Preparation method of antibacterial composite nanofiber material with cascade activity
By constructing a cascaded catalytic system of Au and Cu-TCPP on nanofiber membranes using in-situ electrospinning and solvent filtration loading techniques, the problems of low catalytic efficiency and stability of nanozymes in the microenvironment of infected wounds were solved, achieving high-efficiency antibacterial effect and tissue compatibility.
Patent Information
- Application Number
- CN202610073211.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-01-20
- Publication Date
- 2026-05-26
AI Technical Summary
Existing nanozymes have low catalytic efficiency in the microenvironment of infected wounds, and high concentrations of H2O2 may damage normal tissues. Single nanozyme systems have insufficient catalytic performance under weakly alkaline conditions, and traditional carrier materials have problems such as easy leakage and agglomeration inactivation of nanozymes.
Au composite nanofiber membranes loaded with GOx-Like active gold nanoparticles were prepared by in-situ electrospinning combined with solvent filtration loading technology, and Cu-TCPP was stably anchored on the surface to construct a cascade catalytic system. The catalytic efficiency was enhanced by NIR light.
The efficient cascade catalysis achieved in a weakly alkaline environment avoids the encapsulation of Cu-TCPP, improves the stability and catalytic efficiency of the nanozyme, provides a suitable microenvironment, and enhances the antibacterial effect.
Smart Images

Figure CN122082247A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of functional polymer materials, and in particular to a method for preparing an antibacterial composite nanofiber material with cascade activity. Background Technology
[0002] Antimicrobial resistance in infected wounds is a serious public health problem. Due to the overuse of antibiotics, many pathogens have developed resistance to traditional antibiotics, significantly increasing the difficulty of treating infected wounds. To effectively address this challenge, novel antimicrobial strategies, including nanozymes, have become a research hotspot. Peroxide-like (POD-Like) nanozymes can catalyze the generation of hydroxyl radicals (•OH) from hydrogen peroxide (H2O2) to kill bacteria without inducing bacterial resistance. Among numerous nanozyme materials, metal-organic framework (MOF)-based nanozymes have attracted considerable attention due to their porous structure and abundant active sites. These properties facilitate the adsorption of H2O2 and its catalytic conversion into hydroxyl radicals, especially two-dimensional MOF-based nanozymes, which, with their larger specific surface area and more abundant active sites, are widely used in the antimicrobial field. However, the microenvironment of bacterial infected wounds is weakly alkaline, while the optimal catalytic activity of most POD-Like nanozymes is achieved under acidic conditions, which severely limits their effectiveness in practical applications. Furthermore, the introduction of relatively high concentrations of H2O2 may damage normal tissue. Therefore, the catalytic performance of a single nanozyme is still insufficient to meet the needs of complex biomedical applications, resulting in limited therapeutic effects.
[0003] Therefore, researchers are considering designing multi-enzyme cascade catalytic systems for the treatment of bacterial infections. Effectively immobilizing different enzymes that produce cascade effects together can achieve more efficient substrate conversion and product generation, thereby improving overall therapeutic efficacy. Currently, glucose oxidase (GOx) or glucose oxidase-like enzymes (GOx-Like) are often immobilized with POD-Like nanozymes to construct cascade reactions. GOx and GOx-Like nanozymes consume glucose and oxygen to produce gluconic acid and H2O2. This process not only provides the catalytic substrate (H2O2) for POD-Like nanozymes but also creates a suitable catalytic microenvironment for POD-Like nanozyme catalysis by lowering the local pH.
[0004] Existing systems often rely on electrostatic interactions between nanozymes or inorganic porous materials as carriers for construction, but these often face problems such as nanozyme leakage, aggregation and inactivation, and potential powder toxicity. Electrospun nanofiber membranes, due to their three-dimensional interconnected porous network structure and abundant specific surface area, can serve as carriers for nanozymes. Through strategies such as blend spinning and in-situ growth, enzyme-active components can be stably loaded within the fibers, effectively loading nanozymes; simultaneously, the high mechanical flexibility of the fiber matrix ensures structural stability of the carrier in the wound environment, providing a reliable microenvironment for cascade reactions. However, in previous experiments, the applicant found that the encapsulation of nanozymes within the nanofibers led to a decrease in therapeutic efficacy. Summary of the Invention
[0005] To address the problems of existing technologies, this invention provides a method for preparing an antibacterial composite nanofiber material with cascaded activity. In this antibacterial composite nanofiber material, gold nanoparticles with GOx-Like activity are loaded inside the nanofibers, while Cu-TCPP with POD-Like activity is stably anchored on the surface of the Au composite nanofiber membrane using a special solvent filtration loading technique. This avoids the technical problem of Cu-TCPP being encapsulated inside the nanofibers, which would reduce its therapeutic effect. In a weakly alkaline environment conducive to infection, this antibacterial composite nanofiber material can utilize Au nanozymes as initial enzymes to continuously catalyze the production of gluconic acid and H2O2 from glucose, thereby activating the POD-Like activity of Cu-TCPP to catalyze the generation of hydroxyl radicals to kill bacteria. Furthermore, the introduction of NIR light can enhance the efficiency of this cascaded catalytic system, further improving the antibacterial effect.
[0006] The specific technical solution of this invention is as follows:
[0007] First, a method for preparing an antibacterial composite nanofiber material with cascade activity includes the following steps:
[0008] Step 1: Preparation of Au composite nanofiber membrane (which exhibits GOx-like activity): The gold precursor was added to a solvent and stirred to dissolve; the polymer was added, heated and stirred to dissolve, and a polymer solution was obtained; sodium borohydride solution was added dropwise under stirring to carry out the reaction; after the reaction was completed, electrospinning was performed to obtain the Au composite nanofiber membrane.
[0009] In step 1 above, this invention utilizes in-situ generation of Au nanozymes in a polymer solution followed by electrospinning to prepare a composite nanofiber membrane. This improves the dispersibility and stability of the nanozymes and enhances their catalytic activity. Specifically, this invention obtains a substrate composite membrane loaded with gold nanoparticles (Au NPs) through in-situ reduction and electrospinning. The polymer nanofiber membrane serves as a hydrophilic substrate and a carrier for the nanozymes, providing fundamental support for the subsequent construction of a cascade catalytic system. The gold nanoparticles are stably loaded within the fibers, primarily acting as the initial enzyme in the cascade system, and providing suitable catalytic conditions for the subsequent nanozyme construction through GOx-like activity.
[0010] Step 2: Preparation of Cu-TCPP (which exhibits peroxidase-like (POD-Like) activity): Meso-tetra(4-carboxyphenyl)porphyrin (TCPP) was added to a mixed solvent of N,N-dimethylformamide and ethanol and stirred to dissolve; a mixed solvent of N,N-dimethylformamide and ethanol containing Cu2O was added; polyvinylpyrrolidone (PVP) and trifluoroacetic acid (TFA) were added under stirring and ultrasonically dispersed; the resulting mixture was heated and stirred to react; after the reaction was completed, the product was cooled, washed, and dried to obtain Cu-TCPP.
[0011] In step 2 above, Cu-TCPP is prepared by a solvothermal method. Cu-TCPP serves as a subsequent enzyme in the cascade system. Through POD-Like catalysis, it generates highly oxidizing hydroxyl radicals from the substrate H2O2, causing irreversible oxidative damage to bacterial cell membranes and biomolecules such as proteins and DNA. However, it does not induce antibiotic resistance in bacteria.
[0012] Step 3: Preparation of cascaded composite nanofiber membrane: The Au composite nanofiber membrane was placed in a vacuum filtration device, and Cu-TCPP was ultrasonically dispersed in an N,N dimethylformamide / water mixed solution to obtain a Cu-TCPP dispersion. Under vacuum filtration conditions, the Cu-TCPP dispersion was gradually added to the surface of the Au composite nanofiber membrane to deposit Cu-TCPP on the surface of the Au composite nanofiber membrane. After drying, an antibacterial composite nanofiber material with cascaded activity was obtained.
[0013] In step 3 above, to avoid excessive encapsulation of Cu-TCPP within the nanofibers and thus affecting its therapeutic effect, this invention cleverly employs a solvent filtration loading method to stably attach Cu-TCPP to the surface of the nanofiber membrane rather than its interior. The technical principle of this solvent filtration loading method is as follows: DMF, a good solvent for polymers, is selected as one of the solvent components. Through filtration, an appropriate amount of DMF causes the polymer fiber matrix (e.g., PAN) to swell and slightly dissolve, thereby achieving effective adhesion and stable anchoring of Cu-TCPP without damaging the microstructure of the polymer nanofibers; thus improving the stability and mechanical properties of the composite material.
[0014] In summary, this invention first prepares a composite nanofiber membrane loaded with Au NPs using in-situ electrospinning technology, and then stably loads Cu-TCPP onto the surface of the Au composite nanofiber membrane using solvent filtration loading technology, obtaining an antibacterial composite nanofiber material with cascade activity. The Au NPs and Cu-TCPP loaded in this material achieve therapeutic effects on infected wounds through a cascade reaction constructed by their respective enzyme-like activities. Since the selected nanozymes all possess NIR light absorption characteristics, the prepared composite nanofiber dressing can significantly enhance the overall catalytic efficiency of the cascade reaction through NIR light, achieving a more efficient and controllable therapeutic effect.
[0015] The composite nanofiber material prepared in this invention can achieve cascade catalytic activity under weakly alkaline conditions, and the catalytic efficiency can be significantly enhanced by NIR irradiation. In the prior art, although cascade systems constructed from GOx or GOx-like nanozymes and MOF-based nanozymes with POD-like properties have been reported in the literature, these cascade systems are usually constructed through self-assembly and are mostly in powder form. In practical applications, they may dissociate due to changes in external conditions, affecting long-term stability and potentially causing biotoxicity.
[0016] Preferably, in step 1, the polymer is polyacrylonitrile (PAN), cellulose acetate (CA), or a mixture of both; the concentration of the polymer in the polymer solution is 8-30 wt%.
[0017] This invention uses PAN or CA as the polymer nanofiber matrix, which exhibits hydrophilic properties, facilitating the adsorption and diffusion of substrate molecules on the carrier surface, thereby enhancing catalytic activity. Moreover, the functional groups contained in both do not affect the pH of the microenvironment, thus not affecting the catalytic performance of the initial enzyme in the cascade system.
[0018] More preferably, in step 1, when the polymer is polyacrylonitrile, its concentration is 8-12 wt%; the solvent is N,N dimethylformamide; when the polymer is cellulose acetate, its concentration is 22-30 wt%, the solvent is a mixed solvent of N,N dimethylformamide and acetone, and the volume ratio of N,N dimethylformamide to acetone is 5:5-7:3.
[0019] In step 1, controlling the polymer concentration within a suitable range is beneficial to the spinning process, resulting in nanofiber membranes with good mechanical properties. On the other hand, it can effectively regulate the in-situ reduction process of NaBH4 on the gold precursor, thereby forming smaller and more uniformly distributed Au NPs.
[0020] Preferably, in step 1, the temperature at which the heating agent dissolves is 40-60°C.
[0021] Preferably, in step 1, the gold precursor is tetrachloroauric acid trihydrate (HAuCl4·3H2O); the mass of the gold precursor is 5-20 wt% of the polymer; and the mass ratio of NaBH4 to the gold precursor is 30-50:100.
[0022] In step 1, the ratio of NaBH4 to gold precursor in the polymer solution is also crucial. A suitable ratio is beneficial to the nucleation and growth balance of Au NPs, thereby obtaining nanoparticles with appropriate particle size and maximizing their catalytic performance; at the same time, it ensures that there is no excessive residue of each reactant; and it does not significantly affect the structural stability of the nanofiber membrane.
[0023] Preferably, in step 1, the electrospinning conditions are as follows: needle size 18-22 G, injection pump advance speed 0.001-0.003 mm / s, distance between needle tip and receiver 12-20 cm, spinning voltage 12-25 kV, roller speed 100-300 rpm, injection pump forward and backward movement center position 80-120 mm, swing amplitude 40-50 mm, moving speed 20-50 mm / s, spinning temperature 20-30℃, humidity 50-70%RH, and spinning time 3-6 h.
[0024] Preferably, in step 2, the molar ratio of meso-tetra(4-carboxyphenyl)porphyrin to Cu2O is 1:2-1:8; the ratio of meso-tetra(4-carboxyphenyl)porphyrin to the total amount of the mixed solvent is 0.5-1g:1000mL; the ratio of polyvinylpyrrolidone to the total amount of the mixed solvent is 1g:2000-1000mL; the volume ratio of trifluoroacetic acid to the total amount of the mixed solvent is 1-2:1000; and the volume ratio of N,N-dimethylformamide to ethanol in the mixed solvent is 1-3:1.
[0025] In step 2, the concentrations and ratios of the above components are crucial for optimizing the morphology, structure, and catalytic activity of the material. Specifically: the molar ratio of TCPP to Cu₂O directly determines the coordination saturation of the metal-organic framework; a suitable ratio helps form nanostructures with high specific surface area and abundant active sites. PVP, as a surfactant, effectively regulates the size and dispersibility of Cu-TCPP nanoparticles, preventing aggregation. The amount of TFA added needs precise control; it promotes coordination reactions and optimizes crystal nucleation and growth kinetics, directly affecting the morphology, porosity, and coordination state of copper active centers, ultimately determining its peroxidase-like activity. The ratio of N,N-dimethylformamide to ethanol in the mixed solvent regulates the polarity and diffusion rate of the reaction system, affecting the uniformity of the synthesis reaction and the quality of crystallization.
[0026] Preferably, in step 2, the conditions for ultrasonic dispersion are: ultrasonic power of 100-200 W and ultrasonic time of 10-20 min; the temperature for heating and stirring is 80-100℃ and the reaction time is 4-6 h; the washing is centrifugal washing with a rotation speed of 10000-12000 rpm and a time of 10-20 min.
[0027] In step 2, the ultrasonic treatment, reaction temperature, and time directly affect the nucleation rate and crystal growth process. Appropriate process parameters help to obtain nanomaterials with regular morphology and uniform size.
[0028] Preferably, in step 3, the volume ratio of N,N dimethylformamide to water in the mixed solution is 5-60:100.
[0029] During the filtration process, the ratio of DMF to water affects the loading effect of Cu-TCPP. If the DMF content is too low, the nanofibers cannot fully solute or undergo slight dissolution, resulting in poor adhesion and unstable particle composites. Conversely, if the DMF content is too high, the nanofiber membrane is prone to excessive swelling, affecting the fiber structure and air permeability.
[0030] Preferably, in step 3, the mass ratio of the Cu-TCPP to Au composite nanofiber membrane is 1-10:100.
[0031] In step 3, the Cu-TCPP content directly affects its loading on the nanofiber membrane surface. If the Cu-TCPP loading is too high, it can easily lead to excessive deposition, causing particle instability and affecting the air permeability of the nanofiber membrane; conversely, if the loading is too low, the expected antibacterial effect may not be achieved.
[0032] Preferably, in step 3, the concentration of Cu-TCPP in the Cu-TCPP dispersion is 0.002-0.02 mg / mL.
[0033] Preferably, in step 3, the conditions for ultrasonic dispersion are: ultrasonic power of 100-200 W and ultrasonic time of 5-20 min.
[0034] Secondly, the application of the antibacterial composite nanofiber material with cascade activity prepared by the above method in the preparation of medical wound dressings.
[0035] Compared with the prior art, the beneficial effects of the present invention are:
[0036] (1) This invention employs a composite process combining in-situ electrospinning and solvent filtration loading to successfully construct a nanofiber membrane material with cascade catalytic function. This process achieves the co-loading of Au NPs and Cu-TCPP within the nanofiber membrane, overcoming the shortcomings of traditional GOx, such as easy leakage, inactivation, and low loading capacity, thus ensuring uniform dispersion and high stability of the active components. The cascade catalytic system constructed using the enzyme-like activity of Au NPs and Cu-TCPP significantly enhances the overall catalytic efficiency of the cascade reaction under NIR light response, providing a new approach for the precise treatment of infected wounds. Furthermore, this cascade system can operate efficiently even in the weakly alkaline environment of infection. The microenvironmental regulation capability of the composite fiber membrane ensures the catalytic reaction proceeds, avoiding the problem of decreased catalytic efficiency caused by pH mismatch in single nanozymes.
[0037] (2) The solvent filtration loading technology proposed in this invention is an efficient and reliable method for composite Cu-TCPP nanoparticles with polymer nanofiber membranes. Its advantages lie in the synergistic effect of controlled swelling of the nanofiber surface by the solvent and the dynamic filtration process, achieving uniform and robust loading of Cu-TCPP nanoparticles on the fiber surface. This effectively avoids excessive encapsulation of Cu-TCPP within the nanofibers, thus preserving its therapeutic effect while maintaining the original microstructure and mechanical properties of the nanofibers. Compared with traditional impregnation and coating methods, this method demonstrates superior uniformity, structural integrity, bonding strength, and process scalability, providing a promising technical path for the efficient and stable composite of functional materials with flexible substrates.
[0038] (3) The composite nanofibers prepared in this invention possess both excellent biocompatibility and structural stability. Their cytoplasmic matrix and highly porous structure not only facilitate the absorption of wound exudate but also provide a favorable microenvironment for tissue regeneration. The cascaded composite nanofiber membrane achieves efficient catalysis and excellent antibacterial effects through cascaded catalysis and NIR light assistance, which is of great significance for solving the problem of bacterial resistance and improving the treatment effect of infected wounds. It has high application prospects in the field of biomedical dressings. Attached Figure Description
[0039] Figure 1 The image shows a transmission electron microscope (TEM) image of the Au composite nanofiber membrane prepared in Example 1. The red arrows mark Au nanozymes.
[0040] Figure 2 The image shows a scanning electron microscope (SEM) image of the antibacterial composite nanofiber membrane prepared in Example 1. The red arrows indicate Cu-TCPP.
[0041] Figure 3A comparative graph showing the relative particle stability data of different Cu-TCPP composite fiber membranes obtained by solvent filtration loading method with different amounts of DMF aqueous solution;
[0042] Figure 4 SEM images of PAN fiber membranes treated with solvent filtration of different amounts of DMF aqueous solution; the red circles mark the fiber bonding points.
[0043] Figure 5 This is a graph showing the cascade enzyme activity data of the antibacterial composite nanofiber membrane prepared in Example 1;
[0044] Figure 6 This is a comparison graph showing the enzyme activity of the antibacterial composite nanofiber membrane prepared in Example 1 under NIR light irradiation conditions.
[0045] Figure 7 This is a comparison of the enzyme activity of the antibacterial composite nanofiber membrane prepared in Example 1 and the nanofiber membranes prepared in Comparative Examples 1-3 under NIR light irradiation conditions.
[0046] Figure 8 The antibacterial composite nanofiber membrane prepared in Example 1 is compared with and without NIR light irradiation against Staphylococcus aureus. Among them, Figures a and c are the control groups (no treatment and NIR light treatment only), and Figures b and d are the experimental groups (treated with cascaded composite nanofiber membrane and treated with cascaded composite nanofiber membrane plus NIR light irradiation).
[0047] Figure 9 The figure shows the cytotoxicity test results of the antibacterial composite nanofiber membrane prepared in Example 1. Detailed Implementation
[0048] The present invention will be further described below with reference to embodiments.
[0049] Example 1
[0050] (1) Preparation of Au composite nanofiber membrane: 0.06 g tetrachloroauric acid trihydrate (HAuCl4·3H2O) was added to 4 mL of NN dimethylformamide (DMF) solvent and stirred until completely dissolved; then 0.6 g polyacrylonitrile (PAN) powder was added to the solution and heated and stirred at 60 °C until the polymer was completely dissolved; then the mixed solution was cooled and transferred to an ice-water bath, and freshly prepared sodium borohydride (NaBH4) solution (0.03 g dissolved in 2 mL DMF) was added dropwise under continuous stirring; after the addition was completed, the mixture was stirred at room temperature for a period of time, and then electrospinned. The spinning parameters were as follows: the needle specification was 22 G, the injection pump advance speed was 0.003 mm / s, the distance between the needle tip and the receiver was 15 cm, the voltage was 22 kV, the roller rotation speed was 200 rpm, the center position of the injection pump back and forth movement was 100 mm, the swing amplitude was 50 mm, and the moving speed was 30 The spinning speed was 25 mm / s, the spinning temperature was 25℃, the humidity was 60%RH, and the spinning time was 4 h. Au composite nanofiber membranes were obtained by spinning.
[0051] (2) Preparation of Cu-TCPP: 0.08 g of racemic tetra(4-carboxyphenyl)porphyrin (TCPP) was added to a mixed solvent of DMF and ethanol (C2H5OH) (v / v=3:1, 40 mL) and stirred until completely dissolved; then Cu2O (0.057 g Cu2O dispersed in a mixed solvent of DMF and C2H5OH (v / v=3:1, 40 mL)) was added while stirring continuously; 0.04 g of polyvinylpyrrolidone (PVP) and 80 μL of trifluoroacetic acid (TFA) were added and sonicated at 200 W for 10 min to make it uniformly dispersed; then the mixture was transferred to an oil bath at 80℃ and heated and stirred for 4 h to carry out the reaction; after the reaction was completed, the product was cooled to room temperature and washed by centrifugation at 10000 rpm for 10 min with ethanol and water respectively, and then freeze-dried to obtain Cu-TCPP.
[0052] (3) Preparation of cascaded composite nanofiber membrane: The Au composite nanofiber membrane obtained in step (1) was cut into a rectangular size of 4.5cm×4.5cm (mass about 30 mg) and placed on the filter head of the vacuum filtration device; 0.5 mg Cu-TCPP was dispersed in an aqueous solution of DMF (the ratio of DMF to water was 5:100, and the volume of water was 100 mL), and ultrasonicated at 200 W for 5 min to make it uniformly dispersed; then the Cu-TCPP dispersion was uniformly applied to the surface of the Au composite nanofiber membrane and vacuum filtered to make Cu-TCPP stably deposited on the surface of the Au composite nanofiber membrane; it was naturally dried to obtain an antibacterial composite nanofiber membrane with cascaded activity.
[0053] Example 2
[0054] (1) Preparation of Au composite nanofiber membrane: 0.08 g tetrachloroauric acid trihydrate (HAuCl4·3H2O) was added to a mixed solvent of DMF and ACE (v / v=5:5, 4 mL) and stirred until completely dissolved; then 1.5 g cellulose acetate (CA) powder was added to the solution and heated and stirred at 60 °C until the polymer was completely dissolved; then the mixed solution was cooled and transferred to an ice-water bath, and freshly prepared sodium borohydride (NaBH4) solution (0.04 g dissolved in 2 mL DMF) was added dropwise under continuous stirring; after the addition was completed, the mixture was stirred at room temperature for a period of time, and then electrospinned. The spinning parameters were as follows: the needle specification was 22 G, the injection pump advance speed was 0.001 mm / s, the distance between the needle tip and the receiver was 12 cm, the voltage was 25 kV, the roller rotation speed was 200 rpm, the center position of the injection pump back and forth movement was 100 mm, the swing amplitude was 50 mm, and the moving speed was 30 The spinning speed was 25 mm / s, the spinning temperature was 25℃, the humidity was 60%RH, and the spinning time was 6 h. Au composite nanofiber membranes were obtained by spinning.
[0055] (2) Preparation of Cu-TCPP: 0.08 g of racemic tetra(4-carboxyphenyl)porphyrin (TCPP) was added to a mixed solvent of DMF and ethanol (C2H5OH) (v / v=3:1, 40 mL) and stirred until completely dissolved; then Cu2O (0.057 g Cu2O dispersed in a mixed solvent of DMF and C2H5OH (v / v=3:1, 40 mL)) was added while stirring continuously; 0.04 g of polyvinylpyrrolidone (PVP) and 80 μL of trifluoroacetic acid (TFA) were added and sonicated at 200 W for 10 min to make it uniformly dispersed; then the mixture was transferred to an oil bath at 80℃ and heated and stirred for 4 h to carry out the reaction; after the reaction was completed, the product was cooled to room temperature and washed by centrifugation at 10000 rpm for 10 min with ethanol and water respectively, and then freeze-dried to obtain Cu-TCPP.
[0056] (3) Preparation of cascaded composite nanofiber membrane: The Au composite nanofiber membrane obtained in step (1) was cut into a rectangular size of 4.5cm×4.5cm (mass about 40 mg) and placed on the filter head of the vacuum filtration device; 0.5 mg Cu-TCPP was dispersed in an aqueous solution of DMF (the ratio of DMF to water was 5:100, and the volume of water was 100 mL), and ultrasonicated at 200 W for 5 min to make it uniformly dispersed; then the Cu-TCPP dispersion was uniformly applied to the surface of the Au composite nanofiber membrane and vacuum filtered to make Cu-TCPP stably deposited on the surface of the Au composite nanofiber membrane; it was air-dried naturally to obtain an antibacterial composite nanofiber membrane with cascaded activity.
[0057] Comparative Example 1 (different from Example 1 in that it does not contain Au NPs and Cu-TCPP)
[0058] Preparation of pure PAN nanofiber membrane: 0.6 g of polyacrylonitrile (PAN) powder was added to 6 mL of N,N-dimethylformamide (DMF) solvent, and heated and stirred at 60 °C until the polymer was completely dissolved. The mixture was then cooled to room temperature and stirred for a period of time before electrospinning. The spinning parameters were as follows: needle size 22 G, injection pump feed rate 0.003 mm / s, needle tip-receiver distance 15 cm, voltage 16 kV, roller rotation speed 200 rpm, injection pump back-and-forth movement center position 100 mm, swing amplitude 50 mm, moving speed 30 mm / s, spinning temperature 25 °C, humidity 60% RH, and spinning time 4 h. Pure PAN nanofiber membrane was obtained by spinning.
[0059] Comparative Example 2 (different from Example 1, but without Cu-TCPP composite)
[0060] Preparation of Au composite nanofiber membrane: 0.06 g of tetrachloroauric acid trihydrate (HAuCl4·3H2O) was added to 4 mL of N,N dimethylformamide (DMF) solvent and stirred until completely dissolved. Then, 0.6 g of polyacrylonitrile (PAN) powder was added to the solution, and the mixture was heated and stirred at 60 °C until the polymer was completely dissolved. The mixture was then cooled and transferred to an ice-water bath, and a freshly prepared sodium borohydride (NaBH4) solution (0.03 g dissolved in 2 mL DMF) was added dropwise under continuous stirring. After the addition was complete, the mixture was stirred at room temperature for a period of time before electrospinning. The spinning parameters were as follows: needle size 22 G, injection pump advance speed 0.003 mm / s, needle tip to receiver distance 15 cm, voltage 22 kV, roller rotation speed 200 rpm, injection pump back-and-forth movement center position 100 mm, swing amplitude 50 mm, and moving speed 30 rpm. The spinning speed was 25 mm / s, the spinning temperature was 25℃, the humidity was 60%RH, and the spinning time was 4 h. Au composite nanofiber membranes were obtained by spinning.
[0061] Comparative Example 3 (different from Example 1, without Au NPs)
[0062] (1) Preparation of pure PAN nanofiber membrane: 0.6 g of polyacrylonitrile (PAN) powder was added to 6 mL of N,N-dimethylformamide (DMF) solvent and heated and stirred at 60 °C until the polymer was completely dissolved. The mixture was then cooled at room temperature and stirred for a period of time before electrospinning. The spinning parameters were as follows: needle size was 22 G, injection pump speed was 0.003 mm / s, distance between needle tip and receiver was 15 cm, voltage was 16 kV, roller speed was 200 rpm, injection pump center position was 100 mm, swing amplitude was 50 mm, moving speed was 30 mm / s, spinning temperature was 25 °C, humidity was 60%RH, and spinning time was 4 h. Pure PAN nanofiber membrane was obtained by spinning.
[0063] (2) Preparation of Cu-TCPP: 0.08 g of racemic tetra(4-carboxyphenyl)porphyrin (TCPP) was added to a mixed solvent of DMF and ethanol (C2H5OH) (v / v=3:1, 40 mL) and stirred until completely dissolved; then Cu2O (0.057 g Cu2O dispersed in a mixed solvent of DMF and C2H5OH (v / v=3:1, 40 mL)) was added while stirring continuously; 0.04 g of polyvinylpyrrolidone (PVP) and 80 μL of trifluoroacetic acid (TFA) were added and sonicated at 200 W for 10 min to make it uniformly dispersed; then the mixture was transferred to an oil bath at 80℃ and heated and stirred for 4 h to carry out the reaction; after the reaction was completed, the product was cooled to room temperature and washed by centrifugation at 10000 rpm for 10 min with ethanol and water respectively, and then freeze-dried to obtain Cu-TCPP.
[0064] (3) Preparation of Cu-TCPP composite nanofiber membrane: The pure polymer nanofiber membrane obtained in step (1) was cut into a rectangular size of 4.5 cm × 4.5 cm (mass of about 30 mg) and placed on the filter head of the vacuum filtration device; 0.5 mg Cu-TCPP was dispersed in an aqueous solution of DMF (the ratio of DMF to water was 5:100, and the volume of water was 100 mL), and ultrasonicated at 200 W for 5 min to make it uniformly dispersed; then the Cu-TCPP dispersion was uniformly applied to the surface of the pure PAN nanofiber membrane and vacuum filtered to make Cu-TCPP stably deposited on the surface of the pure PAN nanofiber membrane; it was naturally dried to obtain Cu-TCPP composite nanofiber membrane.
[0065] Performance testing
[0066] (1) Morphological observation: Microstructure observation of the Au composite nanofiber membrane prepared in step (1) of Example 1: The dispersion of Au nanoparticles in the Au composite nanofiber membrane within the fibers was tested using high-power transmission electron microscopy (HRTEM). The morphology of the antibacterial composite nanofiber membrane was tested using scanning electron microscopy (SEM). Figure 1 As shown, Au NPs are spherical and relatively evenly distributed within the PAN fibers. Figure 2 As shown, Cu-TCPP nanosheets are uniformly distributed on the surface of the Au composite nanofiber membrane. These results demonstrate that the two types of particles were successfully composited onto the same fiber membrane.
[0067] (2) Cascade enzyme activity assay: The TMB colorimetric method was used for testing, and NIR irradiation was performed using an 808 nm laser. The composite nanofiber membrane prepared in Example 1 was cut into rectangular shapes of 1 cm × 1 cm, then immersed in 2 mL of PBS solution (pH 7.4, 2 mM) containing 25 mM glucose (Glu), and 40 μL of TMB (40 mM) solution was added directly. The membrane was incubated at 37 °C for 30 min. After incubation, the membrane was removed, and the UV absorption curve of the mixed solution was tested. The control group consisted of only Glu or the fiber membrane. At 3 W / cm² 2 The cascade enzyme activity of the composite nanofiber membrane was tested under NIR light irradiation, with different nanofiber membranes prepared in Comparative Examples 1-3 serving as controls.
[0068] like Figure 5 As shown, a UV absorption peak appeared at 652 nm, indicating that the composite nanofiber membrane prepared in Example 1 can achieve cascade enzyme activity. Figure 6 As shown, after NIR irradiation, the cascade enzyme activity of the composite nanofiber membrane prepared in Example 1 was significantly enhanced, indicating that the nanoenzyme in the composite nanofiber membrane significantly improved the overall catalytic efficiency in response to NIR light. Figure 7 As shown, compared with the composite nanofiber membranes (non-cascaded fiber membranes) prepared in Comparative Examples 1-3, the composite nanofiber membranes could not achieve cascaded enzyme activity under NIR irradiation, indicating that the simultaneous presence of the two cascaded nanoenzymes is a prerequisite for the occurrence of cascaded catalytic reactions.
[0069] (3) Antibacterial efficacy test: The antibacterial efficacy was tested using the dilution plating method. A suspension of Staphylococcus aureus (S. aureus) in the logarithmic growth phase was diluted to 10 μL with PBS solution containing 25 mM Glu (pH 7.4, 2 mM). 7 CFU / mL. This was then added to a 48-well plate (1 mL per well), and a 1 cm × 1 cm fiber membrane was placed inside. During illumination, the illumination distance was set to 5 cm, and the power was 3 W / cm². 2 The irradiation time was 30 min. After the irradiation, the cells were incubated in a shaking incubator for 1.5 h. The group without NIR irradiation was directly incubated at 37℃ for 2 h. After incubation, the bacterial suspensions of different treatments were diluted to appropriate concentration gradients using the 10-fold dilution method. 100 μL of each dilution was spread on nutrient agar plates and incubated in a constant temperature and humidity incubator at 37℃ for 24 h. Photos were taken and the antibacterial rate was calculated.
[0070] like Figure 8As shown, without NIR light irradiation, the composite nanofiber membrane prepared in Example 1 exhibited an antibacterial rate of approximately 87.4% against *S. aureus*. After NIR light irradiation, the antibacterial rate against golden yellow was increased to 99.9%. These results indicate that NIR light can improve antibacterial properties by enhancing enzyme activity.
[0071] (4) Cytotoxicity test: The CCK-8 reagent was used for determination. L929 cells were cultured in DMEM containing 10% FBS and 1% penicillin-streptomycin. When the cells reached a density of 80-90%, they were digested with trypsin to obtain a cell suspension. Subsequently, the cell suspension was diluted and 1×10⁶ cells per well were added. 4 Cells were seeded at a density of 200 μL in 96-well plates and incubated at 37°C and 5% CO2 for 24 h. Then, fibrous membranes (6 mm diameter discs) were gently transferred to the wells containing cells (five replicates per sample) and co-incubated with the cells for 24 h. After incubation, the fibrous membranes were gently removed from the wells, and 110 μL of a mixture of CCK-8 reagent and DMEM medium (v / v = 1:10) was added to each well. After co-incubation for 2 h, the OD value at 450 nm was measured using a microplate reader, and cell viability was calculated using the following formula:
[0072]
[0073] Where ODs represents the OD value of the cells treated with the sample reacting with CCK-8 solution, OD C This is the OD value of a CCK-8 solution that has not undergone any treatment or reaction with cells. B This indicates the OD value of a pure CCK-8 solution.
[0074] like Figure 9 As shown, after co-incubating the composite nanofiber membrane prepared in Example 1 with L929 fibroblasts for 24 h, the cell viability was greater than 80%, indicating that the composite nanofiber membrane has good cell compatibility.
[0075] Example 3 (Effect of DMF dosage on composite membrane particle stability in solvent filtration loading method)
[0076] The effect of DMF loading on the particle stability of composite membranes was investigated using a 0.5 mg Cu-TCPP loading. 0.5 mg Cu-TCPP (prepared as in Example 1) was dispersed in 200 mL of DMF aqueous solutions with different DMF contents (0%, 1%, 2.5%, 5%, and 10%, v / v). After sonication at 200 W for 5 min, the solutions were filtered to obtain composite membranes treated with different concentrations of DMF (other conditions were the same as in Example 1). Then, the different Cu-TCPP composite membranes (1 cm × 1 cm) obtained from different DMF treatments were placed in 2 mL of water and sonicated at 200 W for 5 min. Afterward, the membranes were gently removed, and the UV absorption curves of the treated solutions were measured using a UV spectrophotometer. Using the 0% DMF-treated composite membrane as a control, the relative stability was calculated based on the absorbance at 438 nm using the following formula:
[0077]
[0078] Among them, A C A is the absorbance of the solution after ultrasonic treatment of the control composite membrane. S It is the absorbance of the solution after ultrasonic treatment of composite membranes treated with different amounts of DMF.
[0079] like Figure 3 As shown, it can be observed that the relative stability of the particles gradually increases with the increase of DMF content, and the stability is significantly improved to over 90% when the DMF content reaches 5% or more. The photograph of the Cu-TCPP exfoliated liquid in the inset also proves this result.
[0080] Example 4 (The effect of DMF dosage on the fiber structure of composite membrane in solvent filtration loading method)
[0081] The surface microstructure of PAN nanofiber membranes treated with different amounts of DMF (0%, 1%, 2.5%, 5%, 10%, 20%, 40%, 60%, 70%, and 80%, v / v) was observed using SEM (simulated filtration treatment).
[0082] like Figure 4As shown, the original nanofiber membrane exhibits a state of random fiber stacking without any bonding points. When the PAN nanofiber membrane is treated with an aqueous solution of DMF concentration not exceeding 60%, the nanofiber structure in the membrane is well preserved, and some bonding points can be observed between the nanofibers. This indicates that under the above conditions, DMF induces micro-dissolution of PAN nanofibers, promoting the fusion and connection between fibers, forming bonding points after drying, which is beneficial to structural stability. However, when the DMF concentration increases to above 70%, the structure of the nanofiber membrane is significantly damaged, with excessive swelling of the nanofibers, affecting porosity and air permeability.
[0083] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, alterations, and equivalent transformations made to the above embodiments based on the technical essence of the present invention shall still fall within the protection scope of the present invention.
Claims
1. A method for preparing an antibacterial composite nanofiber material with cascade activity, characterized in that... Includes the following steps: Step 1: Dissolve the gold precursor in a solvent; add the polymer and dissolve it to obtain a polymer solution; add sodium borohydride solution dropwise to carry out the reaction; after the reaction is completed, electrospin to obtain an Au composite nanofiber membrane; Step 2: Dissolve meso-tetra(4-carboxyphenyl)porphyrin in a mixed solvent of N / N dimethylformamide / ethanol; add a mixed solvent of N / N dimethylformamide / ethanol containing Cu2O; add polyvinylpyrrolidone and trifluoroacetic acid, and disperse by ultrasonication; heat and stir the resulting mixture; after the reaction is complete, Cu-TCPP is obtained. Step 3: Place the Au composite nanofiber membrane in a vacuum filtration device, and ultrasonically disperse Cu-TCPP in an N / N dimethylformamide / water mixed solution with a volume ratio of 5-60:100 to obtain a Cu-TCPP dispersion. Under vacuum filtration conditions, gradually add the Cu-TCPP dispersion to the surface of the Au composite nanofiber membrane to deposit Cu-TCPP on the surface of the Au composite nanofiber membrane. Dry the membrane to obtain an antibacterial composite nanofiber material with cascade activity. The mass ratio of Cu-TCPP to Au composite nanofiber membrane is 1-10:
100.
2. The preparation method according to claim 1, characterized in that: In step 1, The polymer is polyacrylonitrile, cellulose acetate, or a mixture of both; The polymer concentration in the polymer solution is 8-30 wt%.
3. The preparation method according to claim 2, characterized in that: In step 1, The polymer is polyacrylonitrile, with a concentration of 8-12 wt%; the solvent is N,N dimethylformamide; or The polymer is cellulose acetate with a concentration of 22-30 wt%, and the solvent is a mixture of N,N dimethylformamide and acetone with a volume ratio of 5:5-7:
3.
4. The preparation method according to claim 1, characterized in that: In step 1, The gold precursor is tetrachloroauric acid trihydrate; The gold precursor comprises 5-20 wt% of the polymer. The mass ratio of NaBH4 to the gold precursor is 30-50:
100.
5. The preparation method according to claim 1, characterized in that: In step 1, the electrospinning conditions are as follows: needle size 18-22 G, injection pump advance speed 0.001-0.003 mm / s, distance between needle tip and receiver 12-20 cm, spinning voltage 12-25 kV, roller speed 100-300 rpm, injection pump forward and backward movement center position 80-120 mm, swing amplitude 40-50 mm, moving speed 20-50 mm / s, spinning temperature 20-30℃, humidity 50-70%RH, and spinning time 3-6 h.
6. The preparation method according to claim 1, characterized in that: In step 2, The molar ratio of the meso-tetra(4-carboxyphenyl)porphyrin to Cu2O is 1:2-1:8; The ratio of the meso-tetra(4-carboxyphenyl)porphyrin to the total amount of the mixed solvent is 0.5-1g:1000mL; The ratio of polyvinylpyrrolidone to the total amount of mixed solvent is 1g:2000-1000mL; The volume ratio of trifluoroacetic acid to the total volume of the mixed solvent is 1-2:1000; The volume ratio of N,N dimethylformamide to ethanol in the mixed solvent is 1-3:
1.
7. The preparation method according to claim 1 or 6, characterized in that: In step 2, The conditions for ultrasonic dispersion are: ultrasonic power of 100-200 W and ultrasonic time of 10-20 min. The heating and stirring temperature is 80-100℃, and the reaction time is 4-6 h; The washing process is centrifugal washing, with a rotation speed of 10,000-12,000 rpm and a time of 10-20 min.
8. The preparation method according to claim 1, characterized in that: In step 3, the concentration of Cu-TCPP in the Cu-TCPP dispersion is 0.002-0.02 mg / mL.
9. The preparation method according to claim 1, characterized in that: In step 3, the conditions for ultrasonic dispersion are: ultrasonic power of 100-200 W and ultrasonic time of 5-20 min.
10. The application of the antibacterial composite nanofiber material with cascade activity prepared by the preparation method according to any one of claims 1-9 in the preparation of medical wound dressings.