Preparation method of polypropylene adhesive for pipeline corrosion prevention

By optimizing the composition and process flow, a polypropylene adhesive was prepared, which solved the problem of insufficient bonding performance of polypropylene in the field of pipeline corrosion protection. It achieved a balance of high strength, flexibility and aging resistance, making it suitable for pipeline corrosion protection construction in powder form, and improving construction efficiency and coating quality.

CN121991605APending Publication Date: 2026-05-08WUXI TENGLONG PLASTIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511881320.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-15
Publication Date
2026-05-08

AI Technical Summary

Technical Problem

Polypropylene has poor adhesion in the field of pipeline corrosion protection. Existing modification methods are insufficient in terms of toughness, construction adaptability, or long-term aging resistance. How to effectively disperse various functional additives in high molecular weight resin systems and ensure the stability of comprehensive performance is a challenge.

Method used

A polypropylene adhesive is prepared by combining a polypropylene matrix resin, anhydride-grafted polypropylene, tackifying resin, elastomer, antioxidant, filler, plasticizer, curing agent and diluent, through low-speed mixing and melt blending in a twin-screw extruder. Combined with powdering treatment with specific particle size, the components are uniformly dispersed and have high-strength adhesion.

Benefits of technology

The prepared polypropylene adhesive exhibits excellent bonding strength, flexibility, and aging resistance, making it suitable for powder storage and application. This improves the efficiency and uniformity of pipeline anti-corrosion construction and extends the service life of the anti-corrosion coating.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of pipeline anticorrosion materials, and discloses a preparation method of a polypropylene adhesive for pipeline anticorrosion, which comprises the following steps: (a) providing polypropylene matrix resin, anhydride grafted polypropylene and the like; (b) putting the polypropylene matrix resin, the anhydride grafted polypropylene, the tackifying resin, the elastomer, the antioxidant and the plasticizer into mixing equipment, and mixing at a low speed from room temperature to 60 DEG C to obtain a premix; and (c) adding the premix, the filler, the curing agent and the diluent into a double-screw extruder together, and carrying out melt blending, extrusion, cooling and granulation to obtain the polypropylene adhesive for pipeline corrosion prevention. Compared with the prior art, the preparation method of the polypropylene adhesive for pipeline corrosion prevention, provided by the invention, has the advantages that through an optimized raw material formula and a specific process flow, the prepared adhesive has excellent bonding strength, flexibility and aging resistance, is suitable for being prepared into a powder form, and has a good application prospect. And storage, transportation and coating in the pipeline anti-corrosion construction are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of pipeline corrosion protection materials, specifically to a method for preparing a polypropylene adhesive for pipeline corrosion protection. Background Technology

[0002] Polypropylene is widely used in pipeline corrosion protection due to its excellent chemical stability, mechanical properties, and low cost. However, polypropylene itself is non-polar, has low surface energy, and high crystallinity, resulting in poor adhesion to metal pipes or other substrates, which limits its direct application in heavy-duty anti-corrosion adhesives.

[0003] To improve the adhesive properties of polypropylene, various methods are commonly employed in existing technologies, such as surface treatment and blending modification. Among these, adding polar components (such as anhydride-grafted polypropylene) through melt blending is an effective approach. However, simple polar modification often results in deficiencies in toughness, workability (such as powdering), or long-term aging resistance. For example, some technical solutions focus on improving adhesion but sacrifice material flexibility; others may introduce complex post-processing for powdering, increasing energy consumption and cost. Furthermore, effectively dispersing multiple functional additives in high molecular weight resin systems while ensuring stable overall performance of the final product remains a technical problem that needs to be solved in this field.

[0004] Therefore, developing a polypropylene adhesive preparation method with reasonable process, excellent comprehensive performance, and especially suitable for pipeline corrosion protection is of great practical significance. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to overcome the above-mentioned technical difficulties and provide a method for preparing polypropylene adhesive for pipeline anti-corrosion. Through optimized raw material formulation and specific process flow, the prepared adhesive has excellent bonding strength, flexibility and aging resistance, and is suitable for being made into powder form, which is convenient for storage, transportation and coating in pipeline anti-corrosion construction.

[0006] To solve the above-mentioned technical problems, the technical solution provided by the present invention is as follows:

[0007] A method for preparing a polypropylene adhesive for pipeline corrosion protection includes the following steps:

[0008] (a) Provide polypropylene matrix resin, anhydride-grafted polypropylene, tackifying resin, elastomer, antioxidant, filler, plasticizer, curing agent and diluent;

[0009] (b) The polypropylene matrix resin, anhydride-grafted polypropylene, tackifying resin, elastomer, antioxidant and plasticizer are placed in a mixing device and mixed at low speed at room temperature to 60°C to obtain a premix.

[0010] (c) The premix obtained in step (b) is added together with filler, curing agent and diluent into a twin-screw extruder, and after melt blending, extrusion, cooling and granulation, a polypropylene adhesive for pipeline corrosion protection is obtained.

[0011] (d) Grind and crush the granulated material to obtain polypropylene adhesive powder;

[0012] The twin-screw extruder has a processing temperature of 180℃~220℃ and a screw speed of 200~400rpm.

[0013] The plasticizer is selected from at least one of phthalates, adipates, or citrates;

[0014] The curing agent is an isocyanate compound;

[0015] The diluent is a low-viscosity solvent.

[0016] Furthermore, in step (a), each component, by weight, includes: 40-70 parts of polypropylene matrix resin, 5-15 parts of anhydride-grafted polypropylene, 5-20 parts of tackifying resin, 5-15 parts of elastomer, 0.1-2 parts of antioxidant, 10-30 parts of filler, 3-10 parts of plasticizer, 1-5 parts of curing agent, and 2-8 parts of diluent.

[0017] Furthermore, the tackifying resin is selected from at least one of petroleum resin, terpene resin, and rosin resin.

[0018] Furthermore, the elastomer is selected from at least one of styrene-butadiene-styrene block copolymers, hydrogenated styrene-butadiene-styrene block copolymers, and polyolefin elastomers.

[0019] Furthermore, the filler is an inorganic filler, selected from at least one of calcium carbonate, talc, wollastonite, and mica powder.

[0020] Furthermore, the antioxidant is a compound system of phenolic antioxidants or phosphorus antioxidants.

[0021] Furthermore, in step (b), the speed of low-speed mixing is 100-500 rpm, and the mixing time is 5-30 minutes.

[0022] Furthermore, in step (d), the particle size of the polypropylene adhesive powder obtained after grinding and pulverizing is 50-200 mesh.

[0023] Furthermore, the diluent is at least one of acetone, ethyl acetate, toluene, or xylene.

[0024] Furthermore, in the melt blending process of step (c), the length-to-diameter ratio of the twin-screw extruder is 30:1 to 48:1.

[0025] It is worth mentioning that the polypropylene adhesive prepared by this invention is packaged in high-strength polypropylene jumbo bags, each with a net weight of 800 kg. Strict waterproofing and moisture protection should be maintained during storage, and the bags should be kept away from spillage. It should be stored under dry conditions, and the shelf life is one year.

[0026] The advantages of this invention compared to the prior art are:

[0027] 1. This invention achieves a good balance between adhesive strength, flexibility and cohesive strength in the final product through the synergistic effect of multiple components such as polypropylene matrix resin, acid anhydride grafted polypropylene (to improve polarity and adhesion), elastomer (for toughening), and tackifying resin (to improve initial adhesion), making it particularly suitable for harsh environments for pipeline corrosion protection.

[0028] 2. This invention employs a two-step mixing process. First, the main polymer and some additives are pre-mixed at low speed to avoid dust dispersion and component segregation. Then, the mixture, along with shear- and temperature-sensitive components (such as curing agents and diluents), is fed into a twin-screw extruder for high-intensity melt dispersion. This process ensures the uniform dispersion of all components, especially small amounts of additives and liquid components, within the polypropylene matrix, guaranteeing product quality stability.

[0029] 3. The present invention, through the steps of granulation followed by grinding and pulverization, produces an adhesive powder with a specific particle size, which is very suitable for pipeline anti-corrosion operations using processes such as electrostatic spraying or fluidized bed dip coating, resulting in high construction efficiency and uniform coating.

[0030] 4. The formulation of this invention incorporates antioxidants and is combined with specific processing temperature control, which effectively delays the thermo-oxidative aging of materials during processing and use, and extends the service life of the anti-corrosion coating. Detailed Implementation

[0031] In the description of this invention, unless otherwise stated, "a plurality of" means two or more. Furthermore, the term "comprising" and any variations thereof are intended to cover non-exclusive inclusion.

[0032] The present invention will now be described in further detail with reference to the embodiments.

[0033] In specific implementation of the embodiments of the present invention:

[0034] Example 1

[0035] A method for preparing a polypropylene adhesive for pipeline corrosion protection:

[0036] Prepare the raw materials according to the following weight ratio: 50 parts of polypropylene matrix resin (homopolymer PP), 10 parts of acid anhydride grafted polypropylene (MAH-g-PP), 15 parts of petroleum resin (C5 petroleum resin), 8 parts of hydrogenated styrene-butadiene-phenylene copolymer (SEBS), 0.5 parts of antioxidant 1010 (phenolic) and antioxidant 168 (phosphorus) compound, 20 parts of calcium carbonate, 5 parts of dioctyl phthalate (DOP), 3 parts of 4,4'-diphenylmethane diisocyanate (MDI), and 5 parts of acetone.

[0037] Preparation steps:

[0038] Step 1: Add polypropylene matrix resin, anhydride-grafted polypropylene, petroleum resin, SEBS, antioxidant compound and DOP into a high-speed mixer and mix at 300 rpm for 15 minutes at room temperature to obtain a premix.

[0039] Step 2: Add the above premixed material, along with calcium carbonate, MDI, and acetone, into the twin-screw extruder through the feed port. The processing temperatures of the twin-screw extruder are set sequentially from the feeding section to the die head as 185℃, 195℃, 205℃, 210℃, and 205℃, with a screw speed of 300 rpm and a length-to-diameter ratio of 40:1.

[0040] Step 3: The material is melt-extruded, cooled in a water tank, and granulated by a pelletizer to obtain adhesive granules.

[0041] Step 4: Feed the adhesive particles into a grinder for crushing, and pass them through a 100-mesh sieve to obtain polypropylene adhesive powder.

[0042] Example 2

[0043] A method for preparing a polypropylene adhesive for pipeline corrosion protection:

[0044] Prepare the raw materials according to the following weight ratio: 60 parts of polypropylene matrix resin (copolymer PP), 8 parts of acid anhydride grafted polypropylene (MAH-g-PP), 12 parts of terpene resin, 10 parts of polyolefin elastomer (POE), 1 part of antioxidant 1076 (phenolic), 25 parts of talc, 4 parts of tributyl citrate, 2 parts of toluene diisocyanate (TDI), and 4 parts of ethyl acetate.

[0045] Preparation steps:

[0046] Step 1: Add polypropylene matrix resin, anhydride-grafted polypropylene, terpene resin, POE, antioxidant 1076 and tributyl citrate to a high-speed mixer and mix at 200 rpm for 20 minutes at 40°C to obtain a premix.

[0047] Step 2: Add the above premixed material, along with talc, TDI, and ethyl acetate, into the twin-screw extruder through the feed port. The processing temperatures of the twin-screw extruder are set sequentially from the feeding section to the die head as 190℃, 200℃, 215℃, 220℃, and 215℃, with a screw speed of 250 rpm and a length-to-diameter ratio of 36:1.

[0048] Step 3: The material is melt-extruded, cooled in a water tank, and granulated by a pelletizer to obtain adhesive granules.

[0049] Step 4: Feed the adhesive particles into a grinder for crushing, and pass them through a 150-mesh sieve to obtain polypropylene adhesive powder.

[0050] The present invention and its embodiments have been described above, and this description is not restrictive. If those skilled in the art are inspired by this description and design similar embodiments without departing from the spirit of the invention, such embodiments should fall within the protection scope of the present invention.

Claims

1. A method for preparing a polypropylene adhesive for pipeline corrosion protection, characterized in that, Includes the following steps: (a) Provide polypropylene matrix resin, anhydride-grafted polypropylene, tackifying resin, elastomer, antioxidant, filler, plasticizer, curing agent and diluent; (b) The polypropylene matrix resin, anhydride-grafted polypropylene, tackifying resin, elastomer, antioxidant and plasticizer are placed in a mixing device and mixed at low speed at room temperature to 60°C to obtain a premix. (c) The premix obtained in step (b) is added together with filler, curing agent and diluent into a twin-screw extruder, and after melt blending, extrusion, cooling and granulation, a polypropylene adhesive for pipeline corrosion protection is obtained. (d) Grind and crush the granulated material to obtain polypropylene adhesive powder; The twin-screw extruder has a processing temperature of 180℃~220℃ and a screw speed of 200~400rpm. The plasticizer is selected from at least one of phthalates, adipates, or citrates; The curing agent is an isocyanate compound; The diluent is a low-viscosity solvent.

2. A method for preparing a polypropylene adhesive for pipeline corrosion protection according to claim 1, characterized in that, In step (a), each component, by weight, includes: 40-70 parts of polypropylene matrix resin, 5-15 parts of anhydride-grafted polypropylene, 5-20 parts of tackifying resin, 5-15 parts of elastomer, 0.1-2 parts of antioxidant, 10-30 parts of filler, 3-10 parts of plasticizer, 1-5 parts of curing agent, and 2-8 parts of diluent.

3. A method for preparing a polypropylene adhesive for pipeline corrosion protection according to claim 2, characterized in that, The tackifying resin is selected from at least one of petroleum resin, terpene resin, and rosin resin.

4. A method for preparing a polypropylene adhesive for pipeline corrosion protection according to claim 2, characterized in that, The elastomer is selected from at least one of styrene-butadiene-styrene block copolymer, hydrogenated styrene-butadiene-styrene block copolymer, and polyolefin elastomer.

5. A method for preparing a polypropylene adhesive for pipeline corrosion protection according to claim 2, characterized in that, The filler is an inorganic filler, selected from at least one of calcium carbonate, talc, wollastonite, and mica powder.

6. A method for preparing a polypropylene adhesive for pipeline corrosion protection according to claim 2, characterized in that, The antioxidant is a compound system of phenolic antioxidants or phosphorus antioxidants.

7. A method for preparing a polypropylene adhesive for pipeline corrosion protection according to claim 1, characterized in that, In step (b), the speed of low-speed mixing is 100-500 rpm, and the mixing time is 5-30 minutes.

8. A method for preparing a polypropylene adhesive for pipeline corrosion protection according to claim 1, characterized in that, In step (d), the particle size of the polypropylene adhesive powder obtained after grinding and pulverizing is 50-200 mesh.

9. A method for preparing a polypropylene adhesive for pipeline corrosion protection according to claim 1, characterized in that, The diluent is at least one of acetone, ethyl acetate, toluene, or xylene.

10. A method for preparing a polypropylene adhesive for pipeline corrosion protection according to claim 1, characterized in that, In the melt blending process of step (c), the length-to-diameter ratio of the twin-screw extruder is 30:1 to 48:1.