Low-cost thick-specification 590MPa nickel-free weathering steel and manufacturing method thereof

By designing low-cost chemical compositions and optimizing processes, a high-strength, nickel-free weathering steel with good weldability was prepared, solving the problems of high cost and insufficient thickness in existing technologies. This resulted in high weather resistance and excellent surface quality, making it suitable for large-scale engineering projects.

CN121320839APending Publication Date: 2026-01-13BAOSHAN IRON & STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410876283.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2026-01-13

AI Technical Summary

Technical Problem

Existing weathering steels, while adding nickel to prevent copper brittle cracking, are too expensive and have limited thickness specifications, failing to meet the needs of large-scale projects. Furthermore, their weather resistance and weldability are insufficient.

Method used

The design employs a low-cost chemical composition, including a reasonable ratio of C, Si, Mn, Cu, Cr, Ti, V, B, Al, and Zr. Through micro-Ti-B treatment and single-pass high-reduction rolling, combined with a rapid cooling process, an equiaxed ferrite + pearlite + a small amount of granular bainite microstructure is formed, avoiding copper brittle cracks and achieving high strength and good weldability.

Benefits of technology

Without adding nickel, a steel plate with a yield strength ≥590MPa, tensile strength ≥710MPa, impact energy of 190~360J at -20℃, yield strength ratio ≤0.85 was prepared. The steel plate surface was free of copper brittle cracks and the thickness could reach 60mm, thus expanding the application range of weathering steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121320839A_ABST
    Figure CN121320839A_ABST
Patent Text Reader

Abstract

The invention discloses low-cost thick-specification 590 MPa nickel-free weathering steel and a manufacturing method thereof. The low-cost thick-specification 590 MPa nickel-free weathering steel comprises the following chemical components in percentage by weight: 0.06 to 0.09 percent of C, 0.65 to 0.85 percent of Si, 0.53 to 0.83 percent of Mn, 0.010 to 0.014 percent of P, less than or equal to 0.003 percent of S, 0.3 to 0.5 percent of Cu, 0.3 to 0.5 percent of Cr, 0.020 to 0.030 percent of Ti, 0.020 to 0.030 percent of V, 0.0015 to 0.0020 percent of B, 0.020 to 0.030 percent of Al, 0.0015 to 0.0020 percent of Zr and the balance of Fe and other inevitable impurities. The chemical components need to simultaneously meet the following requirements: the welding crack sensitive index Pcm is less than or equal to 0.22%; the carbon equivalent CEV is less than or equal to 0.35%; the weather-proof index I is greater than or equal to 6.2; cu / P + 5 * Si > = 25; 0.06% < = (Al + Ti + V) < = 0.085%. According to the weathering steel, the yield strength is larger than or equal to 590 MPa, the tensile strength is larger than or equal to 710 MPa, the impact energy at the temperature of-20 DEG C is 190-360 J, the yield ratio is smaller than or equal to 0.85, and no copper brittleness crack exists on the surface of a steel plate.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of weathering steel, in particular to a low-cost thick-gauge 590MPa nickel-free weathering steel and a manufacturing method thereof. BACKGROUND

[0002] Weathering steel, i.e. low-alloy atmospheric corrosion-resistant steel, is a low-carbon steel with the addition of a small amount of alloying elements Cu, Ni, Cr, P, Mn, Sn, etc. to improve its atmospheric corrosion resistance. In weathering steel products, 0.2-0.5% of copper must generally be added. However, copper elements are prone to enrichment at the interface between the substrate surface layer and the oxide layer after high-temperature oxidation of the steel, forming "copper brittle" crack defects. Therefore, a high-melting point copper-nickel compound is generally formed by adding nickel elements to prevent the formation of copper-induced thermal cracks. The amount of nickel added is related to the content of copper, and the nickel-copper ratio is generally required to be close to 1:1. However, the cost of nickel element is too high, which limits the widespread use of weathering steel in application fields with higher economic requirements.

[0003] Chinese patent 202311320781.8 discloses "a 355MPa low-cost weathering steel and a preparation method thereof", the main chemical composition of the steel plate is as follows: C: 0.06-0.08%, Si: 0.3-0.5%, Mn: 0.45-0.55%, P≤0.018%, Cu: 0.2-0.3%, Cr: 0.45-0.50%, Ni: 0.06-0.08%, La: 30-60ppm, and the rest is Fe and inevitable impurities. On the one hand, the patent adds Ni element and lanthanum La element in the composition, which greatly increases the production cost of the steel plate; on the other hand, the insufficient Cu content leads to a weathering index I of only 3.0-4.0, insufficient corrosion resistance, and a strength level of only 355MPa. Finally, the thickness specification of the steel plate is relatively narrow, which can only cover 1.8-3.0mm, and cannot meet the use requirements of domestic large-scale projects such as bridges, railways, etc.

[0004] Chinese patent 202110856859.2 discloses "a 340MPa low-cost weathering steel for cold-rolled automobiles and a manufacturing method thereof", the main chemical composition of the steel plate is as follows: C≤0.10%, Si: 0.10-0.45%, Mn: 0.30-0.60%, P: 0.06-0.13%, Cu: 0.2-0.4%, Ni: 0.1-0.2%, and the balance is Fe and inevitable impurities. To avoid copper brittleness, the patent also adds Ni element in the composition, which is relatively high in cost and insufficient in strength.

[0005] Chinese patent 202010769262.X discloses "a 400MPa grade high-silicon weathering steel and its preparation method and application", the main chemical composition of the steel plate is: C≤0.12%, Si: 1.20-2.00%, Mn≤1.50%, P: 0.005-0.030%, Cr: 0.20-0.80%, Ni: 0.10-0.40%, Cu: 0.20-0.60%, the balance is Fe and inevitable impurities. The patent weathering index I reaches 6.0 or more, but the addition of Cr, Ni and other precious metal elements increases the cost, and the high Si content affects the welding performance.

[0006] Chinese patent 202010095562.4 discloses "a method for producing economic weathering steel by using RE-P reinforcement and preparation process", the main chemical composition of the steel plate is: C: 0.01-0.08%, Si: 0.10-0.30%, Mn: 1.30-1.70%, P: 0.06-0.10%, Cu: 0.08-0.20%, Al: 0.015-0.06%, Re: 0.02-0.06%, the balance is Fe and inevitable impurities. Since the amount of Cu element added is very small, the probability of copper brittleness is low, so no Ni element is added, but rare earth Re element is still added to refine the grain. Although the alloy cost is not high, the weathering index I is only 1.0-3.0, which reduces the weather resistance.

[0007] With the increasing demand for resource conservation and cost control worldwide, the development of low-cost, high-performance weathering steel has become a research hotspot in the field of materials science. Especially for thick gauge steel, how to achieve 590MPa strength level of high strength and good welding performance, surface quality, while maintaining excellent atmospheric corrosion resistance without using expensive alloy elements such as nickel, is the key challenge of current research. SUMMARY

[0008] The purpose of the present application is to provide a low-cost thick-gauge 590MPa nickel-free weathering steel and its manufacturing method. The obtained weathering steel has high strength and weather resistance, good surface quality, low yield ratio and easy welding characteristics without adding Ni, and the thickest steel can reach 60mm, expanding the use range of high-strength weathering steel, and can be widely used in the production of corrosion-resistant structural parts. The yield strength of the weathering steel is ≥590MPa, the tensile strength is ≥710MPa, the impact energy at -20℃ is 190-360J, the yield ratio is ≤0.85, and the steel plate surface is free of "copper brittleness" cracks.

[0009] To achieve the above purpose, the technical scheme of the present application is as follows:

[0010] A low-cost thick-gauge 590MPa nickel-free weather-resistant steel, the chemical composition of which is as follows: C: 0.06-0.09%, Si: 0.65-0.85%, Mn: 0.53-0.83%, P: 0.010-0.014%, S: ≤0.003%, Cu: 0.3-0.5%, Cr: 0.3-0.5%, Ti: 0.020-0.030%, V: 0.020-0.030%, B: 0.0015-0.0020%, Al: 0.020-0.030%, Zr: 0.0015-0.0020%, and the balance of Fe and other inevitable impurities; and the chemical composition needs to meet the following conditions simultaneously:

[0011] welding crack sensitivity index Pcm≤0.22%;

[0012] carbon equivalent CEV≤0.35%;

[0013] weathering index I≥6.2;

[0014] Cu / P+5*Si≥25;

[0015] 0.06%≤(Al+Ti+V)≤0.085%.

[0016] wherein, Pcm= %C+ %Si / 30+ %Mn / 20+ %Cu / 20+ %Ni / 60+ %Cr / 20+ %Mo / 15+ %V / 10+5% B;

[0017] CEV= %C+ %Mn / 6+ (%Cr+ %Mo+ %V) / 5+ (%Ni+ %Cu) / 15;

[0018] I=26.01(%Cu)+3.88(%Ni)+1.20(%Cr)+1.49(%Si)+17.28(%P)-7.29(%Cu)(%Ni)-9.10(%Ni)(%P)-33.39(%Cu) 2 ;

[0019] In the above formula, only the numerical value before the percentage symbol of the corresponding element content is substituted when calculating, for example, the C content is 0.04%, only 0.04 is substituted when calculating.

[0020] Further, the balance is Fe and other inevitable impurities.

[0021] The microstructure of the weather-resistant steel is equiaxed ferrite+pearlite+ a small amount of granular bainite; wherein the volume fraction of equiaxed ferrite is 40-60%, the volume fraction of granular bainite is ≤10%, the rest is pearlite, the average grain size is 5-8μm, the grain size is ≥10, and the inclusion level is ≤0.4 level.

[0022] The number density of heterogeneous nucleated particles in the microstructure of the weathering steel described in this invention is 6.35 × 10⁻⁶. 4 ~7.65×10 4 / mm 3 The proportion of ferrite heterogeneous nuclei is ≥60%, and the heterogeneous nuclei are Ti(C,N) and V(C,N) composite precipitates.

[0023] The weathering steel described in this invention has a yield strength ≥590MPa, a tensile strength ≥710MPa, an impact energy of 190~360J at -20℃, a yield strength ratio ≤0.85, and no "copper brittleness" cracks on the surface of the steel plate.

[0024] The thickness range of the weathering steel described in this invention is 20–60 mm.

[0025] In the chemical composition design of the low-cost, thick-gauge 590MPa nickel-free weathering steel described in this invention:

[0026] C: In the steel of this invention, carbon can stabilize austenite and improve hardenability, thereby increasing the strength of the steel plate. However, an increase in carbon content will increase brittle phases and carbides, reduce corrosion resistance, and significantly increase the carbon equivalent (CEV) and weld crack sensitivity index (Pcm), thus seriously affecting the toughness and weldability of the steel plate. Therefore, in this invention, the carbon content is controlled at 0.06-0.09%.

[0027] Si: In the steel of this invention, Si plays a similar role to P, increasing the resistivity and corrosion resistance index (I value) of the steel along with other alloying elements (such as Cu, Cr, P, Ni), enhancing the corrosion resistance of the steel under natural conditions, and inhibiting the formation of hot cracks in Cu-containing steel. Therefore, the Si content is controlled at 0.65% to 0.85% in this invention.

[0028] Mn: In the steel of this invention, Mn can improve the strength and hardenability of the steel, playing a role in solid solution strengthening. However, excessive Mn content will lead to severe segregation of the steel, increase costs, and easily generate MnS inclusions, forming cell reactions that can easily detach from the matrix and form voids, reducing the toughness and corrosion resistance of the steel. Therefore, in this invention, the Mn content is controlled at 0.53-0.83%.

[0029] Cu: In the steel of this invention, Cu is the most important corrosion-resistant element, promoting the density and stability of the internal rust layer and thus improving atmospheric corrosion resistance. However, excessively high Cu content can easily cause "copper embrittlement" cracking defects. Furthermore, Cu is a valuable alloying element, and increasing its content leads to a significant increase in steel cost. As can be seen from the I value expression, I reaches its maximum value when the Cu content is 0.39%. Therefore, in this invention, the Cu content is controlled between 0.3% and 0.5%.

[0030] P: In the steel of this invention, P has a strong solid solution strengthening effect, and when combined with Cu, it can significantly improve the corrosion resistance of the steel. Excessive P content can lead to compositional segregation, resulting in hot cracking and deteriorating weldability, while excessively low P content increases steelmaking costs. Therefore, in this invention, the P content is controlled at 0.010–0.014%.

[0031] Cu / P + 5*Si ≥ 25: In the steel of this invention, while higher Cu and Si contents generally result in better weather resistance, the minimum addition amounts need to be determined due to cost and other mechanical property limitations. Furthermore, phosphorus (P) is the most effective alloying element for improving atmospheric corrosion resistance and helps form a uniform rust protective film on the steel surface. However, the presence of P easily leads to internal and external cracks in the steel and also deteriorates its toughness, especially reducing its low-temperature impact toughness. This invention controls Cu / P + 5*Si ≥ 25 to ensure a suitable ratio of copper to phosphorus in the steel, while maintaining a sufficiently high silicon content to form an effective protective film. The copper to phosphorus ratio ensures that copper can form stable compounds with phosphorus, while the silicon content directly affects the formation and stability of the protective film.

[0032] Cr: In the steel of this invention, Cr is the main corrosion-resistant element. Increasing the Cr content can improve the strength and hardenability of the steel, and it does not produce significant component segregation in the steel. However, if the content is too high, it will have an adverse effect on the weldability. Therefore, in this invention, the Cr content is controlled at 0.3% to 0.5%.

[0033] Micro-Ti-B treatment: In the steel of this invention, B can significantly increase the critical cooling rate of martensite or bainite, thereby improving the hardenability of the steel. However, a B content exceeding 0.0020% will lead to the formation of carbides at grain boundaries, affecting toughness. Therefore, this invention controls the B content at 0.0015–0.0020%, close to the upper limit of the embrittlement point. Simultaneously, to ensure sufficient acid-soluble B in the steel, 0.020–0.030% Ti is added to fix N in the steel, preventing the formation of BN and ensuring an effective B content. This allows the steel to maintain good mechanical properties even at a thickness of 60 mm. Furthermore, Ti(C,N) can precipitate during rolling to refine the grains and improve the strength and toughness of the steel. Therefore, the Ti content is controlled at 0.020–0.030% in this invention.

[0034] V-Ti treatment: In the steel of this invention, the combined use of V and Ti mainly serves to refine the grains. During the finishing rolling process, the austenite grains are refined by the deformation-induced precipitation of heterogeneous nucleation particles, such as Ti(C,N) and V(C,N) composite precipitates. At the same time, the precipitated carbonitrides pin dislocations and also play a precipitation strengthening role, so that the room temperature microstructure remains fine equiaxed grains in the untempered state, thereby achieving the effect of elements such as La and Re commonly used in weathering steel. Therefore, the V content in this invention is controlled at 0.020-0.030%.

[0035] Al: In the steel of this invention, the addition of Al can effectively prevent the formation of carbides in the steel, facilitate the solid solution of carbon in austenite, improve the stability of austenite during cooling, and greatly benefit the improvement of the toughness of the steel plate. However, if the aluminum content in the steel is too high, it will increase the difficulty of smelting and casting, raise manufacturing costs, and cause excessive oxide formation, which will deteriorate the quality of the steel plate. Therefore, this invention controls the Al content at 0.020-0.030%.

[0036] Meanwhile, this invention controls the content of Ti(C,N) and V(C,N) heterogeneous nuclei to be 0.06% ≤ (Al+Ti+V) ≤ 0.085%, ensuring that the number density of Ti(C,N) and V(C,N) heterogeneous nuclei formed in the tissue is 6.35 × 10⁻⁶. 4 ~7.65×10 4 / mm 3 The content of heterogeneous ferrite nucleation is ≥60%, which fully utilizes their role in improving corrosion resistance and effectively enhances the weather resistance of the steel plate. Excessive content may lead to increased costs and adverse effects on other properties (such as weldability), while insufficient content has little effect on improving corrosion resistance.

[0037] Zr: In the steel of this invention, Zr can replace expensive La and RE to purify molten steel, reduce hard oxide inclusions, refine the grain structure to achieve uniformity, enhance the polarization resistance of the steel plate, and enhance the enrichment of corrosion-resistant elements (Cu, Cr, etc.) as oxides within the rust layer. This results in the formation of a shallow zirconium oxide passivation film on the steel plate surface, significantly improving the steel's corrosion resistance, especially in a hydrogen sulfide atmosphere. Furthermore, Zr is a strong carbide-forming element, which greatly hinders grain growth, ensuring the strength and toughness of thick steel plates. Simultaneously, the addition of Zr shifts the CCT curve to the right, enhancing the stability of supercooled austenite. This allows for the formation of a fine ferrite and pearlite multiphase structure after reheating from the 410–450°C cooling temperature, thus contributing to a reduction in the yield strength ratio. Therefore, the Zr content in this invention is controlled at 0.0015–0.0020%.

[0038] The composition design employs lower C and Si content, while adding Cu and Zr to improve weather resistance. Adjusting the Cu / P and Si ratio appropriately (Cu / P + 5*Si ≥ 25) ensures that the weathering steel possesses excellent mechanical properties and weather resistance. Adding a small amount of Zr to replace expensive La and RE purifies the molten steel, reduces hard oxide inclusions, refines the grain structure, enhances the polarization resistance of the steel plate, and enhances the enrichment of corrosion-resistant elements (Cu, Cr, etc.) within the rust layer as oxides. This forms a shallow zirconium oxide passivation film on the steel plate surface, significantly improving the steel's corrosion resistance, especially in hydrogen sulfide atmospheres. Utilizing relatively inexpensive V and Ti, and controlling the content to 0.06% ≤ (Al + Ti + V) ≤ 0.085%, ensures that the number density of Ti(C,N) and V(C,N) heterogeneous nucleation particles formed in the microstructure is 6.35 × 10⁻⁶. 4 ~7.65×10 4 / mm 3 The proportion of heterogeneous ferrite nucleation is ≥60%, which fully leverages their role in improving corrosion resistance and effectively enhances the weather resistance of steel plates.

[0039] The method for manufacturing low-cost, thick-gauge 590MPa nickel-free weathering steel according to the present invention includes the following steps:

[0040] 1) Smelting and refining

[0041] The above-mentioned components are smelted, refined, and cast into billets;

[0042] 2) Slab heating

[0043] Heating temperature: 1060~1080℃, holding time: 1~2h;

[0044] 3) Rolling

[0045] Roughing rolling start temperature: 900~1000℃, single-pass rolling reduction rate in roughing stage ≥15%;

[0046] Finishing rolling start temperature: 870~890℃, single-pass rolling reduction rate in the finishing rolling stage ≥20%, finishing rolling temperature: 820~840℃;

[0047] 4) Cooling

[0048] Cooling start temperature: 770~810℃, cooling stop temperature: 410~450℃, cooling rate ≥45℃ / s.

[0049] Preferably, in step 4), the cooling is water cooling.

[0050] Preferably, in step 4), the steel plate is air-cooled to room temperature after the cooling process is stopped.

[0051] In the manufacturing method described in this invention:

[0052] The slab is heated at a relatively low temperature, controlled between 1060 and 1080°C, below the melting point of Cu (1083°C). This is because when the Cu content in the steel is ≥0.2% and the temperature is above 1083°C, selective oxidation occurs on the surface, leading to the transformation of CuO + Fe into FeO + Cu in an oxidizing atmosphere. This reduces the Fe content on the surface and increases the Cu content, forming a Cu-rich phase. This process continues until the Cu content exceeds the solubility of Cu in Fe. At this point, the Cu-rich phase in the steel is in a molten state and begins to melt. When this process reaches a certain point, it causes surface scaly cracking during rolling deformation, resulting in "copper embrittlement" defects. This invention, through research, has found that controlling the heating temperature below the melting point of copper can prevent the dissolution of copper, thus preventing the oxidation and transformation of Cu on the slab surface and eliminating concerns about copper embrittlement.

[0053] Rolling is divided into roughing and finishing. The initial rolling temperature for roughing is 900–1000℃, with a single-pass reduction rate of ≥15% during the roughing stage, which fully breaks down and refines the original austenite grains. The initial rolling temperature for finishing is 870–890℃, with a single-pass reduction rate of ≥20% during the finishing stage. This high reduction rolling elongates the austenite grains along the rolling direction and simultaneously introduces a large number of deformation bands into the grains, increasing the grain boundary area and increasing the dislocation density and nucleation sites in the austenite. The dislocations are carbon. The diffusion of small atoms such as carbon and nitrogen provides a rapid pathway, and carbon and nitrogen atoms easily agglomerate at dislocation pile-ups. At these pile-ups, Ti(C,N) and V(C,N) deformation precipitation is induced. These dispersed, fine metallic carbonitrides can more effectively pin dislocations, further hindering grain growth and ensuring that the average grain size of the original austenite in the microstructure is 5–8 μm, with a grain size ≥10. This increases corrosion resistance and produces deformation strengthening, grain refinement strengthening, and precipitation strengthening. The final rolling temperature is controlled at 820–840℃. Strict control of the final rolling temperature helps prevent the fine deformed grains from recovering and recrystallizing, increasing deformation resistance and producing deformation strengthening, thereby simultaneously improving the strength and toughness of the steel plate.

[0054] During the cooling process, the starting temperature is controlled at 770-810℃, and the cooling rate is greater than that of conventional steel plates. This increases the supercooling degree of the steel plate during cooling. The cooling rate is controlled at ≥45℃ / s, and a large volume of water cooling is used. This is beneficial for improving the nucleation rate and refining the grains, allowing the rolled deformed grains to remain in a broken state at room temperature.

[0055] After air cooling at a stopping temperature of 410–450℃, the steel plate will reheat to the pearlite transformation zone. This releases residual stress, achieving a self-tempering effect. Furthermore, 410–450℃ is the optimal precipitation temperature for heterogeneous nucleation particles such as Ti(C,N) and V(C,N) after the steel plate reheats, which increases the nucleation rate and inhibits grain growth, thereby improving the steel plate's strength and toughness. The final result is a multiphase microstructure consisting of fine equiaxed ferrite, pearlite, and a small amount of granular bainite, achieving a low yield strength ratio while maintaining strength and toughness.

[0056] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0057] 1. This invention employs a low C and low Si content in its composition design. Through the use of Cu, Zr, V, and Ti elements, and by adjusting the appropriate Cu / P and Si ratios, Cu / P + 5*Si ≥ 25 is controlled to ensure the mechanical properties and weather resistance of the steel. Furthermore, by controlling the content to 0.06% ≤ (Al + Ti + V) ≤ 0.085%, the number density of Ti(C, N) and V(C, N) heterogeneous nucleation particles formed in the microstructure is ensured to be 6.35 × 10⁻⁶. 4 ~7.65×10 4 / mm 3 By fully utilizing their role in improving corrosion resistance, the weather resistance of the steel is effectively improved, ensuring that the weather resistance index I of the steel of this invention is ≥6.2. With a low Si content and without the addition of precious metal elements such as Ni and Nb, and with the addition of a small amount of Cr, a steel with high strength, high weather resistance, and excellent weldability is prepared.

[0058] 2. Based on the composition design, this invention controls the heating temperature within a relatively low range of 1060–1080℃ to avoid surface scaly cracking during subsequent rolling deformation caused by oxidation and dissolution under high-temperature oxidation due to excessive Cu content, thus preventing "copper embrittlement" defects. Traditionally, the solution to "copper embrittlement" defects in weathering steel is to add nickel, forming a copper-nickel compound to address the surface copper embrittlement problem caused by Cu enrichment. This invention achieves high weather resistance and good surface quality in steel without adding Ni.

[0059] 3. In the rolling process, this invention employs single-pass high-reduction rolling to increase the dislocation density and nucleation points in austenite. This induces V(C,N) and Ti(C,N) deformation precipitation at dislocation entanglement sites, further hindering grain growth. The average grain size in the microstructure is 5-8 μm, with a grain size ≥10, resulting in deformation strengthening, fine-grain strengthening, and precipitation strengthening. Combined with subsequent rapid cooling, controlling the cooling rate to ≥45℃ / s, and controlling the final rolling temperature and cooling temperature, the rolled deformed grains are retained in a fragmented state at room temperature, fully utilizing the effects of V and Ti to improve the steel's strength. This achieves high strength and weather resistance in a composition system that does not require the addition of precious alloying elements such as La, Re, and Nb. Furthermore, since this invention does not add Nb, it avoids the problem of Nb carbides being unable to dissolve at lower heating temperatures.

[0060] 4. To obtain thick-gauge weathering steel, micro-Ti-B treatment is used in the composition, and the single-pass high reduction and final cooling rate are controlled in the process. This allows the grains to be fully broken down and retained in solid solution, thereby refining the grains in the core of the steel plate. While ensuring the mechanical properties of the material, thick-gauge steel can be produced, with a maximum plate thickness of 60mm. In contrast, the existing technology can only produce weathering steel with a strength level of 590MPa at a maximum thickness of 8mm, which cannot meet the needs of large-scale domestic projects such as bridges and railways. Attached Figure Description

[0061] Figure 1 This is a photograph of the microstructure of the steel plate in Embodiment 1 of the present invention. Detailed Implementation

[0062] The present invention will be further described below with reference to the embodiments and accompanying drawings.

[0063] The components of the embodiments and comparative examples of the present invention are shown in Tables 1 and 2, with the balance containing Fe and other unavoidable impurities.

[0064] The process parameters of the embodiments and comparative examples of the present invention are shown in Table 3, and the steel properties of the embodiments and comparative examples of the present invention are shown in Table 4.

[0065] Figure 1 The image shows a microstructure of the steel plate in Example 1 of this invention. As can be seen from the image, the microstructure of the steel obtained by this invention is equiaxed ferrite + pearlite + a small amount of granular bainite. The volume percentage of equiaxed ferrite is 40-60%, the volume percentage of granular bainite is ≤10%, and the remainder is pearlite. The average grain size is 5-8 μm, the grain size is ≥10, and the inclusion level is ≤0.4.

[0066] The steel plates of the embodiments of the present invention were tested in accordance with the standard TB / T-1993 "Test Method for Cyclic Immersion Corrosion of Weathering Steel for Railways". The corrosion rates of the embodiments and comparative examples after 3 weeks were obtained in a solution containing 0.01 mol / L sodium bisulfite.

[0067] The corrosion resistance test results are shown in Table 5. The comparative example is purchased ordinary weathering steel Q590NH, with specific composition ratios shown in Table 1. The processing and properties of the purchased material conform to the national standard GB / T4171 Weathering Structural Steel. The corrosion rates of Examples 1-8 are all lower than those of the comparative example, and because Ni is not added to these examples, the production cost is significantly reduced.

[0068]

[0069]

[0070]

[0071]

[0072]

[0073]

Claims

1. A low-cost, thick-gauge 590MPa nickel-free weathering steel, with the following chemical composition by weight percentage: C: 0.06–0.09%, Si: 0.65–0.85%, Mn: 0.53–0.83%, P: 0.010–0.014%, S≤0.003%, Cu: 0.3–0.5%, Cr: 0.3–0.5%, Ti: 0.020–0.030%, V: 0.020–0.030%, B: 0.0015–0.0020%, Al: 0.020–0.030%, Zr: 0.0015–0.0020%, with the balance including Fe and other unavoidable impurities; and the chemical composition must simultaneously meet the following requirements: The weld crack sensitivity index Pcm ≤ 0.22%; Carbon equivalent (CEV) ≤ 0.35%; Weather resistance index I ≥ 6.2; Cu / P+5*Si≥25; 0.06%≤(Al+Ti+V)≤0.085%.

2. The low-cost, thick-gauge 590MPa nickel-free weathering steel as described in claim 1, characterized in that, The balance consists of Fe and other unavoidable impurities.

3. The low-cost, thick-gauge 590MPa nickel-free weathering steel as described in claim 1 or 2, characterized in that, The microstructure of the weathering steel is equiaxed ferrite + pearlite + a small amount of granular bainite; wherein the volume percentage of equiaxed ferrite is 40-60%, the volume percentage of granular bainite is ≤10%, and the remainder is pearlite, with an average grain size of 5-8 μm, a grain size ≥10, and an inclusion grade ≤0.

4.

4. The low-cost, thick-gauge 590MPa nickel-free weathering steel as described in claim 1, 2, or 3, characterized in that, The number density of heterogeneous nucleated particles in the microstructure of the weathering steel is 6.35 × 10⁻⁶. 4 ~7.65×10 4 / mm 3 The proportion of ferrite heterogeneous nuclei is ≥60%, and the heterogeneous nuclei are Ti(C,N) and V(C,N) composite precipitates.

5. The low-cost, thick-gauge 590MPa nickel-free weathering steel as described in claim 1, 2, 3, or 4, characterized in that, The weathering steel has a yield strength ≥590MPa, tensile strength ≥710MPa, impact energy of 190~360J at -20℃, yield strength ratio ≤0.85, and no "copper brittleness" cracks on the surface of the steel plate.

6. The low-cost, thick-gauge 590MPa nickel-free weathering steel as described in claim 1, 2, 3, 4, or 5, characterized in that, The thickness of the weathering steel ranges from 20 to 60 mm.

7. The method for manufacturing low-cost, thick-gauge 590MPa nickel-free weathering steel as described in any one of claims 1 to 6, characterized in that, Includes the following steps: 1) Smelting and refining The components described in claim 1 or 2 are smelted, refined, and cast into billets. 2) Slab heating Heating temperature: 1060~1080℃, holding time: 1~2h; 3) Rolling Roughing rolling start temperature: 900~1000℃, single-pass rolling reduction rate in roughing stage ≥15%; Finishing rolling start temperature: 870~890℃, single-pass rolling reduction rate in the finishing rolling stage ≥20%, finishing rolling temperature: 820~840℃; 4) Cooling Cooling start temperature: 770~810℃, cooling stop temperature: 410~450℃, cooling rate ≥45℃ / s.

8. The manufacturing method as described in claim 7, characterized in that, In step 4), the cooling is achieved by water cooling.

9. The manufacturing method as described in claim 7 or 8, characterized in that, In step 4), the steel plate is air-cooled to room temperature after the cooling process is stopped.

Citation Information

Patent Citations

  • Economical weathering-resistant steel produced through using RE-P reinforcement and preparation process

    CN111270135A

  • 400MPa-grade high-silicon weathering steel as well as preparation method and application thereof

    CN111979484A

  • A 340MPa grade cold-rolled low-cost weathering steel for automotive use and its manufacturing method

    CN113637904B

  • 355MPa-grade low-cost weathering steel and preparation method thereof

    CN117587324A