Copper powder surface modifier based on phosphonic acid group, modified copper powder and preparation method of copper powder surface modifier

By using a copper powder surface modifier based on phosphonic acid groups to form Cu-OP covalent coordination bonds and an organic protective layer, the oxidation and dispersion problems of copper powder are solved, and the high-efficiency anti-oxidation and dispersion performance of copper powder are improved.

CN121378336APending Publication Date: 2026-01-23GUANGDONG JINGYUN ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511492542.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-20
Publication Date
2026-01-23

AI Technical Summary

Technical Problem

Copper powder is easily oxidized in air to form Cu2O or CuO, which leads to a decrease in electrical properties. Furthermore, it has poor dispersibility in non-polar media and is prone to agglomeration and sedimentation, affecting its application performance.

Method used

A copper powder surface modifier based on phosphonic acid groups is used. N-octadecyl-methylphosphonic acid amide is generated by reacting octadecylamine with methylphosphonic acid, forming Cu-OP covalent coordination bonds and an organic protective layer. This provides steric hindrance to the long alkyl chain and enhances the oxidation resistance and dispersibility of the copper powder.

Benefits of technology

It significantly improves the oxidation resistance and dispersibility of copper powder, with low oxidation weight gain, good dispersion stability, and good conductivity retention, with a conductivity retention rate of over 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121378336A_ABST
    Figure CN121378336A_ABST
Patent Text Reader

Abstract

The invention discloses a copper powder surface modifier based on phosphonic acid groups, modified copper powder and a preparation method of the copper powder surface modifier. The preparation method of the copper powder surface modifier based on the phosphonic acid group comprises the following steps: step 1, mixing octadecylamine and methylphosphonic acid according to a molar ratio; 2, heating and refluxing in a toluene solvent under the protection of ammonia gas; and 3, removing the solvent, and drying under reduced pressure to obtain the N-octadecyl-methylphosphonic acid amide. A Cu-O-P chemical bond is formed by a-P-OH group in a phosphonic acid amide molecule and a copper surface, so that a modified layer has excellent stability and binding force; meanwhile, a hydrophobic protective barrier is constructed by an octadecyl long chain, so that oxidation is prevented, and the conductivity is kept. The structure has the advantage of double protection of chemical bond combination and steric hindrance, and compared with traditional stearic acid physical adsorption, the performance is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal powder surface modification and its anti-oxidation treatment technology, and particularly to a copper powder surface modifier based on phosphonic acid groups and its preparation technology. Background Technology

[0002] Copper powder is widely used in conductive pastes, electronic packaging materials, metal injection molding, and antibacterial materials due to its excellent electrical and thermal conductivity and processing properties. However, copper powder is highly susceptible to oxidation in air, forming Cu₂O or CuO, which leads to a decrease in electrical properties and changes in surface color. Furthermore, copper powder exhibits poor dispersibility in non-polar media (such as organic solvents or polymer matrices), easily agglomerating and settling, severely impacting its application performance.

[0003] To improve the antioxidant and dispersing properties of copper powder, organic surface modification methods are often used, such as modification with fatty acids, thiol compounds, phosphonates, or silane coupling agents. Traditional fatty acid modification (such as stearic acid) can improve dispersibility, but its bonding force with the copper surface is weak, making it difficult to maintain stability under high temperature or long-term use; thiol compounds, although having strong coordination effects, have a strong odor, are easily oxidized and decomposed, and are relatively expensive. Summary of the Invention

[0004] The purpose of this invention is to address the problems of poor oxidation resistance and insufficient dispersibility of copper powder in the prior art, as proposed in the above-mentioned background art, by proposing a copper powder surface modifier based on phosphonic acid groups and its application method.

[0005] To achieve the above objectives, the present invention provides the following technical solution: This invention first provides a copper powder surface modifier based on phosphonic acid groups, the structural formula of which is as follows: CH3P(O)(OH)(NH-R), wherein the R group is C 16 -C 20 alkyl chain.

[0006] In a preferred embodiment, the R group is octadecyl.

[0007] In a preferred embodiment, it is generated by reacting octadecylamine and methylphosphonic acid.

[0008] The present invention relates to a method for preparing a copper powder surface modifier based on phosphonic acid groups, which includes the following steps: Step 1: Mix octadecylamine and methylphosphonic acid in a molar ratio; Step 2: Heat under ammonia protection in toluene solvent and reflux; Step 3: Remove the solvent and dry under reduced pressure to obtain N-octadecyl-methylphosphonic acid amide.

[0009] In a preferred embodiment, the molar ratio of octadecylamine to methylphosphonic acid is 1:1 to 1.2:1; and the heating reflux time is 8 to 12 hours.

[0010] This invention provides a modified copper powder, comprising copper powder and a surface modifier, wherein the surface modifier is CH3P(O)(OH)(NH-C 18 It chelates to the copper surface to provide steric hindrance for the long alkyl chain.

[0011] In a preferred embodiment, the -P=O of the surface modifier reacts with the Cu on the copper surface. 2+ or Cu + A coordination reaction occurs, forming Cu-OP coordination bonds; And / or the -OH groups on the copper surface undergo condensation and dehydration with the -OH groups of the surface modifier to form Cu-OP bonds.

[0012] In a preferred embodiment, the amount of surface modifier used is 0.1% to 2% of the mass of copper powder.

[0013] The method for preparing modified copper powder provided by this invention includes the following steps: Step 1: Dissolve the surface modifier described in claim 1 or 2 in ethylene glycol; Step 2: Add the modifier solution to the wet copper powder and stir to react; Step 3: Wash and dry to obtain surface-modified copper powder.

[0014] A preferred embodiment includes the following steps: in step 1, the concentration of the surface modifier is 1-3 wt%; in step 2, the reaction conditions are a temperature of 60°C and stirring for 2 hours.

[0015] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention utilizes the -P-OH groups in the phosphonic amide molecule to form Cu-OP chemical bonds with the copper surface, resulting in a modified layer with excellent stability and binding force. Simultaneously, the octadecyl long chain constructs a hydrophobic protective barrier, preventing oxidation while maintaining electrical conductivity. The advantage of this structure lies in the dual protection of chemical bonding and steric hindrance, significantly improving performance compared to traditional stearic acid physical adsorption.

[0016] 2. The oxidation weight gain rate of the phosphonic acid amide-modified sample was only 0.7%, significantly lower than that of stearic acid-modified and unmodified copper powder. This indicates that the phosphonic acid groups form Cu-OP covalent coordination bonds with the copper surface, constructing a dense organic protective layer that effectively inhibits oxygen and moisture penetration; while stearic acid mainly relies on weak van der Waals adsorption, resulting in poor durability.

[0017] 3. The phosphonic amide modified sample still maintained more than 90% conductivity after 72 h of exposure, indicating that the surface...

[0018] The modified layer is stable and has good conductive contact. In contrast, the stearic acid modified sample shows a significant decrease in conductivity due to partial desorption of the capping layer and an increase in the oxide layer.

[0019] 4. The phosphonic acid group in the N-octadecyl-methylphosphonic amide molecule forms a Cu-OP covalent coordination bond with the Cu atoms on the surface of copper powder, firmly adsorbing onto the surface and forming an organic protective layer. The long alkyl chain provides steric hindrance, preventing oxygen and moisture from contacting the copper surface, while enhancing non-polar compatibility, thereby significantly improving the chemical stability and dispersibility of the copper powder. Attached Figure Description

[0020] Figure 1 This is a SEM image of the surface morphology of the modified copper powder.

[0021] Figure 2 These are statistical comparison data on the oxidation weight gain rate, dispersion sedimentation time, and conductivity retention rate of different sample groups.

[0022] Figure 3 This refers to the changes in exposure time and oxidative weight gain rate.

[0023] Figure 4 It is a statistical analysis of settlement time and the proportion of settlement stratification over 24 hours.

[0024] Figure 5 It is a statistical analysis of the initial conductivity, time, and retention rate.

[0025] Figure 6 The study investigated samples obtained by modifying copper powder with modifiers of different weight ratios, and then conducted sedimentation tests. Detailed Implementation

[0026] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided below.

[0027] Example 1: Synthesis of the modifier: 18.5 g (0.074 mol) of octadecylamine and 5.5 g (0.074 mol) of methylphosphonic acid were added to a 250 mL three-necked flask, and 150 mL of anhydrous toluene was added as solvent. The mixture was heated to reflux (approximately 110 °C) under ammonia protection for 10 hours. After the reaction was completed, the mixture was cooled to room temperature, the solvent was removed by rotary evaporation, and the product was dried under reduced pressure (60 °C, 8 hours) to give a pale yellow solid product, N-octadecyl-methylphosphonic acid amide, in 92% yield.

[0028] Example 2: Modification treatment of copper powder: Copper powder preparation: A chemical reduction method was used: CuSO4·5H2O was used as the copper source, ascorbic acid as the reducing agent, and the reaction was carried out at 70℃ for 1 hour. After filtration and washing, wet copper powder (35% moisture content) was obtained. Alternatively, other existing methods can be used to obtain wet copper powder.

[0029] Take 100 g of wet copper powder (100 g refers to the net content of copper powder), add 2 g (accounting for 2 wt% of the copper powder mass) of N-octadecyl-methylphosphonic amide, and dissolve it in 80 mL of ethylene glycol.

[0030] After mixing, the mixture was stirred at 60°C for 2 hours, filtered and washed (with anhydrous ethanol 3 times), and then vacuum dried at 60°C for 12 hours to obtain modified copper powder.

[0031] Characterization analysis: like Figure 1 As shown in the SEM observation, the modified particles have smooth surfaces, uniform particle size distribution, and no obvious agglomeration. Comparison sample A: Unmodified copper powder.

[0032] Comparative sample B: Stearic acid modified copper powder.

[0033] Preparation process of stearic acid modified copper powder: wet copper powder (prepared by chemical reduction method, water content of about 35 wt%): 100 g (net weight of copper powder); stearic acid (purity ≥98%): 2.0 g (about 2.0 wt% of the mass of wet copper powder); anhydrous ethanol (or isopropanol): 80-150 mL (used to dissolve stearic acid and aid washing); the equipment used includes: reaction stirrer, oil bath or water bath, vacuum filter, rotary evaporator or vacuum drying oven with ammonia (optional, used for protection and to reduce oxidation).

[0034] step: 1. Preparation of stearic acid solution: Add approximately 100 mL of anhydrous ethanol to a reflux flask or large beaker, heat to 55-65°C, add 2.0 g of stearic acid to the ethanol, and stir until completely dissolved to obtain a stearic acid solution of approximately 2 wt% (relative to the mass of copper powder). If isopropanol is used, the solubility is better, and the temperature should also be controlled at around 60°C.

[0035] 2. Mix with wet copper powder: Place 100 g (net weight) of wet copper powder in a 250 mL reaction vessel, and slowly add a heated stearic acid ethanol solution (maintaining 60°C) while stirring at 300-600 rpm. Maintain stirring at 60°C for 2 hours to allow stearic acid molecules to fully adsorb and cover the surface of the copper powder.

[0036] 3. After washing and separation modification, the system is separated by vacuum filtration or centrifugation, and the supernatant is discarded. The solid is washed three times with anhydrous ethanol (about 50-80 mL each time) to remove unbound stearic acid and solvent residue.

[0037] 4. Drying: Dry the washed wet solid in a vacuum drying oven at 60°C for 12 hours (or evaporate it to dryness under reduced pressure at 60°C) to obtain stearic acid modified copper powder (remember to weigh and record the yield).

[0038] Test items such as Figure 2 The table data is shown below.

[0039] The results show that the modified copper powder of this invention has several times the antioxidant properties and significantly improved dispersion stability.

[0040] I. Oxidative weight gain test (1) Test purpose: to evaluate the effect of the modifier on the antioxidant properties of copper powder, and to determine the surface protection ability by measuring the mass increase rate of the sample after exposure to air.

[0041] (2) Test Principle: Copper powder readily reacts with oxygen and moisture in the air to form copper oxide (Cu₂O, CuO), which leads to an increase in sample mass. The oxidation weight gain rate (%) is defined as: m t - m0 / m0; where m t m is the initial dried mass, and m0 is the mass after t hours of air exposure.

[0042] (3) Test steps 1. Take 2.0g of each modified copper powder sample (unmodified, stearic acid modified, and phosphonic amide modified) and place them in a dry weighing dish; 2. Expose them in static air at 70°C (high temperature environment) and 80+5% relative humidity (high humidity environment); 3. Weigh them once every 24 hours and monitor them continuously for 72 hours; 4. Before weighing, the samples are vacuum dried at 100°C for 30min to remove surface adsorbed water; 5. Repeat the test 3 times and take the average value.

[0043] Test results in Figure 3 middle, Figure 3 Data from Zhongde shows that the oxidation weight gain rate of the phosphonic acid amide-modified sample was only 0.7%, significantly lower than that of stearic acid-modified and unmodified copper powder. This indicates that the phosphonic acid groups form Cu-OP covalent coordination bonds with the copper surface, constructing a dense organic protective layer that effectively inhibits oxygen and moisture penetration; while stearic acid mainly relies on weak van der Waals adsorption, resulting in poor durability.

[0044] In existing technologies, the smaller the particle size of powder, the easier it is to oxidize due to its larger specific surface area. In particular, the oxidizing power increases significantly when the particle size approaches the nanometer level. To address this, through modification, the particle size obtained in this application is at the micrometer level or hundreds of nanometers. Such small particle size powder still maintains good antioxidant properties, indicating that the surface modifier of this application has a significant effect on the surface modification of copper powder.

[0045] II. Dispersion Settlement Performance Test: (1) Test objective: To evaluate the dispersion stability of modified copper powder in non-polar solvents (such as petroleum ether or cyclohexane) and reflect the effect of surface hydrophobic modification.

[0046] (2) Test principle: A copper powder dispersion of a certain concentration is allowed to stand, and the time required for the supernatant to become transparent or separate into layers is recorded. The longer the time, the better the dispersibility and stability.

[0047] (3) Test steps: 1. Add the copper powder sample to cyclohexane at a mass fraction of 10 wt%; 2. Disperse using an ultrasonic disperser (100 W) for 10 minutes to ensure initial uniformity; 3. Place the sample in a transparent glass tube (20 mm in diameter and 100 mm in height); 4. Observe and record the change in the height of the settlement layer over time at 25℃; 5. When the upper transparent area occupies 50% of the total volume, record it as the settling time T. 50 (Each sample was repeated 3 times and the average value was taken).

[0048] (5) Results Analysis: Statistical data in Figure 4 In Figure 4 In the data: The phosphonic acid amide modified copper powder of this invention shows almost no stratification in cyclohexane after 24 hours, exhibiting excellent dispersion stability.

[0049] III. Conductivity Retention Rate Test (1) Test purpose: to evaluate the effect of the modifier in maintaining the antioxidant properties while protecting the conductivity of copper.

[0050] (2) Test Principle: By measuring the change in volume resistivity or conductivity of the pressed sample, the degree to which the conductivity is retained after modification is reflected. The conductivity retention rate is defined as: σ t / σ0 x 100%; where σ0 is the initial conductivity, σ t The conductivity is the electrical conductivity after 72 hours of air exposure.

[0051] (3) Test steps: 1. Each sample (2 g) was pressed into a φ10 mm x 2 mm disc using a mold; 2. Initial test: The volume resistivity ρ0 (Ω·cm) was measured using the four-probe method, and σ0 = 1 / ρ0 was calculated; 3. Expose the sample to air at 70°C and 80% RH (relative humidity) for 72 hours; 4. Test resistivity ρ again. t Calculate σ t ; 5. Repeat 3 times and take the average.

[0052] (4) Test results are summarized to Figure 5 The table data in the document.

[0053] (5) Analysis and explanation, see details. Figure 5 Data in: The phosphonic amide-modified sample maintained over 90% conductivity after 72 hours of exposure, indicating that the surface modification layer was stable and had good conductive contact. In contrast, the stearic acid-modified sample showed a significant decrease in conductivity due to partial desorption of the coating layer and an increased oxide layer.

[0054] Furthermore, Figure 6 The study investigated samples obtained by modifying copper powder with different weight ratios of modifiers, followed by sedimentation tests. Specifically, samples with a surface modifier-to-net-weight copper powder ratio of 0.5%, 1.0%, 1.5%, and 2.0% were tested, all following the preparation and testing procedures described above. Figure 6 As can be seen, 1.5% and 2.0% were the experimental groups with better dispersion effects, but at this point, the increase in sedimentation effect was already very limited, and further increasing the amount of modifier would not be very meaningful. Therefore, it is better to control it below 2.0%.

[0055] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any indirect modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A copper powder surface modifier based on phosphonic acid groups, characterized in that: The structural formula of the surface modifier is as follows: CH3P(O)(OH)(NH-R), where the R group is C 16 -C 20 alkyl chain.

2. The copper powder surface modifier based on phosphonic acid groups according to claim 1, characterized in that: The R group is an octadecyl group.

3. The copper powder surface modifier based on phosphonic acid groups according to claim 2, characterized in that: It is produced by the reaction of octadecylamine and methylphosphonic acid.

4. The method for preparing the copper powder surface modifier based on phosphonic acid groups according to claim 2 or 3, characterized in that: Includes the following steps: Step 1: Mix octadecylamine and methylphosphonic acid in a molar ratio; Step 2: Heat under ammonia protection in toluene solvent and reflux; Step 3: Remove the solvent and dry under reduced pressure to obtain N-octadecyl-methylphosphonic acid amide.

5. The method for preparing the copper powder surface modifier based on phosphonic acid groups according to claim 4, characterized in that: The molar ratio of octadecylamine to methylphosphonic acid is 1:1 to 1.2:1; the heating reflux time is 8 to 12 hours.

6. A modified copper powder, characterized in that, Includes copper powder and surface modifier, the surface modifier being CH3P(O)(OH)(NH-C 18 It chelates to the copper surface to provide steric hindrance for the long alkyl chain.

7. The modified copper powder according to claim 6, characterized in that, The -P=O of the surface modifier reacts with the Cu on the copper surface. 2+ or Cu + A coordination reaction occurs, forming Cu-OP coordination bonds; And / or the -OH groups on the copper surface undergo condensation and dehydration with the -OH groups of the surface modifier to form Cu-OP bonds.

8. The modified copper powder according to claim 6, characterized in that, The amount of surface modifier used is 0.1% to 2% of the copper powder mass.

9. The method for preparing modified copper powder according to any one of claims 6 to 8, characterized in that, Includes the following steps: Step 1: Dissolve the surface modifier described in claim 1 or 2 in ethylene glycol; Step 2: Add the modifier solution to the wet copper powder and stir to react; Step 3: Wash and dry to obtain surface-modified copper powder.

10. The method for preparing modified copper powder according to claim 9, characterized in that, The process includes the following steps: in step 1, the concentration of the surface modifier is 1-3 wt%; in step 2, the reaction conditions are a temperature of 60℃ and stirring for 2 hours.