Thickening agent for oil field fracturing fluid, preparation method of thickening agent and fracturing fluid

By preparing a thickener containing quaternary ammonium salt cations and sulfonate anions, the problem of unstable performance of fracturing fluid thickeners at high temperatures was solved, and a fracturing fluid with high temperature, salt and shear resistance was achieved, which improved the sand carrying capacity and thickening effect and reduced damage to the reservoir.

CN121852035APending Publication Date: 2026-04-14DONGYING BAO ZE ENERGY TECH CO LTD

Patent Information

Application Number
CN202610330258.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-18
Publication Date
2026-04-14

AI Technical Summary

Technical Problem

Existing fracturing fluid thickeners have problems with residue and residual adhesive, which leads to severe damage to the proppant zone and affects permeability. In addition, traditional synthetic polymers are unstable at high temperatures and cannot meet the needs of high-temperature wells. Powdered polymers have a slow dissolution rate, which affects their performance.

Method used

A thickener with a quaternary ammonium salt cationic structure and sulfonate anion was prepared by combining polymer, synergist, salt-resistant component, structure regulator, suspending agent and emulsifier. The molecular entanglement is achieved through the mutual attraction of anions and cations, which improves the sand carrying capacity. N-vinylpyrrolidone is added to increase the temperature resistance and rigid groups to improve the shear resistance.

Benefits of technology

It achieves temperature, salt, and shear resistance of fracturing fluid, improves sand carrying capacity, reduces damage to reservoir, enhances thickening performance, and has drag reduction, sand carrying, fracture creation, and drainage assistance functions, making it suitable for high-temperature wells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121852035A_ABST
    Figure CN121852035A_ABST
Patent Text Reader

Abstract

The invention provides a thickening agent for an oil field fracturing fluid, a preparation method of the thickening agent and the fracturing fluid, and belongs to the technical field of fracturing fluids. Comprising a polymer, a synergist, a salt-resistant component, a structure regulator, a suspending agent and an emulsifier. The polymer prepared by the invention contains abundant anions and cations, including quaternary ammonium salt cation structures, sulfonate anions and the like, and molecular winding can be realized through mutual attraction of the anions and cations, so that the elasticity modulus is increased, the sand-carrying performance is improved, and the sand-carrying and thickening performance of the thickening agent is improved; the fracturing fluid has good temperature resistance, salt resistance, shearing resistance, water solubility and thickening property, integrates the functions of drag reduction, sand carrying, fracture forming, swelling prevention, discharge aiding, low damage and the like, and has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fracturing fluid technology, specifically to a thickener for oilfield fracturing fluid, its preparation method, and the fracturing fluid itself. Background Technology

[0002] With the gradual depletion of global oil reserves and the increasing difficulty of oil reservoir extraction, fracturing has become an increasingly important oil production enhancement technology. The purpose of fracturing is to maximize reservoir conductivity to increase oil and gas production. The fracturing fluid used must possess characteristics such as high viscosity, high shear resistance, excellent proppant carrying capacity, and environmental friendliness with no residue after disintegration. Thickeners, as the main agents in water-based fracturing fluids, are primarily used to increase the viscosity of the fracturing fluid, reduce filtrate loss, and suspend and carry proppant. During conventional fracturing operations, the fracturing fluid contains a large amount of polymers. After the fracturing fluid filtrates into the formation, polymer residues adhere to the surface of the proppant, and residual gum from the fracturing fluid also accumulates on the proppant band, damaging the proppant band and leading to poor or even ineffective fracturing results.

[0003] Currently, the thickeners used in fracturing fluids include plant gums and their derivatives, cellulose derivatives, biopolysaccharides, and synthetic polymers. Commonly used thickeners include guar gum, hydroxypropyl guar gum, carboxymethyl guar gum, and coumarin gum. Guar gum is a plant gum, typically containing 10-25% water-insoluble matter. Incomplete breaking of the gum by the proppant-carrying fluid leads to the formation of large amounts of residue and residual gum. Simultaneously, fracturing fluid filtration during operations results in dense filter cakes of varying thicknesses. These residues and residual gums trapped in the pores of the proppant particles, as well as the filter cake on the support wall, severely affect the cleanliness of the prop zone and fracture surface, reducing the permeability of the prop zone. Furthermore, the proppant-carrying fluid filtrate also contaminates the reservoir fluid and rock pore media, reducing reservoir matrix permeability and impacting fracturing efficiency. Fracturing fluid containing 0.45% guar gum can cause over 45% damage to the prop zone. Moreover, due to the current severe situation of soaring guar gum prices and tight supply both domestically and internationally, synthetic polymer thickeners are becoming increasingly important for increasing fracturing production.

[0004] Early synthetic polymers, such as polyacrylamide and methylene polyacrylamide, had weaknesses in oilfield development, including sensitivity to salt, poor shear stability, and poor temperature stability. Therefore, these polymers were not widely used. In recent years, oligomeric fracturing fluids have emerged, overcoming the shortcomings of conventional polymers. However, oligomers cannot withstand ultra-high temperatures, making them unsuitable for wells exceeding 150°C. Furthermore, traditional synthetic polymer fracturing fluid thickeners are primarily in solid powder form. Powdered polymers dissolve slowly when preparing solutions, even fast-dissolving products require a certain time to dissolve. This increases workload, inconvenience, and cost when preparing base fluids, and can also cause shear degradation, affecting product performance. Additionally, crosslinking agents are needed during fracturing to carry sand, but the crosslinking effect is unstable and difficult to control, leading to a low sand ratio and insufficient sand carrying capacity, resulting in unsatisfactory or even worse production increases. Meanwhile, powdered polymers, due to their inherent limitations such as slow solubility and crosslinking requirements, cannot adequately meet the integrated operation requirements of low-concentration drag reduction and high-concentration sand carrying. Furthermore, conventional emulsion-type fracturing fluid thickeners, such as polyacrylamide emulsions, are typically used to formulate low-concentration slickwater solutions, resulting in low sand ratios and small sand content, and the stringent crosslinking conditions make it difficult to formulate sand-carrying fluids.

[0005] Chinese patent CN102838978A discloses a method for preparing a self-generating foam composite oil displacement agent in wells. The main components include urea, ammonium nitrate, sodium azide, acetylsalicylic acid, and sodium nitrite. Sodium azide is highly toxic and explosive, while acetylsalicylic acid is deliquescent and ineffective. Chinese patents CN103265938A, CN102627960A, CN104790933A, and CN102086388A all provide a self-generating thermally heated foam fracturing fluid. The thickener used is conventional guar gum, which has a high residue content, severely damaging the conductivity of the fractures. Furthermore, all these systems utilize the reaction of sodium nitrite and ammonium chloride under acidic conditions to release large amounts of gas, without providing a reasonable method for controlling and constructing the system. Chinese patent CN105238382A discloses a clean self-heating pressurized fracturing fluid system and its preparation method. It uses hydrophobic polyacrylamide as a thickener and zirconium salt compound as a crosslinking agent, which significantly reduces the residue content. However, the system's temperature resistance can only reach 100℃, and its heating effect is poor, resulting in low fracturing fluid foam quality. Summary of the Invention

[0006] The purpose of this invention is to provide a thickener for oilfield fracturing fluid, its preparation method, and the resulting fracturing fluid. The polymer contains abundant anions and cations, including quaternary ammonium salt cationic structures and sulfonate anions. Through the mutual attraction of anions and cations, molecular entanglement is achieved, thereby increasing the elastic modulus, improving the sand-carrying capacity, and enhancing the sand-carrying and thickening performance of the thickener. It has good temperature resistance, salt resistance, shear resistance, water solubility, and thickening properties. The resulting fracturing fluid integrates functions such as drag reduction, sand carrying, fracture creation, anti-swelling, drainage assistance, and low damage, and has broad application prospects.

[0007] The technical solution of this invention is implemented as follows: This invention provides a thickener for oilfield fracturing fluid, comprising a polymer, a synergist, a salt-resistant component, a structure modifier, a suspending agent, and an emulsifier; The polymer has the structure shown in Formula I: Formula I; Wherein, a:b:c:d=15-20:25-50:10-20:12-15, and R=C12-18 alkyl chain.

[0008] As a further improvement of the present invention, the mass ratio of the polymer, synergist, salt-resistant component, structure modifier, suspending agent, and emulsifier is 52-65:3-5:1-2:5-7:3-5:1-3; the synergist is selected from at least one of sodium p-aminobenzenesulfonate, fluorinated surfactants, cationic surfactants, and nonionic surfactants; the salt-resistant component is 2-acrylamido-2-methylpropanesulfonic acid or N-benzyl-N-acryloylamino-alkyl sulfonate; the structure modifier is ethylene glycol methyl ether or ethylene glycol butyl ether; the suspending agent is selected from at least one of fumed silica, organobentonite, and montmorillonite; and the emulsifier is a Span series and / or a Tween series emulsifier.

[0009] As a further improvement of the present invention, the polymer is composed of dimer monomers, acrylamide, N -Vinylpyrrolidone and 2-acrylamido-2-methylpropanesulfonic acid were prepared in a mass ratio of 288-452:17-36:11-23:27-35, and the structural formula of the dimer monomer is shown in Formula II: Formula II; Wherein, R is an alkyl chain of C12-18.

[0010] As a further improvement of the present invention, the method for preparing the dimer monomer is as follows: S1. Acrylamide and p-aminobenzyl chloride were reacted under alkaline conditions to prepare intermediate 1, with the following structure: ; S2. Intermediate 2 was prepared by reacting intermediate 1 with sodium 3-chloro-2-hydroxypropanesulfonate, with the following structure: ; S3. Intermediate 2 and 1,2-dibromoethane were reacted under alkaline conditions to prepare intermediate 3, with the following structure: ; S4. Intermediate 3 was reacted with propane sulfonyl lactone to obtain intermediate 4, with the following structure: ; S5. React intermediate 4 and haloalkane under alkaline conditions to obtain the product.

[0011] As a further improvement of the present invention, in step S1, the molar ratio of acrylamide to p-aminobenzyl chloride is 1.2-1.5:1, the base is selected from at least one of triethylamine, diethylamine, ethylenediamine, NaOH, and KOH, the reaction temperature is 50-60℃, and the time is 2-4h; in step S2, the molar ratio of intermediate 1 to sodium 3-chloro-2-hydroxypropanesulfonate is 1.2-1.5:1, and a base is added, the base being NaOH or KOH, the reaction temperature is 65-75℃, and the time is 5-7h; in step S3, the molar ratio of intermediate 2 to 1,2-dibromoethane is 2.1-2.2:1, the base is selected from at least one of triethylamine, diethylamine, ethylenediamine, NaOH, and KOH, the reaction temperature is 80-90℃, and the time is 1-3h.

[0012] As a further improvement of the present invention, in step S4, the molar ratio of intermediate 3 to propane sulcolone is 1:3.9-4, the reaction temperature is 50-60℃, and the time is 25-32h; in step S5, the molar ratio of intermediate 4 to haloalkane is 1:4-4.2, the base is selected from at least one of triethylamine, diethylamine, ethylenediamine, NaOH, and KOH, the reaction temperature is 75-85℃, and the time is 2-4h, and the haloalkane is selected from at least one of 1-chlorododecane, 1-chlorotetradecane, 1-chlorohexadecane, 1-chlorooctadecane, 1-bromododecane, 1-bromotetradecane, 1-bromohexadecane, and 1-bromooctadecane.

[0013] As a further improvement of the present invention, the preparation method of the polymer is as follows: a dimer monomer, acrylamide, ... N Vinylpyrrolidone and 2-acrylamido-2-methylpropanesulfonic acid are dissolved in water, and NaOH is added to adjust the solution to neutral to prepare an aqueous solution with a total monomer concentration of 35-37 wt%. Then, under inert gas protection, chain transfer agent, cosolvent, initiator and water are added to make the total monomer concentration 25-30 wt%. The reaction is heated and stirred, cooled to room temperature, purified, cut, dried and pulverized to obtain the polymer.

[0014] As a further improvement of the present invention, the initiator is selected from at least one of sodium persulfate, potassium persulfate, and ammonium persulfate, and the amount added is 1-2 wt% of the total mass of the system; the co-solvent is acetamide, and the amount added is 1.5-2 wt%; the chain transfer agent is polyethylene glycol dimethacrylate, and the amount added is 0.5-1 wt%; the temperature of the heating and stirring reaction is 55-65°C, and the time is 3-5 h.

[0015] The present invention further protects the preparation of the above-mentioned thickener for oilfield fracturing fluid, comprising the following steps: stirring and mixing polymer, emulsifier, and suspending agent, adding synergist, salt-resistant component and structure modifier, dispersing and mixing evenly to obtain thickener for oilfield fracturing fluid.

[0016] This invention further protects an oilfield fracturing fluid, which is prepared from the following raw materials in the following mass percentages: 0.4-1.5% of the above-mentioned oilfield fracturing fluid thickener, 0.1-0.5% of clay stabilizer SRCS-1, 0.1-0.5% of drainage aid SRCU-1, and the balance being water.

[0017] The present invention has the following beneficial effects: The present invention prepares a dimer monomer, which introduces long-chain hydrophobic chains to increase the side chains and temperature resistance of the polymer. The presence of hydrophobic groups will produce hydrophobic association. As the temperature increases, the hydration film of the hydrophobic groups becomes thinner, the hydrophobic chains become more exposed, the association is enhanced, and the polymer exhibits better temperature and shear resistance. At the same time, the presence of rigid benzene ring structures improves the shear resistance and thermal stability of the polymer. The abundant quaternary ammonium salt structures can neutralize the negative charge on the surface of sand particles, adsorb sand particles, and improve sand carrying capacity. The quaternary ammonium salt groups can also effectively shield the influence of salt ions and improve salt resistance. Meanwhile, the nitrogen-containing structure can promote the formation of intramolecular and intermolecular hydrogen bonds, improve temperature resistance, and the abundant sulfonate groups have the ability to resist external cation attack, effectively enhancing the mechanical properties and salt resistance of the polymer chain segments.

[0018] Introduction N Vinylpyrrolidone (NVP) increases the temperature and shear resistance of thickeners. The five-membered ring structure increases the rigidity of the molecular chain and has low degrees of freedom of movement, making the molecular chain more extended. The five-membered ring structure has greater steric hindrance, making the molecular chain less prone to curling and shrinking, thus improving the shear resistance of the polymer.

[0019] The polymer obtained by this invention contains abundant anions and cations, including quaternary ammonium salt cationic structures and sulfonate anions. Through the mutual attraction of anions and cations, molecular entanglement can be achieved, thereby increasing the elastic modulus, improving the sand-carrying capacity, and enhancing the sand-carrying and thickening performance of the thickener. It has good temperature resistance, salt resistance, shear resistance, water solubility, and thickening properties. The fracturing fluid obtained integrates functions such as drag reduction, sand carrying, fracture creation, anti-swelling, drainage assistance, and low damage, and has broad application prospects. Attached Figure Description

[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 Infrared spectrum of the dimer monomer obtained in Preparation Example 1.

[0022] Figure 2 Infrared spectrum of the polymer prepared in Example 4. Detailed Implementation

[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0024] Preparation Example 1: Preparation of Dimer Monomer The method is as follows: S1. Dissolve 0.12 mol acrylamide, 0.1 mol p-aminobenzyl chloride, and 0.5 mol triethylamine in 200 mL acetonitrile, heat to 50 °C, stir for 2 h, remove solvent under reduced pressure, and separate and purify by column chromatography (ethyl acetate and petroleum ether 10:1) to obtain intermediate 1. ESI-MS calculated value: C 10 H 13 N₂O(M+H) + 177.09, Measured value: 177.1, NMR result: 1 H NMR (300MHz, CDCl3) δ8.10 (br, 1H), 6.82 (d, J =6.4Hz, 2H), 6.45 (m, 1H), 6.37 (d, J=6.4Hz, 2H), 6.13 (m, 1H), 5.72 (m, 1H), 4.22 (s, 2H), 3.85 (br, 2H).

[0025] S2. Dissolve 0.1 mol of sodium 3-chloro-2-hydroxypropanesulfonate in 150 mL of ethylene glycol by heating, add 0.12 mol of intermediate 1, heat to 65 °C, adjust the pH of the mixed solution to 8 with 40% NaOH aqueous solution, stir for 5 h, filter, wash, and dry to obtain intermediate 2; ESI-MS calculated value: C 13 H 18 N₂NaO₅S(M+H) + 337.08, measured value: 337.1, NMR result: 1 H NMR (300MHz, CDCl3) δ7.88 (br, 1H), 6.86 (d, J =6.6Hz, 2H), 6.47 (m, 1H), 6.32 (d, J=6.5Hz, 2H), 6.23 (m, 1H), 5.72 (m, 1H), 4.1 9 (s, 2H), 4.1 (br, 1H), 3.67 (m, 1H), 3.3-3.5 (m, 3H), 3.11 (m, 1H), 1.8 (br, 1H).

[0026] S3. Dissolve 0.21 mol of intermediate 2 in 200 mL of ethylene glycol monoethyl ether, add 0.5 mol of triethylamine and 0.1 mol of 1,2-dibromoethane, heat to 80 °C, stir for 1 h, remove solvent under reduced pressure, and separate and purify by column chromatography (ethyl acetate and petroleum ether 15:1) to obtain intermediate 3. ESI-MS calculated value: C 28 H 37 N4Na2O 10 S2(M+H) + 699.17, measured value: 699.2, NMR result: 1 H NMR (300MHz, CDCl3) δ7.9 (br, 2H), 6.87 (d, J =6.2Hz, 4H), 6.4-6.5 (m, 6H), 6.18 (m, 2H), 5.75 (m, 2H), 4.20 (s, 4H), 4.1 (br, 2H), 3.68 (m, 2H), 3.51 (t, 4H), 3.3-3.45 (m, 4H), 3.0-3.1 (m, 4H).

[0027] S4. Dissolve 0.1 mol of intermediate 3 and 0.39 mol of propane sulpholactone in 200 mL of acetone, heat to 50 °C, stir and react for 25 h, filter, wash the solid, and dry to obtain intermediate 4. ESI-MS calculated value: C 34 H 47 N4Na4O 16 S4(M+H) + 987.14, measured value: 987.1, NMR result: 1 H NMR (300MHz, CDCl3) δ8.05 (br, 2H), 6.89 (d, J =6.4Hz, 4H), 6.45-6.50 (m, 6H), 6.13 (m, 2H), 5.67 (m, 2H), 4.27 (s, 4H), 3.3-3.6 (m, 20H), 3.13 (m, 2H), 2.08 (m, 4H).

[0028] S5. 0.1 mol of intermediate 4, 0.4 mol of 1-chlorododecane, and 1 mol of triethylamine were added to 200 mL of N,N-dimethylformamide. The mixture was heated to 75 °C and stirred for 2 h. After filtration, washing, and drying, the product was obtained with a total yield of 72.2%. The infrared spectrum is shown below. Figure 1 As shown. Infrared spectral analysis is as follows: 3417cm -1 The peak at 2950 cm⁻¹ represents the stretching vibration peak of NH₄⁺ on quaternary ammonium salts. -1 The characteristic absorption peak of the amide group -NH is at 1705 cm⁻¹. -1 The peak at 1485 cm⁻¹ represents the stretching vibration of the amide group C=O. -1 The peak at 1150 cm⁻¹ represents the bending vibration of CH in the alkyl chain. -1 The absorption peak at 990 cm⁻¹ is the stretching vibration peak of the sulfonic acid group -SO₃. -1 The absorption peak for the =CH out-of-plane bending vibration of olefins is at 825 cm⁻¹. -1 The peak at this location is a characteristic absorption peak of the benzene ring.

[0029] Preparation Example 2: Preparation of Dimer Monomer The method is as follows: S1. Dissolve 0.15 mol acrylamide, 0.1 mol p-aminobenzyl chloride, and 0.5 mol triethylamine in 200 mL acetonitrile, heat to 60 °C, stir for 4 h, remove solvent under reduced pressure, and separate and purify by column chromatography (ethyl acetate and petroleum ether 10:1) to obtain intermediate 1. S2. Dissolve 0.1 mol of sodium 3-chloro-2-hydroxypropanesulfonate in 150 mL of ethylene glycol by heating, add 0.15 mol of intermediate 1, heat to 75 °C, adjust the pH of the mixed solution to 8 with 40% NaOH aqueous solution, stir for 7 h, filter, wash, and dry to obtain intermediate 2; S3. Dissolve 0.22 mol of intermediate 2 in 200 mL of ethylene glycol monoethyl ether, add 0.5 mol of triethylamine and 0.1 mol of 1,2-dibromoethane, heat to 90 °C, stir for 3 h, remove solvent under reduced pressure, and purify by column chromatography (ethyl acetate and petroleum ether 15:1) to obtain intermediate 3. S4. Dissolve 0.1 mol of intermediate 3 and 0.4 mol of propane sulpholactone in 200 mL of acetone, heat to 60 °C, stir and react for 32 h, filter, wash the solid, and dry to obtain intermediate 4. S5. Add 0.1 mol of intermediate 4, 0.42 mol of 1-chlorotetradecane, and 1 mol of triethylamine to 200 mL of N,N-dimethylformamide, heat to 85 °C, stir for 4 h, filter, wash, and dry to obtain the product with a total yield of 67.8%.

[0030] Preparation Example 3: Preparation of Dimer Monomer The method is as follows: S1. Dissolve 0.135 mol acrylamide, 0.1 mol p-aminobenzyl chloride, and 0.5 mol triethylamine in 200 mL acetonitrile, heat to 55 °C, stir for 3 h, remove solvent under reduced pressure, and purify by column chromatography (ethyl acetate and petroleum ether 10:1) to obtain intermediate 1. S2. Dissolve 0.1 mol of sodium 3-chloro-2-hydroxypropanesulfonate in 150 mL of ethylene glycol by heating, add 0.135 mol of intermediate 1, heat to 70 °C, adjust the pH of the mixed solution to 8 with 40% NaOH aqueous solution, stir for 6 h, filter, wash, and dry to obtain intermediate 2. S3. Dissolve 0.215 mol of intermediate 2 in 200 mL of ethylene glycol monoethyl ether, add 0.5 mol of triethylamine and 0.1 mol of 1,2-dibromoethane, heat to 85 °C, stir for 2 h, remove solvent under reduced pressure, and purify by column chromatography (ethyl acetate and petroleum ether 15:1) to obtain intermediate 3. S4. Dissolve 0.1 mol of intermediate 3 and 0.395 mol of propane sulpholactone in 200 mL of acetone, heat to 55 °C, stir and react for 28 h, filter, wash the solid, and dry to obtain intermediate 4. S5. Add 0.1 mol of intermediate 4, 0.41 mol of 1-chlorooctadecane, and 1 mol of triethylamine to 200 mL of N,N-dimethylformamide, heat to 80 °C, stir for 3 h, filter, wash, and dry to obtain the product with a total yield of 70.5%.

[0031] Preparation Example 4: Preparation of Polymers The method is as follows: 335 parts by weight of dimer monomer, 27 parts by weight of acrylamide, and 18 parts by weight of... N Vinylpyrrolidone and 30 parts by weight of 2-acrylamido-2-methylpropanesulfonic acid were dissolved in water, and NaOH was added to adjust the solution to neutral to prepare an aqueous solution with a total monomer concentration of 36 wt%. Then, under nitrogen protection, polyethylene glycol dimethacrylate, acetamide, potassium persulfate and water were added to make the total monomer concentration 27 wt%. The mixture was heated to 60°C, stirred for 4 hours, cooled to room temperature, purified, shredded, dried and pulverized to obtain the polymer. The amount of polyethylene glycol dimethacrylate added was 0.7 wt%; the amount of acetamide added was 1.7 wt%; and the amount of potassium persulfate added was 1.5 wt% of the total mass of the system.

[0032] Infrared spectrum as follows Figure 2 As shown. Infrared spectral analysis is as follows: at 3423 cm⁻¹ -1 The peak at 3179 cm⁻¹ represents the stretching vibration of NH₄⁺ on quaternary ammonium salts. -1 The characteristic absorption peak of the amide group -NH is at 1579 cm⁻¹. -1 The peak at 1477 cm⁻¹ represents the stretching vibration of the amide group C=O. -1 The peak at 1122 cm⁻¹ represents the bending vibration of CH in the alkyl chain. -1 The absorption peak at 807 cm⁻¹ is the stretching vibration of the sulfonic acid group -SO₃. -1 The characteristic absorption peak of the benzene ring is at 725 cm⁻¹. -1 The peak at 669 cm⁻¹ is an in-plane rocking peak for alkane (CH₂)ₙ (n≥4). -1 The absorption peak for CS is located at 995-985 cm⁻¹. Additionally, there is an absorption peak in the range of 995-985 cm⁻¹. -1 With 915-905cm -1 The absence of an out-of-plane bending vibration absorption peak for the =CH group of the alkene indicates that the double bond in the C=C group has already undergone a reaction.

[0033] Preparation Example 5: Preparation of Polymers The method is as follows: 288 parts by weight of the dimer monomer prepared in Example 2, 17 parts by weight of acrylamide, and 11 parts by weight of... NVinylpyrrolidone and 27 parts by weight of 2-acrylamido-2-methylpropanesulfonic acid were dissolved in water, and NaOH was added to adjust the solution to neutral to prepare an aqueous solution with a total monomer concentration of 35 wt%. Then, under nitrogen protection, polyethylene glycol dimethacrylate, acetamide, ammonium persulfate and water were added to make the total monomer concentration 25 wt%. The mixture was heated to 55°C, stirred and reacted for 3 hours, cooled to room temperature, purified, shredded, dried and pulverized to obtain the polymer. The amount of polyethylene glycol dimethacrylate added is 0.5 wt%; the amount of acetamide added is 1.5 wt%; and the amount of ammonium persulfate added is 1 wt% of the total mass of the system.

[0034] Preparation Example 6: Preparation of Polymers The method is as follows: 452 parts by weight of the dimer monomer prepared in Preparation Example 3, 36 parts by weight of acrylamide, and 23 parts by weight of... N Vinylpyrrolidone and 35 parts by weight of 2-acrylamido-2-methylpropanesulfonic acid were dissolved in water, and NaOH was added to adjust the solution to neutral to prepare an aqueous solution with a total monomer concentration of 37 wt%. Then, under nitrogen protection, polyethylene glycol dimethacrylate, acetamide, sodium persulfate and water were added to make the total monomer concentration 30 wt%. The mixture was heated to 65°C, stirred and reacted for 5 hours, cooled to room temperature, purified, shredded, dried and pulverized to obtain the polymer. The amount of polyethylene glycol dimethacrylate added is 1 wt%; the amount of acetamide added is 2 wt%; and the amount of sodium persulfate added is 2 wt% of the total mass of the system.

[0035] Comparative Preparation Example 1 The difference from Preparation Example 4 is that no dimer monomer was added.

[0036] Comparative Preparation Example 2 The difference compared to Preparation Example 4 is that no additives were added. N -Vinylpyrrolidone.

[0037] Comparative preparation example 3 The difference from Preparation Example 4 is that 2-acrylamido-2-methylpropanesulfonic acid was not added. Example 1

[0038] This embodiment provides a method for preparing a thickener for oilfield fracturing fluid, comprising the following steps: mixing 60 parts by weight of the polymer obtained in Preparation Example 4, 1 part by weight of Tween-80, 1 part by weight of Span-80, and 4 parts by weight of fumed silica for 10 min; adding 4 parts by weight of sodium p-aminobenzenesulfonate, 1.5 parts by weight of 2-acrylamide-2-methylpropanesulfonic acid, and 6 parts by weight of ethylene glycol methyl ether; and dispersing and mixing at 1000 r / min for 20 min to obtain the thickener for oilfield fracturing fluid. Example 2

[0039] This embodiment provides a method for preparing a thickener for oilfield fracturing fluid, comprising the following steps: mixing 52 parts by weight of the polymer obtained in Preparation Example 5, 1 part by weight of Span-80, and 3 parts by weight of organic bentonite for 10 min; adding 3 parts by weight of fluorocarbon surfactant FC-1, 1 part by weight of N-benzyl-N-acryloylamino-alkyl sulfonate, and 5 parts by weight of ethylene glycol butyl ether; and dispersing and mixing at 1000 r / min for 20 min to obtain a thickener for oilfield fracturing fluid. Example 3

[0040] This embodiment provides a method for preparing a thickener for oilfield fracturing fluid, comprising the following steps: mixing 65 parts by weight of the polymer obtained in Preparation Example 6, 3 parts by weight of Tween-80, and 5 parts by weight of montmorillonite for 10 min, adding 5 parts by weight of sodium p-aminobenzenesulfonate, 2 parts by weight of 2-acrylamide-2-methylpropanesulfonic acid, and 7 parts by weight of ethylene glycol butyl ether, and dispersing and mixing at 1000 r / min for 20 min to obtain the thickener for oilfield fracturing fluid.

[0041] Comparative Examples 1-3 The difference from Example 1 is that the polymer was prepared from Comparative Preparation Examples 1-3.

[0042] Comparative Example 4 The difference compared to Example 1 is that no fumed silica was added.

[0043] Comparative Example 5 The difference from Example 1 is that Tween-80 and Span-80 were not added.

[0044] Test Example 1 The performance of the thickeners for oilfield fracturing fluids prepared in Examples 1-3 and Comparative Examples 1-5, as well as commercially available similar products, was tested.

[0045] Thickening performance test The samples were prepared into 0.1 wt% aqueous solutions, and their apparent viscosities were measured using a six-speed rotational viscometer at room temperature (25°C) and 170 s⁻¹. -1 Measurement at shear rate.

[0046] Salt resistance test A 0.1 wt% aqueous solution was prepared, with the mass fraction controlled at 0.5%. NaCl and CaCl2 were added in a molar ratio of 1:1, with the NaCl concentration being 1 wt%. The apparent viscosity of the solution was measured using a six-speed rotational viscometer, with the conditions controlled at room temperature (25℃) and 170 s. -1 The shear rate.

[0047] Temperature resistance test Each solution was prepared into a 0.1 wt% aqueous solution. The apparent viscosity of the solution at 170°C was measured using a six-speed rotational viscometer, with the shear rate controlled at 170 s⁻¹. -1 .

[0048] Shear resistance test Each was prepared into a 0.1 wt% aqueous solution and subjected to continuous shearing using a six-speed rotational viscometer for 1 hour, with the conditions controlled at room temperature (25°C) and 1024 s. -1 The shear rate.

[0049] The results are shown in Table 1.

[0050] Table 1 ; As can be seen from the table above, the thickeners for oilfield fracturing fluids prepared in Examples 1-3 of this invention have good thickening, temperature resistance, shear resistance, and salt resistance properties.

[0051] Test Example 2 The performance of the thickeners for oilfield fracturing fluids prepared in Examples 1-3 and Comparative Examples 1-5, as well as commercially available similar products, was tested. 600 kg / m³ of thickener was added to each. 3 The sand-carrying capacity of fracturing fluid was tested using 20 / 40 ceramsite with a sand concentration at room temperature and 90°C.

[0052] The results are shown in Table 2.

[0053] Table 2 ; As can be seen from the table above, the thickeners for oilfield fracturing fluids prepared in Examples 1-3 of this invention have good sand-carrying performance. Example 4

[0054] This embodiment provides an oilfield fracturing fluid, which is prepared by mixing the following raw materials in the following mass percentages: the oilfield fracturing fluid prepared in Example 1 contains 1% thickener, 0.1% clay stabilizer SRCS-1, 0.1% drainage aid SRCU-1, and the balance is water. Example 5

[0055] This embodiment provides an oilfield fracturing fluid, which is prepared by mixing the following raw materials in the following mass percentages: the oilfield fracturing fluid prepared in Example 2 contains 1.5% thickener, 0.5% clay stabilizer SRCS-1, 0.5% drainage aid SRCU-1, and the remainder is water. Example 6

[0056] This embodiment provides an oilfield fracturing fluid, which is prepared by mixing the following raw materials in the following mass percentages: the oilfield fracturing fluid prepared in Example 3 contains 1.2% thickener, 0.3% clay stabilizer SRCS-1, 0.3% drainage aid SRCU-1, and the remainder is water.

[0057] Comparative Examples 6-10 Compared with Example 4, the thickener for oilfield fracturing fluid was prepared from Comparative Examples 1-5.

[0058] Test Example 3 The performance of the oilfield fracturing fluids prepared in Examples 4-6 and Comparative Examples 6-10, as well as commercially available similar products, was tested. The results are shown in Table 3.

[0059] Static suspension sand test was used to determine the settling velocity of sand particles in oilfield fracturing fluid. Oilfield fracturing fluid was poured into a 100ml graduated cylinder, and the liquid level height h was measured with a ruler. Selected quartz sand was gently placed onto the liquid surface, and a stopwatch was started to record the time t at which the first particles reached the bottom of the graduated cylinder. The sand ratio was 20%.

[0060] The calculation method for sedimentation velocity is: sedimentation velocity v = liquid level height / sedimentation time = h / t.

[0061] Table 3 ; As can be seen from the table above, the oilfield fracturing fluids prepared in Examples 4-6 of this invention have good sand-carrying capacity.

[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A thickener for oilfield fracturing fluid, characterized in that, The product comprises a polymer, a synergist, a salt-resistant component, a structure modifier, a suspending agent, and an emulsifier; the mass ratio of the polymer, synergist, salt-resistant component, structure modifier, suspending agent, and emulsifier is 52-65:3-5:1-2:5-7:3-5:1-3; the synergist is selected from at least one of sodium p-aminobenzenesulfonate, fluorinated surfactants, cationic surfactants, and nonionic surfactants; the salt-resistant component is 2-acrylamido-2-methylpropanesulfonic acid or N-benzyl-N-acryloylamino-alkyl sulfonate; the structure modifier is ethylene glycol methyl ether or ethylene glycol butyl ether; the suspending agent is selected from at least one of fumed silica, organobentonite, and montmorillonite; and the emulsifier is a Span series and / or a Tween series emulsifier. The polymer has the structure shown in Formula I: Equation I; Wherein, a:b:c:d=15-20:25-50:10-20:12-15, and R=C12-18 alkyl chain.

2. The thickener for oilfield fracturing fluid according to claim 1, characterized in that, The polymer is composed of dimer monomers, acrylamide, N -Vinylpyrrolidone and 2-acrylamido-2-methylpropanesulfonic acid were prepared in a mass ratio of 288-452:17-36:11-23:27-35, and the structural formula of the dimer monomer is shown in Formula II: Formula II; Wherein, R is an alkyl chain of C12-18.

3. The thickener for oilfield fracturing fluid according to claim 2, characterized in that, The dimer monomer is prepared as follows: S1. Acrylamide and p-aminobenzyl chloride were reacted under alkaline conditions to prepare intermediate 1, with the following structure: ; S2. Intermediate 2 was prepared by reacting intermediate 1 with sodium 3-chloro-2-hydroxypropanesulfonate, with the following structure: ; S3. Intermediate 2 and 1,2-dibromoethane were reacted under alkaline conditions to prepare intermediate 3, with the following structure: The molar ratio of intermediate 2 to 1,2-dibromoethane is 2.1-2.2:

1. S4. Intermediate 3 was reacted with propane sulfonyl lactone to obtain intermediate 4, with the following structure: ; S5. Intermediate 4 and the haloalkane are reacted under alkaline conditions to obtain the product; wherein the haloalkane is selected from at least one of 1-chlorododecane, 1-chlorotetradecane, 1-chlorohexadecane, 1-chlorooctadecane, 1-bromododecane, 1-bromotetradecane, 1-bromohexadecane, and 1-bromooctadecane.

4. The thickener for oilfield fracturing fluid according to claim 3, characterized in that, In step S1, the molar ratio of acrylamide to p-aminobenzyl chloride is 1.2-1.5:1, and the base is selected from at least one of triethylamine, diethylamine, ethylenediamine, NaOH, and KOH. The reaction temperature is 50-60℃, and the reaction time is 2-4 hours. In step S2, the molar ratio of intermediate 1 to sodium 3-chloro-2-hydroxypropanesulfonate is 1.2-1.5:1, and a base, NaOH or KOH, is added. The reaction temperature is 65-75℃, and the reaction time is 5-7 hours. In step S3, the base is selected from at least one of triethylamine, diethylamine, ethylenediamine, NaOH, and KOH. The reaction temperature is 80-90℃, and the reaction time is 1-3 hours.

5. The thickener for oilfield fracturing fluid according to claim 3, characterized in that, In step S4, the molar ratio of intermediate 3 to propane sulpholactone is 1:3.9-4, the reaction temperature is 50-60℃, and the time is 25-32h; in step S5, the molar ratio of intermediate 4 to haloalkane is 1:4-4.2, the base is selected from at least one of triethylamine, diethylamine, ethylenediamine, NaOH, and KOH, the reaction temperature is 75-85℃, and the time is 2-4h.

6. The thickener for oilfield fracturing fluid according to claim 2, characterized in that, The polymer is prepared as follows: a dimer monomer, acrylamide, ... N Vinylpyrrolidone and 2-acrylamido-2-methylpropanesulfonic acid are dissolved in water, and NaOH is added to adjust the solution to neutral to prepare an aqueous solution with a total monomer concentration of 35-37 wt%. Then, under inert gas protection, chain transfer agent, cosolvent, initiator and water are added to make the total monomer concentration 25-30 wt%. The reaction is heated and stirred, cooled to room temperature, purified, cut, dried and pulverized to obtain the polymer.

7. The thickener for oilfield fracturing fluid according to claim 6, characterized in that, The initiator is selected from at least one of sodium persulfate, potassium persulfate, and ammonium persulfate, and the amount added is 1-2 wt% of the total mass of the system; the co-solvent is acetamide, and the amount added is 1.5-2 wt%; the chain transfer agent is polyethylene glycol dimethacrylate, and the amount added is 0.5-1 wt%; the heating and stirring reaction temperature is 55-65℃, and the time is 3-5 h.

8. A method for preparing a thickener for oilfield fracturing fluid as described in any one of claims 1-7, characterized in that, The process includes the following steps: mixing polymer, emulsifier, and suspending agent, adding synergist, salt-resistant component, and structure modifier, dispersing and mixing evenly to obtain a thickener for oilfield fracturing fluid.

9. An oilfield fracturing fluid, characterized in that, It is prepared from the following raw materials in the following mass percentages: 0.4-1.5% of the thickener for oilfield fracturing fluid as described in any one of claims 1-7, 0.1-0.5% of the clay stabilizer SRCS-1, 0.1-0.5% of the drainage aid SRCU-1, and the balance being water.

Citation Information

Patent Citations

  • Gas self-generating reaction formula of gas self-generating foam system

    CN102086388A

  • Self-gas-generating foam fracturing fluid, its production method and application method

    CN102627960A

  • Preparation method and application of autogeneration gas foam composite oil-displacing agent under shaft

    CN102838978A

  • Foam-like fracturing system, preparation method and filling method thereof

    CN103265938A

  • Coal seam gas-generating fracturing fluid and construction technology thereof

    CN104790933A

Cited By

  • Thickening agent for self-crosslinking slickwater, preparation method of thickening agent and fracturing fluid

    CN122037906A