High-stability double-layer core-shell coated pure copper silver-substituted conductive paste and preparation method thereof

By designing a double-layer core-shell structure copper powder and optimizing specific additive solvents, the oxidation and compatibility issues of copper-to-silver paste have been resolved, resulting in a highly stable and low-cost conductive paste suitable for electronic products such as printed circuit boards.

CN121839247APending Publication Date: 2026-04-10高广军
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202610265919.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-05
Publication Date
2026-04-10

AI Technical Summary

Technical Problem

Existing copper-to-silver conductive pastes suffer from problems such as easy oxidation of copper powder, poor storage stability, and poor curing compatibility, resulting in substandard performance and high switching costs. Furthermore, they are constrained by patent barriers imposed by industry giants, making large-scale commercialization difficult.

Method used

The copper powder adopts a dual-core-shell structure design, with an inner nano-silver passivation layer and an outer organic composite coating layer. Combined with specific additives and solvents, it forms a full-cycle antioxidant system that is compatible with existing silver paste curing processes, reduces silver content, and optimizes paste composition to improve stability and compatibility.

Benefits of technology

It achieves highly stable and low-cost conductive paste with a long shelf life at room temperature, strong compatibility, reduced production costs, and avoids patent infringement risks, making it suitable for small and medium-sized customers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides high-stability double-layer core-shell coated pure copper silver-substituted conductive paste and a preparation method thereof, and belongs to the technical field of electronic special materials. The copper-resistant coating comprises the following components in percentage by mass: 82%-90% of antioxidant copper powder with a double-layer core-shell structure, 3%-6% of bismuth-boron-zinc lead-free low-melting-point glass powder, 3%-7% of a modified epoxy resin compound organic carrier, 2%-5% of a gradient volatilization compound solvent and 0.5%-2% of a special compound additive for copper. Through the double-layer core-shell copper powder design of inner-layer nano-silver passivation and outer-layer organic composite coating and in cooperation with a liquid-phase synergistic anti-oxidation system, the volume resistivity after slurry curing is smaller than or equal to 3.5 * 10 <-5 > omega.cm, the resistivity change rate after 1000-hour damp-heat aging at 85 DEG C / 85% RH is smaller than or equal to 10%, the normal-temperature storage period without opening a tank is larger than or equal to 6 months, direct curing can be conducted in the conventional air atmosphere of 120-160 DEG C, and the high-temperature-resistant copper paste can be applied to the field of high-temperature storage. The silver paste is completely compatible with production and application production lines of existing silver paste, equipment transformation is not needed, the comprehensive cost is reduced by more than 80% compared with pure silver paste, and the silver paste can be widely applied to the fields of PCBs, membrane switches, flexible electronics, photovoltaic back electrodes, LED packaging and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electronic special materials technology, specifically relating to a highly stable double-layer core-shell coated pure copper silver substitute conductive paste and its preparation method. Background Technology

[0002] Conductive paste is a core material in the manufacturing process of electronic products such as printed circuit boards, flexible electronic devices, photovoltaic cells, and LED packaging. Its conductivity, stability, and lifespan directly determine the performance and reliability of the final electronic devices. Currently, the mainstream conductive paste used in the industry is silver paste. Silver has excellent conductivity and chemical stability, but it is a scarce precious metal with high prices and volatile market fluctuations. This not only significantly increases the production costs of downstream industries but also results in a serious waste of precious metal resources.

[0003] Copper has a conductivity similar to silver, and its abundant reserves and low price in the Earth's crust make it an ideal material to replace silver in the preparation of conductive pastes. However, existing copper-based conductive pastes still face three core technological challenges that the industry urgently needs to address: First, copper powder is chemically reactive and easily oxidizes throughout the entire process of paste storage, printing, and curing, forming non-conductive copper oxide. This leads to a significant decrease in the conductivity of the paste, or even complete failure. Existing ordinary pure copper paste generally has a volume resistivity ≥1×10⁻⁶ after curing. -4 Ω·cm, which cannot meet the performance requirements of mid-to-high-end application scenarios; Second, the slurry has poor storage stability. Ordinary copper slurry can generally be stored for less than 3 months at room temperature without opening the tank. It is very easy for problems such as powder agglomeration, sedimentation, slurry stratification, oxidation and scrapping to occur, which cannot meet the needs of industrial production and warehousing and transportation. Third, the curing compatibility is poor. Most existing high-performance copper pastes require nitrogen-protected curing, laser sintering, or narrow temperature window curing processes, which cannot be directly compatible with the conventional curing production lines of existing silver pastes. Downstream customers need to invest a lot of money to modify their equipment to replace them, resulting in extremely high switching costs, which seriously restricts the large-scale commercialization of copper-based silver pastes.

[0004] Meanwhile, the core technology patents for existing high-end copper-to-silver pastes are basically monopolized by domestic and international industry giants such as DuPont, Heraeus, and Polymer Materials. Copper pastes produced by small and medium-sized manufacturers generally suffer from substandard performance, lack of independent intellectual property rights, and high infringement risks, making it impossible to provide downstream small and medium-sized customers with stable, compliant, and cost-effective products. Therefore, developing a pure copper-to-silver conductive paste that combines high conductivity, high storage stability, full production line compatibility, low cost, and no patent infringement risks has extremely strong market demand and commercial value. Summary of the Invention

[0005] The purpose of this invention is to overcome the above-mentioned shortcomings of the prior art and provide a highly stable double-layer core-shell coated pure copper silver substitute conductive paste and its preparation method. Through the core design of copper powder with a double-layer core-shell structure, combined with the synergistic optimization of the whole system formula and process, the industry pain point of easy oxidation of copper powder is solved from the root. At the same time, the paste achieves high storage stability, full production line compatibility and extreme cost advantage, completely avoids existing patent barriers and can form independent intellectual property protection.

[0006] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: A highly stable double-layer core-shell coated pure copper-silver substitute conductive paste, comprising the following components by mass fraction (100%): Double-layer core-shell structure anti-oxidation copper powder 82%-90%; Bismuth-boron-zinc based lead-free low-melting-point glass powder, 3%-6%; Modified epoxy resin is compounded with 3%-7% organic carrier; Gradient evaporation compound solvent 2%-5%; Copper-specific compound additives: 0.5%-2%.

[0007] Furthermore, the dual-core-shell structure antioxidant copper powder uses micron-sized spherical high-purity copper powder as the core, with an inner layer of 20-50nm thick nano-silver passivation layer and an outer layer of 100-200nm thick silane coupling agent and epoxy resin composite organic coating layer; the purity of the dual-core-shell structure antioxidant copper powder is ≥99.9%, particle size D50=1.5-2.5μm, sphericity ≥90%, and tap density ≥4.5g / cm³. 3 Silver content ≤1%.

[0008] This invention utilizes an inner nano-silver passivation layer to form a dense barrier on the surface of the copper powder core, blocking contact between oxygen and water and the copper core. This fundamentally prevents oxidation of the copper powder throughout the entire storage, printing, and curing cycle, solving the industry problem of blackening and a sharp drop in conductivity when ordinary copper powder is heated and cured. The outer organic composite coating layer further enhances the oxidation resistance of the copper powder and achieves perfect compatibility between the copper powder and the organic carrier, eliminating powder agglomeration and sedimentation problems. This allows the slurry to be stored at room temperature for ≥6 months without opening the can, far exceeding the industry average of 3 months. At the same time, with a silver content of only ≤1%, it achieves performance far exceeding that of ordinary pure copper powder, balancing cost reduction and performance improvement.

[0009] Furthermore, the bismuth-boron-zinc-based lead-free low-melting-point glass powder has a softening point of 420-480℃, a particle size D50 of 0.8-1.2μm, and is lead-free and cadmium-free. This glass powder exhibits excellent compatibility with copper powder systems, and will not undergo a displacement reaction with copper powder during curing, thus preventing secondary oxidation of the copper powder. Simultaneously, it can fully melt during medium-temperature curing, forming a dense inorganic adhesive layer, increasing the adhesion between the slurry and the substrate from 1B to over 4B compared to ordinary products. No significant peeling is observed in the cross-cut adhesion test, and the cured film's resistance to damp heat and thermal shock is significantly improved.

[0010] Furthermore, the modified epoxy resin compound, with an organic carrier comprising 100% by mass, includes: 55%-65% bisphenol A type epoxy resin E-20, 15%-25% linear phenolic epoxy resin, and 10%-20% carboxyl-terminated nitrile rubber modified epoxy resin. This compound system balances the hardness and flexibility of the cured film, meeting both the high hardness requirements of rigid PCBs and the bending resistance requirements of flexible PET / PI circuit boards, achieving full-scenario application coverage. Simultaneously, it exhibits excellent compatibility with the organic coating layer of copper powder, preventing slurry stratification and powder sedimentation at the system level. It also boasts a wide curing temperature window, fully curing within the range of 120-160℃, perfectly compatible with all existing silver paste production lines of downstream customers, requiring no equipment modification and incurring zero switching costs.

[0011] Furthermore, the gradient evaporation compound solvent, by mass fraction of 100%, includes: 55%-65% diethylene glycol butyl ether acetate, 25%-35% terpineol, and 5%-15% dodecyl alcohol ester. Through the gradient compounding design of solvents with different boiling points, slow and uniform evaporation without skinning is achieved during the pre-baking stage, and complete evaporation without residue during the curing stage. This fundamentally eliminates the problems of screen clogging during printing and pinholes and bubbles in the cured film layer, allowing for continuous printing for 4 hours after opening the can without screen clogging, far exceeding the 1-hour printing limit of ordinary single-solvent products.

[0012] Furthermore, the copper-specific compound additives, by mass fraction of 100%, include: 20%-30% dispersant, 15%-25% thixotropic agent, 10%-20% liquid phase antioxidant, 15%-25% adhesion promoter, 10%-15% defoamer, and 5%-10% leveling agent.

[0013] Further, the dispersant is BYK-111, the thixotropic agent is hydrophobic fumed silica R972, the liquid-phase antioxidant is a benzotriazole derivative, the adhesion promoter is silane coupling agent KH-560, the defoamer is BYK-066N, and the leveling agent is BYK-333.

[0014] This invention utilizes a copper-specific compound additive system to create a dual antioxidant synergistic effect with double-layer core-shell structured copper powder, while comprehensively optimizing the dispersibility, thixotropy, leveling, and adhesion of the slurry, thereby achieving a synergistic improvement in the overall performance of the slurry.

[0015] Furthermore, the optimal composition ratio of the high-stability double-layer core-shell coated pure copper-silver substitute conductive paste of the present invention, based on a 100% mass fraction, is: Double-layer core-shell structure anti-oxidation copper powder 86%; 4% bismuth-boron-zinc lead-free low-melting-point glass powder; The modified epoxy resin compound contains 5% organic carrier; Gradient evaporation compound solvent 3.5%; Copper-specific compound additives 1.5%.

[0016] This invention also provides a method for preparing the above-mentioned highly stable double-layer core-shell coated pure copper-for-silver conductive paste, comprising the following steps: S1 Dry Mixing Preparation: Weigh out double-layer core-shell structure antioxidant copper powder and bismuth boron zinc-based lead-free low-melting-point glass powder according to the ratio, place them in a three-dimensional mixer, mix at 30 rpm for 10-20 minutes to obtain a uniformly mixed inorganic powder mixture. S2 Wet Pre-dispersion: Weigh the modified epoxy resin compound, organic carrier, gradient volatile compound solvent, and copper-specific compound additive according to the formula, and mix them evenly to obtain an organic phase mixture; add the inorganic powder mixture obtained in step S1 to the organic phase mixture, place it in a high-speed disperser, and disperse it at 1200-1800 rpm for 25-35 minutes to completely wet the powder and obtain a pre-dispersion slurry; S3 Grinding and Refining: The pre-dispersed slurry obtained in step S2 is fed into a three-roll mill and circulated for grinding 3-5 times. The roller gap is gradually reduced from 40-60μm to 8-12μm, and the final slurry fineness is controlled to be ≤10μm to obtain the ground slurry. S4 Vacuum degassing: Place the ground slurry obtained in step S3 into a vacuum degassing machine and degas for 8-15 minutes at a vacuum degree of -0.08~-0.1MPa and a speed of 20-40rpm to eliminate air bubbles inside the slurry, thus obtaining the finished pure copper silver substitute conductive slurry.

[0017] Furthermore, the curing process of the finished pure copper silver-substitute conductive paste is as follows: pre-baking at 120℃ for 10 minutes, curing at 150℃ in a conventional air atmosphere for 30 minutes, without the need for nitrogen protection, fully compatible with existing silver paste curing production lines, and without any equipment modification.

[0018] Compared to existing technologies, it has the following beneficial effects: 1. This invention fundamentally solves the core industry pain point of copper powder's easy oxidation. Through a dual-layer core-shell structure design—inner layer of nano-silver passivation + outer layer of organic composite coating—combined with a liquid-phase specialized antioxidant, a closed-loop dual-antioxidant system is formed throughout the entire lifecycle. The resulting slurry, after curing, has a volume resistivity ≤3.5×10⁻⁶. -5 Ω·cm, reaching the mainstream level of commercial products in the industry, resistivity change rate ≤10% after 1000 hours of damp heat aging at 85℃ / 85%RH, and room temperature storage period ≥6 months without opening the can, far exceeding the performance of ordinary products in the industry.

[0019] 2. This invention achieves perfect compatibility across the entire production line. The paste can be completely cured in a normal air atmosphere at 120-160℃ without the need for special processes such as nitrogen protection or laser sintering. Downstream customers can directly replace their existing silver paste without modifying any production equipment, resulting in zero switching costs and significantly reducing the barriers to product promotion and application.

[0020] 3. This invention has an extreme cost advantage. The silver content of the paste is ≤1%, which is almost negligible. The overall production cost is reduced by more than 80% compared with pure silver paste and by more than 50% compared with silver-coated copper paste of the same performance. It perfectly meets the cost reduction needs of downstream industries and has extremely strong market competitiveness.

[0021] 4. This invention completely circumvents the core patent barriers of domestic and foreign industry giants. The technical solution has complete novelty and inventiveness, and can be directly applied for as an independent invention patent, forming exclusive intellectual property protection. There is no risk of infringement, and downstream customers can cooperate with confidence in the long term.

[0022] 5. The preparation process of this invention is simple and controllable. All raw materials can be purchased domestically. No special high-end equipment is required. Small-scale and large-scale production can be achieved in ordinary university laboratories and pilot-scale bases. It can be quickly commercialized and perfectly meets the small-batch, multi-batch, and customized needs of small and medium-sized customers. Detailed Implementation

[0023] The present invention will be further described in detail below with reference to specific embodiments. The following embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. All other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0024] Example 1 This embodiment provides a highly stable double-layer core-shell coated pure copper-silver substitute conductive paste, with the following component ratio based on 100% by mass: Double-layer core-shell structure anti-oxidation copper powder 86%; 4% bismuth-boron-zinc lead-free low-melting-point glass powder; The modified epoxy resin compound contains 5% organic carrier; Gradient evaporation compound solvent 3.5%; Copper-specific compound additives 1.5%.

[0025] Among them, the double-layer core-shell structure anti-oxidation copper powder has the following characteristics: purity ≥99.9%, D50=2μm, sphericity ≥90%, and tap density ≥4.5g / cm³. 3 The inner layer is a 30nm nano-silver passivation layer, and the outer layer is a 150nm silane coupling agent + epoxy resin composite organic coating layer with a silver content of 0.8%. Bismuth-boron-zinc lead-free low-melting-point glass powder: softening point 450℃, D50=1μm, lead-free and cadmium-free; The modified epoxy resin compound is formulated with an organic carrier: 60% bisphenol A type epoxy resin E-20, 20% linear phenolic epoxy resin, and 20% carboxyl-terminated butadiene-acrylonitrile rubber modified epoxy resin; Gradient volatile compound solvent: 60% diethylene glycol butyl ether acetate, 30% terpineol, and 10% dodecyl alcohol ester; Copper-specific compound additives: BYK-111 dispersant 0.4%, hydrophobic fumed silica R972 0.3%, benzotriazole derivative 0.2%, silane coupling agent KH-560 0.3%, BYK-066N defoamer 0.2%, BYK-333 leveling agent 0.1%.

[0026] The conductive paste preparation method of this embodiment includes the following steps: S1 Dry Mixing Preparation: Weigh out double-layer core-shell structure antioxidant copper powder and bismuth boron zinc-based lead-free low-melting-point glass powder according to the ratio, place them in a three-dimensional mixer, mix at 30 rpm for 15 minutes to obtain a uniformly mixed inorganic powder mixture. S2 Wet Pre-dispersion: Weigh the modified epoxy resin compound, organic carrier, gradient volatile compound solvent, and copper-specific compound additive according to the ratio, and mix them evenly to obtain an organic phase mixture; add the inorganic powder mixture obtained in step S1 to the organic phase mixture, place it in a high-speed disperser, and disperse it at 1500 rpm for 30 minutes to completely wet the powder and obtain a pre-dispersion slurry. S3 Grinding and Refining: The pre-dispersed slurry obtained in step S2 is fed into a three-roll mill and circulated and ground 4 times. The roller spacing is gradually reduced from 50μm to 10μm, and the final slurry fineness is controlled to be ≤10μm to obtain the ground slurry. S4 Vacuum degassing: Place the ground slurry obtained in step S3 into a vacuum degassing machine and degas for 10 minutes at a vacuum degree of -0.09MPa and a rotation speed of 30rpm to eliminate air bubbles inside the slurry, thus obtaining the finished pure copper silver substitute conductive slurry.

[0027] The curing process of the finished slurry in this embodiment is as follows: pre-baking at 120℃ for 10 minutes, curing at 150℃ in a conventional air atmosphere for 30 minutes, without the need for nitrogen protection.

[0028] Example 2 This embodiment provides a highly stable double-layer core-shell coated pure copper-silver substitute conductive paste, with the following component ratio based on 100% by mass: Double-layer core-shell structure anti-oxidation copper powder 82%; Bismuth-boron-zinc series lead-free low-melting-point glass powder 6%; The modified epoxy resin compound contains 7% organic carrier; Gradient evaporation compound solvent 4%; 1% copper-specific compound additive.

[0029] The remaining raw material parameters, preparation methods, and curing processes are completely consistent with those in Example 1.

[0030] Example 3 This embodiment provides a highly stable double-layer core-shell coated pure copper-silver substitute conductive paste, with the following component ratio based on 100% by mass: Double-layer core-shell structure anti-oxidation copper powder (90%); 3% bismuth-boron-zinc lead-free low-melting-point glass powder; The modified epoxy resin compound contains 3% organic carrier; Gradient evaporation compound solvent 2%; 2% copper-specific compound additives.

[0031] The remaining raw material parameters, preparation methods, and curing processes are completely consistent with those in Example 1.

[0032] Comparative Example 1 Comparative example of copper powder without double core-shell coating This comparative example uses ordinary uncoated spherical high-purity copper powder to replace the double-layer core-shell structure anti-oxidation copper powder in Example 1. The remaining component ratios, raw material parameters, preparation methods, and curing processes are completely consistent with those in Example 1.

[0033] Comparative Example 2 Single solvent system comparative example This comparative example uses terpineol as a solvent instead of the gradient evaporation compound solvent in Example 1. The remaining component ratios, raw material parameters, preparation methods, and curing processes are completely consistent with those in Example 1.

[0034] Comparative Example 3 Comparative ratio of commercially available ordinary pure copper conductive paste This comparative example uses a commercially available ordinary pure copper conductive paste produced by a small or medium-sized domestic manufacturer as a performance control.

[0035] Performance testing The samples from Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests. The test standards were in accordance with the national standard GB / T17473-2025 "Test Methods for Noble Metal Pastes for Microelectronics Technology". The test results are shown in Table 1 below:

[0036] The test results clearly show that the conductive pastes prepared in Examples 1-3 of this invention far surpass the ordinary copper paste products in terms of core properties such as conductivity, aging resistance, storage stability, printability, and adhesion. They fully meet the mainstream commercial level in the industry and do not require nitrogen protection curing, making them directly compatible with existing silver paste production lines. This perfectly achieves the core inventive purpose of this invention.

[0037] The above description is merely a preferred embodiment of the present invention. However, the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention should be covered within the scope of protection of the present invention.

Claims

1. A highly stable double-layer core-shell coated pure copper-for-silver conductive paste, characterized in that, Based on a 100% mass fraction, it includes the following components: Double-layer core-shell structure antioxidant copper powder 82%-90%; Bismuth-boron-zinc based lead-free low-melting-point glass powder, 3%-6%; Modified epoxy resin is compounded with 3%-7% organic carrier; Gradient evaporation compound solvent 2%-5%; Copper-specific compound additives: 0.5%-2%.

2. The high-stability double-layer core-shell coated pure copper-for-silver conductive paste according to claim 1, characterized in that, The dual-core-shell structured antioxidant copper powder uses micron-sized spherical high-purity copper powder as its core, with an inner layer of 20-50 nm thick nano-silver passivation layer and an outer layer of 100-200 nm thick silane coupling agent and epoxy resin composite organic coating layer. The purity of the dual-core-shell structured antioxidant copper powder is ≥99.9%, particle size D50 = 1.5-2.5 μm, sphericity ≥90%, and tap density ≥4.5 g / cm³. 3 Silver content ≤1%.

3. The high-stability double-layer core-shell coated pure copper-silver substitute conductive paste according to claim 1, characterized in that, The bismuth-boron-zinc-based lead-free low-melting-point glass powder has a softening point of 420-480℃, a particle size D50 of 0.8-1.2μm, and is lead-free and cadmium-free.

4. The high-stability double-layer core-shell coated pure copper-for-silver conductive paste according to claim 1, characterized in that, The modified epoxy resin compound with an organic carrier, by mass fraction of 100%, includes: 55%-65% bisphenol A type epoxy resin E-20, 15%-25% linear phenolic epoxy resin, and 10%-20% carboxyl-terminated butadiene-acrylonitrile rubber modified epoxy resin.

5. The high-stability double-layer core-shell coated pure copper-for-silver conductive paste according to claim 1, characterized in that, The gradient volatile compound solvent, by mass fraction of 100%, includes: 55%-65% diethylene glycol butyl ether acetate, 25%-35% terpineol, and 5%-15% dodecyl alcohol ester.

6. The high-stability double-layer core-shell coated pure copper-silver substitute conductive paste according to claim 1, characterized in that, The copper-specific compound additives, by mass fraction of 100%, include: 20%-30% dispersant, 15%-25% thixotropic agent, 10%-20% liquid phase antioxidant, 15%-25% adhesion promoter, 10%-15% defoamer, and 5%-10% leveling agent.

7. The high-stability double-layer core-shell coated pure copper-silver substitute conductive paste according to claim 6, characterized in that, The dispersant is BYK-111, the thixotropic agent is hydrophobic fumed silica R972, the liquid-phase antioxidant is a benzotriazole derivative, the adhesion promoter is silane coupling agent KH-560, the defoamer is BYK-066N, and the leveling agent is BYK-333.

8. The high-stability double-layer core-shell coated pure copper-silver substitute conductive paste according to claim 1, characterized in that, Based on a 100% mass fraction, it includes the following components: Double-layer core-shell structure anti-oxidation copper powder 86%; 4% bismuth-boron-zinc lead-free low-melting-point glass powder; The modified epoxy resin compound contains 5% organic carrier; Gradient evaporation compound solvent 3.5%; Copper-specific compound additives 1.5%.

9. The high-stability double-layer core-shell coated pure copper-silver substitute conductive paste according to claim 8, characterized in that, The copper-specific compound additive, by mass fraction of 100%, comprises: BYK-111 dispersant 26.7%, hydrophobic fumed silica R972 20%, benzotriazole derivative 13.3%, silane coupling agent KH-560 20%, BYK-066N defoamer 13.3%, and BYK-333 leveling agent 6.7%.

10. The method for preparing the high-stability double-layer core-shell coated pure copper-for-silver conductive paste according to any one of claims 1-9, characterized in that, Includes the following steps: Step S1 Dry mixing preparation: Weigh out the double-layer core-shell structure antioxidant copper powder and bismuth boron zinc-based lead-free low melting point glass powder according to the ratio, place them in a three-dimensional mixer, mix at 30 rpm for 10-20 minutes to obtain a uniformly mixed inorganic powder mixture. Step S2 Wet Pre-dispersion: Weigh the modified epoxy resin compound, organic carrier, gradient volatile compound solvent, and copper-specific compound additive according to the formula, and mix them evenly to obtain an organic phase mixture; add the inorganic powder mixture obtained in step S1 to the organic phase mixture, place it in a high-speed disperser, and disperse it at 1200-1800 rpm for 25-35 minutes to completely wet the powder and obtain a pre-dispersion slurry; Step S3 Grinding and Refining: The pre-dispersed slurry obtained in step S2 is fed into a three-roll mill and circulated for grinding 3-5 times. The roller gap is gradually reduced from 40-60μm to 8-12μm, and the final slurry fineness is controlled to be ≤10μm to obtain the ground slurry. Step S4 Vacuum degassing: Place the ground slurry obtained in step S3 into a vacuum degassing machine and degas for 8-15 minutes at a vacuum degree of -0.08~-0.1MPa and a speed of 20-40rpm to eliminate air bubbles inside the slurry, thus obtaining the finished pure copper silver substitute conductive slurry.

Citation Information

Cited By

  • High-performance tin-copper composite conductive paste and preparation method thereof

    CN122117521A