Method for recycling PA66 / PET (Polyamide 66 / Polyethylene Terephthalate) mixed waste

By using an adipic acid autocatalytic system to synergistically hydrolyze PA66/PET mixed waste, the complexity of traditional recycling methods is solved, and high-performance polyesteramide is efficiently recycled, making it suitable for the engineering plastics field.

CN121449970APending Publication Date: 2026-02-03TECHNICAL INST OF PHYSICS & CHEMISTRY - CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202511214837.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-28
Publication Date
2026-02-03

AI Technical Summary

Technical Problem

The recycling and treatment of mixed PA66 and PET waste is complex. Traditional methods require step-by-step processing and are costly. The hydrolysis products have complex compositions, making it difficult to achieve efficient recycling and regeneration.

Method used

Adipic acid autocatalytic system was used to synergistically hydrolyze PA66/PET mixed waste under single reaction conditions. The hydrolysis products were directly repolymerized into high-performance polyesteramide. The performance of the recycled materials was optimized through esterification and polycondensation reactions.

Benefits of technology

It achieves efficient hydrolysis of PA66 and PET, with hydrolysis rates of 85% and 50-70% respectively. The recycled materials have excellent mechanical properties and thermal stability, making them suitable for the field of engineering plastics and forming a complete resource recycling system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121449970A_ABST
    Figure CN121449970A_ABST
Patent Text Reader

Abstract

The invention discloses a method for recycling PA66 / PET (Polyamide 66 / Polyethylene Terephthalate) mixed waste. The recycling and regenerating method comprises the following steps: under the action of a catalyst, carrying out hydrolysis reaction on the PA66 / PET mixed waste; wherein the catalyst is adipic acid, and the use amount of the catalyst is 10-30 wt% of the amount of the mixed waste according to the mass percentage. An adipic acid autocatalysis system is adopted, efficient hydrolysis of PA66 and PET is achieved at the same time under the single reaction condition, the defect that step-by-step treatment is needed in a traditional process is overcome, the hydrolysis rate of PET is larger than or equal to 85%, the hydrolysis rate of PA66 is 50-70%, hydrolysis products can be further polymerized into polyesteramide with excellent mechanical performance and thermal stability, and the preparation method is suitable for industrial production. And the spanning from degradation recovery to upgrading regeneration is realized.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of high polymer materials. More particularly, it relates to a recycling method of PA66 / PET mixed waste. BACKGROUND

[0002] Polyamide (PA) and polyester (PET) mixed fabric is a fabric that combines the advantages of both PA and PET. This fabric has been widely used in clothing, home textiles and other fields, mainly due to its unique physical properties and cost advantages. PA, also known as nylon, has good elasticity and wear resistance, while PET is known for its high strength, quick drying and easy washing. When these two fibers are mixed together, the resulting fabric retains the elasticity of PA and the durability of PET. In addition, the mixed fabric usually has good wrinkle resistance and shape retention, allowing clothes to maintain a good appearance after long wear.

[0003] It is worth noting that the widespread use of PA and PET mixed systems has also led to the complexity of waste components. It is estimated that more than one million tons of waste PA and blended fabrics are generated in China every year, which will cause serious resource waste and environmental risk if there is a lack of efficient recycling methods. In the current environmental context, the recycling and reuse of polymer waste has become a global focus. PA66 and PET are two widely used thermoplastic polymers, and their waste recycling is of great significance for resource conservation and environmental protection. However, due to the differences in chemical structure and physical properties between PA66 and PET, the recycling of their mixed waste becomes particularly complex. PA66 and PET have large differences in physical and chemical properties, and traditional mixed recycling has conflicts in hydrolysis conditions (PET requires acid / alkali hydrolysis, PA66 requires high temperature hydrolysis). Even after hydrolysis, the hydrolysis products are relatively complex, and it is difficult to separate and purify the monomers, which is a complex process with high cost (such as hexamethylene diamine recovery rate <60%). SUMMARY

[0004] Therefore, the purpose of the present application is to provide a recycling method of PA66 / PET mixed waste. The present application realizes the synergistic hydrolysis of two polymers through a adipic acid self-catalytic system, avoiding the defects of traditional process that requires step-by-step treatment. At the same time, the hydrolysis products can be directly repolymerized to form high-performance polyester amide, realizing the leap from "downgrade recycling" to "upgrade regeneration".

[0005] To achieve the above purpose, the technical scheme adopted by the present application is as follows:

[0006] The present application discloses a recycling method of PA66 / PET mixed waste, comprising the following steps:

[0007] Under the action of the catalyst, the PA66 / PET mixed waste is subjected to a hydrolysis reaction;

[0008] The catalyst is adipic acid, and the amount of the catalyst is 10-30wt% of the mixed waste.

[0009] Further, the amount of the catalyst can be 10wt%, 15wt%, 20wt%, 25wt%, 30wt% or the like of the mixed waste, preferably 10-25wt%, more preferably 15-20wt%.

[0010] In the technical solution of the present application, considering that the PET content in the current textile waste (such as polyester blended fabric) and engineering plastic waste (such as electronic and electrical shell) is controlled at 20-50wt%, therefore, the mass ratio of PA66 and PET in the mixed waste is selected as 3-4:1. Of course, the present application only studies the composition distribution of the currently more common PA66 / PET mixed waste, and the skilled person should understand that the PA66 / PET mixed waste with other proportions is also applicable.

[0011] Further, the reaction temperature of the hydrolysis reaction is 200-240℃, and the reaction time is 6-12h, so that the hydrolysis rate of PET in the hydrolysis reaction is 85-100%, and the hydrolysis rate of PA66 is 50-70%.

[0012] Further, the reaction temperature of the hydrolysis reaction is preferably 200-220℃.

[0013] Further, the solvent used in the hydrolysis reaction is water. Using water as the only solvent improves environmental protection.

[0014] Further, the amount of the solvent is 100-1000wt% of the mixed waste; for example, the amount of water can be 100wt%, 200wt%, 300wt%, 400wt%, 500wt%, 600wt%, 700wt%, 800wt%, 900wt%, 1000wt% or the like of the mixed waste, preferably 200-800wt%, more preferably 300-600wt%.

[0015] Further, the hydrolysis reaction is carried out in a closed environment.

[0016] Further, the recycling method further comprises preparing a polyester amide by repolymerizing the hydrolysis product obtained in the hydrolysis reaction;

[0017] The repolymerization comprises an esterification reaction and a polycondensation reaction in sequence.

[0018] Further, the re-polymerization comprises the following steps:

[0019] The oligomers and / or monomers (such as adipic acid, hexamethylene diamine, ethylene glycol, etc.) obtained from the hydrolysis reaction are subjected to an esterification reaction with additional monomers for preparing polyester amide and a polymerization catalyst;

[0020] The product obtained from the esterification reaction is subjected to a polycondensation reaction to obtain polyester amide.

[0021] Further, the hydrolysis reaction product used for re-polymerization in the present application can be either a monomer compound obtained after complete hydrolysis reaction, or an oligomer obtained after incomplete hydrolysis reaction, or a mixture of oligomer and monomer. Regardless of monomer, oligomer or mixture of the two, the performance of the polyester amide obtained after the subsequent re-polymerization reaction is not greatly affected. Therefore, the present application can obtain polyester amide in a relatively lower energy consumption and in a shorter time.

[0022] Further, the monomers used for preparing polyester amide are selected from one or more of adipic acid, hexamethylene diamine and ethylene glycol.

[0023] Further, the polymerization catalyst used for preparing polyester amide is selected from a titanate catalyst (such as tetrabutyl titanate).

[0024] Further, the esterification reaction is carried out under normal pressure and at a reaction temperature of 130-200℃.

[0025] The polycondensation reaction is carried out under a vacuum degree of 10-100 Pa and at a reaction temperature of 200-290℃.

[0026] Further, the re-polymerization process is as follows: high-strength polyester amide is prepared by two-step melt polycondensation + gradient temperature rise (torque real-time feedback regulation) to solve the problem of mechanical property degradation of the regenerated material. Under the condition of oil bath temperature control, the reaction system is raised from 130-170℃ to 150-290℃ at a gradient temperature rise program of 20-40℃ / h for esterification reaction. After the esterification water is stable (the water output no longer increases), 1wt% of glycerol based on the mass of adipic acid is added as a branching agent, and 0.25wt% of tetrabutyl titanate based on the total system mass is added as a catalyst, and the stirring is continued for 20 min to ensure uniform dispersion. After entering the polycondensation stage, the pressure gradient is reduced by a dynamic vacuum control system: the initial stage starts at 0.1 MPa (absolute pressure about 10 kPa), and the oil bath temperature is gradually raised to 230-290℃. The system pressure is reduced to below 100 Pa in stages through a precision pressure regulating valve. When the torque growth stops, the reaction is stopped, the product is discharged, and polyester amide is obtained.

[0027] Further, the polyester amide material has the following characteristics: an alternating structure of amide bonds and ester bonds in the molecular chain; a number average molecular weight (Mn) of 15000-35000 g / mol; an intrinsic viscosity of 0.6-1.2 dL / g; a tensile strength of 12.45-56.62 MPa; an elongation at break of 15.15-54.5%; and a melting temperature of 151-230 DEG C.

[0028] The regenerated polyester amide (PEA) exhibits excellent performance controllability, and by adjusting the ratio of hexamethylene diamine (HMD) to ethylene glycol (EG) (the molar ratio of HMD to EG is 0.4-0.7:0.9-0.6), the hardness of the material can be controlled, specifically, the tensile strength can be precisely adjusted in the range of 12.45-56.62 MPa, and the elongation at break can be controlled between 15.15-26.93% according to requirements, realizing the conversion from a rigid material to a flexible material. In addition, when the optimized formula of HMD and EG is 6:7, for example, HMD is 0.6 mol and EG is 0.7 mol, the material exhibits excellent tensile strength of 45.43 MPa and balanced elongation at break of 23.57%, which has a significant advantage in engineering applications.

[0029] The beneficial effects of the present application are as follows:

[0030] 1. The adipic acid autocatalytic system is used to realize the efficient hydrolysis of PA66 and PET under single reaction conditions, avoiding the defects of the traditional process which needs step-by-step treatment. Further, by optimizing the hydrolysis conditions, the PET hydrolysis rate is ensured to be greater than or equal to 85%, and the PA66 hydrolysis rate is 50-70%. The recycling method solves the problems of difficult recycling and complex operation of textile waste and engineering plastic waste, and saves resources.

[0031] 2. Since water is the only solvent in the recycling method, no strong acid or organic solvent is introduced, the reaction conditions are mild, the operation is simple, and the environment is friendly.

[0032] 3. The liquid phase product obtained by the hydrolysis reaction can be directly used for polyester amide synthesis without purification, the utilization rate of the liquid phase components is high, the obtained polyester amide has excellent mechanical properties and thermal stability, and is suitable for engineering plastic field. And by adjusting the reaction materials, polyester amide with tensile strength of 12.45-56.62 MPa and elongation at break of 15.15-54.5% can be obtained, which meets the diversified needs from flexible seals to engineering structural parts.

[0033] 4. The solid phase product obtained by the hydrolysis reaction can be selectively recovered terephthalic acid (TPA) by alkali treatment (0.5-1 mol / L NaOH) for reuse, and the whole recycling method forms a complete resource recycling system. BRIEF DESCRIPTION OF DRAWINGS

[0034] The specific embodiments of the present application will be further described with reference to the drawings.

[0035] Figure 1 A hydrolysis process flow chart of PA66 / PET mixed waste in Example 1 is shown. DETAILED DESCRIPTION

[0036] In order to more clearly illustrate the application, the application will be further described below with reference to the preferred embodiments and the accompanying drawings. Like components are denoted by the same reference numerals in the drawings. It should be understood by those skilled in the art that the specific descriptions below are illustrative rather than limiting, and the protection scope of the application should not be limited thereto.

[0037] Example 1

[0038] In combination Figure 1 As shown, PA66 / PET mixed waste (mass ratio 4:1, PA66 1.6±0.05 g, PET 0.4±0.05 g), catalyst adipic acid (0.2-0.6 g) and 10 mL deionized water were added into a polytetrafluoroethylene-lined hydrothermal reactor, and the temperature was raised to 200-240°C at a rate of 10°C / min, and the reaction was carried out under normal pressure and 25 rpm stirring for 6-12 h. After the reaction was completed, the temperature was naturally cooled to room temperature, and the solid-liquid phase was separated by vacuum filtration (0.22 μm filter membrane). The solid phase was unreacted PA66 and terephthalic acid (TPA), and the liquid phase was a mixed solution of ethylene glycol (EG), AA and hexamethylene diamine (HMD). After the solid phase was treated with 1 mol / L NaOH solution for 2 h to dissolve TPA, it was filtered again. The residual solid was incompletely hydrolyzed PA66, and the filtrate was acidified with dilute sulfuric acid to precipitate TPA crystals with a purity of ≥98% and a yield of ≥95%. The liquid phase was directly used for subsequent polymerization. To quantitatively evaluate the hydrolysis rate, after vacuum filtration with a 0.22 μm filter membrane, the solid phase was vacuum dried at 50°C to a constant weight (Δm <0.1%), and then the unreacted PET content was determined by 0.1 mol / L NaOH dispersion and acid-base titration. The PET and PA66 hydrolysis conversion rates under different hydrolysis conditions are shown in Table 1.

[0039] Table 1 PET and PA66 hydrolysis conversion rates under different hydrolysis conditions

[0040] Hydrolysis temperature / °C Hydrolysis time / h Catalyst amount / g PET conversion / % PA66 conversion / % 200 12 0.2 86.7 52.8 200 10 0.4 87.1 55.2 200 8 0.6 88.4 58.6 210 12 0.2 88.3 53.2 210 10 0.4 89.2 53.7 210 8 0.6 90.6 56.4 220 12 0.2 92.6 57.8 220 10 0.3 94.7 59.3 220 8 0.4 95.4 62.1 220 6 0.6 96.3 65.4 240 12 0.2 97.8 68.2 240 10 0.3 99.0 70.5 240 8 0.4 99.2 72.8 240 6 0.6 99.2 75.2

[0041] Example 2

[0042] The 200 g of PA66 / PET mixed waste (mass ratio 4:1, PA66 is 160 g, and PET is 40 g), adipic acid (30 g) and 1 L of deionized water were added into a polytetrafluoroethylene-lined hydrothermal reactor. The temperature was raised to 210°C at a rate of 10°C / min, and the reaction was carried out under normal pressure and 25 rpm stirring for 10 h. After the reaction was completed, it was naturally cooled to room temperature, and the solid-liquid phase was separated by vacuum filtration (0.22 μm filter membrane). The solid phase was unreacted PA66 and terephthalic acid (TPA), and the liquid phase was a mixed solution of ethylene glycol (EG), AA and hexamethylene diamine (HMD). The solid phase was dissolved by 1 mol / L NaOH solution for 2 h, and then the residual solid was PA66 which was not completely hydrolyzed. The filtrate was acidified with dilute sulfuric acid to precipitate TPA crystals with a purity of ≥98% and a yield of ≥95%. The liquid phase was directly used for subsequent polymerization. The results showed that the PA66 hydrolysis conversion rate was 55.1±0.9%, and the PET conversion rate was 99.3±0.7%.

[0043] The vacuum filtration method was used to separate the solid and liquid of the hydrolysis reaction liquid, and a pure liquid monomer mixture was provided for subsequent PEA synthesis. The specific operation is as follows: a Buchner funnel is sealed and connected with a filtration bottle, a wet filter paper is laid inside, a rubber tube is connected to a vacuum pump and adjusted to a negative pressure of-0.08 MPa to-0.095 MPa, the mixed liquid is slowly poured into the funnel, the liquid level is controlled not to exceed 2 / 3 of the volume, and the filtration is carried out under constant pressure until the filtrate passes through; then the filter cake is washed with deionized water, the vacuum connection is disconnected and the vacuum pump is closed after drying; the final collected filtrate contains about 23.26 g of ethylene glycol (EG) (recovery rate 90%), about 45.16 g of hexamethylene diamine (HMD), and about 86.84 g of adipic acid (AA) (including 30 g of catalyst added initially).

[0044] Re-polymerization part: AA, HMD and EG in liquid phase were directly used for PEA synthesis, 59.16 g AA, 1.24 g HMD and 32.54 g EG were added to make the monomer molar ratio AA:HMD:EG = 1:0.4:0.9, and a two-step melt polycondensation process was used in the synthesis process: first, the esterification stage, the mixed liquid was placed in a three-necked flask equipped with mechanical stirring, nitrogen protection and water separation device, and the inert reaction environment was established by three vacuum-nitrogen replacement cycles. The temperature was raised from 130 to 150 °C at a rate of 30 °C / h, and the water output was monitored in real time through the water separator during this period. When the actual water collection amount exceeded 85% of the theoretical value, it was determined that the esterification stage was completed; second, the polycondensation stage, the functional additives were introduced step by step: first, 1% (1.46 g) of glycerol based on the mass of adipic acid was added as a branching agent, and then 0.25% (0.6205 g) of tetrabutyl titanate based on the total system mass was added as an ester exchange catalyst, and the stirring was continued for 20 min to ensure uniform dispersion. After entering the polycondensation stage, the pressure gradient type reduction was implemented through the dynamic vacuum control system: the initial stage started at 0.1 MPa (absolute pressure about 10 kPa), and the system pressure was reduced to below 100 Pa through a precision pressure regulating valve in stages as the oil bath temperature gradually increased to 230 °C. During this process, the extension of the molecular chain was monitored in real time by the following characteristics: (1) the apparent viscosity of the melt increased significantly, resulting in a continuous rise in stirring torque; (2) the melt showed typical non-Newtonian fluid characteristics, and a clear rod climbing effect was observed. When the torque value reached the preset threshold of 50 N·m, the reaction was immediately terminated to prevent excessive crosslinking, and finally the molten copolymer was quickly extruded through nitrogen pressurization to obtain sample PEA-1.

[0045] Example 3

[0046] The hydrolysis process and the re-polymerization process were the same as in Example 2, except that the esterification temperature was adjusted from 150 to 170 °C, and the polycondensation temperature was 260 °C, to obtain sample PEA-4.

[0047] Example 4

[0048] The hydrolysis process and the re-polymerization process were the same as in Example 2, except that the esterification temperature was adjusted from 170 to 190 °C, and the polycondensation temperature was 290 °C, to obtain sample PEA-7.

[0049] Example 5

[0050] The hydrolysis process and the re-polymerization process were the same as in Example 2, except that the amount of monomer added was changed to 59.16 g AA, 24.44 g HMD and 20.14 g EG, making the monomer molar ratio AA:HMD:EG = 1:0.6:0.7, and finally obtaining sample PEA-2.

[0051] Example 6

[0052] The hydrolysis and re-polymerization processes were the same as in Example 3, except that the amount of monomers added was changed to 59.16 g AA, 24.44 g HMD and 20.14 g EG, so that the molar ratio of monomers was AA:HMD:EG = 1:0.6:0.7, and finally sample PEA-5 was obtained.

[0053] Example 7

[0054] The hydrolysis and re-polymerization processes were the same as in Example 4, except that the amount of monomers added was changed to 59.16 g AA, 24.44 g HMD and 20.14 g EG, so that the molar ratio of monomers was AA:HMD:EG = 1:0.6:0.7, and finally sample PEA-8 was obtained.

[0055] Example 8

[0056] The hydrolysis and re-polymerization processes were the same as in Example 2, except that the amount of monomers added was changed to 59.16 g AA, 36.04 g HMD and 13.94 g EG, so that the molar ratio of monomers was AA:HMD:EG = 1:0.7:0.6, and finally sample PEA-3 was obtained.

[0057] Example 9

[0058] The hydrolysis and re-polymerization processes were the same as in Example 3, except that the amount of monomers added was changed to 59.16 g AA, 36.04 g HMD and 13.94 g EG, so that the molar ratio of monomers was AA:HMD:EG = 1:0.7:0.6, and finally sample PEA-6 was obtained.

[0059] Example 10

[0060] The hydrolysis and re-polymerization processes were the same as in Example 4, except that the amount of monomers added was changed to 59.16 g AA, 36.04 g HMD and 13.94 g EG, so that the molar ratio of monomers was AA:HMD:EG = 1:0.7:0.6, and finally sample PEA-9 was obtained.

[0061] The thermal properties of the samples synthesized in Examples 2-10 are shown in Table 2, and the mechanical properties are shown in Table 3.

[0062] Table 2 Thermal properties of polyester amides with different ratios and process conditions

[0063]

[0064] Note: T d 5% T5% represents the temperature at which the mass loss reaches 5% during programmed temperature, and is a key indicator for evaluating the thermal stability of a material; Tm is the melting point, which refers to the temperature of the endothermic peak when a crystalline polymer changes from a solid state to a molten state.

[0065] Table 3 Mechanical properties of polyester amides under different ratios and process conditions

[0066]

[0067] Obviously, the above embodiments of the present application are only examples for clearly illustrating the present application, and are not intended to limit the implementation manners of the present application. Based on the above description, other different forms of changes or variations can be made by those skilled in the art, and it is impossible to enumerate all the implementation manners here. Any obvious changes or variations derived from the technical solutions of the present application are still within the protection scope of the present application.

Claims

1. A method for recycling and regenerating PA66 / PET mixed waste, characterized in that, Includes the following steps: The PA66 / PET mixed waste was hydrolyzed under the action of a catalyst; The catalyst is adipic acid, and the amount of the catalyst used is 10-30 wt% of the mixed waste.

2. The recycling and regeneration method according to claim 1, characterized in that, The catalyst is used in an amount of 10-25 wt% of the mixed waste, based on a mass percentage.

3. The recycling and regeneration method according to claim 1, characterized in that, The mass ratio of PA66 to PET in the mixed waste is 3-4:

1.

4. The recycling and regeneration method according to claim 1, characterized in that, The hydrolysis reaction temperature is 200-240℃, and the reaction time is 6-12h, so that the hydrolysis rate of PET is 85-100% and the hydrolysis rate of PA66 is 50-70%.

5. The recycling and regeneration method according to claim 1, characterized in that, The solvent used in the hydrolysis reaction is water.

6. The recycling and regeneration method according to claim 5, characterized in that, The amount of solvent used, by mass percentage, is 100-1000 wt% of the mixed waste.

7. The recycling and regeneration method according to claim 1, characterized in that, The hydrolysis reaction takes place in a closed environment.

8. The recycling and regeneration method according to claim 1, characterized in that, The recycling method further includes repolymerizing the hydrolysis product obtained from the hydrolysis reaction to prepare polyesteramide; The repolymerization includes sequential esterification and polycondensation reactions.

9. The recycling and regeneration method according to claim 8, characterized in that, The re-aggregation includes the following steps: The oligomers and / or monomers obtained from the hydrolysis reaction are subjected to esterification with additional monomers and polymerization catalysts for the preparation of polyesteramides. The product obtained from the esterification reaction was subjected to a polycondensation reaction to obtain polyesteramide.

10. The recycling and regeneration method according to claim 9, characterized in that, The esterification reaction is carried out under normal pressure and at a reaction temperature of 130-200℃. The conditions for the polycondensation reaction are a vacuum of 10-100 Pa and a reaction temperature of 200-290 °C.

Citation Information

Cited By

  • Method for recycling waste colored chinlon

    CN121628094A