel particles based on ultrasonic cooperation as mentioned above, the carbonization ultrasonic reaming in S3 has the following specific content: S3.1, low-temperature carbonization: low-temperature carbonization of the dewatered sludge after gradient drying by a fluidized bed low-temperature carbonization furnace, carbonization temperature 180℃, time 20-30 min; S3.2, ultrasonic hole expansion: simultaneously applying 40kHz / 5kW ultrasound to construct 0.5-5μm dominant open pores, and remodeling the pore size distribution through cavitation-acoustic streaming coupling effect; Through cavitation shock wave extrusion, large pore walls are crushed, through microjet shear, closed pores are opened, through sonochemical oxidation, active oxygen is produced, and the surface of the pores is etched to increase the diffusion micropores.
[0012] In the foregoing sludge and biomass blending solidified fuel particle preparation method based on ultrasonic cooperation, the ultrasonic blending modification of S5 is provided by a 40kHz piezoelectric transducer radially inserted into a double screw main machine, and the specific content is as follows: S5.1, conveying section: double screw rotation speed 40rpm, ultrasonic power 200w; S5.2, melting section: double screw rotation speed 45rpm, ultrasonic power 300w; S5.3, mixing section: double screw rotation speed 50rpm, ultrasonic power 400w; S5.4, homogenization section: double screw rotation speed 48rpm, ultrasonic power 0w.
[0013] In the foregoing sludge and biomass blending solidified fuel particle preparation method based on ultrasonic cooperation, the power density of the ultrasonic treatment is 15-18W / g, the penetration depth is 1.5mm, and the blending time is ≤10min; the ultrasonic field application direction and the material flow direction form an angle of 30°-60°; a radiation head is further provided to synchronously apply a 20MHz radio frequency field, and the insertion depth of the radiation head is 1 / 3-1 / 2 of the material layer thickness.
[0014] In the foregoing sludge and biomass blending solidified fuel particle preparation method based on ultrasonic cooperation, the low-temperature pressing forming of S6 has the following specific content: Pressing is carried out at 70-90℃, and cylindrical solid particles are formed, with a length of 40mm and an aspect ratio of 4:1-6.7:1.
[0015] In the foregoing sludge and biomass blending solidified fuel particle preparation method based on ultrasonic cooperation, the low-temperature curing of S7 has the following specific content: The curing environment has an O2 concentration of <5%, an environmental temperature of 40-50℃, and a particle layer airflow speed of 0.05-0.1m / s.
[0016] Compared with the prior art, the present application has the following beneficial effects: 1. Synergistic effect innovation: add the composite additive compounded by Ca(OH)2+ sodium lignosulfonate + Fe2(SO4)3, the protein in the sludge is cross-linked under the action of the additive to form a natural bonding network, thereby more than 70% of the chemical binder can be replaced, the use of the chemical binder is reduced, and the binder is reduced to 1 / 5 compared with the existing traditional process; 2. Process coupling breakthrough: through ultrasonic synergy, the ultrasonic field promotes the penetration of the additive into the sludge micelle, breaks the wax layer on the surface of the biomass, the penetration depth can reach 0.9-1.5mm, the sludge micelle rupture rate is more than 90%, and the blending efficiency is greatly improved; 3. Production cost reduction: the fuel particles are prepared by gradient drying, low-temperature pressing and low-temperature curing, which reduces the energy consumption compared with the traditional preparation process, and greatly reduces the production cost.
[0017] Therefore, the present application has the advantages of less binder, high production efficiency and low cost. BRIEF DESCRIPTION OF DRAWINGS
[0018] Figure 1 is the process flow chart of the preparation method of the present application. DETAILED DESCRIPTION
[0019] The present application will be further described below in combination with the drawings and examples, but it is not used as the basis for limiting the present application.
[0020] Example 1. The preparation method of the sludge and biomass blending solidified fuel particle preparation method based on ultrasonic synergy, contains 30-40wt% of dewatered sludge, 60-70wt% of biomass and 0.5-3.5wt% of composite additive; the dewatered sludge is prepared from sludge dewatering including at least municipal sludge, papermaking sludge and printing and dyeing sludge, and the water content of the dewatered sludge is ≤60%; the biomass at least includes tree trunk, tree bark, furniture scrap and sawdust, and the particle size of the biomass is 0.5-2mm; the composite additive is Ca(OH)2, sodium lignosulfonate and Fe2(SO4)3; the mass ratio of Ca(OH)2: sodium lignosulfonate: Fe2(SO4)3 is 2:1:0.5.
[0021] The preparation method of the sludge and biomass blending solidified fuel particle preparation method based on ultrasonic synergy, as shown in Figure 1 , the steps are as follows: S1, biomass raw material pretreatment: the biomass is crushed to obtain biomass particles with a particle size of 0.5-2mm; S2, sludge gradient drying: the hot air circulation system performs gradient drying on the sludge, and the sludge is dewatered in stages at 75-115℃, and the dewatered sludge is obtained; the energy consumption is reduced by 35%, and the volatile matter is retained; S3, carbonization ultrasonic reaming: carbonize the dewatered sludge in the fluidized bed at 180℃ for 20-30min, and synchronously apply 40kHz / 5kW ultrasonic; the proportion of effective pore size (0.5-5μm) is increased from 45% to 83%; S4, additive injection; S5, ultrasonic blending modification: blend the dewatered sludge and biomass particles by double screw extrusion with 200-400W ultrasonic oscillation to obtain a blend; the mixing uniformity reaches 98.5%; S6, low-temperature pressing forming: the blend is pressed and formed by a ring mold forming machine at 70-90℃ in the mold at a pressure of 15-25MPa; the prepared particles have a density of >1.1g / cm³; S7, low-temperature curing: the finished particles are obtained by curing at 40-50℃ in a ventilated environment for 20-28h; the compressive strength is increased to above 800N; S8, finished product packaging.
[0022] S2, sludge gradient drying, the specific content is as follows: S2.1, free water removal: the sludge enters the phase change dehydration zone to remove free water, the dehydration temperature is 75-85℃, and the dehydration time is 40-50min; the evaporation latent heat is relatively low (2300 kJ / kg); S2.2, bound water removal: the sludge enters the bound water removal zone to remove bound water, the dehydration temperature is 105-115℃, and the dehydration time is 15-25min; the evaporation latent heat is relatively high (2600 kJ / kg).
[0023] The phase change dehydration zone stage (low temperature section) preferentially evaporates low-energy free water (accounting for 70% of the total), avoiding energy waste caused by treating free water in the bound water removal stage (high temperature section); The bound water removal stage (high temperature section) is only for difficult-to-remove bound water, shortening the high temperature time (reducing heat loss), and comprehensively reducing the total evaporation latent heat demand; The traditional constant temperature 120℃ process has an evaporation energy consumption of 780 kWh per ton of water; and the gradient drying adopted in the present application has an evaporation energy consumption of 507 kWh per ton of water (reduced by 35.1%).
[0024] S3, carbonization ultrasonic reaming, which is carried out in the powdery semi-finished product stage (moisture content ≤8%) after gradient drying and before low-temperature forming, the specific content is as follows: S3.1, low-temperature carbonization: the dewatered sludge after gradient drying is subjected to low-temperature carbonization by a fluidized bed low-temperature carbonization furnace, the carbonization temperature is 180℃, and the time is 20-30min; At 180℃, hemicellulose releases bound water to generate furfural polymers (natural binder), effectively avoiding high-temperature cracking and retaining >90% of aliphatic hydrocarbon volatile matter (contribution to heat value >15MJ / kg). S3.2, ultrasonic reaming: 40 kHz / 5 kW ultrasonic is applied synchronously to build 0.5-5 μm dominant open pores (accounting for >80% of pore volume, to improve burning rate), to reshape pore size distribution through cavitation-acoustic streaming coupling effect, to avoid conventional particle pores concentrated in <0.1 μm (ineffective micropores) or >50 μm (structurally weak), to improve the path of volatile matter rapid escape, and to achieve a combustion efficiency of 92.5% (compared with 78-85% for traditional particles); Through cavitation shock wave extrusion, large pore walls are crushed with local pressure >50 MPa, thereby eliminating >20 μm ineffective large pores; Through microjet shear, closed pores are punched with flow rate >100 m / s, thereby generating 1-5 μm through pores; Through acoustic chemical oxidation, active oxygen is generated to etch the pore surface and increase 0.5-1 μm diffusion micropores.
[0025] S5 ultrasonic blending modification, in which a 40 kHz piezoelectric transducer (converting electrical energy into mechanical vibration waves) is radially inserted into a 40 kHz piezoelectric transducer (converting electrical energy into mechanical vibration waves) installed on a double screw main machine, the coupling component is a titanium alloy horn (Φ25 mm), which penetrates the machine cylinder wall (sealing level IP68), and the processing specific content is as follows: First, start the screw (low speed 20 rpm), feed up to 30% of the volume, turn on the ultrasonic (initial 200 W), and gradually increase the speed to the target speed (5 rpm every 5 min); S5.1, conveying section: double screw speed 40 rpm, ultrasonic power 200 w; low-frequency cavitation breaks down sludge flocs, releasing bound water; S5.2, melting section: double screw speed 45 rpm, ultrasonic power 300 w; acoustic streaming effect (>10 m / s) promotes biomass lignin melting; S5.3, mixing section: double screw speed 50 rpm, ultrasonic power 400 w; acoustic chemical modification generates hydroxyl radicals to degrade dye molecules in printing and dyeing sludge; S5.4, homogenization section: double screw speed 48 rpm, ultrasonic power 0 w; eliminate bubbles to prevent particle micropore collapse.
[0026] The power density of the ultrasonic treatment is 15-18 W / g, the penetration depth is 1.5 mm, and the blending time is ≤10 min; the ultrasonic field application direction forms an angle of 30°-60° with the material flow direction; a radiation head is further provided to synchronously apply a 20 MHz radio frequency field, and the insertion depth of the radiation head is 1 / 3-1 / 2 of the material layer thickness.
[0027] S6 low-temperature pressing forming, which is the core technology of sludge biomass fuel particle forming, and its core principle lies in the use of biomass thermal plasticity transformation and sludge colloidal adhesion, and the specific content is as follows: The pressing is carried out at 70-90℃, and the pressed solid particles are cylinders with a diameter of 6 / 8 / 10 mm, a length of 40 mm, and a length-diameter ratio of 4:1-6.7:1, and the volatile combustion path is fully optimized.
[0028] S7 is low-temperature curing, and the specific content is as follows: The curing environment has an O2 concentration of less than 5% (to inhibit the generation of dioxins, and when O2 is greater than 8%, the amount of dioxin generated is 0.25 ng TEQ / kg), an environmental temperature of 40-50℃, and a particle layer airflow speed of 0.05-0.1 m / s, so as to avoid cracking on the surface of the particles.
[0029] Example 2. The preparation method of the sludge and biomass blending solidified fuel particle preparation method based on ultrasonic synergy is basically the same as that of Example 1, and the difference lies in that: The sludge contains 39wt% of dewatered sludge, 60wt% of biomass, and 1wt% of composite additives; the dewatered sludge is papermaking sludge; the biomass is a tree trunk; and the composite additives are Ca(OH)2, sodium lignosulfonate, and Fe2(SO4)3, and the mass ratio of Ca(OH)2:sodium lignosulfonate:Fe2(SO4)3 is 2:1:0.5.
[0030] The particle size of the biomass particles is Φ8 mm.
[0031] The fuel particles prepared by the application have a calorific value of ≥18.5 MJ / kg (210% higher than single sludge), and no additional coal combustion is required during the combustion process; The NOx emission of the combustion is ≤80 mg / m³, and the heavy metal solidification rate is >97%, which greatly reduces the NOx emission concentration, and if a dust-nitrogen coupling integrated device is configured subsequently, the NOx can be easily reduced to the national ultra-low standard (NOx≤50 mg / m³); The combustion rate reaches 0.92 mm / s (42% higher than the traditional one); Only a conventional biomass boiler can easily handle the blended solidified fuel particles, without any other adjustment to the boiler.
[0032] According to the calculation of 50,000 tons of sludge treatment per year, the following values can be obtained by applying the application: • 45 mu of landfill land is reduced per year; • 32,000 tons of fuel particles are produced, replacing 18,000 tons of standard coal; • The ultrasonic intensification process can reduce the additive cost by 1.75 million yuan; • The CO2 emission reduction amount reaches 46,000 tons / year; • Because the NOx emission of the combustion is ≤80 mg / m³, the denitration ammonia water consumption can be reduced by 20 tons / year, and the catalyst replacement frequency is also reduced. X
[0033] Comparative experiment I) Composite additive experiment comparison Application experiment data comparison of 0.5-3.5wt% composite additive (Ca(OH)2: sodium lignosulfonate: Fe2(SO4)3=2:1:0.5) in sludge-biomass fuel particles (test standards: GB / T 28750 and ISO 17225-7) I) Experimental design and control group
[0034] II) Comparison of key performance data 1. Fuel heat value and combustion efficiency
[0035] Conclusion: 1.0% additive concentration is the optimal value, heat value increased by 16.7%, and carbon residue rate decreased by 47%; Excessive addition (>1.5%) actually leads to a decrease in heat value.
[0036] 2. Heavy metal solidification effect
[0037] Mechanism of action: Ca(OH)2 provides an alkaline environment (pH≈11.5) to promote the formation of insoluble hydroxides of heavy metals; Iron sulfate hydrolysis generates colloidal Fe(OH)3, which adsorbs heavy metals such as Cd / Pb in sludge to form stable co-precipitation (solidification rate↑5-8%).
[0038] Sodium lignosulfonate enhances solidification through phenolic hydroxyl chelation (As solidification rate↑87%).
[0039] 3. Particle physical strength
[0040] Explanation: Sodium lignosulfonate as a natural binder improves the toughness of the particles; By ultrasonic dispersion of Fe2(SO4)3, the particle strength is maintained >800N.
[0041] Excessive Ca(OH)2 leads to an increase in particle brittleness (>1.5% when the strength decreases).
[0042] III) Comparison of combustion emissions (1.0% additive vs. control group)
[0043] Emission reduction mechanism: Ca(OH)2sulfur fixation: CaSO4generation rate > 95%; Fe 3+ Catalytic decomposition of NO in combustion X (selective non-catalytic reduction SNCR effect), can make NO X emission reduction of 15-30%; Sodium lignosulfonate inhibits dioxin: destroys the synthesis path of chlorobenzene precursors.
[0044] Four, multivariate comparative experiments 1, additive ratio vs total additive amount (compressive strength response)
[0045] 2, ultrasonic power vs total additive amount (heat value response)
[0046] Interaction mechanism: high ultrasonic power (400W) can break the additive agglomerates → allow higher additive amount (1.2-1.3%) without reducing heat value; Breakthrough cognition: traditional theory believes that "additive amount ↑ must lead to heat value ↓", but ultrasonic intervention breaks this limitation.
[0047] Two, raw material ratio experiment Sludge and mixed biomass blended fuel particles, raw material ratio performance verification: One, core parameter setting of the experiment
[0048] Two, performance comparison of three types of sludge particles (Φ8mm benchmark) 1: Physical and mechanical properties
[0049] Conclusion: Papermaking sludge has the best particle density and strength due to high fiber content; printing and dyeing sludge needs to be pretreated to reduce moisture content.
[0050] 2: Combustion characteristics (1.0% additive)
[0051] Explanation: Printing and dyeing sludge has a 12.3% reduction in heat value due to residual inorganic salts (about 18%), which needs to be supplemented with high-heat-value biomass (such as tree trunk chips).
[0052] Three, the influence of particle size on performance (papermaking sludge system) 3: Comparison of Φ6 / 8 / 10mm particles
[0053] Conclusion: Φ8mm is balanced in energy consumption, combustion stability and emission control, which is suitable for mainstream industrial boilers; Φ6mm has fast burning speed, but dust emission increases by 15% (need to strengthen dust removal).
[0054] Four, environmental protection and safety data (Φ8mm particles) 4: Heavy metal leaching and emission
[0055] The natural detoxification characteristics of lignin in paper sludge make the dioxin generation very low.
Claims
1. A method for the production of sludge and biomass co-blended, solidified fuel pellets based on ultrasonic synergy, characterized by: The application relates to a preparation method of a sludge-biomass blended solidified fuel particle based on ultrasonic coordination, which comprises the following steps: S1, biomass raw material pretreatment: biomass is crushed to obtain biomass particles with a particle size of 0.5-2 mm; S2, sludge gradient drying: a hot air circulation system is used to perform gradient drying on sludge to obtain dewatered sludge by section dehydration at 75-115 DEG C; the water content of the dewatered sludge is less than or equal to 60%; S3, carbonization ultrasonic hole expansion: the dewatered sludge is carbonized in a fluidized bed at 180 DEG C for 20-30 min, and 40 kHz / 5 kW ultrasonic waves are synchronously applied; S4, additive injection; S5, ultrasonic blending modification: the dewatered sludge and the biomass particles are blended by means of double-screw extrusion and 200-400 W ultrasonic oscillation to obtain a blended product; S6, low-temperature pressing forming: the blended product is formed by a ring die forming machine, and is pressed and formed in a mold at 70-90 DEG C under a pressure of 15-25 MPa; S7, low-temperature curing: the product is cured in a ventilated environment at 40-50 DEG C for 20-28 h to obtain finished particles; and S8, finished product packaging.
2. The preparation method of the sludge-biomass blended solidified fuel particle based on ultrasonic coordination according to claim 1, comprising the following steps: S1, biomass raw material pretreatment: biomass is crushed to obtain biomass particles with a particle size of 0.5-2 mm; S2, sludge gradient drying: a hot air circulation system is used to perform gradient drying on sludge to obtain dewatered sludge by section dehydration at 75-115 DEG C; the water content of the dewatered sludge is less than or equal to 60%; S3, carbonization ultrasonic hole expansion: the dewatered sludge is carbonized in a fluidized bed at 180 DEG C for 20-30 min, and 40 kHz / 5 kW ultrasonic waves are synchronously applied; S4, additive injection; S5, ultrasonic blending modification: the dewatered sludge and the biomass particles are blended by means of double-screw extrusion and 200-400 W ultrasonic oscillation to obtain a blended product; S6, low-temperature pressing forming: the blended product is formed by a ring die forming machine, and is pressed and formed in a mold at 70-90 DEG C under a pressure of 15-25 MPa; S7, low-temperature curing: the product is cured in a ventilated environment at 40-50 DEG C for 20-28 h to obtain finished particles; S8, finished product packaging.
3. The method of claim 2, wherein the method further comprises: S2, sludge gradient drying, specific content as follows: S2.1, free water removal: sludge enters the phase change dehydration zone to remove free water, dehydration temperature 75-85 DEG C, dehydration time 40-50 min; S2.2, bound water removal: sludge enters the bound water removal zone to remove bound water, dehydration temperature 105-115 DEG C, dehydration time 15-25 min.
4. The method of claim 2, wherein the method further comprises: S3, carbonization ultrasonic hole expansion, specific content as follows: S3.1, low-temperature carbonization: the dewatered sludge after gradient drying is subjected to low-temperature carbonization by a fluidized bed low-temperature carbonization furnace, carbonization temperature 180 DEG C, time 20-30 min; S3.2, ultrasonic hole expansion: 40 kHz / 5 kW ultrasonic waves are synchronously applied to construct 0.5-5 mu m dominated open pores, and the pore size distribution is remodeled through cavitation-acoustic flow coupling effect; Through cavitation shock wave extrusion, large pore walls are crushed, through microjet shear, closed pores are opened, through acoustic chemical oxidation, active oxygen is produced, and the surface of the pore is etched to increase diffusion micropores.
5. The ultrasonic synergy based sludge and biomass co-blended solidified fuel pellet production method as claimed in claim 2, wherein, S5, ultrasonic blending modification, ultrasonic waves are provided by a 40 kHz piezoelectric transducer radially inserted into a double-screw host machine, specific content as follows: S5.1, conveying section: double-screw rotation speed 40 rpm, ultrasonic power 200 w; S5.2, melting section: double-screw rotation speed 45 rpm, ultrasonic power 300 w; S5.3, mixing section: double screw rotation speed 50 rpm, ultrasonic power 400 w; S5.4, homogenizing section: double screw rotation speed 48 rpm, ultrasonic power 0 w.
6. The method of claim 5, wherein the method further comprises: The power density of the ultrasonic treatment is 15-18 W / g, the penetration depth is 1.5 mm, and the blending time is ≤10 min; the ultrasonic field application direction forms an angle of 30°-60° with the material flow direction; a radiation head is further provided to synchronously apply a 20 MHz radio frequency field, and the insertion depth of the radiation head is 1 / 3-1 / 2 of the thickness of the material layer.
7. The ultrasonic synergy based sludge and biomass co-blended solidified fuel pellet production method as claimed in claim 2, wherein, The low-temperature pressing forming in S6 has the following specific content: The pressing is performed at 70-90°C to form a cylindrical solid particle with a length of 40 mm and an aspect ratio of 4:1-6.7:
1.
8. The ultrasonic synergy based sludge and biomass co-blended solidified fuel pellet production method as claimed in claim 2, wherein, The low-temperature curing in S7 has the following specific content: The curing environment has an O2 concentration of <5%, an environmental temperature of 40-50°C, and a particle layer airflow speed of 0.05-0.1 m / s.
Citation Information
Patent Citations
Compounded sludge dewatering conditioner and application and method thereof
CN103241922A
Preparation method of phosphogypsum-based sludge drying agent and application of preparation method in drying sludge
CN104045298A
Deep treatment method for sewage of breeding plants
CN106277579A
Compound agent for repairing heavy metal contaminated soil and application thereof
CN108641726A
Method for preparing high calorific value fuel from municipal sludge and biomass synergistically
CN108753403A
Cited By
A biomass sludge composite fuel and its preparation method
CN122542289A