Ferroelectric field effect transistor memory and preparation method thereof

By using a gate electrode material with low work function and a Zr-doped HfO2 ferroelectric layer, the erasure problem of FeFET devices was solved, the reliability of the storage window and multi-value storage was enhanced, and a better erasure effect was achieved.

CN121152214APending Publication Date: 2025-12-16INST OF MICROELECTRONICS CHINESE ACAD OF SCI LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410722765.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2025-12-16

AI Technical Summary

Technical Problem

FeFET devices suffer from an erase problem, resulting in insufficient storage windows and making it difficult to achieve effective polarization switching and multi-value storage.

Method used

Ferroelectric field-effect transistor memory is fabricated using a gate electrode material with low work function (such as molybdenum), combined with a Zr-doped HfO2 ferroelectric layer and a semiconductor channel layer, through an atomic layer deposition process, thereby enhancing the voltage division and electric field strength of the ferroelectric layer.

Benefits of technology

The storage window of the FeFET memory has been increased, the reliability and efficiency of multi-value storage have been enhanced, and the erasure performance of the device has been improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121152214A_ABST
    Figure CN121152214A_ABST
Patent Text Reader

Abstract

The invention relates to a ferroelectric field effect transistor memory and a preparation method thereof in the technical field of microelectronics, the ferroelectric field effect transistor memory comprises a substrate layer, a gate electrode, a ferroelectric layer, a semiconductor channel layer and a source and drain electrode layer which are stacked in sequence, and the work function WF of the material of the gate electrode is less than 4.5 eV. According to the ferroelectric field effect transistor memory, the partial voltage of the semiconductor channel layer can be reduced, the partial voltage and the electric field intensity of the ferroelectric layer can be increased, the erasing effect of the FeFET memory can be effectively improved, and the memory window of the FeFET memory can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of microelectronics technology, and in particular to a ferroelectric field-effect transistor memory and its fabrication method. Background Technology

[0002] Ferroelectric field-effect transistors (FeFETs) based on HfO2 material hold promise for next-generation memory devices, exhibiting significant advantages including high speed, low power consumption, non-destructive read capability, and CMOS compatibility. To achieve sufficiently large I²S / I ... ON / I OFF To achieve high impedance (one of the requirements for fast read speed of FeFET), realize multi-value storage, and improve the reliability of memory operation, it is necessary to widely separate the high-resistivity and low-resistivity states of V. th Distribution, i.e., realizing a large storage window.

[0003] The advantage of a large memory window is that it enhances the ability of each cell to store more than one bit of data. This allows for an increase in effective bit density without reducing device size. To ensure the reliable operation of multi-valued operations, the following prerequisites must be met: (1) there must be a sufficient memory window between any two states; (2) each state must have stable retention characteristics, stable durability, good consistency, and anti-interference capabilities. When the memory window falls below a certain value, the stored information cannot be identified.

[0004] FeFET devices commonly suffer from an erase problem, which limits their storage window. During the erase process, the semiconductor channel layer is in a high-resistivity state with a high voltage division, which reduces the voltage division of the ferroelectric layer, making it difficult to achieve an ideal erase effect. In some cases, the voltage division of the ferroelectric layer drops so low that the electric field strength is less than the coercive field, hindering effective polarization switching and significantly reducing the erase performance. Summary of the Invention

[0005] In view of the problems existing in the background technology, this application provides a ferroelectric field-effect transistor memory and its fabrication method. The ferroelectric field-effect transistor memory can reduce the voltage division of the semiconductor channel layer, increase the voltage division and electric field strength of the ferroelectric layer, effectively improve the erasure effect of the FeFET memory, and increase the storage window of the FeFET memory.

[0006] According to one aspect of the present invention, a ferroelectric field-effect transistor memory is provided, comprising a substrate layer, a gate electrode, a ferroelectric layer, a semiconductor channel layer and a source / drain electrode layer stacked sequentially, wherein the work function WF of the material of the gate electrode is less than 4.5 eV.

[0007] In some embodiments of the present invention, the gate electrode is made of molybdenum.

[0008] In some embodiments of the present invention, the thickness of the gate electrode is 10-100 nm.

[0009] In some embodiments of the present invention, the material of the ferroelectric layer is Zr-doped HfO2.

[0010] In some embodiments of the present invention, the thickness of the ferroelectric layer is 3-20 nm.

[0011] In some embodiments of the present invention, the material of the semiconductor channel layer is an oxide semiconductor or polycrystalline silicon.

[0012] According to another aspect of the present invention, a method for fabricating a ferroelectric field-effect transistor memory is provided, comprising: providing a substrate layer; fabricating a gate electrode on the substrate layer using a material with a work function WF less than 4.5 eV; fabricating a ferroelectric layer on the gate electrode; fabricating a semiconductor channel layer on the ferroelectric layer; fabricating a source / drain electrode layer on the semiconductor channel layer; and obtaining a ferroelectric field-effect transistor memory.

[0013] In some embodiments of the present invention, the preparation of the gate electrode includes: depositing the gate electrode on the substrate using a deposition process; coating the gate electrode with photoresist, exposing and developing it, etching it, and removing the photoresist to achieve gate electrode patterning.

[0014] In some embodiments of the present invention, the photoresist coated on the gate electrode is a negative photoresist, which is then pre-baked at 150°C for 2 minutes, exposed, post-baked at 120°C for 2 minutes, and then immersed in the developing solution for 30 seconds for development.

[0015] In some embodiments of the present invention, the preparation of the ferroelectric layer includes: preparing a Zr-doped HfO2 ferroelectric layer on the gate electrode using an atomic layer deposition process, with a deposition temperature range of 280-350°C; coating the ferroelectric layer with photoresist, exposing and developing it, and then etching and removing the photoresist to achieve patterning of the ferroelectric layer.

[0016] This application provides a ferroelectric field-effect transistor (FET) memory. This FET memory utilizes a gate electrode material with a low work function (WF), resulting in a lower intrinsic threshold voltage (V) for the FET memory with a gate electrode material having a work function WF less than 4.5 eV. thUnder the same erase voltage, the FeFET memory has a higher conductivity and a smaller voltage drop in the semiconductor channel layer, which increases the voltage drop in the ferroelectric layer. This allows the electric dipoles of the ferroelectric layer to be effectively and fully flipped, resulting in a better erase effect. This, in turn, increases the memory window of the FeFET. The increased memory window is beneficial for the application of FeFET in multi-value storage and improves the reliability of the memory in practical applications. Attached Figure Description

[0017] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0018] Figure 1 This is a schematic diagram of the overall structure of the ferroelectric field-effect transistor memory according to an embodiment of this application;

[0019] Figure 2 This is a graph showing the relationship between the TCAD simulation storage window and the work function of the gate electrode metal;

[0020] Figure 3 This is a schematic diagram illustrating the principle of improving the storage window through the gate electrode metal work function engineering.

[0021] The reference numerals in the attached figures represent the following: 1. Substrate layer; 2. Gate electrode; 3. Ferroelectric layer; 4. Semiconductor channel layer; 5. Source / drain electrode layer. Detailed Implementation

[0022] It should be understood that the described embodiments are merely some, not all, of the embodiments in this application. All other embodiments obtained by those skilled in the art based on the embodiments in this application without inventive effort are within the scope of protection of this application.

[0023] In the following description, when referring to the accompanying drawings, the same numbers in different drawings denote the same or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this application. Rather, they are merely examples of apparatuses and methods consistent with some aspects of this application as detailed in the appended claims.

[0024] In the description of this application, it should be understood that the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances. Furthermore, in the description of this application, unless otherwise stated, "a plurality of" means two or more.

[0025] This application discloses a ferroelectric field-effect transistor memory. For example... Figure 1 As shown, the ferroelectric field-effect transistor memory includes a substrate layer 1, a gate electrode 2, a ferroelectric layer 3, a semiconductor channel layer 4, and a source / drain electrode layer 5 stacked sequentially.

[0026] Among them, the work function WF of the material of the gate electrode 2 is less than 4.5 eV.

[0027] The storage window and erase process of ferroelectric field-effect transistors (FETs) are strongly correlated. Using a gate electrode material with a low work function (WF) enables FeFET memories with a gate electrode material having a work function WF less than 4.5 eV to have a lower intrinsic threshold voltage (V). th Under the same erase voltage, the conductivity of the semiconductor channel layer 4 of the FeFET memory is higher and the voltage division is smaller, which increases the voltage division of the ferroelectric layer 3. The electric dipoles of the ferroelectric layer 3 are effectively and fully flipped, resulting in a better erase effect. This, in turn, increases the storage window of the FeFET. The increase in storage window is beneficial for the application of FeFET in multi-value storage and improves the reliability of the memory in practical applications.

[0028] In some embodiments of the present invention, the gate electrode 2 is made of molybdenum, which has a work function WF of 4.37 eV, and can achieve a storage window of more than 1.9 V.

[0029] Furthermore, the thickness of the gate electrode 2 is 10-100nm, for example, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, etc.

[0030] It should be noted that in other embodiments, the gate electrode 2 can also be made of other conductive materials, as long as the work function WF of the conductive material is less than 4.5 eV, such as Ta, Ga, Ti, etc., with molybdenum Mo being the preferred material.

[0031] In some embodiments of the present invention, the material of the ferroelectric layer 3 is Zr-doped HfO2.

[0032] In this embodiment, the molar ratio of Hf to Zr in the ferroelectric layer 3 is close to 1:1 to achieve the maximum remanent polarization intensity. It should be understood that other component ratios of Hf and Zr in the ferroelectric layer 3 that are close to this value are also acceptable and are not limited here.

[0033] Furthermore, the thickness of the ferroelectric layer 3 is 3-20nm, for example, 3nm, 5nm, 10nm, 15nm, 20nm, etc.

[0034] In some embodiments of the present invention, the material of the semiconductor channel layer 4 is an oxide semiconductor or polysilicon or other materials with semiconductor properties.

[0035] Preferably, the oxide semiconductor can be indium gallium zinc oxide (IGZO).

[0036] Furthermore, the In:Ga:Zn molar ratio of indium gallium zinc oxide (IGZO) is approximately 1:1:1. It should be understood that other component ratios close to this value are also acceptable and are not limited here.

[0037] In some embodiments of the present invention, the substrate layer 1 is made of SiO2 / Si (a silicon dioxide SiO2 thin film is coated on the surface of a silicon Si substrate).

[0038] The thickness of SiO2 is 100-500nm, and the thickness of Si is 300-600μm.

[0039] In some embodiments of the present invention, the source / drain electrode layer 5 includes a source and a drain, and the materials of the source and drain are Ti / Au (titanium Ti as the base layer and gold Au as the conductive layer) or Ni / Au (nickel Ni as the base layer and gold Au as the conductive layer).

[0040] In the Ti / Au configuration, the Ti thickness is 10 nm and the Au thickness is 30 nm; in the Ni / Au configuration, the Ni thickness is 10 nm and the Au thickness is 30 nm.

[0041] It should be noted that Ti / Au and Ni / Au can also be of other thicknesses, which are not limited here.

[0042] This embodiment also proposes a fabrication method for fabricating the above-mentioned ferroelectric field-effect transistor memory, which specifically includes the following steps:

[0043] S1: Provide a substrate layer and clean the substrate layer.

[0044] In this embodiment, the substrate layer is sequentially soaked in acetone, cleaned and dried with anhydrous ethanol; then soaked and rinsed with deionized water and dried.

[0045] S2: The gate electrode is fabricated on the substrate using a material with a work function WF less than 4.5 eV.

[0046] In this embodiment, a gate electrode is deposited on a substrate using a deposition process. Then, photoresist is coated onto the gate electrode, exposed and developed, etched, and the photoresist is removed to achieve gate electrode patterning.

[0047] Preferably, the deposition process for depositing the gate electrode on the substrate includes, but is not limited to, thin film deposition processes such as ion beam sputtering, DC sputtering, reactive sputtering, magnetron sputtering, atomic layer deposition (ALD), and electron beam evaporation, which can ensure the conductivity of the gate electrode, the integrity of the gate electrode / ferroelectric layer interface, and the flatness of the electrode film (especially the gate electrode).

[0048] Preferably, the photoresist coated on the gate electrode is a negative photoresist, then pre-baked at 150°C for 2 minutes, exposed, post-baked at 120°C for 2 minutes, immersed in developer for 30 seconds, and then rinsed with deionized water and dried.

[0049] In another embodiment, the photoresist on the gate electrode can also be a positive photoresist, and the hardening and exposure operations can be adjusted accordingly, which will not be described in detail here.

[0050] Preferably, the gate electrode is etched using a dry etching method to remove excess metal, and then the photoresist is removed in a photoresist remover solution.

[0051] S3: Fabricate a ferroelectric layer on the gate electrode.

[0052] In this embodiment, a Zr-doped HfO2 ferroelectric layer is first prepared on the gate electrode using atomic layer deposition (ALD). Then, photoresist is coated, exposed, developed, etched, and the photoresist is removed to achieve the patterning of the ferroelectric layer.

[0053] Preferably, the deposition temperature range for preparing the Zr-doped HfO2 ferroelectric layer is 280-350℃.

[0054] Specifically, in this embodiment, the precursor for Hf is tetra(ethylmethylamido)hafnium(IV) (TEMAH), with the chemical formula Hf(NCH3C2H5)4; the precursor for Zr is tetra(ethylmethylamido)zirconium(IV) (TEAZ), with the chemical formula Zr(NCH3CH5)4; and deionized water is used as the oxygen source. The deposition temperature range is typically 280-300°C. The Zr and Hf precursors are heated to 100-140°C, the deionized water is kept at room temperature of 20°C, and N2 is selected as the carrier gas with a flow rate of 40-80 sccm.

[0055] It should be noted that in other implementations, the precursor and oxygen source may also be selected from other options.

[0056] Preferably, a negative adhesive is coated on the Zr-doped HfO2 ferroelectric layer, pre-baked at 150°C for 2 min, exposed and then post-baked at 120°C for 2 min, developed by immersing in developer for 30 s, and then rinsed with deionized water and dried.

[0057] In another embodiment, the photoresist on the ferroelectric layer can also be a positive photoresist, and the hardening and exposure operations can be adjusted accordingly, which will not be described in detail here.

[0058] Preferably, the ferroelectric layer etching includes, but is not limited to, dry etching or wet etching to remove excess ferroelectric material, and then the photoresist is removed in the photoresist remover.

[0059] S4: Fabricate a semiconductor channel layer on the ferroelectric layer.

[0060] In this embodiment, a semiconductor channel layer is first deposited on the ferroelectric layer using a deposition process. Then, photoresist is coated, exposed and developed on the semiconductor channel layer, and etched and the photoresist is removed to pattern the semiconductor channel layer. After that, photoresist is coated again on the semiconductor channel layer and exposed and developed.

[0061] Preferably, the deposition process for depositing the semiconductor channel layer on the ferroelectric layer includes, but is not limited to, magnetron sputtering, ALD, pulsed laser deposition (PLD), etc., which can ensure the semiconductor properties of the semiconductor channel layer, the integrity of the ferroelectric layer / semiconductor channel layer interface, and the flatness of the semiconductor thin film.

[0062] Preferably, a negative adhesive is coated on the semiconductor channel layer, pre-baked at 150°C for 2 minutes, exposed and then post-baked at 120°C for 2 minutes, developed by immersing in developer for 30 seconds, and then rinsed with deionized water and dried.

[0063] In another embodiment, the photoresist on the semiconductor channel layer can also be a positive photoresist, and the hardening and exposure operations can be adjusted accordingly, which will not be described in detail here.

[0064] Preferably, the semiconductor channel layer etching includes, but is not limited to, dry etching or wet etching to remove excess semiconductor material, and then the photoresist is removed in the photoresist remover.

[0065] In another embodiment, a stripping process can also be used to pattern the semiconductor channel layer, and the photoresist can be adjusted accordingly. For example, the stripping process specifically involves: soaking in an acetone solution until the photoresist and excess material fall off; then soaking in anhydrous ethanol to remove the acetone; and finally rinsing with deionized water and drying.

[0066] S5: Fabricate source and drain electrode layers on the semiconductor channel layer.

[0067] In this embodiment, the source and drain electrodes are fabricated using electron beam evaporation or other deposition processes.

[0068] Preferably, the deposition process includes, but is not limited to, magnetron sputtering, ALD, PLD, etc., which can ensure the conductivity of the source and drain electrodes, the integrity of the semiconductor channel layer / source / drain electrode layer interface, and the flatness of the electrode film.

[0069] S6: Annealing after removing photoresist and excess metal.

[0070] In this embodiment, the annealing process includes, but is not limited to, rapid thermal annealing, furnace tube annealing, microwave annealing, etc. The general annealing conditions are a temperature of 300°C, a time of 100s, and a nitrogen atmosphere.

[0071] Furthermore, the annealing process temperature can be between 300℃ and 500℃, the annealing time can be adjusted, and the annealing atmosphere can be nitrogen, oxygen, or other atmospheres, as long as the ferroelectric properties of the ferroelectric material and the semiconductor properties of the semiconductor material are guaranteed.

[0072] like Figure 2 and Figure 3 As shown, the FeFET memory fabricated using the above method achieves a larger storage window compared to the conventional tin (TiN) or tungsten (W) gate electrode fabrication. This is because the FeFET memory with a low work function gate electrode has a lower resistance state in its semiconductor channel layer (semiconductor layer) compared to the FeFET memory with a high work function gate electrode. This results in a higher conductivity and lower voltage division within the semiconductor channel layer, increasing the voltage division of the ferroelectric layer. Consequently, the electric dipoles of the ferroelectric layer are effectively and fully flipped, achieving a better erasure effect and thus improving the storage window of the FeFET.

[0073] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A ferroelectric field-effect transistor memory, characterized in that, It includes a substrate layer, a gate electrode, a ferroelectric layer, a semiconductor channel layer and a source / drain electrode layer stacked sequentially, wherein the work function WF of the gate electrode material is less than 4.5 eV.

2. The ferroelectric field-effect transistor memory according to claim 1, characterized in that, The gate electrode is made of molybdenum.

3. The ferroelectric field-effect transistor memory according to claim 2, characterized in that, The thickness of the gate electrode is 10-100 nm.

4. The ferroelectric field-effect transistor memory according to claim 1, characterized in that, The ferroelectric layer is made of Zr-doped HfO2.

5. The ferroelectric field-effect transistor memory according to claim 4, characterized in that, The thickness of the ferroelectric layer is 3-20 nm.

6. The ferroelectric field-effect transistor memory according to claim 1, characterized in that, The semiconductor channel layer is made of oxide semiconductor or polycrystalline silicon.

7. A method for fabricating a ferroelectric field-effect transistor memory, characterized in that, include: Provide a substrate layer; The gate electrode is fabricated on the substrate using a material with a work function WF less than 4.5 eV; A ferroelectric layer is fabricated on the gate electrode; A semiconductor channel layer is fabricated on the ferroelectric layer; Source and drain electrode layers are fabricated on the semiconductor channel layer; A ferroelectric field-effect transistor memory was obtained.

8. The method for fabricating a ferroelectric field-effect transistor memory according to claim 7, characterized in that, The fabrication of the gate electrode includes: A gate electrode is deposited on the substrate using a deposition process; Photoresist is coated onto the gate electrode, exposed and developed, etched, and the photoresist is removed to achieve gate electrode patterning.

9. The method for fabricating a ferroelectric field-effect transistor memory according to claim 8, characterized in that, The photoresist coated on the gate electrode is a negative photoresist, then it is pre-baked at 150°C for 2 minutes, exposed, post-baked at 120°C for 2 minutes, and then immersed in the developing solution for 30 seconds for development.

10. The method for fabricating a ferroelectric field-effect transistor memory according to claim 7, characterized in that, The fabrication of the ferroelectric layer includes: A Zr-doped HfO2 ferroelectric layer was prepared on the gate electrode using atomic layer deposition (ALD) at a temperature range of 280-350 °C. Photoresist is coated onto the ferroelectric layer, exposed and developed, etched, and the photoresist is removed to achieve the patterning of the ferroelectric layer.