TOPCon solar cell

By using laser patterning technology to advance the phosphorus-doped polycrystalline silicon layer in TOPCon solar cells, the problems of reduced doping concentration and poor metal contact caused by excessively thin polycrystalline silicon layers are solved, thus improving the cell efficiency.

CN222015419UActive Publication Date: 2024-11-15HANWHA SOLARONE QIDONG
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202323558317.0
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2024-11-15
Estimated Expiration
2033-12-26

AI Technical Summary

Technical Problem

In existing TOPCon solar cells, the excessively thin polycrystalline silicon layer leads to a decrease in doping concentration, poorer metal contact, increased risk of metallization burn-through, and reduced cell efficiency.

Method used

Laser patterning technology is used to advance excess phosphorus in a phosphorus-doped polycrystalline silicon layer to form a heavily phosphorus-doped polycrystalline silicon layer, thereby increasing the doping concentration and junction depth, ensuring good metal contact, and avoiding the risk of burn-through.

Benefits of technology

By reducing parasitic absorption in the polycrystalline silicon layer, the short-circuit current is increased, the metal contact is improved, and the efficiency of the solar cell is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222015419U_ABST
    Figure CN222015419U_ABST
Patent Text Reader

Abstract

The utility model relates to a TOPCon solar cell, comprising an N-type silicon wafer, the back surface of the N-type silicon wafer is sequentially provided with a tunneling oxide layer and a phosphorus lightly doped polycrystalline silicon layer from inside to outside, and the cell also comprises a phosphorus heavily doped polycrystalline silicon layer and a back surface electrode, the phosphorus heavily-doped polycrystalline silicon layer is formed by laser propulsion on the side, provided with the tunneling oxide layer, of the phosphorus lightly-doped polycrystalline silicon layer towards the N-type silicon wafer, the back passivation layer is arranged on the side, away from the tunneling oxide layer, of the phosphorus heavily-doped polycrystalline silicon layer, one end of the back electrode penetrates through the phosphorus lightly-doped polycrystalline silicon layer, the tunneling oxide layer makes contact with the phosphorus heavily-doped polycrystalline silicon layer, and the other end of the back electrode makes contact with the N-type silicon wafer. And the other end extends out of the back passivation layer. According to the TOPCon solar cell provided by the utility model, metal contact is ensured, and the risk of metallization burnthrough is avoided, so that the efficiency of the cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to a TOPCon solar cell. Background Art

[0002] In recent years, with the rapid development of photovoltaic technology, TOPCon passivation contact technology has become the mainstream technology for solar cell production. The TOPCon passivation contact structure combines an ultra-thin tunneling oxide layer with a heavily doped polysilicon layer, so that the silicon oxide layer can reduce the interface state density between the silicon substrate and the doped polysilicon through chemical passivation, while allowing the majority carriers to be transported through the tunneling principle, while the minority carriers are difficult to tunnel through the silicon oxide layer due to the higher potential barrier and the field effect of doped polysilicon, thereby improving the passivation performance while reducing metal recombination, thereby improving the efficiency of solar cells. Considering the impact of the parasitic absorption of the polysilicon layer on current loss, the thickness of the polysilicon layer will be selected to be thinner and thinner, but too thin polysilicon will reduce the overall doping concentration, worsen the metal contact, and increase the risk of metallization burn-through, both of which will affect the improvement of solar cell efficiency. Utility Model Content

[0003] The utility model aims to provide a TOPCon solar cell.

[0004] In order to achieve the above purpose, the technical solution adopted by the utility model is:

[0005] A TOPCon solar cell comprises an N-type silicon wafer, wherein a tunneling oxide layer and a lightly phosphorus-doped polysilicon layer are sequentially arranged on the back side of the N-type silicon wafer from the inside to the outside, and the cell further comprises a heavily phosphorus-doped polysilicon layer and a back electrode, wherein the heavily phosphorus-doped polysilicon layer is formed by laser propulsion on one side of the lightly phosphorus-doped polysilicon layer toward the N-type silicon wafer where the tunneling oxide layer is arranged; a back passivation layer is arranged on the side of the heavily phosphorus-doped polysilicon layer away from the tunneling oxide layer, one end of the back electrode is in contact with the heavily phosphorus-doped polysilicon layer, and the other end extends outside the back passivation layer.

[0006] A tunneling oxide layer and intrinsic amorphous silicon are grown on the back of the silicon wafer; then the intrinsic amorphous silicon layer is subjected to a phosphorus diffusion process to form the phosphorus lightly doped polysilicon layer; and laser patterning is further performed on the phosphorus lightly doped polysilicon layer to form a phosphorus heavily doped polysilicon layer.

[0007] In some embodiments, the heavily phosphorus-doped polysilicon layer partially extends into the back side of the N-type silicon wafer.

[0008] In some embodiments, the thickness of the tunnel oxide layer is 0.5-2 nm, and the growth method of the tunnel oxide layer is CVD deposition method, high temperature thermal oxidation method, ozone oxidation method, and ultraviolet oxidation method.

[0009] In some embodiments, the intrinsic amorphous silicon layer is deposited by LPCVD method, using SiH4 and N2 as reaction gases, the flow rate of SiH4 is 100~1000sccm, the flow rate of N2 is 100~10000sccm, the deposition temperature is 580℃-630℃, and the thickness is 50-130nm.

[0010] In some embodiments, the phosphorus lightly doped polysilicon layer is prepared by using a low-pressure diffusion furnace, using POCl3, O2, and N2 as reaction gases, and the square resistance of the phosphorus lightly doped polysilicon layer region is 30-60 ohm / sq.

[0011] In some embodiments, laser doping is used to push the excess phosphorus in the PSG on the phosphorus lightly doped polysilicon layer into the poly and the silicon substrate to form a phosphorus heavily doped polysilicon layer with a square resistance of 15-40 ohm / sq.

[0012] In some embodiments, the laser is green light or purple light, the laser doped pattern corresponds to the metallization pattern, and the laser width is 50-110 nm.

[0013] In some embodiments, the square resistance of the lightly phosphorus-doped polysilicon layer is higher than the square resistance of the heavily phosphorus-doped polysilicon layer, the doping concentration of the lightly phosphorus-doped polysilicon layer is lower than the doping concentration of the heavily phosphorus-doped polysilicon layer, and the junction depth of the lightly phosphorus-doped polysilicon layer is less than the junction depth of the heavily phosphorus-doped polysilicon layer.

[0014] In some embodiments, the square resistance of the heavily phosphorus-doped polysilicon layer is 15~40ohm / sq; the square resistance of the lightly phosphorus-doped polysilicon layer is 30-60ohm / sq; the doping concentration of the lightly phosphorus-doped polysilicon layer is 1E20~3E20; the doping concentration of the heavily phosphorus-doped polysilicon layer is 2E20~4E20; the junction depth of the lightly phosphorus-doped polysilicon layer is 0.1~0.15um; the junction depth of the heavily phosphorus-doped polysilicon layer is 0.15~0.2um.

[0015] The front side of the N-type silicon wafer is provided with a boron-doped P+ layer, a front passivation anti-reflection layer, and a front electrode in sequence from the inside to the outside. The N-type silicon wafer undergoes a boron diffusion process on its front side to form a boron-doped P+ layer (P+ emitter); the front passivation anti-reflection layer is an aluminum oxide layer and a silicon nitride layer.

[0016] Due to the application of the above technical solution, the utility model has the following advantages compared with the prior art:

[0017] The TOPCon solar cell provided by the utility model, after phosphorus doping polysilicon, uses laser patterning to push the surplus phosphorus in PSG into poly and silicon substrate, thereby forming a phosphorus lightly doped polysilicon layer and a phosphorus heavily doped polysilicon layer, and can reduce the thickness of poly in the lightly phosphorus doped polysilicon layer domain to reduce the parasitic absorption of polysilicon, and at the same time, through the action of laser in the phosphorus heavily doped polysilicon layer domain, increase the phosphorus concentration and promote the junction depth, ensure metal contact, and avoid the risk of metallization burn-through, thereby improving the efficiency of the battery, and the process is simple and easy to integrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Attached Figure 1 It is a schematic diagram of the structure after forming a phosphorus lightly doped polysilicon layer in the embodiment;

[0019] Attached Figure 2 A schematic diagram of the structure of forming a heavily phosphorus-doped polysilicon layer according to an embodiment;

[0020] Attached Figure 3 This is a structural diagram of the TOPCon solar cell provided by the utility model.

[0021] In the above figures: 1- N-type silicon wafer; 2- boron-doped P+ layer; 3- front passivation anti-reflection layer; 4- tunneling oxide layer; 5- phosphorus-lightly doped polysilicon layer; 6- phosphorus-heavy doped polysilicon layer; 7- back passivation layer; 8- back electrode; 9- front electrode. DETAILED DESCRIPTION

[0022] The technical solution of the utility model will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments of the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.

[0023] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0024] See also Figures 1 to 3The TOPCon solar cell shown comprises an N-type silicon wafer 1, on the back of which a tunneling oxide layer 4 and a phosphorus lightly doped polysilicon layer 5 are sequentially arranged from the inside to the outside, and the cell further comprises a phosphorus heavily doped polysilicon layer 6 and a back electrode 8. The phosphorus heavily doped polysilicon layer 6 is formed by laser propulsion on the side of the phosphorus lightly doped polysilicon layer 5 toward the N-type silicon wafer where the tunneling oxide layer 4 is arranged, and a back passivation layer 7 is arranged on the side of the phosphorus heavily doped polysilicon layer 6 away from the tunneling oxide layer 4. One end of the back electrode 8 penetrates the phosphorus lightly doped polysilicon layer 5, the tunneling oxide layer 4 and contacts the phosphorus heavily doped polysilicon layer 6, and the other end extends to the outside of the back passivation layer 7. On the front of the N-type silicon wafer, a boron doped P+ layer 2, a front passivation anti-reflection layer 3, and a front electrode 9 are sequentially arranged from the inside to the outside, and the front passivation anti-reflection layer 3 is an aluminum oxide layer and a silicon nitride layer.

[0025] Although thin poly can reduce the current loss caused by parasitic absorption of the polysilicon layer, too thin polysilicon reduces the overall doping concentration, deteriorates metal contact, and increases the risk of metallization burn-through. Therefore, after phosphorus-doped polysilicon, laser patterning is used to push the excess phosphorus in PSG into the poly and silicon substrate (i.e., N-type silicon wafer 1), thereby increasing the phosphorus concentration in the n++poly region and advancing the junction depth, ensuring metal contact and avoiding the risk of metallization burn-through, thereby improving the efficiency of the battery.

[0026] The method for preparing the TOPCon solar cell of this example comprises the following steps:

[0027] Step 1: Clean the double-sided texture of the N-type silicon wafer.

[0028] Step 2: Perform a boron diffusion process on the front side of the silicon wafer to form a P+ emitter (boron-doped P+ layer 2).

[0029] Step 3: The back side of the silicon wafer is then wet chemically polished and cleaned.

[0030] Step 4: grow an ultra-thin tunneling oxide layer 4 and an intrinsic amorphous silicon layer on the polished surface of the silicon wafer, the material of the tunneling oxide layer 4 is silicon dioxide, the thickness of the tunneling oxide layer 4 is 0.5-2nm, and the growth method of the tunneling oxide layer 4 is CVD deposition method, high temperature thermal oxidation method, ozone oxidation method, and ultraviolet oxidation method.

[0031] The intrinsic amorphous silicon layer is deposited by the LPCVD method, using SiH4 and N2 as reaction gases, with a SiH4 flow rate of 100-1000sccm and a N2 flow rate of 100-10000sccm, a deposition temperature of 580°C-630°C, and a thickness of 90-110nm.

[0032] Step 5: Perform a phosphorus diffusion process on the intrinsic amorphous silicon layer to form a phosphorus-doped n+ poly region. The sheet resistance of the phosphorus lightly doped polysilicon layer 5 (phosphorus-doped n+ poly region) is 40 ohm / sq, the junction depth is 0.13 um, and the surface concentration is 2E20.

[0033] Specifically include:

[0034] (1) Place the silicon wafer in a phosphorus expansion furnace tube and heat it to 800°C-830°C. During the heating process, the furnace tube is evacuated, leak tested and voltage stabilized; (2) The silicon wafer is pre-oxidized in an oxygen atmosphere, with an O2 flow rate of 500-3000sccm, a temperature stably controlled at 800°C-830°C, a time controlled at 100-500s, and a pressure controlled at 20-300mbar; (3) Start the first step of deposition, with the temperature controlled at 800°C-830°C, and N2-POCl3, O2 and N2 are introduced into the furnace tube, wherein the N2-POCl3 flow rate is 800-1600sccm, the O2 gas flow rate is 500-1000sccm, the introduction time is 800-1200s, and the pressure is controlled at 20-300mbar; (4) The temperature is raised to 860-920°C again, and the second step of deposition begins during the heating process. N2-POCl3, O2 and N2 are introduced into the furnace tube, wherein the flow rate of N2-POCl3 is 800-1600sccm, the flow rate of O2 gas is 500-1000sccm, and the introduction time is 60-300s; the pressure is controlled at 20-300mbar; (5) After the temperature is raised to 860-920°C, the push-in is started, the time is 400-700s, and the pressure is controlled at 20-300mbar; (6) The temperature is lowered to 830-860°C, and the cooling process starts The third step of deposition begins. N2-POCl3, O2 and N2 are introduced into the furnace tube, wherein the flow rate of N2-POCl3 is 800-1600sccm, the flow rate of O2 gas is 500-1000sccm, and the introduction time is 400-1000s; the pressure is controlled at 20-300mbar; (7) The temperature is reduced to 780℃, and the cooling process begins and then oxidation is carried out. The flow rate of O2 gas is 1000-2000sccm, and the introduction time is 600-1200s; the pressure is controlled at 100-300mbar; (8) The pressure is increased and the temperature is reduced; (9) Exit the boat.

[0035] Step 6: Laser patterning is performed on a part of the phosphorus-doped n+ poly region (phosphorus-lightly doped polysilicon layer 5) (not the entire phosphorus-doped n+ poly region) to form an n++poly region (phosphorus-heavy doped polysilicon layer 6) with a square resistance of 30 ohm / sq, a junction depth of 0.25 um, and a surface concentration of 4E20;

[0036] Step 7: Clean the silicon wafer to remove the wrap-around plating and BSG and PSG;

[0037] Step 8: A front passivation layer and a front anti-reflection layer are sequentially deposited on the front side of the silicon wafer, i.e., the boron-doped P+ emitter side. The front passivation layer is an aluminum oxide layer, and the front anti-reflection layer is a silicon nitride layer.

[0038] Step nine: depositing a back passivation layer 7 on the back side of the silicon wafer, i.e., the side of the phosphorus-doped n+ poly layer, wherein the back passivation layer 7 is a silicon nitride layer;

[0039] Step 10: Screen printing and sintering to form the front electrode 9 and the back electrode 8 respectively.

[0040] In step six, a plurality of phosphorus heavily doped polysilicon layers 6 are provided, a gap is maintained between two adjacent phosphorus heavily doped polysilicon layers 6, and a plurality of back electrodes 8 are provided, and the phosphorus heavily doped polysilicon layers 6 correspond to the back electrodes 8 one by one.

[0041] The TOPCon solar cell in this example forms a high-low junction on the passivation contact surface by selective laser doping, wherein a thin poly is used in the non-metallic area to reduce the parasitic absorption of the polysilicon layer and increase the short-circuit current, and the metal area is further selectively laser doped to push more phosphorus in the PSG on the phosphorus diffusion surface into the poly layer and the silicon substrate, thereby increasing the overall phosphorus concentration and improving the metal contact, thereby increasing the efficiency of the passivation contact solar cell.

[0042] The above embodiments are only for illustrating the technical concept and features of the utility model, and their purpose is to enable people familiar with the technology to understand the content of the utility model and implement it accordingly, and they cannot be used to limit the protection scope of the utility model. Any equivalent changes or modifications made according to the spirit of the utility model should be included in the protection scope of the utility model.

Claims

1. A TOPCon solar cell, comprising an N-type silicon wafer, wherein a tunneling oxide layer and a phosphorus lightly doped polysilicon layer are sequentially arranged on the back of the N-type silicon wafer from the inside to the outside, characterized in that: The battery also includes a phosphorus-heavy doped polysilicon layer and a back electrode. The phosphorus-heavy doped polysilicon layer is formed by laser propulsion on one side of the phosphorus-lightly doped polysilicon layer toward the N-type silicon wafer through a tunneling oxide layer. A back passivation layer is provided on the side of the phosphorus-heavy doped polysilicon layer away from the tunneling oxide layer. One end of the back electrode penetrates the phosphorus-lightly doped polysilicon layer, the tunneling oxide layer and contacts the phosphorus-heavy doped polysilicon layer, and the other end extends outside the back passivation layer.

2. The TOPCon solar cell according to claim 1, characterized in that: There are multiple phosphorus heavily doped polysilicon layers, and a gap is maintained between two adjacent phosphorus heavily doped polysilicon layers. There are multiple back electrodes, and the phosphorus heavily doped polysilicon layers correspond to the back electrodes one by one.

3. The TOPCon solar cell according to claim 2, characterized in that: The square resistance of the lightly phosphorus-doped polysilicon layer is higher than that of the heavily phosphorus-doped polysilicon layer, the doping concentration of the lightly phosphorus-doped polysilicon layer is lower than that of the heavily phosphorus-doped polysilicon layer, and the junction depth of the lightly phosphorus-doped polysilicon layer is less than that of the heavily phosphorus-doped polysilicon layer.

4. The TOPCon solar cell according to claim 3, characterized in that: The sheet resistance of the heavily phosphorus-doped polysilicon layer is 15-40 ohm / sq; the sheet resistance of the lightly phosphorus-doped polysilicon layer is 30-60 ohm / sq.

5. The TOPCon solar cell according to claim 3, characterized in that: The junction depth of the lightly phosphorus-doped polysilicon layer is 0.1-0.15um; the junction depth of the heavily phosphorus-doped polysilicon layer is 0.15-0.2um.

6. The TOPCon solar cell according to claim 1, characterized in that: The back passivation layer is a silicon nitride layer.

7. The TOPCon solar cell according to claim 1, characterized in that: The material of the tunnel oxide layer is silicon dioxide; the thickness of the tunnel oxide layer is 0.5-2nm.

8. The TOPCon solar cell according to claim 1, characterized in that: The front side of the N-type silicon wafer is provided with a boron-doped P+ layer, a front passivation anti-reflection layer, and a front electrode in sequence from the inside to the outside.

9. The TOPCon solar cell according to claim 8, characterized in that: The front passivation anti-reflection layer is an aluminum oxide layer and a silicon nitride layer.

Citation Information

Cited By

  • Tunneling oxide layer passivation contact battery and preparation method thereof

    CN120224839A

  • Tunneling oxide layer passivation contact cell and preparation method thereof

    CN120224839B

  • Solar cell and production method of the same

    EP4804764A1