A hierarchically distributed porous carbon material and a preparation method and application thereof
By using temperature gradient carbonization treatment of magnesium salts and carbon source materials and acid washing and sintering processes, a layered porous carbon material was prepared, which solved the problems of environmental pollution and high cost of existing porous carbon materials, and improved the electrochemical performance of silicon-carbon composite materials and the performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202411943719.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-27
- Publication Date
- 2026-06-30
Smart Images

Figure CN122301169A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery materials technology, and in particular to a porous carbon material with a layered distribution, its preparation method, and its application. Background Technology
[0002] Existing methods for preparing porous carbon materials commonly employ either the template method or the chemical activation method. The template method primarily uses hard templates such as silica, but removing these templates requires hydrofluoric acid washing, leading to severe environmental pollution. The chemical activation method mainly uses potassium hydroxide, potassium carbonate, phosphoric acid, and zinc chloride as activators, and requires prolonged heating in high-temperature equipment. Conventional chemical activation methods not only use a large proportion of activators, causing severe pollution from washing wastewater and resulting in high costs, but also involve long heating times and high energy consumption, leading to substantial expenses.
[0003] Existing methods for preparing porous carbon materials suffer from problems such as a low proportion of mesopores, insufficient pore size and volume, and a high proportion of large mesopores. Therefore, when using existing porous carbon materials to prepare silicon-carbon composites, the silicon deposition capability is relatively poor, and the resulting silicon-carbon composites have low lithium storage capacity and electrical conductivity, which hinders the preparation of high-rate and high-stability performance. Summary of the Invention
[0004] The purpose of this invention is to address the shortcomings of existing technologies by providing a porous carbon material with a hierarchical pore structure, its preparation method, and its applications. The method involves mixing magnesium salts and carbon source materials in a specific ratio, granulating the mixture, and then performing a temperature gradient carbonization process to obtain magnesium oxide-containing carbonized particles. The magnesium oxide is then removed by acid washing, followed by washing with deionized water and / or anhydrous ethanol until the solution is neutral. After drying, a precursor is obtained, which is then sintered to obtain a porous carbon material with a hierarchically distributed pore structure. This preparation method, by controlling the ratio of magnesium salts to carbon source materials, yields porous carbon materials with specific pore sizes and volumes, resulting in porous carbon materials with high specific surface areas and excellent silicon deposition capabilities, thus meeting the needs of various specific applications.
[0005] To achieve the above objectives, in a first aspect, embodiments of the present invention provide a porous carbon material with a hierarchical distribution, wherein the pores of the porous carbon material include: a first micropore, a second micropore, a first mesopore, a second mesopore, a third mesopore, and a fourth mesopore;
[0006] The pore size of the first micropore is less than 1 nm; the number of the first micropore accounts for less than 10% of the total number of pores in the porous carbon material.
[0007] The pore size of the second micropore is greater than or equal to 1 nm and less than 2 nm; the number of the second micropore accounts for a percentage of the total number of pores in the porous carbon material that is greater than or equal to 5% and less than or equal to 15%.
[0008] The pore size of the first mesopore is greater than or equal to 2 nm and less than 4 nm; the percentage of the number of the first mesopores to the total number of pores in the porous carbon material is greater than or equal to 15% and less than or equal to 25%.
[0009] The pore size of the second mesopore is greater than or equal to 4 nm and less than 7 nm; the number of the second mesopore accounts for a percentage of the total number of pores in the porous carbon material that is greater than or equal to 50% and less than or equal to 70%.
[0010] The pore size of the third mesopore is greater than or equal to 7 nm and less than 10 nm; the number of the third mesopores accounts for a percentage of the total number of pores in the porous carbon material that is greater than or equal to 1% and less than or equal to 10%.
[0011] The pore size of the fourth mesopore is greater than or equal to 10 nm and less than or equal to 50 nm; the number of the fourth mesopore accounts for less than 1% of the total number of pores in the porous carbon material.
[0012] Preferably, the porous carbon material has a specific surface area of 800 m². 2 / g~1500m 2 / g;
[0013] The porous carbon material has a pore volume of 0.8 cm³. 3 / g~1.3cm 3 Between / g.
[0014] In a second aspect, embodiments of the present invention provide a method for preparing the porous carbon material with a hierarchical distribution as described in the first aspect above, the preparation method comprising:
[0015] Step S1: Mix magnesium salt and carbon source material in a certain proportion and granulate to obtain composite particles;
[0016] Step S2: The composite particles are subjected to carbonization treatment to obtain carbonized particles;
[0017] Step S3: The carbonized particles are acid-washed, then washed with deionized water and / or anhydrous ethanol, and dried to obtain the precursor.
[0018] Step S4: The precursor is sintered to obtain a porous carbon material with a layered distribution after discharge.
[0019] Preferably, the magnesium salt comprises one or more of the following: magnesium glycinate, magnesium sulfate, magnesium nitrate, magnesium lactate, magnesium citrate, magnesium gluconate, magnesium acetate, magnesium acetylatum, and magnesium malate.
[0020] The carbon source material includes one or more of the following: phenolic resin, furan resin, polyester resin, polyamide resin, ion exchange resin, polyethylene, polypropylene, starch, asphalt, straw, sawdust, bagasse, rice husk, and coconut shell.
[0021] The mass ratio of the magnesium salt to the carbon source material is 1:1 to 3:1.
[0022] The mixed granulation method includes any one of the following: solid phase ball milling, liquid phase ball milling, spray drying, VC mixing, sol-gel method, and evaporation method.
[0023] Preferably, the carbonization process includes: placing the composite particles in a high-temperature furnace, and using a gradient heating method under a protective atmosphere, first heating to 200℃~280℃ at a heating rate of 1℃ / min, holding at that temperature for 2 hours, and then heating to 600℃~1000℃ at a heating rate of 3℃ / min~6℃ / min, holding at that temperature for 2 hours~6 hours.
[0024] Preferably, the pickling includes: immersing the carbonized particles in a hydrochloric acid aqueous solution with a molar concentration of 5 mol / L for 24 to 48 hours; the mass ratio of the carbonized particles to the hydrochloric acid aqueous solution is 3:1 to 4:1.
[0025] The deionized water wash shall be performed at least three times;
[0026] The anhydrous ethanol wash shall be performed at least three times.
[0027] Preferably, the sintering process includes: placing the precursor in a high-temperature furnace, heating it to 900°C to 1400°C at a heating rate of 1°C / min to 10°C / min under a protective atmosphere, and holding it at that temperature for 2 hours to 6 hours.
[0028] Thirdly, embodiments of the present invention provide a silicon-carbon composite material, the silicon-carbon composite material comprising the porous carbon material with a hierarchical distribution as described in the first aspect above, nano-silicon particles deposited in the pores of the porous carbon material, and a carbon coating layer covering the outermost surface of the porous carbon material.
[0029] Fourthly, embodiments of the present invention provide a negative electrode sheet, wherein the negative electrode sheet comprises the silicon-carbon composite material described in the third aspect above.
[0030] Fifthly, embodiments of the present invention provide a lithium-ion battery, the lithium-ion battery comprising the negative electrode sheet described in the fourth aspect above.
[0031] This invention provides a method for preparing a porous carbon material with a hierarchical pore structure. Magnesium salt and carbon source material are mixed and granulated in a specific ratio. The mixture is then subjected to a temperature gradient carbonization process to obtain carbonized particles containing magnesium oxide. The magnesium oxide is removed by acid washing, followed by washing with deionized water and / or anhydrous ethanol until the solution is neutral. The particles are then dried to obtain a precursor, which is then sintered to finally obtain a porous carbon material with a hierarchical pore structure. This preparation method achieves a hierarchical pore size and ratio by controlling the mass ratio of magnesium salt and carbon source material, as well as the heating rate, temperature, and holding time during the carbonization and sintering processes. The preparation method provided by this invention has a simple production process, low cost, and is suitable for mass production.
[0032] The porous carbon material prepared by the preparation method provided in this invention has a layered distribution of pores. The pore structure has a specific layered distribution, with a small proportion of micropores and mesopores with a diameter between 2 nm and 10 nm. The proportion of mesopores with a diameter greater than or equal to 4 nm and less than 7 nm is the highest. The regular pore size distribution gives the porous carbon material a rich specific surface area and excellent silicon deposition capability, which can meet specific application requirements. For example, using the porous carbon material provided in this invention for silicon deposition and carbon coating, a silicon-carbon composite material with a high amount of nano-silicon deposition and good uniformity can be obtained. This can improve the electrochemical performance of the silicon-carbon composite material. Applying the silicon-carbon composite material to lithium-ion batteries can improve the lithium storage capacity and conductivity of lithium-ion batteries, thereby improving the first-cycle coulombic efficiency and specific capacity of lithium-ion batteries. Attached Figure Description
[0033] Figure 1 A flowchart illustrating a method for preparing porous carbon materials with a hierarchical distribution, as provided in an embodiment of the present invention.
[0034] Figure 2 This is a scanning electron microscope (SEM) image of a porous carbon material with a hierarchical distribution provided in Embodiment 8 of the present invention.
[0035] Figure 3 The X-ray diffraction (XRD) pattern of the porous carbon material with a hierarchical distribution provided in Embodiment 8 of the present invention.
[0036] Figure 4 The pore size distribution diagram of the porous carbon material with a hierarchical distribution provided in Embodiment 8 of the present invention is shown.
[0037] Figure 5 The pore size distribution diagram of the porous carbon material with a hierarchical distribution provided in Embodiment 9 of the present invention is shown. Detailed Implementation
[0038] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0039] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0040] This invention provides a porous carbon material with a hierarchical distribution, comprising: a first micropore, a second micropore, a first mesopore, a second mesopore, a third mesopore, and a fourth mesopore. The specific surface area of the porous carbon material is 800 m². 2 / g~1500m 2 / g, pore volume 0.8cm 3 / g~1.3cm 3 Between / g.
[0041] The hierarchical distribution of the pore structure in porous carbon materials is as follows:
[0042] The diameter of the first micropore is less than 1 nm; the number of the first micropores accounts for less than 10% of the total number of pores in the porous carbon material;
[0043] The pore size of the second micropore is greater than or equal to 1 nm and less than 2 nm; the percentage of the number of the second micropores in the total number of pores of the porous carbon material is greater than or equal to 5% and less than or equal to 15%.
[0044] The diameter of the first mesopore is greater than or equal to 2 nm and less than 4 nm; the percentage of the number of the first mesopores in the total number of pores of the porous carbon material is greater than or equal to 15% and less than or equal to 25%.
[0045] The pore size of the second mesopore is greater than or equal to 4 nm and less than 7 nm; the number of the second mesopore accounts for more than or equal to 50% and less than or equal to 70% of the total number of pores in the porous carbon material;
[0046] The diameter of the third mesopore is greater than or equal to 7 nm and less than 10 nm; the percentage of the number of third mesopores in the total number of pores in the porous carbon material is greater than or equal to 1% and less than or equal to 10%.
[0047] The pore size of the fourth mesopore is greater than or equal to 10 nm and less than or equal to 50 nm; the number of fourth mesopores accounts for less than 1% of the total number of pores in the porous carbon material.
[0048] This invention provides a method for preparing the above-mentioned porous carbon material with hierarchical distribution, such as... Figure 1 As shown, the specific steps include:
[0049] Step S1: Mix magnesium salt and carbon source material in a certain proportion and granulate to obtain composite particles;
[0050] Among them, magnesium salts include one or more of the following: magnesium glycinate, magnesium sulfate, magnesium nitrate, magnesium lactate, magnesium citrate, magnesium gluconate, magnesium acetate, magnesium acetylatum, and magnesium malate.
[0051] Carbon source materials include one or more of the following: phenolic resin, furan resin, polyester resin, polyamide resin, ion exchange resin, polyethylene, polypropylene, starch, asphalt, straw, sawdust, bagasse, rice husk, and coconut shell.
[0052] The mass ratio of magnesium salt to carbon source material is 1:1 to 3:1, and can be any ratio within the above range, such as 1:1, 1.5:1, 2:1, 2.5:1, 3:1, etc., but is not limited to the listed mass ratios. Other unlisted mass ratios within this range are also applicable.
[0053] All the methods for mixed granulation are existing conventional methods, including: solid phase ball milling, liquid phase ball milling, spray drying, VC mixing, sol-gel method, and evaporation method.
[0054] Specifically, the inlet temperature range of the spray dryer used in the spray drying method is 150℃~250℃, and the outlet temperature range is 50℃~150℃; the rotation speed of the ball mill in the solid phase ball milling method and the liquid phase ball milling method can be between 300rpm and 1000rpm.
[0055] Step S2: Carbonize the composite particles to obtain carbonized particles.
[0056] The carbonization process specifically includes: placing the composite particles in a high-temperature furnace and using a gradient heating method under a protective atmosphere. First, the temperature is increased to 200℃~280℃ at a heating rate of 1℃ / min and held for 2 hours. Then, the temperature is increased to 600℃~1000℃ at a heating rate of 3℃ / min~6℃ / min and held for 2 hours~6 hours.
[0057] Step S3: The carbonized particles are acid-washed, then washed with deionized water and / or anhydrous ethanol, and dried to obtain the precursor.
[0058] The pickling process includes immersing the carbonized particles in a hydrochloric acid aqueous solution with a molar concentration of 5 mol / L for 24 to 48 hours; the mass ratio of carbonized particles to hydrochloric acid aqueous solution is 3:1 to 4:1.
[0059] Wash with deionized water at least three times, and / or with anhydrous ethanol at least three times, until the solution is neutral.
[0060] Step S4: The precursor is sintered to obtain a porous carbon material with a layered distribution after discharge.
[0061] The sintering process includes: placing the precursor in a high-temperature furnace, heating it to 900℃ to 1400℃ at a heating rate of 1℃ / min to 10℃ / min under a protective atmosphere, and holding it at that temperature for 2 hours to 6 hours.
[0062] This invention uses a mixture of magnesium salt and carbon source material to form composite particles, which are then carbonized through a gradient heating process. Specifically, the temperature is first raised to 200℃~280℃ at a heating rate of 1℃ / min and held for 2 hours to stabilize the structure of the composite particles at a low temperature. Then, the temperature is raised to 600℃~1000℃ at a heating rate of 3℃ / min~6℃ / min to carbonize the material at a high temperature. During the carbonization process, the magnesium salt in the composite particles decomposes into magnesium oxide and gases (such as water vapor and carbon dioxide) at high temperature. The magnesium oxide remains in the carbonized material of the composite particles. After removing the magnesium oxide, sintering is performed to obtain porous carbon material.
[0063] This invention uses magnesium salts instead of directly using magnesium oxide as a template agent to prepare porous carbon materials. On the one hand, magnesium salts can decompose into magnesium oxide and gas at high temperatures, and the generated gas can also etch the surface of the carbon material to form a porous structure. On the other hand, if magnesium oxide is used directly, the pore size will be fixed, which cannot meet the requirement of controlling the pore size. The magnesium oxide particles obtained by the decomposition of magnesium salts have a smaller particle size. At the same time, by adjusting the heating rate, temperature, and time of the carbonization process, as well as the temperature and time of the sintering process, a porous carbon material with a hierarchical distribution of pore size and ratio can be obtained.
[0064] In addition, compared with the hard template method of directly preparing porous carbon materials using silicon dioxide, the present invention does not require hydrofluoric acid washing, is pollution-free, has a short sintering time, and is low in cost.
[0065] This invention provides a silicon-carbon composite material, comprising the aforementioned porous carbon material with a hierarchical distribution, nano-silicon particles deposited in the pores of the porous carbon material, and a carbon coating layer covering the outermost surface of the porous carbon material.
[0066] The method for preparing a silicon-carbon composite material provided in this embodiment of the invention is a known prior art method, specifically as follows:
[0067] The aforementioned porous carbon material with hierarchical distribution is placed in a deposition apparatus and heated to 400℃~700℃ under a protective atmosphere. A mixture of carrier gas and silicon source gas is introduced and kept at this temperature for 2 hours to 5 hours. This allows the silicon source gas to decompose, resulting in silicon elements that are deposited in the pores and on the surface of the porous carbon material and grow into nano-silicon particles. After cooling to room temperature, a silicon-carbon precursor material is obtained. The carrier gas and protective gas include nitrogen or argon. The silicon source gas includes one or more of silane, disilane, and dichlorosilane. The volumetric flow rate ratio of the carrier gas to the silicon source gas is [1:1]~[3:1]. The flow rate range of the carrier gas to the silicon source gas is 10L / min~50L / min.
[0068] The silicon-carbon precursor material is placed in a coating device and heated to 500℃~600℃ under a protective atmosphere. A mixture of carrier gas and carbon source gas is introduced and kept at this temperature for 2 hours to 3 hours. This allows the carbon source gas to decompose and carbon elements to be deposited on the surface of the silicon-carbon precursor material to form a carbon coating layer, thus obtaining a silicon-carbon composite material. The protective gas or carrier gas includes nitrogen or argon. The carbon source gas includes one or more of methane, acetylene, ethylene, and propylene. The volumetric flow rate ratio of the carrier gas to the carbon source gas is [3:1]~[4:1]. The flow rate of the mixed gas is 5L / min~40L / min.
[0069] The silicon-carbon composite material prepared based on a porous carbon material with a hierarchical distribution, as provided in the embodiments of the present invention, can be used as a negative electrode active material to prepare a negative electrode sheet, which can be applied in lithium-ion batteries. The silicon-carbon composite material prepared using the porous carbon material provided in the embodiments of the present invention has a high deposition amount and good uniformity of nano-silicon particles due to the hierarchical distribution of the pore structure of the porous carbon material. Applying this silicon-carbon composite material to lithium-ion batteries can improve the first-cycle coulombic efficiency and specific capacity of the battery.
[0070] To better understand the technical solution provided by the present invention, the following uses several specific examples to illustrate the preparation process and characteristics of the porous carbon material with hierarchical distribution of the present invention.
[0071] Example 1
[0072] This embodiment provides a process for preparing a porous carbon material with a hierarchical distribution, the specific process of which is as follows.
[0073] (1) Place 32g of magnesium glycine and 20g of phenolic resin in a ball mill and ball mill at 400rpm for 6 hours to obtain composite particles.
[0074] (2) The composite particles are heated to 260°C at a heating rate of 1°C / min under a nitrogen atmosphere and held for 2 hours. Then, they are heated to 900°C at a heating rate of 5°C / min and held for 2 hours. The particles are then cooled naturally to obtain carbonized particles.
[0075] (3) The carbonized particles were soaked in a 5 mol / L hydrochloric acid solution at 80°C for 24 hours, washed three times with deionized water, then washed three times with anhydrous ethanol, and then dried in an oven at 90°C for 24 hours to obtain the precursor.
[0076] (4) The precursor is placed in a box furnace and sintered under a nitrogen atmosphere. It is heated to 1200°C at a heating rate of 5°C / min, held for 4 hours, and then cooled naturally to obtain a porous carbon material with a layered distribution.
[0077] Example 2
[0078] This embodiment provides a preparation process for a porous carbon material with a hierarchical distribution. The difference from Example 1 is that the sintering temperature in step (4) is 900°C, while the other preparation processes are the same as in Example 1.
[0079] Example 3
[0080] This embodiment provides a process for preparing a porous carbon material with a hierarchical distribution, the specific process of which is as follows.
[0081] (1) 50g of magnesium gluconate and 20g of ion exchange resin were soaked in an aqueous solution for 24 hours, and then the exchanged resin was filtered out and dried at 80°C for 24 hours to obtain composite particles.
[0082] (2) The composite particles are heated to 260°C at a heating rate of 1°C / min under a nitrogen atmosphere and held for 2 hours. Then, they are heated to 900°C at a heating rate of 5°C / min and held for 2 hours for carbonization treatment. The particles are then cooled naturally to obtain carbonized particles.
[0083] (3) The carbonized particles were soaked in a 5 mol / L hydrochloric acid solution at 80°C for 24 hours, washed three times with deionized water, then washed three times with anhydrous ethanol, and then dried in an oven at 90°C for 24 hours to obtain the precursor.
[0084] (4) The precursor is placed in a box furnace and sintered under a nitrogen atmosphere. It is heated to 1200°C at a heating rate of 5°C / min, held for 4 hours, and then cooled naturally to obtain a porous carbon material with a layered distribution.
[0085] Example 4
[0086] This embodiment provides a preparation process for a porous carbon material with a layered distribution. The difference from Example 3 is that the proportion of raw materials in step (1) is different, and 60g of magnesium gluconate and 20g of ion exchange resin are impregnated in an aqueous solution; the sintering temperature in step (4) is 900℃; and the other preparation processes are the same as in Example 3.
[0087] Example 5
[0088] This embodiment provides a preparation process for a porous carbon material with a layered distribution, which differs from that of Example 3 in that: the proportion of raw materials in step (1) is different, that is, 32g of magnesium gluconate and 20g of ion exchange resin are impregnated in an aqueous solution; the second heating temperature in step (2) is 700℃; the sintering temperature in step (4) is 1400℃; and the other preparation processes are the same as those in Example 3.
[0089] Example 6
[0090] This embodiment provides a process for preparing a porous carbon material with a hierarchical distribution, the specific process of which is as follows.
[0091] (1) Place 50g of magnesium nitrate and 20g of asphalt in a ball mill, add ethanol solution, and ball mill at 400rpm for 6 hours. Then dry at 80℃ for 24 hours to obtain composite particles.
[0092] (2) The composite particles are heated to 260°C at a heating rate of 1°C / min under a nitrogen atmosphere and held for 2 hours. Then, they are heated to 700°C at a heating rate of 5°C / min and held for 2 hours. The particles are then cooled naturally to obtain carbonized particles.
[0093] (3) The carbonized particles were soaked in a 5 mol / L hydrochloric acid solution at 80°C for 24 hours, washed three times with deionized water, then washed three times with anhydrous ethanol, and then dried in an oven at 90°C for 24 hours to obtain the precursor.
[0094] (4) The precursor is placed in a box furnace and sintered under a nitrogen atmosphere. It is heated to 1200°C at a heating rate of 5°C / min, held for 4 hours, and then cooled naturally to obtain a porous carbon material with a layered distribution.
[0095] Example 7
[0096] This embodiment provides a preparation process for a porous carbon material with a layered distribution. The difference from Example 6 is that the proportion of raw materials in step (1) is different, using 32g of magnesium nitrate and 20g of pitch; the sintering temperature in step (4) is 1400℃; and the other preparation processes are the same as in Example 6.
[0097] Example 8
[0098] This embodiment provides a process for preparing a porous carbon material with a hierarchical distribution, the specific process of which is as follows.
[0099] (1) Dissolve 32g of magnesium citrate and 20g of water-soluble starch in deionized water, and then spray dry to obtain composite granules. The spray dryer used for spray drying has an inlet temperature range of 200℃ and an outlet temperature range of 80℃.
[0100] (2) The composite particles are heated to 260°C at a heating rate of 1°C / min under a nitrogen atmosphere and held for 2 hours. Then, they are heated to 600°C at a heating rate of 5°C / min and held for 2 hours. The particles are then cooled naturally to obtain carbonized particles.
[0101] (3) The carbonized particles were soaked in a 5 mol / L hydrochloric acid solution at 80°C for 24 hours, washed three times with deionized water, then washed three times with anhydrous ethanol, and then dried in an oven at 90°C for 24 hours to obtain the precursor.
[0102] (4) The precursor is placed in a box furnace and sintered under a nitrogen atmosphere. It is heated to 1200°C at a heating rate of 5°C / min, held for 4 hours, and then cooled naturally to obtain a porous carbon material with a layered distribution.
[0103] SEM image of the porous carbon material with hierarchical distribution prepared in this embodiment, as shown below. Figure 2 As shown.
[0104] The XRD pattern of the porous carbon material with hierarchical distribution prepared in this embodiment is shown below. Figure 3 As shown in the figure, the standard diffraction peaks of porous carbon materials are displayed.
[0105] The pore size distribution diagram of the porous carbon material with hierarchical distribution prepared in this embodiment is as follows: Figure 4 As shown, the pore size distribution is mainly concentrated in the range of 4nm to 7nm.
[0106] Example 9
[0107] This embodiment provides a preparation process for a porous carbon material with a hierarchical distribution. The difference from Example 8 is that the sintering temperature in step (4) is 900°C, while the other preparation processes are the same as in Example 8.
[0108] The pore size distribution diagram of the porous carbon material with hierarchical distribution prepared in this embodiment is as follows: Figure 5 As shown, the pore size distribution is mainly concentrated in the range of 2nm to 10nm.
[0109] Example 10
[0110] This embodiment provides a process for preparing a porous carbon material with a hierarchical distribution, the specific process of which is as follows.
[0111] (1) Place 32g of magnesium citrate and 20g of asphalt in a ball mill, add ethanol solution, and ball mill at 400rpm for 6 hours. Then dry at 80℃ for 24 hours to obtain composite particles.
[0112] (2) The composite particles are heated to 260°C at a heating rate of 1°C / min under a nitrogen atmosphere and held for 2 hours. Then, they are heated to 900°C at a heating rate of 5°C / min and held for 2 hours. The particles are then cooled naturally to obtain carbonized particles.
[0113] (3) The carbonized particles were soaked in a 5 mol / L hydrochloric acid solution at 80°C for 24 hours, washed three times with deionized water, then washed three times with anhydrous ethanol, and then dried in an oven at 90°C for 24 hours to obtain the precursor.
[0114] (4) The precursor is placed in a box furnace and sintered under a nitrogen atmosphere. It is heated to 1200°C at a heating rate of 5°C / min, held for 4 hours, and then cooled naturally to obtain a porous carbon material with a layered distribution.
[0115] Example 11
[0116] This embodiment provides a preparation process for a porous carbon material with a layered distribution, which differs from that of Example 10 in that: the proportion of raw materials in step (1) is different, using 50g of magnesium citrate and 20g of pitch; the sintering temperature in step (4) is 900℃; and the other preparation processes are the same as those in Example 10.
[0117] Example 12
[0118] This embodiment provides a preparation process for a type of porous carbon material with a hierarchical distribution, the specific process of which is as follows.
[0119] (1) Place 32g of magnesium acetate and 20g of asphalt in a ball mill, add ethanol solution, and ball mill at 400rpm for 6 hours. Then dry at 80℃ for 24 hours to obtain composite particles.
[0120] (2) The composite particles are heated to 260°C at a heating rate of 1°C / min under a nitrogen atmosphere and held for 2 hours. Then, they are heated to 700°C at a heating rate of 5°C / min and held for 2 hours. The particles are then cooled naturally to obtain carbonized particles.
[0121] (3) The carbonized particles were soaked in a 5 mol / L hydrochloric acid solution at 80°C for 24 hours, washed three times with deionized water, then washed three times with anhydrous ethanol, and then dried in an oven at 90°C for 24 hours to obtain the precursor.
[0122] (4) The precursor is placed in a box furnace and sintered under a nitrogen atmosphere. It is heated to 1400°C at a heating rate of 5°C / min, held for 4 hours, and then cooled naturally to obtain a porous carbon material with a layered distribution.
[0123] Example 13
[0124] This embodiment provides a preparation process for a porous carbon material with a layered distribution. The difference from Example 12 is that the proportion of raw materials in step (1) is different, using 50g of magnesium acetate and 20g of pitch; the sintering temperature in step (4) is 900℃; and the other preparation processes are the same as in Example 12.
[0125] Example 14
[0126] This embodiment provides a process for preparing a porous carbon material with a hierarchical distribution, the specific process of which is as follows.
[0127] (1) Dissolve 32g of magnesium acetate and 20g of water-soluble starch in deionized water, and then spray dry to obtain composite granules. The spray dryer used for spray drying has an inlet temperature range of 200℃ and an outlet temperature range of 80℃.
[0128] (2) The composite particles are heated to 260°C at a heating rate of 1°C / min under a nitrogen atmosphere and held for 2 hours. Then, they are heated to 700°C at a heating rate of 5°C / min and held for 2 hours. The particles are then cooled naturally to obtain carbonized particles.
[0129] (3) The carbonized particles were soaked in a 5 mol / L hydrochloric acid solution at 80°C for 24 hours, washed three times with deionized water, then washed three times with anhydrous ethanol, and then dried in an oven at 90°C for 24 hours to obtain the precursor.
[0130] (4) The precursor is placed in a box furnace and sintered under a nitrogen atmosphere. It is heated to 1200°C at a heating rate of 5°C / min, held for 4 hours, and then cooled naturally to obtain a porous carbon material with a layered distribution.
[0131] Example 15
[0132] This embodiment provides a preparation process for a porous carbon material with a layered distribution. The difference from Example 14 is that the proportion of raw materials in step (1) is different, using 50g of magnesium acetate and 20g of water-soluble starch; the sintering temperature in step (4) is 900℃; and the other preparation processes are the same as in Example 14.
[0133] Example 16
[0134] This embodiment provides a process for preparing a porous carbon material with a hierarchical distribution, the specific process of which is as follows.
[0135] (1) Dissolve 50g of magnesium sulfate and 20g of asphalt in a ball mill, add ethanol solution, and ball mill at 400rpm for 6 hours. Then dry at 80℃ for 24 hours to obtain composite particles.
[0136] (2) The composite particles are heated to 260°C at a heating rate of 1°C / min under a nitrogen atmosphere and held for 2 hours. Then, they are heated to 900°C at a heating rate of 5°C / min and held for 2 hours. The particles are then cooled naturally to obtain carbonized particles.
[0137] (3) The carbonized particles were soaked in a 5 mol / L hydrochloric acid solution at 80°C for 24 hours, washed three times with deionized water, then washed three times with anhydrous ethanol, and then dried in an oven at 90°C for 24 hours to obtain the precursor.
[0138] (4) The precursor is placed in a box furnace and sintered under a nitrogen atmosphere. It is heated to 900°C at a heating rate of 5°C / min, held for 4 hours, and then cooled naturally to obtain a porous carbon material with a layered distribution.
[0139] Example 17
[0140] This embodiment provides a preparation process for a porous carbon material with a layered distribution. The difference from Example 16 is that the proportion of raw materials in step (1) is different, using 32g of magnesium sulfate and 20g of pitch; the sintering temperature in step (4) is 1400℃; and the other preparation processes are the same as in Example 16.
[0141] To better illustrate the effects of the embodiments of the present invention, comparative examples 1-4 are compared with the above embodiment 8.
[0142] Comparative Example 1
[0143] This comparative example provides a preparation process for porous carbon materials. The difference from Example 8 is that the heating rate of the first heating in step (2) is different. The composite particles are first heated to 260°C at a heating rate of 5°C / min under a nitrogen atmosphere, held at that temperature for 2 hours, then heated to 600°C at a heating rate of 5°C / min, held at that temperature for 2 hours, and then allowed to cool naturally to obtain carbonized particles. The other preparation processes are the same as in Example 8.
[0144] Comparative Example 2
[0145] This comparative example provides a preparation process for porous carbon materials. The difference from Example 8 is that in step (1), the ratio of magnesium salt to carbon source material is larger, which is 80:20. 80g of magnesium citrate and 20g of water-soluble starch are used.
[0146] Comparative Example 3
[0147] This comparative example provides a preparation process for porous carbon materials. The difference from Example 8 is that the carbonization process in step (2) does not use a gradient heating process. Instead, it directly heats the material to 600°C at a heating rate of 5°C / min and holds it at that temperature for 2 hours for carbonization.
[0148] Comparative Example 4
[0149] This comparative example provides a preparation process for porous carbon materials. The difference from Example 8 is that in step (1), the ratio of magnesium salt to carbon source material is smaller, using 16g of magnesium citrate and 20g of water-soluble starch.
[0150] The physicochemical properties and electrochemical performance of the porous carbon materials prepared in Examples 1-17 and Comparative Examples 1-4 were tested:
[0151] 1. The pore size distribution was analyzed by BET test using a gas adsorption analyzer (Quantachrom-IQ2-XR). The specific surface area, average pore size, and pore volume of the porous carbon materials prepared in Examples 1-17 and Comparative Examples 1-4 were obtained. The test structures are detailed in Table 1.
[0152]
[0153]
[0154] Table 1
[0155] The test data in Table 1 show that: Compared with Comparative Example 1, Example 8 had a higher heating rate during carbonization, resulting in a smaller pore structure, insufficient mesoporous structure, and a smaller specific surface area in the prepared porous carbon material; Compared with Comparative Example 2, Example 8 used a larger ratio of magnesium salt to carbon source material, leading to the formation of more magnesium oxide during subsequent sintering steps, thus resulting in a larger pore size in Comparative Example 2 compared to Example 8; Compared with Comparative Example 3, Example 8 did not use gradient heating during carbonization, resulting in an unstable structure in the early carbonization process and the formation of larger pores during later carbonization steps; Compared with Comparative Example 4, Example 8 had a smaller ratio of magnesium salt to carbon source material, resulting in less magnesium oxide formation during subsequent sintering steps, smaller pore structure, insufficient mesoporous structure, and a smaller specific surface area.
[0156] 2. Let the first micropore (<1nm), second micropore (1nm~2nm), first mesopore (2nm~4nm), second mesopore (4nm~7nm), third mesopore (7nm~10nm), and fourth mesopore (≥10nm) in the porous carbon materials prepared in Examples 1-17 and Comparative Examples 1-4 be a, b, c, d, e, and f, respectively. The distribution ratios of a, b, c, d, e, and f were detected using an ASAP2460 pore size analyzer. The test results are detailed in Table 2.
[0157] serial number a b c d e f Example 1 8.25% 7.73% 18.92% 60.25% 4.36% 0.49% Example 2 6.32% 8.79% 17.37% 60.32% 6.32% 0.88% Example 3 9.26% 12.98% 20.10% 53.22% 3.98% 0.46% Example 4 5.81% 7.23% 16.48% 64.90% 4.78% 0.80% Example 5 9.58% 13.36% 23.26% 50.21% 3.25% 0.34% Example 6 7.83% 11.53% 14.59% 58.46% 6.78% 0.81% Example 7 8.92% 13.47% 17.52% 54.60% 4.87% 0.62% Example 8 9.46% 13.89% 22.96% 50.24% 3.16% 0.29% Example 9 6.78% 10.83% 16.62% 57.74% 7.28% 0.75% Example 10 9.76% 14.42% 20.52% 51.44% 3.38% 0.48% Example 11 6.01% 8.36% 15.69% 60.03% 8.97% 0.94% Example 12 9.97% 14.95% 21.57% 50.18% 3.05% 0.28% Example 13 6.46% 9.34% 16.16% 59.11% 8.07% 0.86% Example 14 9.85% 14.63% 20.41% 51.49% 3.26% 0.36% Example 15 6.95% 9.91% 17.59% 57.53% 7.28% 0.74% Example 16 6.21% 9.24% 16.51% 59.03% 8.18% 0.83% Example 17 9.29% 13.46% 20.40% 52.42% 4.01% 0.42% Comparative Example 1 14.26% 27.24% 25.65% 20.14% 12.30% 0.41% Comparative Example 2 2.75% 6.17% 21.42% 35.78% 27.21% 6.67% Comparative Example 3 3.05% 7.12% 23.35% 37.78% 24.32% 4.38% Comparative Example 4 13.58% 23.78% 31.54% 24.24% 6.57% 0.29%
[0158] Table 2
[0159] As can be seen from the test data in Table 2, the porous carbon material with hierarchical pore distribution obtained by the preparation method provided in this embodiment has a higher proportion of second mesopores (4nm~7nm). Mesopores in this range are more conducive to subsequent silicon deposition, thus improving the silicon deposition capability of the porous carbon material.
[0160] 3. Using the porous carbon materials prepared in Examples 1-17 and Comparative Examples 1-4, silicon-carbon anode materials were prepared. Then, anode sheets were prepared using the silicon-carbon anode materials and assembled into coin cells for testing. The specific process is as follows:
[0161] First, silicon-carbon composite materials were prepared using the porous carbon materials obtained in Examples 1-17 and Comparative Examples 1-4. The specific process was as follows: The porous carbon materials were placed in a vapor deposition furnace and heated to 400°C under a nitrogen atmosphere. A mixed gas of nitrogen with a flow rate of 30 L / min and silane with a flow rate of 20 L / min was introduced and kept at this temperature for 3 hours. This allowed the silane to decompose and obtain silicon elements, which were deposited in the pores and on the surface of the porous carbon materials and grew into nano-silicon particles. After cooling to room temperature, silicon-carbon precursor materials were obtained. The silicon-carbon precursor materials were then placed in a coating furnace and heated to 600°C under a nitrogen atmosphere. A mixed gas of nitrogen with a flow rate of 30 L / min and acetylene with a flow rate of 10 L / min was introduced and kept at this temperature for 2 hours. This allowed the acetylene to decompose and obtain carbon elements, which were deposited on the surface of the silicon-carbon precursor materials to form a carbon coating layer, thus obtaining the silicon-carbon composite materials of Examples 1-17 and Comparative Examples 1-4.
[0162] Electrode preparation: The silicon-carbon composite materials of Examples 1-17 and Comparative Examples 1-4 were respectively mixed with Super P conductive agent, sodium carboxymethyl cellulose, and styrene-butadiene rubber in a mass ratio of 16:2:1:1 to prepare aqueous negative electrode slurry. The solid content of the slurry was controlled at about 45 wt%. The slurry was homogenized using a homogenizer. The slurry was coated on copper foil with a coating thickness of 70 μm. After drying at 80 °C, rolling, cutting, and vacuum drying at 110 °C for 12 hours, the electrode was obtained.
[0163] Assemble the half-cell: Using the electrode prepared above, with lithium metal sheet as counter electrode and reference electrode, and with CR2025 matching battery case, Celgard2500 separator and LiPF6 electrolyte with a molar concentration of 1 mol / L, wherein the solvent of the electrolyte is ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1, the half-cell is assembled in a glove box.
[0164] The assembled button cell half-cells were tested: constant current cyclic charge-discharge tests were performed simultaneously on the Xinwei testing system, with a test voltage range of 0.01V to 2V. The tests were conducted at room temperature. First, the cells were discharged to 0.5V at 0.1C (1C = 2000mAh / g), then discharged to 0.1V at 0.05C, and then discharged to 0.01V at 0.02C, followed by a 10-minute rest period. Next, the cells were charged to 1.5V at 0.1C and then rested for 10 minutes. The charge and discharge capacities after the first cycle were recorded, and the coulombic efficiency of the first cycle was calculated. After 5 cycles in the same manner, the charge capacity was recorded. The test results are shown in Table 3 below.
[0165]
[0166] Table 3
[0167] As can be seen from the test data in Table 3, the silicon content, first-cycle coulombic efficiency, and fifth-cycle specific capacity of Examples 1-17 are all greater than those of Comparative Examples 1-4. This indicates that when silicon-carbon composite materials prepared using porous carbon materials with hierarchical distribution in Examples 1-17 are used, silicon deposition is more favorable, thereby improving the first-cycle coulombic efficiency and specific capacity of silicon-carbon composite materials when applied to lithium-ion batteries.
[0168] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A porous carbon material with a hierarchical distribution, characterized in that, The porous carbon material has the following pores: a first micropore, a second micropore, a first mesopore, a second mesopore, a third mesopore, and a fourth mesopore; The pore size of the first micropore is less than 1 nm; the number of the first micropore accounts for less than 10% of the total number of pores in the porous carbon material. The pore size of the second micropore is greater than or equal to 1 nm and less than 2 nm; the number of the second micropore accounts for a percentage of the total number of pores in the porous carbon material that is greater than or equal to 5% and less than or equal to 15%. The pore size of the first mesopore is greater than or equal to 2 nm and less than 4 nm; the percentage of the number of the first mesopores to the total number of pores in the porous carbon material is greater than or equal to 15% and less than or equal to 25%. The pore size of the second mesopore is greater than or equal to 4 nm and less than 7 nm; the number of the second mesopore accounts for a percentage of the total number of pores in the porous carbon material that is greater than or equal to 50% and less than or equal to 70%. The pore size of the third mesopore is greater than or equal to 7 nm and less than 10 nm; the number of the third mesopores accounts for a percentage of the total number of pores in the porous carbon material that is greater than or equal to 1% and less than or equal to 10%. The pore size of the fourth mesopore is greater than or equal to 10 nm and less than or equal to 50 nm; the number of the fourth mesopore accounts for less than 1% of the total number of pores in the porous carbon material.
2. The porous carbon material according to claim 1, characterized in that, The porous carbon material has a specific surface area of 800 m². 2 / g~1500m 2 / g; The porous carbon material has a pore volume of 0.8 cm³. 3 / g~1.3cm 3 Between / g.
3. A method for preparing a porous carbon material with a hierarchical distribution as described in any one of claims 1-2, characterized in that, The preparation method includes: Step S1: Mix magnesium salt and carbon source material in a certain proportion and granulate to obtain composite particles; Step S2: The composite particles are subjected to carbonization treatment to obtain carbonized particles; Step S3: The carbonized particles are acid-washed, then washed with deionized water and / or anhydrous ethanol, and dried to obtain the precursor. Step S4: The precursor is sintered to obtain a porous carbon material with a layered distribution after discharge.
4. The preparation method according to claim 3, characterized in that, The magnesium salt includes one or more of the following: magnesium glycinate, magnesium sulfate, magnesium nitrate, magnesium lactate, magnesium citrate, magnesium gluconate, magnesium acetate, magnesium acetylatum, and magnesium malate. The carbon source material includes one or more of the following: phenolic resin, furan resin, polyester resin, polyamide resin, ion exchange resin, polyethylene, polypropylene, starch, asphalt, straw, sawdust, bagasse, rice husk, and coconut shell. The mass ratio of the magnesium salt to the carbon source material is 1:1 to 3:
1. The mixed granulation method includes any one of the following: solid phase ball milling, liquid phase ball milling, spray drying, VC mixing, sol-gel method, and evaporation method.
5. The preparation method according to claim 3, characterized in that, The carbonization process includes: placing the composite particles in a high-temperature furnace, and using a gradient heating method under a protective atmosphere, first heating to 200℃~280℃ at a heating rate of 1℃ / min, holding at that temperature for 2 hours, and then heating to 600℃~1000℃ at a heating rate of 3℃ / min~6℃ / min, holding at that temperature for 2 hours~6 hours.
6. The preparation method according to claim 3, characterized in that, The pickling process includes immersing the carbonized particles in a hydrochloric acid aqueous solution with a molar concentration of 5 mol / L for 24 to 48 hours; the mass ratio of the carbonized particles to the hydrochloric acid aqueous solution is 3:1 to 4:
1. The deionized water wash shall be performed at least three times; The anhydrous ethanol wash shall be performed at least three times.
7. The preparation method according to claim 3, characterized in that, The sintering process includes: placing the precursor in a high-temperature furnace, heating it to 900℃ to 1400℃ at a heating rate of 1℃ / min to 10℃ / min under a protective atmosphere, and holding it at that temperature for 2 hours to 6 hours.
8. A silicon-carbon composite material, characterized in that, The silicon-carbon composite material includes the porous carbon material with a hierarchical distribution as described in any one of claims 1-2, nano-silicon particles deposited in the pores of the porous carbon material, and a carbon coating layer covering the outermost surface of the porous carbon material.
9. A negative electrode sheet, characterized in that, The negative electrode sheet comprises the silicon-carbon composite material described in claim 8.
10. A lithium-ion battery, characterized in that, The lithium-ion battery includes the negative electrode sheet as described in claim 9.