Sandwich-toughened ceramic-based fuel element and additive manufacturing method thereof
By introducing a sandwich toughening structure into SiC fuel elements and utilizing SiC whiskers and chemical vapor infiltration technology, the problems of crack suppression and damage tolerance improvement in complex structures are solved, achieving a balance between structural reliability and manufacturability.
Patent Information
- Application Number
- CN202610203572.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-02-12
- Publication Date
- 2026-05-26
- Estimated Expiration
- 2046-02-12
AI Technical Summary
Existing technologies struggle to achieve effective crack suppression and damage tolerance improvement in complex SiC fuel elements, especially without introducing independent cladding structures. This makes it difficult to balance manufacturability and toughening effects, resulting in insufficient structural reliability.
A method for preparing ceramic-based fuel elements with sandwich toughening is adopted. This method involves introducing low-solid-content SiC whisker slurry or generating whisker structures in situ during additive manufacturing, combined with chemical vapor infiltration pre-deposition and overall densification treatment, to form a sandwich toughened structure.
It improves the fracture toughness and structural stability of SiC-based fuel elements, enhances service reliability, is suitable for complex geometric designs, and reduces the risk of failure caused by local defects.
Smart Images

Figure CN121726126B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of nuclear reactor fuel technology and relates to the additive manufacturing of silicon carbide-based composite material elements, specifically to a sandwich-toughened ceramic-based fuel element and its additive manufacturing method. Background Technology
[0002] As advanced nuclear reactors increasingly demand higher levels of safety, integration, and manufacturing efficiency, fuel elements are evolving from traditional separate fuel and structure designs towards a highly integrated fuel-structure configuration. New reactor concepts, exemplified by the Transformational Challenge Reactor (TCR), propose using advanced manufacturing technologies to achieve integrated fabrication of fuel elements and supporting structures, thereby shortening design and manufacturing cycles and improving the overall engineering efficiency of core components. In this technological approach, additive manufacturing is considered a crucial means of realizing fuel elements with complex geometries and integrated functions.
[0003] Silicon carbide (SiC) has become an important candidate material for integrated fuel elements due to its excellent high-temperature mechanical properties, corrosion resistance, and good radiation resistance potential. Using additive manufacturing processes such as Digital Light Processing (DLP), SiC-based fuel elements can achieve integrated molding of complex shapes, thin-walled structures, and internal channels, providing new design space for the synergistic optimization of fuel element performance in neutronics, heat transfer, and structural properties. However, the integrated molding of complex structures also presents new challenges for SiC elements in terms of structural continuity and sensitivity to manufacturing defects.
[0004] SiC is a typical brittle ceramic material with limited fracture toughness and damage tolerance, and is highly sensitive to residual porosity, interface defects, and geometric abrupt changes. In additively manufactured integrated fuel elements, structural features such as hyperbolic shapes, thin-walled regions, and open transition zones inevitably introduce localized stress concentrations. Under service conditions of coupled thermal gradients and mechanical loads, once microcracks form, they easily propagate along the element structure, thereby weakening the overall structural integrity and service reliability of the fuel element. Therefore, relying solely on the intrinsic properties of the integral SiC material is insufficient to meet the high safety margin requirements of integrated fuel elements in complex service environments.
[0005] To address the toughening requirements of SiC elements, existing technologies mostly focus on overall material modification or single-layer shell structure reinforcement designs. However, in highly integrated fuel-structure components, these methods often struggle to simultaneously address the manufacturability of complex structures, the feasibility of subsequent fuel filling and encapsulation processes, and the uniformity requirements of the densification process. In particular, without introducing an independent cladding structure, a suitable structural design solution for additively manufactured integrated fuel elements remains lacking in terms of how to effectively suppress cracks and improve damage tolerance within the outer structure of the component. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide a sandwich-toughened ceramic-based fuel element and its additive manufacturing method, thereby solving the technical problems of existing additively manufactured SiC fuel elements being prone to brittle failure under high-temperature service conditions, insufficient structural reliability due to stress concentration in corner and thin-walled areas, and the difficulty of existing integral composite or material modification processes in simultaneously achieving manufacturability and toughening effect under complex structural conditions.
[0007] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0008] An additive manufacturing method for sandwich-toughened ceramic-based fuel elements, such as... Figure 1 As shown, the method specifically includes the following steps:
[0009] Step 1: The shell is prepared using additive manufacturing process.
[0010] Step 2, preparation of toughened interlayer: inject low solid content, low viscosity SiC whisker slurry into the interlayer space, and then perform curing treatment. After the slurry is cured, a toughened interlayer is formed in the interlayer space; then degreasing treatment is performed.
[0011] Specifically, step two can be replaced by: immersing the interlayer space in a raw material slurry containing Si and C, pouring out the excess slurry and drying it, repeating this process three times, and then performing heat treatment to generate self-grown whiskers in situ within the interlayer space, thereby obtaining a toughened interlayer.
[0012] Step 3, pre-deposition treatment: using trichloromethylsilane as the source gas, hydrogen as the carrier gas, and hydrogen and argon as dilution gases, chemical vapor infiltration pre-deposition is performed on the shell with toughening interlayer to initially reinforce the double shell and toughening interlayer.
[0013] Step 4, fuel filling and sealing: Fill the fuel tank with mixed fuel, reserve sealing height at the opening of the fuel tank, and use SiC slurry to simultaneously seal the opening of the fuel tank and the interlayer space, and then dry the sealed overall structure.
[0014] Step 5, Overall densification treatment: Using trichloromethylsilane as the source gas, hydrogen as the carrier gas, and hydrogen and argon as dilution gases, the dried element is deposited using an enhanced chemical vapor infiltration method to obtain a ceramic-based fuel element with a sandwich toughened structure.
[0015] The present invention also has the following technical features:
[0016] Specifically, in step one, the additive manufacturing process is digital light processing photopolymerization forming technology; including: using a base plate as the starting building layer for additive manufacturing, continuously building the outer wall and inner wall layer by layer on the base plate, so that the outer wall, inner wall and base plate form an integrated structure, and obtaining the shell of the ceramic-based fuel element.
[0017] Specifically, in step two, vibration or negative pressure is used to assist in the grouting process.
[0018] Specifically, in step two, the curing conditions are: maintaining a temperature of 75–85°C for 12–18 hours. Preferably, maintaining a temperature of 80°C for 20 hours.
[0019] Specifically, in step two, when using the SiC whisker slurry injection method, the degreasing treatment conditions are as follows: heating at a rate of 0.8–2.2 °C / min to 450–580 °C, holding at that temperature for 5–6 h, and then cooling at a rate of 2–5 °C / min. Preferably, heating at a rate of 1–2 °C / min to 500–550 °C, holding at that temperature for 5–6 h, and then cooling at a rate of 3 °C / min.
[0020] Specifically, in step two, when the in-situ self-grown whisker method is used, the total mass fraction of Si and C in the raw material slurry is 15% to 25%.
[0021] Specifically, in step two, when using the in-situ self-grown whisker method, the heat treatment conditions are as follows: under argon protection, the heating rate is 0.8 to 2.2 °C / min, and after reaching 450 to 580 °C, it is held for 5 to 6 hours to complete the degreasing treatment. Then, the temperature is increased to 1100 °C at a heating rate of 1 °C / min and held for 3 hours, and then cooled to room temperature with the furnace.
[0022] Specifically, in step three, the molar ratio of hydrogen to trichloromethylsilane is 8–12:1, the carrier gas hydrogen flow rate is 2–5 L / min, the dilution gas hydrogen flow rate is 1–3 L / min, and the dilution gas argon flow rate is 2–5 L / min. Preferably, the molar ratio of hydrogen to trichloromethylsilane is 9:1, the carrier gas hydrogen flow rate is 3 L / min, the dilution gas hydrogen flow rate is 2 L / min, and the dilution gas argon flow rate is 3 L / min.
[0023] Specifically, in step three, the pre-deposition conditions are: deposition temperature of 950–1150℃, deposition pressure of 2.5–3.5 kPa, and deposition time of 35–55 h. Preferably, the deposition temperature is 1050℃, the deposition pressure is 3 kPa, and the deposition time is 40–50 h.
[0024] Specifically, in step four, the package height is 0.8–1.8 mm. Preferably, the package height is 1–1.5 mm.
[0025] Specifically, in step four, the mixed fuel consists of TRISO particles and SiC matrix powder, with a volume ratio of 4–6:4–6. Preferably, the volume ratio is 5.5:4.5.
[0026] Specifically, in step four, the SiC slurry is composed of silicon carbide powder and deionized water, with a mass ratio of 8 to 12:1. Preferably, the mass ratio is 9:1.
[0027] Specifically, in step four, the drying conditions are: drying at 70–90°C for 12–18 hours. Preferably, drying at 80°C for 15 hours.
[0028] Specifically, in step five, the deposition conditions are: deposition temperature of 1050–1300℃, deposition pressure of 8–12 kPa, and deposition time of 100–135 h. Preferably, the deposition temperature is 1150–1200℃, the deposition pressure is 9–10 kPa, and the deposition time is 110–120 h.
[0029] Specifically, in step five, the molar ratio of hydrogen to trichloromethylsilane is 9–13:1, the carrier gas hydrogen flow rate is 2–6 L / min, the dilution gas hydrogen flow rate is 2–5 L / min, and the dilution gas argon flow rate is 4–8 L / min. Preferably, the molar ratio of hydrogen to trichloromethylsilane is 11:1, the carrier gas hydrogen flow rate is 4–5 L / min, the dilution gas hydrogen flow rate is 3 L / min, and the dilution gas argon flow rate is 5–6 L / min.
[0030] The present invention also protects a sandwich-toughened ceramic-based fuel element prepared by the method described above, comprising a shell, a filled fuel and a toughened sandwich layer; the toughened sandwich layer is prepared from a slurry with a SiC whisker content of 10-12 wt% and an apparent viscosity of 0.5 Pa·s at 25°C.
[0031] Specifically and optionally, the toughening interlayer may be prepared by in-situ reaction of a slurry with a total Si and C content of 15% to 25%.
[0032] Specifically, the housing includes a base plate, an outer wall integrally formed on the base plate, an inner wall coaxially formed inside the outer wall, an annular gap between the outer wall and the inner wall as a sandwich space, and a sandwich opening provided at the top of the housing for subsequent sandwich filling and sealing.
[0033] Specifically, the thickness of the interlayer space is 0.1 to 0.2 mm, which is one-tenth the thickness of the base plate.
[0034] Specifically and optionally, a cooling pipe is arranged axially at the center of the inner wall, and six cooling pipes are evenly distributed circumferentially around it; the space enclosed by the outer surface of the cooling pipes, the inner surface of the inner wall, and the upper surface of the bottom plate constitutes a fuel compartment. The outer wall is a hollow hexagonal prism structure, including six side walls; the inner wall is a hollow hexagonal prism structure, including six side walls. Seven circular through holes are opened on the bottom plate, the diameter of which matches the inner diameter of the cooling pipes; the through holes correspond one-to-one with the cooling pipes and are connected to form a through cooling channel.
[0035] Specifically and optionally, the space enclosed by the inner surface of the inner wall and the upper surface of the bottom plate is the fuel compartment. Both the outer and inner walls are hollow cylindrical structures.
[0036] Compared with the prior art, the present invention has the following technical effects:
[0037] (I) This invention involves injecting and solidifying a low-solids-content, low-viscosity SiC whisker slurry into the interlayer space, or generating a self-grown whisker structure in situ within the interlayer space through heat treatment of a Si and C-containing raw material system. In other words, by introducing an interlayer toughening structure without significantly increasing the structural complexity of the element, it can effectively improve the fracture toughness, crack resistance, structural stability, and service stability of SiC-based fuel elements.
[0038] (II) This invention achieves integrated manufacturing of the double-layer shell and the interlayer space through DLP additive manufacturing, which has good manufacturability, is suitable for complex geometry and structural expansion design requirements, and can manufacture high-temperature nuclear fuel elements with various structural forms.
[0039] (III) The present invention adopts the process route of “interlayer opening - synchronous packaging - overall densification”, which can improve the sealing consistency and overall densification effect, and reduce the failure risk caused by local defects. Attached Figure Description
[0040] Figure 1 Flowchart of additive manufacturing process for sandwich-toughened ceramic-based fuel elements.
[0041] Figure 2 This is a physical image of the housing of the ceramic-based fuel element in Example 1.
[0042] Figure 3for Figure 2 A sectional view of the model along the A-A' direction.
[0043] Figure 4 This is a schematic diagram of the base plate structure of the ceramic-based fuel element housing in Example 1.
[0044] Figure 5 This is a comparison diagram of the reaction force-displacement relationship of the sandwich-toughened ceramic-based fuel element prepared in Example 2.
[0045] Figure 6 This is a model diagram of the sandwich-toughened ceramic-based fuel element housing prepared in Example 4.
[0046] The labels in the diagram represent: 1-bottom plate, 2-outer wall, 3-inner wall, 4-interlayer space, 5-cooling pipe, 6-fuel compartment.
[0047] The specific content of the present invention will be further explained in detail below with reference to the embodiments. Detailed Implementation
[0048] It should be noted that, unless otherwise specified, all raw materials and control products used in this invention are those known in the art.
[0049] Following the above technical solutions, specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent modifications made based on the technical solutions of this application fall within the protection scope of the present invention.
[0050] Example 1
[0051] This embodiment provides a housing for a ceramic-based fuel element, such as... Figures 2 to 4 As shown, the shell includes a base plate (1), an outer wall (2) is integrally provided on the base plate (1), an inner wall (3) is coaxially provided inside the outer wall (2), the annular gap between the outer wall (2) and the inner wall (3) is a sandwich space (4), and a sandwich opening is provided at the top of the shell for subsequent sandwich filling and sealing; a cooling pipe (5) is provided at the center of the inner wall (3) along the axial direction, and six cooling pipes (5) are evenly distributed around it along the circumferential direction; the space enclosed by the outer surface of the cooling pipe (5), the inner surface of the inner wall (3) and the upper surface of the base plate (1) is a fuel tank (6).
[0052] As a specific embodiment, the outer wall (2) is a hollow hexagonal prism structure, including six sidewalls; the inner wall (3) is a hollow hexagonal prism structure, including six sidewalls. In this embodiment, designing the outer wall (2) and inner wall (3) as hexagonal prism structures allows for seamless stacking of units [similar to a honeycomb structure], maximizing space utilization. In the reactor core, hexagonal fuel assemblies can be arranged more closely, increasing the amount of fuel per unit volume, thereby improving the reactor power density.
[0053] As a specific solution in this embodiment, the base plate (1) is provided with seven circular through holes, the diameter of which matches the inner diameter of the cooling pipe (5); the through holes correspond one-to-one with the cooling pipe (5) and are connected to form a through cooling channel for the cooling medium to circulate.
[0054] As a specific solution in this embodiment, the thickness W1 of the interlayer space (4) is 0.2 mm.
[0055] As a specific embodiment, the thickness H1 of the base plate (1) is 2 mm and the distance between opposite sides L1 is 86 mm; the height H2 of the outer wall (2) is 98 mm, the wall thickness T2 is 2.4 mm, and the distance between opposite sides L2 is 86 mm; the height H3 of the inner wall (3) is 98 mm, the wall thickness T3 is 2.4 mm, and the distance between opposite sides L3 is 76 mm.
[0056] As a specific embodiment, the cooling pipe (5) is a hollow cylindrical structure with a height H4 of 98 mm, a wall thickness T4 of 2 mm, and an outer diameter L4 of 18 mm.
[0057] Example 2
[0058] This embodiment provides an additive manufacturing method for a sandwich-toughened ceramic-based fuel element, which specifically includes the following steps:
[0059] Step 1: Prepare the shell using additive manufacturing process: Using the base plate (1) as the starting building layer for additive manufacturing, build the outer wall (2), inner wall (3) and cooling pipe (5) layer by layer on the base plate (1) so that the outer wall (2), inner wall (3) and cooling pipe (5) form an integrated structure with the base plate (1) to obtain the shell of the ceramic-based fuel element of Example 1.
[0060] In this embodiment, the process includes: mixing β-phase silicon carbide powder with a resin monomer system, a dispersant, and a photoinitiator to prepare a SiC ceramic slurry. The average particle size of the SiC powder is 8 μm. The resin monomer is a dual-monomer system composed of HDDA and TMPTA, with HDDA accounting for 50% of the mass fraction in (HDDA+TMPTA). The dispersant is a compound dispersant of KOS110 and Solspers™ 17000 in a mass ratio of 1:1, with a total addition amount of 5 wt.%. The photoinitiator is TPO, with an addition amount of 2 wt.%. The solid content of the slurry is 40 vol.%. The slurry is ball-milled for 3 h to achieve uniform dispersion, followed by DLP printing. The DLP printing parameters are: layer thickness 20 μm, light intensity 30 mW / cm², and single-layer exposure time 60 s.
[0061] Step 2, preparation of toughened interlayer: Low solid content and low viscosity SiC whisker slurry is injected into the interlayer space (4). The SiC whisker content in the slurry is 12wt%, and the apparent viscosity of the slurry at 25℃ is 0.5Pa·s. Vibration or negative pressure is used during the injection of slurry to improve the filling ability of the slurry in the interlayer space and improve the uniformity of whisker distribution in the interlayer space (4). Then, the slurry is kept at 80℃ for 20h. After the slurry solidifies, a toughened interlayer reinforced with SiC whiskers is formed in the interlayer space (4). Then, degreasing treatment is performed to remove the organic phase. The degreasing treatment conditions are: heating at a rate of 2℃ / min to 550℃, holding for 2h, and then cooling at 3℃ / min; then cooling to room temperature with the furnace.
[0062] Step 3: Pre-deposition treatment: Chemical vapor infiltration pre-deposition is performed on the shell with the toughened interlayer. During deposition, trichloromethylsilane is used as the source gas, hydrogen as the carrier gas, and hydrogen and argon as dilution gases. The molar ratio of hydrogen to trichloromethylsilane is 9:1. The deposition temperature is controlled at 1050℃, the flow rate of the carrier gas hydrogen is 3 L / min, the flow rate of the dilution gas hydrogen is 2 L / min, and the flow rate of the dilution gas argon is 3 L / min. The deposition pressure is 3 kPa, and the deposition time is 50 h. This provides preliminary reinforcement to the double-layer shell and the toughened interlayer.
[0063] Step 4, fuel filling and encapsulation: Fill the fuel tank (6) with mixed fuel, leave an encapsulation height of about 1.5 mm at the opening of the fuel tank (6), and simultaneously encapsulate the fuel tank (6) and the opening of the interlayer space (4) with SiC slurry with a high solid content of 90% (i.e., the mass ratio of silicon carbide powder to deionized water is 9:1). Then, dry the encapsulated overall structure at 80°C for 10 h. It should be noted that in actual use, the mixed fuel is a mixture of TRISO particles and SiC matrix powder (volume ratio 5.5:4.5). In this embodiment, zirconia microspheres are used as simulated TRISO particles instead of TRISO particles.
[0064] Step 5, Overall Densification Treatment: The dried element was deposited using enhanced chemical vapor infiltration (CVI). Trichloromethylsilane was used as the source gas, hydrogen as the carrier gas, and hydrogen and argon as dilution gases. The molar ratio of hydrogen to trichloromethylsilane was 11:1. The deposition temperature was controlled at 1200℃, the hydrogen flow rate was 5 L / min, the hydrogen flow rate was 3 L / min, and the argon flow rate was 6 L / min. The deposition pressure was 10 kPa, and the deposition time was 120 h, ultimately yielding a sandwich-toughened ceramic-based fuel element.
[0065] Figure 5 The diagram shows a comparison of the reaction force-displacement relationship of the sandwich-toughened ceramic-based fuel element. The ceramic-based fuel element containing whiskers exhibits a higher reaction force under the same displacement conditions, indicating that its mechanical load-bearing capacity is improved, thus demonstrating a good toughening effect.
[0066] Example 3
[0067] This embodiment provides an additive manufacturing method for a sandwich-toughened ceramic-based fuel element, which specifically includes the following steps:
[0068] In this embodiment, step one is completely identical to step one in embodiment 2.
[0069] Step 2, preparation of toughened interlayer: A raw material slurry containing Si powder and C powder is poured into the interlayer space (4), wherein the mass ratio of Si powder to C powder is 1:1, and the total mass fraction of powder in the slurry is 20%. After pouring out the excess slurry, it is dried and repeated three times. Under argon protection, the heating rate is 1℃ / min, and after reaching 550℃, it is held for 6 hours. Then, the temperature is increased to 1100℃ at a heating rate of 1℃ / min and held for 3 hours to generate self-grown whiskers in situ in the interlayer space (4). Then, it is cooled to room temperature with the furnace. A toughened interlayer reinforced with SiC whiskers is formed in the interlayer space (4).
[0070] In this embodiment, steps three to five are completely identical to steps three to five in embodiment 2.
[0071] Example 4
[0072] This embodiment provides a housing for a ceramic-based fuel element, such as... Figure 6 As shown, the shell includes a base plate (1), an outer wall (2) is integrally provided on the base plate (1), an inner wall (3) is coaxially provided inside the outer wall (2), the annular gap between the outer wall (2) and the inner wall (3) is a sandwich space (4), and a sandwich opening is provided at the top of the shell for subsequent sandwich filling and sealing; the space enclosed by the inner surface of the inner wall (3) and the upper surface of the base plate (1) is a fuel tank (6).
[0073] As a specific embodiment, both the outer wall (2) and the inner wall (3) are hollow cylindrical structures.
[0074] As a specific solution in this embodiment, the thickness w1 of the interlayer space (4) is 0.1 mm.
[0075] As a specific solution in this embodiment, the thickness h1 of the base plate (1) is 1mm and the diameter d1 is 40mm; the height h2 of the outer wall (2) is 49mm, the wall thickness t2 is 1.2mm and the outer diameter d2 is 40mm; the height h3 of the inner wall (3) is 49mm, the wall thickness t3 is 1.2mm and the inner diameter d3 is 35mm.
[0076] Example 5
[0077] This embodiment provides an additive manufacturing method for a sandwich-toughened ceramic-based fuel element, which specifically includes the following steps:
[0078] Step 1: Prepare the shell using additive manufacturing process: Using the base plate (1) as the starting building layer for additive manufacturing, build the outer wall (2) and inner wall (3) layer by layer on the base plate (1) so that the outer wall (2), inner wall (3) and base plate (1) form an integrated structure, and obtain the shell of the ceramic-based fuel element of Example 3.
[0079] Step 2, preparation of toughened interlayer: Low solid content and low viscosity SiC whisker slurry is injected into the interlayer space (4). The SiC whisker content in the slurry is 10wt%, and the apparent viscosity of the slurry at 25℃ is 0.4Pa·s. Vibration or negative pressure is used during the injection of slurry to improve the filling ability of the slurry in the interlayer space and improve the uniformity of whisker distribution in the interlayer space (4). Then, the slurry is kept at 80℃ for 20h. After the slurry solidifies, a toughened interlayer reinforced with SiC whiskers is formed in the interlayer space (4). Then, degreasing treatment is performed to remove the organic phase. The degreasing treatment conditions are: heating at a rate of 1℃ / min to 500℃, holding at 1.5h, and then cooling at 3℃ / min; then cooling to room temperature with the furnace.
[0080] Step 3: Pre-deposition treatment: Chemical vapor infiltration pre-deposition is performed on the shell with the toughened interlayer. During deposition, trichloromethylsilane is used as the source gas, hydrogen as the carrier gas, and hydrogen and argon as dilution gases. The molar ratio of hydrogen to trichloromethylsilane is 9:1. The deposition temperature is controlled at 1050℃, the flow rate of the carrier gas hydrogen is 3 L / min, the flow rate of the dilution gas hydrogen is 2 L / min, and the flow rate of the dilution gas argon is 3 L / min. The deposition pressure is 3 kPa, and the deposition time is 40 h. This provides preliminary reinforcement to the double-layer shell and the toughened interlayer.
[0081] Step 4, fuel filling and encapsulation: Fill the fuel tank (6) with mixed fuel, leave an encapsulation height of about 1 mm at the opening of the fuel tank (6), and simultaneously encapsulate the opening of the fuel tank (6) and the interlayer space (4) with SiC slurry with a high solid content of 90% (i.e., the mass ratio of silicon carbide powder to deionized water is 9:1). Then, dry the encapsulated overall structure at 80°C for 15 hours. It should be noted that in actual use, the mixed fuel is a mixture of TRISO particles and SiC matrix powder (volume ratio 5.5:4.5). In this embodiment, zirconia microspheres are used as simulated TRISO particles instead of TRISO particles.
[0082] Step 5, Overall Densification Treatment: The dried element is deposited using enhanced chemical vapor infiltration (CVI). During deposition, trichloromethylsilane is used as the source gas, hydrogen as the carrier gas, and hydrogen and argon as dilution gases. The molar ratio of hydrogen to trichloromethylsilane is 11:1. The deposition temperature is controlled at 1150℃, the hydrogen flow rate is 4 L / min, the hydrogen flow rate is 3 L / min, and the argon flow rate is 5 L / min. The deposition pressure is 9 kPa, and the deposition time is 110 h, thus obtaining a ceramic-based fuel element with a sandwich-toughened structure.
[0083] In summary, the present invention improves the crack resistance and structural stability of the element by introducing a toughening structure with clearly defined structural functional partitions into the element shell, without significantly increasing the structural complexity and manufacturing difficulty of the element. This meets the requirements of advanced reactors, such as TCRs, for the safety and engineering adaptability of new fuel elements.
Claims
1. An additive manufacturing method for a sandwich-toughened ceramic-based fuel element, characterized in that, A ceramic-based fuel element, comprising a housing, fuel filling, and a toughened interlayer; The toughened interlayer is prepared by in-situ reaction of a slurry containing Si powder and C powder, wherein the mass ratio of Si powder to C powder is 1:1, and the total mass fraction of Si powder and C powder in the slurry is 15% to 25%. The shell includes a base plate (1), an outer wall (2) is integrally provided on the base plate (1), an inner wall (3) is coaxially provided inside the outer wall (2), the annular gap between the outer wall (2) and the inner wall (3) is a sandwich space (4), and a sandwich opening is provided at the top of the shell for subsequent sandwich filling and sealing. The method specifically includes the following steps: Step 1: Fabricate the shell using a photopolymerization additive manufacturing process. Using the base plate (1) as the starting building layer for additive manufacturing, the outer wall (2), inner wall (3) and cooling pipe (5) are continuously built layer by layer on the base plate (1), so that the outer wall (2), inner wall (3) and cooling pipe (5) and the base plate (1) form an integrated structure, and the shell is obtained; Step 2, preparation of toughened interlayer: The interlayer space is impregnated with a raw material slurry containing Si and C, and then heat-treated to generate self-grown whiskers in situ within the interlayer space, thereby obtaining the toughened interlayer. The heat treatment conditions are as follows: under argon protection, the heating rate is 1℃ / min, reaching 550℃ and holding for 6 hours, then heating at a rate of 1℃ / min to 1100℃ and holding for 3 hours to generate self-grown whiskers in situ within the interlayer space; subsequently, the furnace is cooled to room temperature. Step 3, pre-deposition treatment: using trichloromethylsilane as the source gas, hydrogen as the carrier gas, and hydrogen and argon as dilution gases, chemical vapor infiltration pre-deposition is performed on the shell with toughening interlayer to initially reinforce the double shell and toughening interlayer. Step 4, fuel filling and sealing: Fill the fuel tank with mixed fuel, reserve sealing height at the opening of the fuel tank, and use SiC slurry to simultaneously seal the opening of the fuel tank and the interlayer space, and then dry the sealed overall structure. Step 5, Overall densification treatment: Using trichloromethylsilane as the source gas, hydrogen as the carrier gas, and hydrogen and argon as dilution gases, the dried element is deposited using an enhanced chemical vapor infiltration method to obtain a ceramic-based fuel element with a sandwich toughened structure.
2. The additive manufacturing method for the sandwich-toughened ceramic-based fuel element as described in claim 1, characterized in that, The toughened interlayer may be made of SiC whisker slurry, with SiC whisker content of 10-12 wt% and apparent viscosity of 0.5 Pa·s at 25°C. Step two may be as follows: inject low-solids-content, low-viscosity SiC whisker slurry into the interlayer space, followed by curing treatment. After the slurry cures, a toughened interlayer is formed in the interlayer space. Then, the shell is degreased. The curing treatment conditions are: holding at 75-85℃ for 12-18h; the degreasing treatment conditions are: heating at a rate of 0.8-2.2℃ / min to 450-580℃, holding at that temperature for 1.2-2.2h, and then cooling at a rate of 2-5℃ / min.
3. The additive manufacturing method for the sandwich-toughened ceramic-based fuel element as described in claim 1, characterized in that, In step three, the pre-deposition conditions are: deposition temperature of 950–1150℃, deposition pressure of 2.5–3.5 kPa, and deposition time of 35–55 h; In step three, the molar ratio of hydrogen to trichloromethylsilane is 8–12:1, the flow rate of carrier gas hydrogen is 2–5 L / min, the flow rate of dilution gas hydrogen is 1–3 L / min, and the flow rate of dilution gas argon is 2–5 L / min.
4. The additive manufacturing method for the sandwich-toughened ceramic-based fuel element as described in claim 1, characterized in that, In step four, the drying conditions are: drying at 70–90℃ for 12–18 hours.
5. The additive manufacturing method for the sandwich-toughened ceramic-based fuel element as described in claim 1, characterized in that, In step four, the mixed fuel consists of TRISO particles and SiC matrix powder, with a volume ratio of 4-6:4-6. In step four, the SiC slurry is composed of silicon carbide powder and water, with a mass ratio of 8 to 12:
1.
6. The additive manufacturing method for the sandwich-toughened ceramic-based fuel element as described in claim 1, characterized in that, In step five, the deposition conditions are: deposition temperature of 1050–1300℃, deposition pressure of 8–12 kPa, and deposition time of 100–135 h; In step five, the molar ratio of hydrogen to trichloromethylsilane is 9–13:1, the flow rate of carrier gas hydrogen is 2–6 L / min, the flow rate of dilution gas hydrogen is 2–5 L / min, and the flow rate of dilution gas argon is 4–8 L / min.
Citation Information
Patent Citations
Multilayer structure of SiC / SiC (silicon carbide) composite cladding tube and preparation method thereof
CN103818056A
Accident-resistant fuel core cladding tube and preparation method thereof
CN109020589A
Prismatic TRISO particle dispersion additive fuel element as well as preparation method and application thereof
CN119889750A