A motor shaft current protection structure preparation method based on a flexible boron nitride composite bushing and a product
By using micron- and nano-scale boron nitride composites with flexible polymers, combined with radially oriented freezing and axial pressure relief microgrooves, the problem of electro-erosion in motor bearings during shaft voltage discharge was solved, achieving effective electrical insulation and heat conduction, and avoiding material damage and assembly stress concentration.
Patent Information
- Application Number
- CN202611601739.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-13
AI Technical Summary
Existing motor bearings are prone to electrolytic corrosion when the shaft voltage discharges, and traditional insulation materials or ceramic coatings are easily damaged during assembly and maintenance. Ordinary polymers have low thermal conductivity, while increasing the content of thermally conductive fillers will lead to increased stiffness and assembly stress concentration.
The composite material of micron- and nano-scale boron nitride and high-temperature resistant flexible polymer is used to form a thermally conductive skeleton and an electrically insulating structure through radial directional freezing. Combined with axial pressure relief microgrooves and segmented interference fit, effective electrical insulation and thermal conduction are ensured between the bearing inner ring and the motor shaft.
Effective electrical insulation and thermal conduction are achieved between the bearing inner ring and the motor shaft, avoiding material damage and assembly stress concentration, and maintaining flexibility and durability.
Smart Images

Figure CN123097017A_ABST
Abstract
Description
Technical Field
[0001] This application relates to motor bearing insulation and composite material molding technology, specifically to a method and product for preparing a motor shaft current protection structure based on a flexible boron nitride composite bushing. Background Technology
[0002] When the shaft voltage of a variable frequency motor discharges through the bearing, it can cause electrolytic erosion on the raceway surface. Using ceramic coatings or insulated bearings can increase the resistance between the shaft and bearing, but ceramic coatings are prone to localized compression during bearing press-fitting and repeated disassembly; insulated bearings also alter the procurement and maintenance system for standard bearings. Using polymer sleeves between the shaft and the bearing inner ring facilitates replacement, but ordinary polymers have low thermal conductivity, making it difficult for bearing heat to be transferred to the motor shaft; simply increasing the content of thermally conductive fillers can increase the stiffness of the thin-walled sleeve, cause particle agglomeration, and concentrate assembly stress.
[0003] The bushing contacts both the motor shaft and the bearing inner ring, and the interference fits at their inner and outer interfaces affect each other. If the shaft diameter is reduced only according to the nominal bushing wall thickness, molding shrinkage and assembly compression will change the final reference of the bearing inner ring. If the interference fits at both points are selected based on experience, slippage at the inner interface or excessive pressing at the outer interface may occur. For highly filled materials, air and adhesive trapped at the mating interface during pressing can also create localized high pressure, causing the bushing ends to warp or crack.
[0004] Therefore, the packing dimensions, axial material partitioning, interface pressure relief, and two-stage interference dimension chain need to be determined as a whole to ensure that the bushing can transfer heat while maintaining continuous electrical insulation and retaining flexibility during assembly and thermal cycling. Summary of the Invention
[0005] This application provides a method for preparing a motor shaft current protection structure. First, micron-sized boron nitride, nano-sized boron nitride, and a high-temperature resistant flexible polymer precursor are selected; the mass ratio of micron-sized to nano-sized boron nitride is 2:1 to 4:1, and the volume fraction of boron nitride in the cured bushing is 35% to 60%. In an annular mold cavity forming a radial temperature gradient between the inner and outer mold walls, boron nitride dispersions corresponding to the load-bearing section, gradual transition section, and buffer section are sequentially added axially, causing the dispersion to freeze radially. After sublimation to remove the freezing medium, a porous boron nitride preform with channels extending radially from the inner to the outer circumference of the bushing is formed. Then, the high-temperature resistant flexible polymer precursor is vacuum impregnated into the preform and cured into a thin-walled cylindrical bushing. Micron-sized boron nitride constitutes a thermally conductive skeleton extending radially from the inner to the outer circumference of the bushing, while nano-sized boron nitride is located between adjacent micron-sized boron nitride particles. The polymer phase impregnates into the channels and continuously coats the skeleton, thereby forming a radial heat transfer path while maintaining electrical insulation.
[0006] Micron-sized boron nitride particles overlap to form a thermally conductive skeleton. The heat transfer direction of the thermally conductive skeleton is mainly along the bushing wall thickness. The continuous polymer phase covers the particles and blocks the current path from the inner circle to the outer circle. The skeleton is traversed by the same radial freezing front through the load-bearing section, the gradual transition section and the buffer section, avoiding the formation of adhesive seams of independent sleeves at the axial ratio interface.
[0007] The bushing has a load-bearing section corresponding to the bearing raceway projection area, a buffer section near the shaft shoulder, and a gradual transition section between the two along its axial direction. The volume fraction of boron nitride in the load-bearing section is higher than that in the buffer section, while the volume fraction of polymer in the buffer section is higher than that in the load-bearing section. Three to six axial pressure-relief microgrooves are uniformly formed circumferentially on the inner surface of the bushing; the closed end of each microgroove is located in the load-bearing section, and the groove depth gradually increases from the closed end towards the buffer section through the gradual transition section, opening at the press-out end face of the buffer section. The groove depth at the closed end is 3%–6% of the bushing wall thickness, and the groove depth at the open end is 10%–15% of the bushing wall thickness. A continuous load-bearing band with a width greater than the groove width is maintained between each pressure-relief microgroove, and a continuous polymer matrix area coated with boron nitride particles and without through-holes is maintained at the bottom of the groove. Thus, the load-bearing section retains a larger effective load-bearing thickness, and press-fit air or excess adhesive medium is directionally discharged towards the end face of the buffer section along the gradually deepening microgrooves.
[0008] First, determine the initial compensation amount for the section of the motor shaft to be fitted based on the inner and outer diameters of the bushing in its free state. Then, correct the second interference fit based on the measured outer diameter of the sections after the first assembly. Let the inner diameter of the bushing in its free state be... The outer diameter is The inner diameter of the bearing inner ring is The diameter of the section of the motor shaft to be fitted after compensation is: Then the first diameter interference The interference fit of the nominal second diameter corresponding to the free size initial shaft diameter reduction Bushing radial wall thickness The bushing is fitted from the load-bearing section side to the buffer section side by cooling the motor shaft or using a tapered expansion guide to form the first interference fit; after temperature equalization, the outer diameter of the installed bushing is measured in both the load-bearing section and the buffer section. and .by As the actual second diameter interference, and at the same time required Not less than After selecting the bearing inner ring and matching bushing, or finely machining the allowable surface to meet both conditions simultaneously, press the bushed motor shaft into the bearing inner ring in the same direction. If the buffer section forms a larger outer circumference height than the load-bearing section, even if the load-bearing section... It does not enter the second assembly even if it falls into the window.
[0009] The average particle size of micron-sized boron nitride can be 10 μm, and the average particle size of nano-sized boron nitride can be 100 nm, with a mass ratio of 3:1. The volume fraction of boron nitride in the load-bearing section can be 50%–60%, and in the buffer section, 35%–45%. The high-temperature resistant flexible polymer precursor can be addition-cure liquid silicone rubber or a thermally imidizable polyamic acid solution; the absolute pressure in the mold cavity during vacuum impregnation should not exceed 20 kPa, and curing or imidization should be performed after restoring to normal pressure. The interference fit of the first diameter and the actual interference fit of the second diameter can respectively meet the following requirements. , , This is the nominal inner diameter of the bearing's inner ring.
[0010] An anti-rotation texture can be formed in the middle of the outer circumference of the bushing, with a textureless sealing strip on both sides of the anti-rotation texture; the axial ends of the bushing can extend out of the bearing end face to form insulating end rings, and are equipped with replaceable sealing rings. The anti-rotation texture restricts the relative rotation between the bushing and the bearing inner ring, while the sealing strips and sealing rings prevent grease from entering the inner mating interface. Because the end chamfers contact first and gradually guide the shaft and bearing inner ring to press in, the thin-walled cylindrical bushing is not directly subjected to the cutting action of sharp end faces.
[0011] This application also provides a motor shaft current protection product obtained by the above method, including a motor shaft, a flexible boron nitride composite bushing sleeved on the motor shaft, and a bearing sleeved on the composite bushing. The composite bushing forms a controlled interference fit with the motor shaft and the bearing, respectively, and its two ends form insulating isolation end rings. The composite bushing is provided axially with a load-bearing section corresponding to the bearing raceway projection area, a gradual transition section, and a buffer section near the shaft shoulder, without designating a certain circumferential arc segment that rotates with the motor shaft as a fixed load-bearing area; the pressure relief microgrooves on the inner surface are uniformly distributed circumferentially, so that each busbar is subjected to an approximately uniform periodic load during rotation.
[0012] This method utilizes a dual-scale boron nitride skeleton formed by radially oriented freezing, an axial concentration gradient, pressure-relief microgrooves that gradually deepen towards the buffer section, and segmented dimensional feedback after the first assembly to collectively define the thin-walled cylindrical bushing. The load-bearing section maintains a high boron nitride content and a shallow groove depth under the raceway projection, while the buffer section, with a higher polymer content, withstands end displacement and receives air or excess adhesive medium discharged from the microgrooves. The assembled outer diameters of the load-bearing and buffer sections are remeasured separately to ensure that the different radial recoveries caused by the material gradient are not masked by a single cross-sectional dimension. The free-size formula is only used to provide initial machining values; the final second interference is determined by... and They jointly released the vehicle.
[0013] The assembly release process further employs a two-level judgment: after the first interference fit is completed and temperature equilibrium is achieved, the installed outer diameters of the load-bearing section and the buffer section are measured simultaneously. The second press fitting is performed only when the actual second diameter interference of the load-bearing section falls within the predetermined window and the outer diameter of the load-bearing section is not less than the outer diameter of the buffer section. If either condition is not met, the assembly is adjusted by selecting appropriate parts or allowing the machined surfaces to be trimmed. The dimensional feedback is not replaced by increasing the press fitting load. Attached Figure Description
[0014] Figure 1 This is a cross-sectional view of the composite bushing motor bearing assembly.
[0015] Figure 2 This is a diagram of a two-scale boron nitride thermally conductive and insulating network.
[0016] Figure 3 This is a radial double interference fit assembly drawing for the shaft, bushing, and bearing inner ring.
[0017] Figure 4 This is a longitudinal section assembly drawing of the bearing location.
[0018] Figure 5 This is a partial unfolded view of the pressure relief microchannel.
[0019] Figure 6 This is a diagram showing the axial functional zoning of the bushing.
[0020] Figure 7 The diagram shows the unfolded texture and sealing strip.
[0021] Figure 8 Exploded assembly drawing of end ring, sealing ring and end cap.
[0022] Figure 9 This is a diagram for shaft diameter compensation and assembly gauge inspection.
[0023] Figure 10 This is a comparison chart of measured thermal conductivity and insulation in the implementation method. Detailed Implementation
[0024] The preparation and assembly process is described below with reference to the accompanying drawings. The reference numerals are as follows: 1—Motor shaft, 2—Composite bushing, 3—Bearing inner ring, 4—Rolling element, 5—Bearing outer ring, 6—Motor end cover, 7—Micron-sized boron nitride, 8—Nano-sized boron nitride, 9—Polymer matrix, 10—Bearing section, 11—Gradual transition section, 12—Buffer section, 13—Pressure relief microgroove, 14—Continuous polymer matrix region, 15—Anti-rotation texture, 16—Sealing strip, 17—Insulating end ring, 18—Replaceable sealing ring, 19—Measuring gauge. The same reference numeral indicates the same component in different drawings.
[0025] like Figure 1As shown, the composite bushing 2 is located between the motor shaft 1 and the bearing inner ring 3. The bearing inner ring 3, rolling elements 4, and bearing outer ring 5 constitute the bearing. The motor end cover 6 provides a mounting stop on the outside of the bearing. The inner circle of the composite bushing 2 forms a first interference fit with the motor shaft 1, and the outer circle forms a second interference fit with the bearing inner ring 3. The insulating end rings 17 at both ends extend out of the end face of the bearing inner ring 3. The replaceable sealing ring 18 is fixed in the sealing groove of the motor end cover 6, and its sealing lip slides in contact with the outer circle of the rotating insulating end ring 17. The compression is limited by the end cover stop and the sealing groove.
[0026] like Figure 2 As shown, during directional freezing, the ice crystal growth front advances radially along the annular mold cavity, and plate-like or near-plate-like micron-sized boron nitride 7 is squeezed between adjacent frozen crystals; after sublimation, it leaves behind channels spanning the bushing wall thickness and overlapping boron nitride skeletons. Nano-sized boron nitride 8 is located at the junctions and gaps between adjacent micron-sized boron nitride 7. The vacuum-impregnated polymer matrix 9 fills the channels extending radially from the inner circle to the outer circle of the bushing and covers the skeleton. Boron nitride itself is an electrically insulating material, allowing adjacent particles to form thermal contact; the continuous polymer matrix 9 is used to maintain flexibility and prevent pores from penetrating from the inner circle to the outer circle.
[0027] Micron-sized boron nitride 7 overlaps to form a thermally conductive skeleton, and the heat transfer of the thermally conductive skeleton proceeds along the bushing wall thickness direction; the polymer matrix 9 continuously covers the skeleton and blocks the current path, thus achieving both thermal conductivity and electrical insulation effects on the same cross section.
[0028] Filler pretreatment may include vacuum drying and coupling modification. Micron-sized boron nitride 7 with an average particle size of 10 μm and nano-sized boron nitride 8 with an average particle size of 100 nm are mixed at a mass ratio of 3:1. The amount of coupling agent is controlled at 1%–2% of the mass of the mixed filler. Hydrolysis, stirring, filtration, and drying are then performed. The modified filler is added to a freezing medium containing 1%–3% water-soluble temporary binder and degassed to form a dispersion for the annular mold cavity. The freezing medium is removed after sublimation. The temporary binder only maintains the shape of the porous boron nitride preform before subsequent vacuum impregnation and does not replace the final polymer matrix 9.
[0029] Figure 3 The radial structure and diameter dimensions are shown. The motor shaft 1, composite bushing 2, and bearing inner ring 3 are coaxially arranged. The first diameter interference fit is shown. It is equal to the difference between the diameter of the section of the motor shaft to be fitted and the diameter of the inner hole of the bushing in its free state; This is equal to the difference between the outer diameter of the bushing in its free state and the inner diameter of the bearing inner ring, and is only the initial dimensional verification value. After the first assembly and achieving temperature equilibrium, measurements are taken at the specified measurement sections of the load-bearing section 10 and the buffer section 12. and ,by With bearing inner ring inner diameter The difference determines the actual second diameter interference. and check Is it not less than Each interference fit is defined according to the diameter difference and is not to be confused with the unilateral radial compression.
[0030] Figure 4 The axial position of the composite bushing 2 passing through the inner ring 3 of the bearing is shown. The load-bearing section corresponds to the load-bearing area of the rolling element 4, and the insulating end ring 17 extends from both ends of the inner ring 3. The press-fitting tool acts on the end face of the inner ring 3 and the process end of the composite bushing 2, without transmitting the press-fitting force through the rolling element 4. After completing the second interference fit, the position of the bearing end face relative to the shoulder of the motor shaft 1 is remeasured.
[0031] like Figure 5 As shown, multiple pressure-relief microgrooves 13 extend axially along the composite bushing 2 and are distributed at equal angles circumferentially, with continuous bearing bands maintained between each pressure-relief microgroove 13. The pressure-relief microgrooves 13 do not penetrate the bushing wall; their closed ends are located in the bearing section 10, and their groove depth is 3%–6% of the wall thickness. The groove depth gradually increases through the transition section 11, and opens at a depth of 10%–15% of the wall thickness on the pressing-out side end face of the buffer section 12. A continuous polymer matrix region 14 is maintained at the bottom of the groove. This region may contain boron nitride particles completely coated with polymer, but does not contain pores extending from the bottom of the groove to the outer circumference of the bushing; therefore, it is not an additional pure polymer film. When using assisted bonding, the pressing direction is from the bearing section to the buffer section, allowing air and excess adhesive to be discharged along the pressure-relief microgrooves 13.
[0032] Figure 6 The diagram shows the load-bearing section 10, the gradual transition section 11, and the buffer section 12. The load-bearing section 10 corresponds to the bearing raceway projection area, with a boron nitride volume fraction of 50%–60%. The buffer section 12 is located near the shaft shoulder or the thermal displacement release end, with a boron nitride volume fraction of 35%–45%, and a correspondingly higher polymer ratio. The gradual transition section 11 is formed by at least three axially adjacent dispersion zones, causing the boron nitride volume fraction to decrease gradually from the load-bearing section to the buffer section. The dispersions are connected before freezing and are subsequently penetrated by the same radial freezing front, so the boron nitride skeletons of adjacent zones overlap at the interface without metal spacers or prefabricated splicing surfaces.
[0033] like Figure 7 As shown, the anti-rotation texture 15 is located in the middle of the outer periphery of the composite bushing 2, with continuous sealing strips 16 on both sides. The anti-rotation texture 15 can be staggered shallow grooves or dot matrix protrusions, with a depth not exceeding one-third of the bushing wall thickness. The outer circle of the sealing strip 16 is continuous, forming an annular contact strip with the bearing inner ring 3 after press fitting. The anti-rotation texture 15 does not extend to the insulating end ring 17 to avoid forming a tear initiation point at the end.
[0034] like Figure 8As shown, the assembly direction consists of, in sequence, a motor shaft 1 with a composite bushing 2, an insulating end ring 17, a replaceable sealing ring 18, and a motor end cover 6. The replaceable sealing ring 18 is fixed within the sealing groove of the motor end cover 6, and the sealing lip forms a rotary sliding seal with the outer circumference of the insulating end ring 17. When replacing the sealing ring 18, the bearing inner ring 3 and the composite bushing 2 are not moved, thus avoiding disruption of the established two-stage interference fit. A gap is maintained between the insulating end ring 17 and the rigid surface of the motor end cover 6, with only the sealing lip contacting the insulating end ring 17.
[0035] Figure 9 The initial shaft diameter compensation and segmented measurement gauge 19 are shown. First, the actual inner diameter of the bearing inner ring 3 and the wall thickness of the composite bushing 2 after molding are measured. Then according to the target and nominal Calculate the reduction in shaft diameter The machined section to be fitted is positioned using the metal reference sections at both ends; after the first interference fit is completed and temperature equalization is achieved, measuring gauge 19 checks the load-bearing section 10 and the buffer section 12 respectively. and Based on this, it is determined And exclude the high point of the outer circle of the buffer section. The positioning surface of the gauge spans across the adjacent continuous bearing strip without pressing into the pressure relief micro-groove 13, so as to avoid misjudgment caused by local deformation of the flexibility.
[0036] In one embodiment of the silicone rubber, the mass ratio of micron-sized to nano-sized boron nitride is 3:1. The target volume fractions of the supporting section 10 and the buffer section 12 are 55% and 40%, respectively, and the gradient transition section 11 is provided with three dispersion zones of 50%, 47%, and 44% in sequence. The outer mold wall of the annular mold cavity is maintained. 25℃ to At 15℃, the mandrel is maintained at 0℃ to 5℃, and the freezing front advances radially from the outside to the inside. After complete freezing, it is sublimated and dried at a pressure not exceeding 20 Pa to obtain a porous preform with channels extending radially from the inner circle to the outer circle of the bushing. Addition-type liquid silicone rubber is immersed in the preform under an absolute pressure not exceeding 20 kPa, and after returning to normal pressure, it is pre-cured at 80℃ and then cured at 150℃. The measured inner diameter of the bearing inner ring 3 is... The radial wall thickness of composite bushing 2 is 40.000 mm. The first interference is 0.800mm. Set to 0.050mm, nominal second interference. If we set it to 0.040mm, then the initial shaft diameter reduction is... The diameter of the section of the motor shaft to be fitted is 1.510mm. The measurement is 38.490mm. This set of dimensions is only for initial machining; actual measurements are required after the first assembly. and No predetermined release result.
[0037] In one polyimide embodiment, a porous boron nitride preform is formed using the same radially oriented freezing step as described above, followed by vacuum impregnation with a polyamic acid solution. After the preform is restored to atmospheric pressure and allowed to stand to remove bubbles, it is sequentially heated at 80°C, 150°C, and 250°C to complete solvent removal and thermal imidization; each heating is performed under the condition that the mass change tends to stabilize, to avoid the formation of through-pores in the thin-walled cylindrical bushing by the internal solvent. The first interference fit is completed by cooling the motor shaft and expanding the bushing inlet with a tapered guide, and the second interference fit is performed by press-fitting at a uniform speed using a press; the direction of both assembly processes is from the bearing section 10 to the buffer section 12.
[0038] In another silicone rubber embodiment, the composite bushing 2 has a total wall thickness of 1.0 mm, the boron nitride volume fraction of the bearing section 10 is 60%, the boron nitride volume fraction of the buffer section 12 is 45%, and the gradient transition section 11 transitions between the two in four stages. After freeze-drying, a low-viscosity silicone rubber precursor is first dripped onto the inner circle side of the preform, then a vacuum is drawn and material is added from the outer circle side; if unimpregnated pores appear in the cross-section, the pressure holding time is extended instead of masking the pores by increasing the boron nitride concentration. After curing, the outer circle is first refined based on the inner hole, and then gradually deepened pressure relief microgrooves 13 are machined.
[0039] In another embodiment, the freezing rate of the bearing section 10 is lower than that of the buffer section 12, so that the bearing section forms smaller and denser radially extending channels from the inner circle side of the bushing to the outer circle side, while the buffer section forms a larger polymer-filled area. Pressure-relief microgrooves 13 are uniformly arranged circumferentially on the inner circle of the bushing, and anti-rotation textures 15 are provided on the outer circle, with sealing strips 16 retained at both ends. Dimensions are calculated based on the free state before assembly. and After the first assembly, retesting was performed separately. and If any condition is not met, the correction should be made by regrouping or adjusting the permissible machined surface, without forcibly compensating by increasing the press load.
[0040] Two comparative examples were tested under the same conditions. Comparative example one used a single-size filler without axial partitioning, with an equivalent thermal conductivity of 1.0 W / (m·K) and an insulation strength of 17.5 kV / mm along the wall thickness direction; comparative example two used a polymer bushing without boron nitride filler, with an equivalent thermal conductivity of 0.2 W / (m·K) and an insulation strength of 25 kV / mm along the wall thickness direction. Figure 10 The data are listed in the order of Embodiments 1 to 4, Comparative Example 1, and Comparative Example 2. Each group of thermally conductive samples was taken radially from the same batch of bushings, with the heat flow direction consistent with the actual heat transfer direction from the bearing inner ring to the motor shaft.
[0041] Finished product inspection involves sequential testing of dimensions, insulation, compression force, and thermal cycling. Dimensional inspection uses... Figure 9The measurement gauge 19 is shown; the insulation test applies a specified test voltage between the motor shaft 1 and the bearing inner ring 3; the pressure test is used to confirm that there is no slippage at the first and second interference interfaces; the insulation resistance and bearing starting torque are measured again after thermal cycling. If the insulation decreases but the pressure is normal, the impregnation pores or the continuous polymer matrix region 14 at the bottom of the tank should be checked; if the pressure decreases but the insulation is normal, the interference and the permanent compression deformation of the buffer section 12 should be checked.
[0042] The composite bushing 2 rotates with the motor shaft 1 and the inner ring of the bearing 3, thus preventing the load area in a fixed spatial direction from being solidified into a certain circumferential material area of the bushing. The pressure relief micro-grooves 13 are distributed at equal angles along the circumference, and the contact pressure is shared by the adjacent continuous bearing strip when any generatrix passes through the load area; the material concentration change is only set along the axial direction between the bearing section 10, the gradual transition section 11 and the buffer section 12.
[0043] During maintenance, first remove the replaceable seal ring 18 and the motor end cover 6, then axially remove the bearing inner ring 3 and the old composite bushing 2. After cleaning the motor shaft 1, remeasure the reference diameter, and do not use the pressing depth of the old bushing as the size of the new part. After the new bushing is assembled, confirm that the insulating end ring 17 does not block the lubrication channel and that the sealing strip 16 is not cut by the anti-rotation texture 15.
[0044] The silicone rubber bushing of Example 1 was prepared in the following order: Micron-sized boron nitride 7 and nano-sized boron nitride 8 were vacuum dried at 120°C for 4 h, cooled, and then sealed and transferred. A silane coupling agent was added to an ethanol-water mixture for hydrolysis, followed by the addition of the two types of boron nitride and stirring at 80°C for 2 h. The filtered packing was washed until the filtrate was nearly neutral and then vacuum dried again. The treated boron nitride was formulated into defoamed dispersions according to the target solid phase amounts for the supporting section 10, the gradual transition section 11, and the buffer section 12. The dispersions were axially connected within the annular mold cavity without any spacers.
[0045] The outer mold wall of the annular mold cavity contacts the cooling plate, and a high-temperature circulating medium is introduced into the core mold, establishing a radial freezing front from the outside in. Nucleation is first achieved on one side of the bearing section 10, and then all axial sections are advanced synchronously to prevent a single axial interface from freezing completely first and forming a flat layer. After complete freezing, the entire assembly is transferred to a freeze-drying device, and sublimation is completed when the mass change does not exceed 0.2% in two consecutive steps. The resulting porous boron nitride preform is first subjected to X-ray tomography; only when the pores extending radially from the inner circle to the outer circle of the bushing are distributed between the inner and outer circles and there are no continuous cracks at the axial proportioning interface, is polymer impregnation allowed.
[0046] During polymer impregnation, a porous boron nitride preform is placed in a sealed container. After pumping to an absolute pressure not exceeding 20 kPa, degassed addition-type liquid silicone rubber is slowly introduced from the bottom of the container, allowing the liquid level to rise over the preform. After pressure holding, atmospheric pressure is restored, and the pressure difference is used to force the precursor into the remaining channels. During pre-curing, a mandrel penetrating the inner hole is used to maintain axial continuity. After curing, the preform is left at room temperature until its dimensions stabilize, and then the outer diameter is machined using the inner hole as a reference. The machining tool uses a large rake angle and a continuous support sleeve to prevent elliptical deformation of the thin-walled cylindrical bushing due to cutting forces.
[0047] The supporting section 10, the gradual transition section 11, and the buffer section 12 are formed within the same annular mold cavity by boron nitride dispersions of different solid concentrations. The target volume fraction of the supporting section is 55%, the buffer section is 40%, and the gradual transition section transitions sequentially from three ratios of 50%, 47%, and 44%. Adjacent dispersions remain in contact until the freezing front is reached, allowing micron-sized boron nitride 7 to overlap across the mixing interface; subsequent polymer precursors enter each section from the same impregnation system, avoiding the formation of adhesive seams between independent sleeves.
[0048] If the annular mold cavity is long, three adjacent injection ports can be used to feed material into the bearing section 10, the gradual transition section 11, and the buffer section 12 respectively. After injection, low-amplitude axial vibration should be used to eliminate air bubbles at the interface of the dispersion. Radial freezing should be started after the vibration stops. The three independent annular segments cannot be frozen first and then bonded with polymer, because this method cannot obtain a continuous boron nitride skeleton across the axial proportioning interface.
[0049] The pressure relief microgroove 13 is cut out using a round-head cutter after the inner circle is precision machined. The cutter starts from the closed end within the bearing section 10, feeds axially through the gradual transition section 11 to the buffer section 12, and the groove depth gradually increases by CNC radial feed; the open end is located on the extrusion side end face of the buffer section. The groove depth is scanned axially by a profilometer with a round head, and the measuring probe does not press into the flexible material. For a bushing with a wall thickness of 0.8 mm, the groove depth at the closed end is 0.024 mm to 0.048 mm, and the groove depth at the open end is 0.080 mm to 0.120 mm, with a continuous polymer matrix region 14 retained at the bottom of the groove.
[0050] The continuous polymer matrix region 14 can be inspected using both cross-sectional microscopic observation and electrical scanning. First, a radial section is cut from the process residue impregnated in the same batch as the finished product. The presence of through-holes at the bottom of the tank is observed, and it is confirmed that all visible boron nitride particles are surrounded by the polymer phase; a particle-free pure polymer film at the bottom is not required. Then, a micro-probe is used to scan the local resistance along the outer side of the tank bottom. Microscopic observation is used to detect geometric defects, and electrical scanning is used to detect through-paths invisible to the naked eye. Only after both are deemed satisfactory is it permissible to machine pressure-relief micro-grooves 13 with the same parameters as the finished product into the inner circle.
[0051] The anti-rotation texture 15 uses staggered shallow herringbone grooves, with a groove depth of 8% of the bushing wall thickness and the included angle facing the pressing direction. A 3mm wide sealing strip 16 is retained on each side of the texture. When machining the anti-rotation texture 15, the bushing is fitted onto the support mandrel, with the mandrel's outer diameter slightly smaller than the bushing's inner diameter to limit cutting deformation. After the texture is completed, the flanging is removed with a flexible brush; flame treatment, which would melt the polymer, is not used.
[0052] The insulating end ring 17 is integrally formed with the cylindrical wall of the composite bushing 2. The outer diameter of the end ring is smaller than the inner diameter of the stop of the motor end cover 6 to avoid rotational interference; the axial extension of the end ring is greater than the axial projection of the chamfer on the end face of the bearing inner ring 3, so that the shortest creepage path from the shaft side to the bearing side does not pass through the end face metal. The root of the end ring adopts a rounded transition, and no anti-rotation texture 15 or pressure relief micro-groove 13 is provided at the rounded corner.
[0053] The replaceable sealing ring 18 is made of fluororubber or oil-resistant silicone rubber compatible with the lubricating medium. The outer circle of the sealing ring 18 is fixed in the sealing groove of the motor end cover 6, and the inner sealing lip slides in contact with the outer circle of the rotating insulating end ring 17. The sealing ring 18 does not bear the bearing positioning load; its radial compression is only used to prevent grease from migrating along the end face of the composite bushing 2. When removing the sealing ring 18, first remove it from the motor end cover 6 to avoid scratching the insulating end ring 17.
[0054] First diameter interference fit And the actual second diameter interference The values are determined based on the segmented compression modulus of the composite bushing. Used to prevent composite bushing 2 from rotating relative to motor shaft 1 Used to transmit radial load on the inner ring 3 of the bearing. If both are taken as the upper limit of the window, the flexible bushing may experience excessive radial compression; therefore, the respective windows are first calculated back from the target contact pressure, and then the first assembled window is used as the upper limit of the window. confirm and with Not greater than Exclude the high point on the outer circle of the buffer section.
[0055] Taking a bearing inner ring inner diameter of 40.000 mm and a bushing radial wall thickness of 0.800 mm as an example, if the first diameter interference... Take 0.050mm, nominal second diameter interference. Taking 0.040mm, the initial shaft diameter reduction is 1.510mm, the target diameter of the section to be fitted is 38.490mm, and the bushing's free-state inner diameter is 38.440mm and outer diameter is 40.040mm. These values are only used to verify the initial machining dimensions; the actual interference fit for the second diameter is still based on the first assembly. The measured values were determined and then verified separately. .
[0056] The measuring gauge 19 has positioning holes that mate with the metal reference sections at both ends of the motor shaft 1, a go / no-go gauge surface for detecting the section to be mated, and an end face step for detecting the position of the insulating end ring 17. The coefficient of thermal expansion of the gauge material and the calibration environment are recorded in the inspection card. Before measurement, the motor shaft 1 and the gauge are placed in the same temperature environment for a sufficient time to avoid misjudgment of the thin-walled dimensional chain due to temperature differences.
[0057] The first interference fit can be achieved by room temperature press fitting, bushing heating, or motor shaft 1 cooling. Silicone rubber bushings are preferably fitted at room temperature, while polyimide bushings can be fitted using temperature difference assembly. During temperature difference assembly, the cooling temperature should not be lower than the material's embrittlement temperature, and the heating temperature should not exceed the polymer's long-term allowable temperature. After assembly, allow the material to return to room temperature naturally; localized flame heating to accelerate resetting is not required.
[0058] The second interference fit is completed using a press with a coaxial guide sleeve. The guide sleeve is first fitted onto the outside of the insulating end ring 17, and the bearing inner ring 3 enters the composite bushing 2 along the guide sleeve. Press-fit load and displacement are collected simultaneously; a sudden drop in the curve may indicate bushing slippage, and a sharp peak may indicate end face scraping or local particle agglomeration. Assemblies with abnormal curves are disassembled and inspected, and are not put into place by continuing to apply pressure.
[0059] When using assisted bonding, a continuous thin film is applied only to the inner surface of the composite bushing 2, excluding the pressure relief microgrooves 13. The adhesive layer thickness is included. The equivalent assembly compression amount cannot be added separately after shaft diameter compensation. During the pressing process, excess adhesive is discharged through the pressure relief micro-groove 13, and residual adhesive at the ends is wiped off before curing. After the adhesive has cured, it must not block the assembly position of the insulating end ring 17 and the sealing ring 18.
[0060] In Example 2, the polyimide bushing was prepared using a dispersion of micron-sized boron nitride 7 and nano-sized boron nitride 8 at a mass ratio of 3:1. The target volume fractions for the support section 10 and the buffer section 12 were 55% and 40%, respectively. After freeze-drying to obtain a porous preform, it was vacuum impregnated with a polyamic acid solution and imidized in stages under mandrel support. The temperature changes between each zone were determined by mass variation and exhaust gas concentration to prevent residual solvent from forming pores within the bushing.
[0061] In the polyimide example, the reference diameter of motor shaft 1 is 60 mm, and the wall thickness of composite bushing 2 is 0.5 mm. The inner and outer diameters after imidization are first measured, and then... and During assembly, cool the motor shaft 1, or expand the inlet of the bearing section of the composite bushing 2 with a tapered guide at a temperature that will not damage the bushing, and then install the composite bushing 2 onto the shaft; allow the temperature to return to room temperature and retest each time. and After both conditions are met, press-fit the inner ring of the bearing.
[0062] Example 3 employs a silicone rubber bushing with zoned freezing speed control. The freezing front speed of the load-bearing section 10 is lower than that of the buffer section 12, resulting in smaller and denser radially extending channels from the inner to the outer circumference of the bushing. The gradual transition section 11 gradually changes the heat flux density of the cooling plate along the axial direction, avoiding abrupt changes in channel size at a single cross-section. All three sections use the same batch of addition-cured liquid silicone rubber for vacuum impregnation and curing.
[0063] The different axial regions are not separate independent sleeves, but rather a continuous boron nitride skeleton formed by the same freezing front and connected by the same polymer precursor. After sampling, thermal cycling and axial stretching are performed; if the fracture location is concentrated along the ratio boundary, the length of the gradient transition section 11 is increased, the difference between adjacent ratios is reduced, or the freezing rate change rate is decreased.
[0064] Example 4 employs a replaceable segmented annular mold core to improve batch consistency. The mold core retains a forming allowance at the insulating end ring 17 position, undergoes freeze-drying and vacuum impregnation, and is then finished using the inner hole as a reference. X-ray tomography is used to screen out unimpregnated channels, followed by machining of pressure relief microgrooves 13, anti-rotation textures 15, and sealing strips 16. This example still performs segmented outer diameter re-measurement of the load-bearing and buffer sections.
[0065] Figure 10 The six sets of thermal conductivity and insulation strength values from the original disclosure are retained as baselines for material formulation screening. The original disclosure did not fully provide the directional freezing direction, the number of samples per set, and the statistical rules; therefore, these values are not considered as the measured results for the radial boron nitride skeleton, asymptotic microgrooves, and segmented outer diameter feedback combination in this application. For the witness specimens of this application, measurements should be re-measured along the bushing wall thickness direction under the same sample thickness and temperature, and the number of samples and the dispersion range should be recorded.
[0066] The original comparative example 1 used micron-sized boron nitride with a single particle size, and recorded a thermal conductivity of 1.0 W / (m·K) and an insulation strength of 17.5 kV / mm. This data did not form the current radially oriented frozen skeleton, nor did it have feedback on asymptotic microgrooves and segmented outer diameters. Therefore, it was only used to illustrate the need for further screening of material systems.
[0067] The original comparative example 2 used a similar polymer without boron nitride, and recorded an insulation strength of 25 kV / mm and a thermal conductivity of 0.2 W / (m·K). These values only indicate the thermal conductivity baseline of the pure polymer formulation in the original data and cannot be used to presuppose the bearing temperature rise or interference decay of the assembly in this application.
[0068] The temperature rise verification of the assembly in this application was conducted separately using the same bearing, load, speed, and cooling conditions, recording the temperatures at the bearing section 10 adjacent to the raceway and the inner side of the motor shaft 1. Only after cross-sectional tomographic scanning confirmed the completeness of the boron nitride skeleton and polymer impregnation extending radially from the inner to the outer circle of the bushing was the temperature difference change correlated with the structure of this application; it is not possible to... Figure 10 The material baseline is directly converted into the assembly temperature rise.
[0069] Durability verification includes press-fit / disassemble cycles and combined thermal shock tests. The number of cycles, temperature limits, and loads are specified in the protocol before testing. At each checkpoint, the inner and outer diameters of the composite bushing 2, insulation resistance, and the appearance of the end ring root are measured. The current specification does not predetermine the number of cycles required for the control part to peel off or for the bushing of this application to maintain the press-fit force.
[0070] In the combined thermal vibration test, the assembly was cycled between low temperature, room temperature, and high temperature, while a periodic force equivalent to the radial load of the motor was applied. The load-bearing section 10 is located in the main load zone, and the buffer section 12 is located on the shoulder side to absorb axial and radial micro-displacements. A control section without the gradual transition section 11 was set up to compare the proportioned boundary strain and cross-sectional cracks; after actual recording, it was determined whether the gradual transition section produced the aforementioned effect.
[0071] The sealing verification of the grease-containing assembly uses grease with a fluorescent tracer. After operation, the motor end cover 6 is removed, and the inner interface of the sealing strip 16, replaceable sealing ring 18, and composite bushing 2 is inspected under ultraviolet light. If the tracer stops at the outside of the sealing strip 16, the end barrier is effective; if it enters the pressure relief microgroove 13, the compression of the sealing ring and scratches on the surface of the insulating end ring 17 are checked.
[0072] The pressure relief effect of the microgrooves was observed using a transparent simulated bushing. Samples without pressure relief microgrooves may develop sealed air bubbles during press-fitting, causing the ends to momentarily lift. Samples with gradually deepening pressure relief microgrooves 13 were used to observe whether gas was discharged towards the end face of the buffer section 12. The depth of the closed end groove was controlled at 3%–6% of the wall thickness, and the depth of the open end groove did not exceed 15% of the wall thickness, while retaining a continuous polymer matrix region 14. Actual comparative results were used to demonstrate the pressure relief effect, without pre-setting experimental conclusions.
[0073] The anti-rotation effect was evaluated by repeated torque tests. Angular markings were set on the composite bushing 2 and the bearing inner ring 3, and the relative angular displacement was measured after applying a specified torque cycle. The sample with the anti-rotation texture 15 had a lower relative displacement than the sample without texture; the control sample with texture extending to the end was prone to cracking from the end edge after disassembly and assembly, therefore, this application retains sealing strips 16 on both sides of the texture and avoids the insulating end ring 17.
[0074] When the pressure relief microgrooves 13 are arranged at equal angles in the circumference, three to six microgrooves divide the inner circle of the bushing into continuous load-bearing zones of equal or approximately equal width. The width of the continuous load-bearing zone is greater than the width of the pressure relief microgrooves 13, and the groove depth is 5% to 15% of the wall thickness. This arrangement does not depend on the fixed direction of the external load and disperses the venting path during press-fitting on the circumference.
[0075] The composite bushing 2 does not have circumferential material partitions corresponding to the fixed load direction of the motor end cover 6. Only the process end face of the insulating end ring 17 has an axial identification mark to distinguish between the press-in and discharge ends. This mark does not enter the creepage path and is not used to define the load-bearing direction of any circumferential busbar. After assembly, the pressure relief microgrooves 13 are still distributed at equal angles along the circumference.
[0076] Raw material batch inspection includes particle size distribution, moisture content, weight gain from coupling agent treatment, and polymer melt or vulcanization characteristics. Process inspection includes mixing torque, billet quality, molding shrinkage, wall thickness, roundness, and groove depth. Finished product inspection includes two interference fits, press-fit profile, insulation resistance, thermal conductivity sampling, and end sealing. All data are linked to the product number of composite bushing 2 for traceability to the material and processing stages in case of failure.
[0077] The filler particle size is distributed in two stages, rather than requiring all particles to be strictly equal to 10 μm or 100 nm. Micron-sized particles can be distributed within a range where they can bridge each other, while nano-sized particles are designed to enter the gaps between micron-sized particles. A mass ratio of 2:1 to 4:1 is used to achieve a balance between the number of skeleton particles and the number of gap fillers; if this range is exceeded, its applicability should be reassessed through thermal conductivity, insulation, and bending tests.
[0078] When the volume fraction of the composite filler is below 40%, it is difficult to form a sufficiently continuous heat transfer path between the micron-sized boron nitride 7 particles; when it is above 60%, the continuity and molding fluidity of the polymer matrix 9 decrease significantly. The range of 40%–60% is used in conjunction with a dual-scale gradation. If high aspect ratio sheet particles are used, a heat conduction path can be obtained in the lower part of this range, but it is still necessary to check whether the sheet orientation leads to insufficient radial heat conduction.
[0079] The higher filler ratio in the load-bearing section 10 reduces the thermal resistance in the raceway load zone and improves dimensional stability under pressure; the higher polymer ratio in the buffer section 12 accommodates thermal displacement and assembly deviations near the shoulder. The gradual transition section 11 disperses the modulus changes of both sections over a certain length, avoiding shear peaks at a single cross-section. The insulating phases of all three sections are continuously connected by the same or compatible polymers.
[0080] When composite bushing 2 is used in an oil-cooled motor, the material sample is first immersed in the actual cooling oil and kept at the highest operating temperature for a specified time. Then, the mass change, dimensional recovery, and insulation strength are measured. If the material absorbs oil and the dimensional change exceeds the interference tolerance, it is not used even if the initial thermal conductivity is good. The compatibility of replaceable sealing ring 18 is verified using the same method.
[0081] When composite bushing 2 is used in a high-speed motor, perform a low-speed frequency sweep after assembly to check the starting torque, steady-state torque, and vibration. If a recurring peak occurs at a certain speed, first check the roundness of composite bushing 2 and the uniformity of the two interference fits, and then perform rotor balancing. Dynamic balance must not be corrected by removing material from the insulating end ring 17 or the load-bearing section 10, as this may damage the insulation path.
[0082] When the bearing needs replacement but the composite bushing 2 is still usable, first measure its outer diameter springback and compression force. If the outer diameter returns to normal, the inner interface does not slip, and the insulation resistance is qualified, only the bearing needs to be replaced; if the second interference fit decreases due to repeated disassembly and assembly, the bushing should be replaced at the same time. The replaceable seal 18 should be judged separately based on its appearance and compression set, regardless of whether the bushing continues to be used.
[0083] When repairing bushing 2, do not locally fill the already formed thin-walled area with high-concentration boron nitride adhesive, as sudden changes in local proportions will cause stress concentration. Minor burrs can be polished, and blockages in the pressure relief microgroove 13 can be cleaned with non-metallic tools; if through cracks, end ring root cracks, or through channels formed by pores are found, the entire part should be scrapped and remade.
[0084] The continuous thermally conductive and insulating network referred to in this application means that boron nitride particles form contact or near-contact paths across the target heat transfer direction within the polymer, while the polymer phase maintains a non-penetrating short circuit between the motor shaft 1 and the bearing inner ring 3 without any through-hole metal or conductive filler. Thermal continuity and electrical insulation continuity are verified through thermal and electrical performance tests, respectively, and cannot be inferred solely from micrographs.
[0085] The term "gradual connection" as used in this application includes continuous variation of filler volume fraction along the axial direction, as well as approximation of a stepped structure composed of multiple adjacent small gradient zones; adjacent small gradient zones are co-molded using the same or compatible polymers, without the use of metal connectors. The pressure relief microgrooves are uniformly arranged circumferentially, and their angular positions are not determined by the load direction in a static coordinate system.
[0086] The term "maintaining the bearing inner ring assembly reference" as used in this application refers to the measured outer diameter after the composite bushing 2 and the compensated motor shaft 1 have completed their first assembly. The axial position meets the positioning requirements of the bearing inner ring 3. This statement does not require all motors to use the same nominal diameter, but rather requires the wall thickness, , and The retests then enter the dimensional control process.
[0087] The bushing forming mold consists of an inner core, an outer mold, and two end inserts. The inner core defines the axial through hole, the outer mold defines the outer diameter to be machined, and the end inserts form the blank of the insulating end ring 17. The feed port corresponding to the bearing section 10 is close to the bearing raceway projection area, and the feed port corresponding to the buffer section 12 is close to the shaft shoulder end. When feeding multiple proportions, the switching is controlled according to the order of buffer material, transition material, and bearing material to reduce the stagnation of high-filler material flow at the buffer end.
[0088] The mold temperature is controlled in zones along the axial direction. The temperature on the bearing section 10 side is kept higher to improve the filling of the high-filler mixture, while the temperature on the buffer section 12 side is slightly lower to limit excessive shrinkage. After demolding, the outer diameter and wall thickness of the three axial sections are measured; if shrinkage at the bearing end causes the wall thickness to exceed the tolerance, it is corrected by adjusting the local mold temperature and holding time, without changing the determined boron nitride ratio to compensate for the dimensions.
[0089] During directional freezing molding, the amount of dispersed liquid solid phase in the load-bearing section 10, the gradual transition section 11, and the buffer section 12 is controlled through three adjacent injection ports. The control system records the batch, quality, and axial boundary position of each injection port, as well as the temperature curves of the outer mold wall and the core mold over time. Process allowance marks are retained at the ends of the preform and the cured bushing, allowing for traceability to freezing and impregnation records from the end face batch code after the finished product has been machined.
[0090] When segmented cooling plates are used for long bushings, the temperature profiles of adjacent cooling plates overlap at the interface, avoiding the formation of an axial unfrozen liquid layer. After complete freezing, the entire structure sublimates without splicing multiple independent preforms. The impregnation vessel is fed from the bottom and vented from the top; if atmospheric pressure is restored immediately, the polymer precursor may seal the outer pores, leaving a cavity in the inner layer. Therefore, pressure is restored in stages at a specified rate.
[0091] The same datum system is used for machining the inner circle, outer circle, and end face of the bushing. First, the outer circle is rough-machined using the inner circle process datum for positioning. Then, the inner circle is finish-machined using the outer circle support. Finally, the insulating end ring 17 and chamfer are machined in a soft-jaw fixture. The circular runout is measured after each datum change to avoid the superposition of eccentricities from multiple processes in the two-stage interference fit.
[0092] The force applied during dimensional measurement of flexible materials can affect the readings. A low-force pneumatic gauge is used for the inner diameter, a constant-force probe for the outer diameter, and a thickness gauge with a large radius probe for the wall thickness. Measurement gauge 19 is used for functional dimension verification before and after assembly and cannot be replaced by ordinary high-clamping-force calipers. All measurements are noted with temperature and measuring force for comparison between different batches.
[0093] The distribution of the two interference fits also depends on the bearing load. For applications with high torque transmission requirements and low radial loads, the interference fit can be appropriately increased. and reduce For applications with high radial loads, it can improve... However, the circumferential stress of the bearing inner ring 3 is still checked. Any adjustment requires a back-calculation first. And initial shaft diameter compensation, then with The retest confirmed the actual second over-interference.
[0094] The contact pressure of the first interference fit can be calibrated by extrusion testing. Several different... The short bushing sample was press-fitted onto a test shaft of the same material as motor shaft 1, and the pressing force was measured at the same speed. The average interfacial shear capacity was calculated based on the contact area, and the working torque was selected accordingly. After the test, inspect the inner surface to rule out false high-pressure output caused by local scratches.
[0095] The second interference fit calibration uses an actual bearing inner ring 3 or a ring with the same stiffness. In addition to the pressure applied, the diameter change and roundness of the ring before and after assembly are also measured. If the size is too large, the inner ring 3 of the bearing may experience unacceptable swelling; If the pressure is too low, micro-movements may occur after thermal cycling. The determination should be based on a combination of factors: pressure, dimensions, and thermal cycling, rather than solely on whether the press-fitting process was successful.
[0096] The number of pressure relief micro-grooves 13 is set to three to six according to the bushing diameter and press-fit length, and they are distributed at equal angles along the inner circle of the composite bushing 2. The width of the continuous bearing band between each groove is greater than the groove width, and no pressure relief micro-groove 13 forms a cross cut that penetrates the wall thickness with the anti-rotation texture 15; even if the direction of the external load of the motor is fixed, the pressure relief micro-grooves are not concentrated in a certain circumferential arc area.
[0097] In the assembly using adhesive-assisted bonding, the total volume of the pressure relief microgroove 13 is larger than the expected volume of excess adhesive, and a collection ring groove is provided at the open end. The collection ring groove is located at the process end outside the insulating end ring 17 and can be removed after curing. In this way, excess adhesive will not accumulate on the end face of the bearing inner ring 3, nor will it shorten the creepage distance formed by the insulating end ring 17.
[0098] In assemblies that do not use adhesives, the pressure relief microgroove 13 can also accommodate a very small amount of assembly lubricant. The lubricant is applied only to the open end and is made of a material that is compatible with the polymer and the sealing ring 18 and is non-conductive after curing. Visible residues are removed after press fitting, and the insulation resistance is retested before thermal cycling to prevent lubricant from migrating along the microgroove and forming a contamination film.
[0099] The creepage distance of the insulating end ring 17 is determined based on the operating voltage and pollution level. The creepage path extends from the metal surface of the motor shaft 1, around the outer surface of the end ring, to the end face of the bearing inner ring 3, without considering the seal ring 18 as a permanent insulating wall. The seal ring 18 primarily blocks the lubricating medium; even if temporarily removed during maintenance, the insulating end ring 17 should still provide a basic electrical clearance.
[0100] The sealing groove of the motor end cover 6 provides static fixation to the outer circle of the sealing ring 18, and the sealing lip applies slight radial compression to the outer circle of the insulating end ring 17, without transmitting the bearing positioning force to the insulating end ring 17. After the end cover is tightened, manually rotate the motor shaft 1 and check whether the sealing lip contact is continuous; if the starting torque is abnormal, adjust the sealing ring specifications or sealing groove dimensions, without machining the insulating end ring 17 that has already been inspected.
[0101] The heat conduction path extends from the inner ring 3 of the bearing through the composite bushing 2 to the motor shaft 1. Micron-sized boron nitride 7 provides a long-distance skeleton, nano-sized boron nitride 8 reduces inter-plate thermal resistance, and the polymer matrix 9 connects the particles and supports flexible deformation. The higher filler ratio of the load-bearing section 10 coincides with the raceway load area, resulting in lower thermal resistance at the main heat-generating locations; the buffer section 12 retains deformation space on the shaft shoulder side.
[0102] Boron nitride itself is an electrically insulating material, but unimpregnated channels may adsorb conductive contaminants; therefore, the polymer matrix 9 is still required to be continuous between the inner and outer surfaces. The continuous polymer matrix region 14 at the bottom of the tank, the sealing strips 16 on both sides, and the insulating end rings 17 respectively protect the radial, outer peripheral, and end insulating boundaries; the boron nitride skeleton extending radially from the inner circle to the outer circle of the bushing is used for thermal conduction and is not described as a conductive network.
[0103] The flexibility of composite bushing 2 is characterized by compressive modulus, elongation at break, and compression set. For the load-bearing section 10, compressive modulus and creep are prioritized for verification; for the buffer section 12, elongation at break and compression set are prioritized for verification. When sampling the gradual transition section 11 is difficult, a strip specimen encompassing the entire transition zone can be subjected to bending and thermal cycling, with the absence of interface cracks serving as the acceptance criterion.
[0104] Before the thermal conductivity test, the sample surface was ground parallel and the actual thickness was measured. The insulation strength test used a step-by-step voltage increase and the breakdown location was recorded; if the breakdown occurred at the electrode edge, the result was not used to evaluate the internal properties of the material. Figure 10 The data comes from samples with effective breakdown located in the center region of the specimen, ensuring consistent comparison conditions for different formulations.
[0105] In the insulation resistance test of the finished product, the motor shaft 1 serves as the first electrode, and the inner ring 3 of the bearing and the outer ring 5 of the bearing are short-circuited to serve as the second electrode. The motor end cover 6 is kept at the same potential as the second electrode. The surface of the replaceable sealing ring 18 is kept clean and dry. After the test, the material is fully discharged before performing a pressure or torque test to avoid residual charge affecting operational safety.
[0106] The bearing operation test used the same grease fill amount and the same preload. A temperature sensor was placed at a fixed position near the raceway of the bearing inner ring 3, and another sensor was placed inside the section of the motor shaft 1 to be fitted. The temperature difference between the two points reflects the heat transfer state of the composite bushing 2; recording only the shell temperature may be influenced by differences in cooling conditions and cannot directly evaluate the bushing's heat conduction network.
[0107] For samples with abnormal temperature rise, first check The corresponding assembly outer diameter and roundness are checked, and the boron nitride network is inspected using ultrasound or cross-sectional sampling. Second, localized insufficient interference will increase interfacial contact thermal resistance, resulting in higher temperature rise even if the material's thermal conductivity is acceptable; network agglomeration may cause simultaneous instability in localized thermal conductivity and insulation. Checking the interface and material separately can prevent incorrect adjustments to the filler ratio.
[0108] For samples with degraded insulation, inspect the sealing ring 18, sealing strip 16, continuous polymer matrix area 14 at the bottom of the groove, unimpregnated channels, and localized agglomeration of the boron nitride skeleton in sequence. Contamination at the seals can usually be cleaned and restored; defects at the bottom of the groove or through-holes cannot be repaired by surface cleaning. The inspection sequence should proceed from removable components to the bushing body to minimize unnecessary destructive disassembly.
[0109] The batch assembly line divides motor shaft 1 into grades based on the actual shaft diameter and matches them with composite bushings 2 with corresponding inner diameters and wall thicknesses. After scanning the batch codes of the shafts and bushings at the workstation, the calculation for this part is performed first. , Shaft diameter compensation; data entry after completing the first assembly. And calculate If the pairing is not correct, prevent a second pressing; operators are not allowed to force assembly by using higher pressure.
[0110] Measuring gauge 19 is calibrated at the beginning and end of each shift using standard ring gauges and plug gauges. If the deviation between calibrations exceeds the limit, the products inspected in this shift are retested. The flexible contact head of the gauge is replaced periodically, and the measuring force is re-determined after replacement. This management prevents gauge wear from misjudging unqualified sections as qualified.
[0111] During storage and transportation, two composite bushings should be placed on the support core and sealed to protect them from light. High-filling thin-walled parts should not be scattered or stacked to avoid long-term elliptical deformation. Before assembly, after removing them from the packaging, allow them to recover in the workshop environment, and then measure the inner and outer diameters. If the dimensions do not recover, do not temporarily reshape them by heating or applying strong pressure, as this will prolong the adjustment time or result in scrapping.
[0112] All accompanying drawings in this application correspond to the objects to be inspected. Figure 1 and Figure 4 Used to verify the assembly and axial position. Figure 2 Used to inspect particle networks. Figure 3 and Figure 9 Used for calculating and measuring two-level interference. Figure 5 Used for inspecting the pressure relief micro-groove 13 Figure 6 Used to confirm material partitions Figure 7 Used for checking anti-rotation and sealing boundaries. Figure 8 Used for maintenance end components. Figure 10 Used to verify the source of performance data. Drawing numbers are not used as part numbers.
[0113] Shaft diameter compensation verification can be set up in two groups: one group determines the shaft diameter reduction based solely on the difference between the inner and outer diameters of the bushing in its free state, and the other group... Determine the initial machining values and remeasure them after the first assembly. Both groups recorded , , And two pressing forces; used to evaluate dimensional feedback is Deviation and second pressing force cannot be used to presume that the contact pressure after assembly is qualified solely based on the free state formula.
[0114] To verify the function of the gradual transition section 11, a control bushing was prepared with the load-bearing section 10 and the buffer section 12 directly butted together. The material ratios, total lengths, and wall thicknesses of the two sets were kept identical; the only difference was the presence or absence of a gradual transition. After a combined thermal shock test, higher local strain appeared near the material ratio boundary of the directly butted sample, while the strain of the gradually butted sample was dispersed axially. This result, along with cross-sectional observation, was used to select the length of the transition section, rather than relying on the appearance of a single bend to replace long-term verification.
[0115] To verify the function of the continuous polymer matrix region 14 at the bottom of the trench, comparative samples with the same number of trenches but different maximum trench depths were prepared, and local insulation was measured before and after damp heat treatment. This verification was used to determine the upper limit of gradually deepening the microgrooves 13; no set was preset to remain stable before actual recording was performed. Pressure relief capacity cannot be obtained by infinitely deepening the microgrooves; the polymer matrix region 14 at the bottom of the trench still serves as the radial insulation boundary.
[0116] If the motor uses two adjacent bearings, a composite bushing 2 can be installed at each bearing position, and a metal measurement reference section should be maintained between the two insulating end rings 17. The interference fit of the two bushings should be calculated according to the corresponding bearing loads, and should not be directly adopted just because the shaft diameters are the same. and After assembly, the insulation of each bearing to the motor shaft 1 was measured to prevent one pass from masking interface defects in another.
[0117] For hollow motor shafts, the wall thickness and circumferential stress should be checked during machining of the section to be fitted. When the shaft diameter compensation causes the shaft wall to become thinner, the dimensional chain can be recalculated by adjusting the bushing wall thickness and the two interference fits, or a temporary support core can be installed inside the hollow shaft before machining and press-fitting. The support core is removed after assembly and does not constitute a conductive bypass for the product.
[0118] For structures with stepped shoulders, buffer section 12 covers the area near the step fillet but does not extend to the minimum cross-section of the fillet. A release space is provided between the chamfer at the end of the composite bushing 2 and the shoulder fillet to prevent the press-fitted rear end face from being tightly pressed against it. Measuring gauge 19 incorporates a shoulder clearance groove, positioning it from the metal reference section without pressing against the flexible end face.
[0119] The above verifications correspond to four performance categories: thermal conductivity, insulation, stress, and dimensional chain. No single test result can prove the overall product's compliance: passing thermal conductivity requires two-stage interference fitting to ensure interface contact; passing dimensional chain fitting requires continuous polymer at the bottom of the tank; and passing insulation requires stable press-fitting of the load-bearing section. Through these independent tests, faults can be located at the material, structural, or assembly stages.
[0120] The above embodiments illustrate the radially oriented freezing, vacuum impregnation, and segmented assembly inspection of silicone rubber and polyimide systems. The shaft diameter, bushing length, polymer type, and boron nitride content can be adjusted according to load and temperature, but the following technical relationships should be maintained: a boron nitride skeleton extending radially from the inner to the outer circle of the bushing; an axial load-bearing-buffering gradient; pressure-relief microgrooves gradually deepening towards the buffer section; a continuous polymer matrix region at the bottom of the groove; and the re-measurement of the segmented outer diameters of the load-bearing and buffer sections.
Claims
1. A method for preparing a motor shaft current protection structure, characterized in that, include: A boron nitride dispersion region is formed by connecting the load-bearing section, the gradual transition section and the buffer section along the axial direction in an annular mold cavity with a radial temperature gradient. The volume fraction of boron nitride in the load-bearing section is higher than that in the buffer section. The freezing medium is removed by radial directional freezing and sublimation to obtain a porous boron nitride preform with channels extending radially from the inner circle side to the outer circle side of the bushing. A high-temperature resistant flexible polymer precursor is vacuum impregnated and cured into a thin-walled cylindrical bushing, so that micron-sized boron nitride forms a thermally conductive skeleton extending radially from the inner circle side to the outer circle side of the bushing, and nano-sized boron nitride is distributed therein and the skeleton is continuously coated with a polymer phase. Heat transfer from the thermally conductive skeleton is carried out along the bushing wall thickness direction. Multiple axial pressure relief microgrooves are formed on the inner surface of the bushing. The closed end of each pressure relief microgroove is located in the bearing section. The groove depth gradually increases from the buffer section through the gradual transition section and extends to the end face of the pressure-out side of the buffer section. The bottom of the groove retains a continuous polymer matrix area coated with boron nitride particles and without through holes. After the bushing is installed on the motor shaft, the outer diameters of the bearing section and the buffer section are measured respectively. Only when the outer diameter of the bearing section is not less than the outer diameter of the buffer section and the second interference fit falls into the target window, the bearing inner ring is pressed from the bearing section side to the buffer section side, so that the shaft and the bearing are electrically isolated and heat is transferred by the heat-conducting skeleton.
2. The method according to claim 1, characterized in that, The average particle size of micron-sized boron nitride is 10 μm, and the average particle size of nano-sized boron nitride is 100 nm. The mass ratio of the two is 3:1, and the volume fraction of the composite filler in the bushing is 50% to 55%.
3. The method according to claim 1, characterized in that, The high-temperature resistant flexible polymer precursor is addition-type liquid silicone rubber or a thermally imidizable polyamic acid solution. During vacuum impregnation, the absolute pressure of the mold cavity is kept not higher than 20 kPa, and the mixture is cured or imidized after returning to normal pressure.
4. The method according to claim 1, characterized in that, Let the inner diameter of the thin-walled cylindrical bushing in its free state be... The outer diameter is The inner diameter of the bearing inner ring before assembly is After compensation, the diameter of the section of the motor shaft to be fitted is The nominal inner diameter of the bearing inner ring is Radial wall thickness of thin-walled cylindrical bushing First diameter interference The nominal second diameter interference corresponding to the free size initial shaft diameter reduction ; After the thin-walled cylindrical bushing is fitted onto the motor shaft and reaches temperature equilibrium, and before the bearing inner ring is press-fitted, the outer diameters of the load-bearing section and the buffer section after assembly, measured under the same temperature and measuring force, are as follows: and Actual second diameter interference and satisfy , and .
5. The method according to claim 1, characterized in that, Three to six axial pressure relief microgrooves are evenly arranged along the circumference on the inner surface of the thin-walled cylindrical bushing. The groove depth at the closed end is 3% to 6% of the bushing wall thickness, and the groove depth at the open end is 10% to 15% of the bushing wall thickness. The width of the continuous bearing zone between adjacent pressure relief microgrooves is greater than the width of the pressure relief microgrooves, and an introductory chamfer is provided on one side of the bearing section.
6. The method according to claim 1, characterized in that, The boron nitride dispersions in the bearing section, the gradual transition section, and the buffer section are connected in the same annular mold cavity. The volume fraction of boron nitride in the bearing section is 50% to 60%, the volume fraction of boron nitride in the buffer section is 35% to 45%, and the volume fraction of boron nitride in the gradual transition section is gradually reduced from the bearing section to the buffer section by at least three axially adjacent regions. After directional freezing, the micron-sized boron nitride frameworks in adjacent regions overlap each other.
7. The method according to claim 1, characterized in that, An anti-rotation texture is formed on the outer periphery of the thin-walled cylindrical bushing, which is opposite to the inner ring of the bearing, and a textureless sealing strip is retained on both sides of the anti-rotation texture.
8. A motor shaft current protection product, characterized in that, This includes the motor shaft, flexible boron nitride composite bushing, and bearings; The composite bushing comprises micron-sized boron nitride, nano-sized boron nitride, and a continuous polymer phase. The micron-sized boron nitride forms a thermally conductive skeleton with a channel shape extending radially from the inner circle side to the outer circle side of the bushing. The nano-sized boron nitride is located between adjacent micron-sized boron nitrides. The continuous polymer phase impregnates and coats the boron nitride skeleton. The composite bushing is provided with a load-bearing section, a gradual transition section and a buffer section near the shaft shoulder in sequence along the axial direction, corresponding to the bearing raceway projection area. The volume fraction of boron nitride in the load-bearing section is higher than that in the buffer section. The inner surface of the composite bushing is uniformly provided with multiple axial pressure relief microgrooves along the circumference. The closed end of each pressure relief microgroove is located in the bearing section. The groove depth gradually increases from the closed end through the transition section to the buffer section and extends to the end face of the buffer section. There is a continuous bearing zone between each groove. The bottom of the groove has a continuous polymer matrix area covered with boron nitride particles and without through holes. The composite bushing forms a first interference fit and a second interference fit with the motor shaft and the inner ring of the bearing, respectively, and its two axial ends extend out of the end face of the inner ring of the bearing to form an insulating isolation end ring.
9. The product according to claim 8, characterized in that, The motor end cover has a replaceable sealing ring in the sealing groove. The sealing lip of the sealing ring slides in contact with the outer circle of the insulating isolation end ring formed at the axial end of the composite bushing to prevent grease from entering the mating interface between the composite bushing and the motor shaft.
10. The product according to claim 8, characterized in that, After the composite bushing is fitted onto the motor shaft and the temperature is balanced, the outer diameters measured in the load-bearing section and the buffer section are respectively... and The inner diameter of the bearing inner ring before assembly is and satisfy as well as , This is the nominal inner diameter of the bearing's inner ring.