Porous film

A porous membrane with controlled roughness, bubble point, and porosity addresses the issue of suspended solids adhesion, maintaining efficient filtration performance by reducing clogging and enhancing mechanical strength.

JP2024171901APending Publication Date: 2024-12-12SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023089183
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Porous membranes made of polytetrafluoroethylene face issues with filtration efficiency decline due to adhesion of suspended solids like humic substances, leading to clogging during filtration processes.

Method used

The porous membrane is designed with a surface arithmetic mean roughness Ra of 70 nm or less, an isopropanol bubble point of 180 kPa or more and 250 kPa or less, and a porosity of 40% to 80% by volume, enhancing chemical resistance, mechanical strength, and maintaining filtration performance by reducing suspended matter adhesion.

Benefits of technology

The membrane effectively suppresses filtration efficiency loss by minimizing suspended matter adhesion, ensuring high filtration efficiency and liquid permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024171901000001_ABST
    Figure 2024171901000001_ABST
Patent Text Reader

Abstract

To provide a porous film capable of preventing a deterioration in filtration efficiency caused by fastening of turbid substances at filtration.SOLUTION: A porous film includes a polytetrafluoroethylene or a modified polytetrafluoroethylene as a main component, in which arithmetic average roughness Ra on a surface thereof is 70 nm or less, and an isopropanol bubble point is 180 kPa to 250 kPa, inclusive.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to porous membranes. [Background technology]

[0002] A porous film using polytetrafluoroethylene has the properties of polytetrafluoroethylene such as high heat resistance, chemical stability, weather resistance, non-flammability, high strength, non-adhesiveness, low friction coefficient, etc., and the properties of flexibility and low dielectric constant due to porosity. Therefore, porous films mainly composed of polytetrafluoroethylene are widely used as precision filtration filters for dispersion media and gases in the semiconductor-related field, liquid crystal-related field, and food and medical-related field. In the prior art, a porous film laminate using a porous film mainly composed of polytetrafluoroethylene or modified polytetrafluoroethylene capable of capturing fine particles with a particle diameter of less than 0.1 μm has been proposed as a filtration filter (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-94579 A Summary of the Invention

[0004] A porous membrane according to one embodiment of the present disclosure contains polytetrafluoroethylene or modified polytetrafluoroethylene as a main component, has an arithmetic mean surface roughness Ra of 70 nm or less, and an isopropanol bubble point of 180 kPa or more and 250 kPa or less. [Brief description of the drawings]

[0005] [Figure 1] FIG. 1 is a schematic partial cross-sectional view showing a porous membrane according to one embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0006] [Problem that this disclosure aims to solve] As the filtration process is carried out on a porous membrane, impurities adhere to the membrane surface. Impurities that tend to adhere include turbid matter, including natural organic compounds such as humic substances present in the raw water. When turbid matter adheres, clogging occurs easily, which reduces the filtration efficiency of the liquid that should be filtered.

[0007] An object of the present disclosure is to provide a porous membrane capable of suppressing a decrease in filtration efficiency caused by adhesion of turbidity during filtration.

[0008] [Effects of this disclosure] The porous membrane of the present disclosure can suppress a decrease in filtration efficiency caused by adhesion of turbidity during filtration.

[0009] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described.

[0010] The porous membrane according to one embodiment of the present disclosure comprises: (1) The main component is polytetrafluoroethylene or modified polytetrafluoroethylene, the arithmetic mean surface roughness Ra is 70 nm or less, and the isopropanol bubble point is 180 kPa or more and 250 kPa or less.

[0011] The porous membrane is mainly composed of polytetrafluoroethylene or modified polytetrafluoroethylene, so that the chemical resistance and mechanical strength can be improved. The arithmetic mean roughness Ra of the surface of the porous membrane is 70 nm or less, so that the physical adhesion of turbidity to the surface of the porous membrane can be reduced, so that the decrease in filtration efficiency can be suppressed. In addition, the isopropanol bubble point of the porous membrane is 180 kPa or more and 250 kPa or less, so that the filtration performance can be maintained well. Therefore, the porous membrane can suppress the decrease in filtration efficiency caused by the adhesion of turbidity during filtration.

[0012] Here, the term "main component" refers to the component with the highest content ratio in terms of mass, for example, a component with a content ratio of more than 50 mass%, or 70 mass% or more, or 95 mass% or more. "Turbidity" includes, in addition to natural organic compounds such as humic substances, for example, sand, particles such as silica and calcium carbonate, iron powder, microorganisms, and wood chips. "Isopropanol bubble point" is a value measured using isopropanol in accordance with JIS-K3832 (1990), which indicates the minimum pressure required to push liquid out of a hole, and is an index corresponding to the average hole diameter. The above-mentioned "arithmetic mean roughness Ra" refers to a value measured in accordance with JIS-B0601:2013 with a cutoff value (λc) of 2.5 mm and an evaluation length (l) of 8 mm.

[0013] (2) In the above (1), the porosity of the porous membrane may be 40% by volume or more and 80% by volume or less. In this way, by setting the porosity of the porous membrane in the above range, the strength of the porous membrane can be maintained while the liquid permeability can be sufficiently increased. Here, the "porosity" refers to the percentage of the total volume of the pores in the porous membrane relative to the volume of the porous membrane having pores. The porosity can be calculated by (V1-V0)×100 / V1, where V0 is the actual volume calculated from the mass and density of the solid content of the porous membrane having pores, and V1 is the apparent volume of the porous membrane having pores, including the pores.

[0014] [Details of the embodiment of the present disclosure] Hereinafter, a porous membrane according to an embodiment of the present disclosure will be described in detail with reference to the drawings.

[0015] <Porous membrane> FIG. 1 is a schematic partial cross-sectional view showing a porous membrane according to an embodiment of the present disclosure. The sheet-like porous membrane 1 is mainly composed of polytetrafluoroethylene or modified polytetrafluoroethylene. The porous membrane 1 is composed of a biaxially stretched porous membrane. This biaxially stretched porous membrane is made porous by stretching the surface of a sheet mainly composed of polytetrafluoroethylene or modified polytetrafluoroethylene in two directions perpendicular to each other. The porous membrane 1 allows the liquid or gas to be filtered to permeate in the thickness direction while preventing the permeation of fine impurities.

[0016] Polytetrafluoroethylene and modified polytetrafluoroethylene are fluororesins with excellent chemical resistance and solvent resistance, which increases the range of choices for the types of liquids or gases to be filtered. In addition, polytetrafluoroethylene and modified polytetrafluoroethylene are fluororesins with high hydrophobicity, which prevents liquids from leaking from the porous membrane 1 and improves gas permeability.

[0017] The modified polytetrafluoroethylene refers to polytetrafluoroethylene in which, for example, hexafluoropropylene (HFP), alkyl vinyl ether (AVE), or chlorotrifluoroethylene (CTFE) is copolymerized in a small proportion with respect to tetrafluoroethylene. The ratio of these components to tetrafluoroethylene may be 1 / 50 (molar ratio) or less.

[0018] The lower limit of the average thickness of the porous membrane 1 may be 2 μm or 5 μm. On the other hand, the upper limit of the average thickness of the porous membrane 1 may be 50 μm or 40 μm. If the average thickness is less than 2 μm, the strength of the porous membrane 1 may be insufficient. On the other hand, if the average thickness exceeds 50 μm, the porous membrane 1 may become unnecessarily thick, and the pressure loss during permeation of the filtrate may be large. By setting the average thickness of the porous membrane 1 within the above range, the strength of the porous membrane 1 and the filtration efficiency can be compatible. The "average thickness" refers to the average value of thicknesses at any 10 points, and is measured using a standard digital thickness gauge.

[0019] The upper limit of the arithmetic mean roughness Ra of the surface of the porous membrane 1 is 70 nm, and may be 65 nm, 60 nm, or 55 nm. If the arithmetic mean roughness Ra of the surface of the porous membrane 1 exceeds 70 nm, the turbidity may be easily physically adhered to the porous membrane 1, and the filtration efficiency of the porous membrane 1 may be reduced. The arithmetic mean roughness Ra of the surface of the porous membrane 1 can be adjusted by the stretching conditions and sintering conditions during production. On the other hand, the lower limit of the arithmetic mean roughness Ra is not particularly limited, and may be 0 nm.

[0020] The lower limit of the isopropanol bubble point of the porous membrane 1 is 180 kPa, and may be 185 kPa. On the other hand, the upper limit of the isopropanol bubble point of the porous membrane 1 is 250 kPa, and may be 245 kPa. If the isopropanol bubble point of the porous membrane 1 is less than 180 kPa, impurities may not be separated sufficiently. If the isopropanol bubble point of the porous membrane 1 is more than 250 kPa, the water permeability of the porous membrane 1 may be insufficient, and the filtration efficiency of the porous membrane 1 may be reduced.

[0021] The lower limit of the porosity of the porous membrane 1 may be 40 volume % or 50 volume %. Meanwhile, the upper limit of the porosity may be 80 volume % or 70 volume %. If the porosity is less than 40 volume %, the liquid permeability of the porous membrane 1 may be insufficient. On the other hand, if the porosity is more than 80 volume %, the mechanical strength of the porous membrane 1 may be insufficient.

[0022] In addition to polytetrafluoroethylene and modified polytetrafluoroethylene, the porous membrane 1 may contain other fluororesins and additives within the scope of not impairing the desired effects of the present disclosure. Examples of the additives include inorganic fillers, metal powders, metal oxide powders, and metal sulfide powders for improving abrasion resistance and facilitating pore generation.

[0023] [Method of manufacturing porous membrane] Next, an example of a method for producing the porous membrane will be described. The method for producing the porous membrane includes a step of forming a powder of polytetrafluoroethylene or modified polytetrafluoroethylene into a block-shaped primary molded body (primary molded body forming step), a step of extruding the primary molded body into a sheet (extrusion molding step), a step of stretching the sheet body in biaxial directions while heating it (stretching step), and a step of sintering the stretched sheet body at a temperature equal to or higher than the melting point of polytetrafluoroethylene or modified polytetrafluoroethylene (sintering step).

[0024] (Primary compact forming process) In the primary compact forming process, a material obtained by mixing a liquid lubricant with a powder of polytetrafluoroethylene or modified polytetrafluoroethylene is compressed and molded into a block-shaped primary compact by a compression molding machine. As the raw material polytetrafluoroethylene or modified polytetrafluoroethylene, for example, fine powder of polytetrafluoroethylene or modified polytetrafluoroethylene is used. Specifically, examples of the raw material include fine powder of polytetrafluoroethylene or modified polytetrafluoroethylene produced by emulsion polymerization and molding powder of polytetrafluoroethylene or modified polytetrafluoroethylene produced by suspension polymerization.

[0025] As the liquid lubricant to be mixed with the polytetrafluoroethylene or modified polytetrafluoroethylene powder (hereinafter also referred to as raw material powder), various lubricants that have been conventionally used in the paste extrusion method can be used. For example, naphtha, white oil, and other petroleum-based solvents, hydrocarbon oils such as undecane, aromatic hydrocarbons such as toluene and xylol, alcohols, ketones, esters, silicone oil, fluorochlorocarbon oil, solutions in which polymers such as polyisobutylene and polyisoprene are dissolved in these solvents, mixtures of two or more of these, and aqueous solutions containing surfactants can be mentioned.

[0026] The lower limit of the amount of the liquid lubricant may be 20 parts by mass or 22 parts by mass with respect to 100 parts by mass of the raw powder. On the other hand, the upper limit of the amount of the liquid lubricant may be 28 parts by mass or 25 parts by mass with respect to 100 parts by mass of the raw powder. If the amount of the liquid lubricant is less than 20 parts by mass, the lubricity may be insufficient, making it difficult to extrude the material into a sheet in the next extrusion molding process. On the other hand, if the amount of the liquid lubricant is more than 28 parts by mass, the sheet may be easily torn in the subsequent stretching process.

[0027] (Extrusion molding process) In the extrusion molding process, the primary molded body is molded into a sheet using an extruder. This extrusion molding is carried out at a temperature lower than the melting point of polytetrafluoroethylene or modified polytetrafluoroethylene, and is generally carried out at room temperature.

[0028] In the extrusion process, the sheet extruded from the die may be heated to volatilize the liquid lubricant. By removing the liquid lubricant in this manner, the sheet can be stably stretched in the subsequent stretching process.

[0029] (Stretching process) In the stretching step, the sheet body, which is a molded body, is stretched in biaxial directions while being heated. This step allows pores to be formed and a porous membrane to be obtained. In this step, the sheet body is stretched successively in the longitudinal direction (flow direction) and the transverse direction (width direction) perpendicular to the longitudinal direction, thereby obtaining a biaxially stretched porous membrane.

[0030] The longitudinal stretching ratio in the biaxial stretching may be from 1.5 to 10, or from 2 to 8. The transverse stretching ratio may be from 3 to 16, or from 4 to 15.

[0031] The lower limit of the heating temperature during stretching may be 200°C or 220°C. Meanwhile, the upper limit of the heating temperature during stretching may be 300°C or 280°C. If the heating temperature during stretching is less than 200°C, the stretching speed of the sheet body may not be sufficiently high. Meanwhile, if the heating temperature during stretching exceeds 300°C, the sheet body may be ruptured due to temperature fluctuations exceeding the melting point of polytetrafluoroethylene or modified polytetrafluoroethylene.

[0032] (Sintering process) In the sintering step, the stretched sheet is sintered at a temperature equal to or higher than the melting point of polytetrafluoroethylene or modified polytetrafluoroethylene. This relaxes the biaxial orientation of the porous film and allows it to be adjusted to a good range. The heating temperature in the sintering step may be 350°C or higher and 600°C or lower, and the heating time may be 5 minutes or higher and 60 minutes or lower.

[0033] The heating furnace in the sintering process may be a furnace having a structure in which the object is placed on a mesh belt conveyor and moved from the furnace entrance to the furnace exit side. A heater source such as an electric heater is installed inside the heating furnace, and the object is heated and cooled while being moved from the furnace entrance into the furnace, and then transferred to the furnace exit side.

[0034] The porous membrane can suppress a decrease in filtration efficiency caused by adhesion of suspended matter during filtration.

[0035] [Other embodiments] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is not limited to the configurations of the above-described embodiments, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.

[0036] In the above embodiment, the porous membrane is in a sheet shape, but the shape of the porous membrane is not particularly limited, and may be, for example, a hollow fiber porous membrane. EXAMPLES

[0037] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0038] <Porous membrane test No.1~No.6> Fine powder of polytetrafluoroethylene was used as the raw material powder. The raw material powder was mixed with naphtha, a liquid lubricant, in an amount of 18 parts by mass per 100 parts by mass of the raw material powder, and compressed into a block shape using a preforming machine. Then, a sheet body was formed using an extruder. The cylinder and die temperatures were set to 50°C.

[0039] Next, the above sheet was biaxially stretched at 140° C. to obtain a sheet having an average thickness shown in Table 1.

[0040] Next, the stretched sheet bodies of Test No. 1 to No. 6 were sintered. Specifically, the sheet bodies of Test No. 1 and No. 2 were sintered by heating the heater of a heating furnace equipped with a mesh belt conveyor to 380°C, placing the sheet bodies on the mesh belt conveyor, and conveying them while pressing them with a load of 600 N. The sheet bodies of Test No. 3 to No. 6 were sintered in a normal heating furnace set to 500°C.

[0041] [Measurement of physical properties] (Isopropanol (IPA) bubble point) The IPA bubble point [kPa] was measured in accordance with JIS-K3832 (1990) using isopropanol as the test liquid.

[0042] (Arithmetic mean roughness Ra) The arithmetic mean roughness Ra [nm] of the porous membrane surfaces of No. 1 to No. 6 was measured in accordance with JIS-B0601:2013 with a cutoff value (λc) of 2.5 mm and an evaluation length (l) of 8 mm.

[0043] (porosity) The actual volume V0 calculated from the mass and density of the solid content of the porous membranes No. 1 to No. 6 and the apparent volume V1 including the pores of each porous membrane were calculated, and the porosity (unit: volume %) was calculated from these V0 and V1 values ​​by the following formula. The calculation of the porosity was performed for n=6, and the average value was calculated. Porosity [volume%] = (V1-V0) x 100 / V1

[0044] (Amount of adhered turbidity) Sodium humate was used as the turbid substance. A 10,000 ppm sodium humate solution obtained by dissolving sodium humate in pure water was then passed through the circular porous sheet membranes No. 1 to No. 6 (Φ50: 1962.5 mm 2 The amount of turbidity adhered to the surface of each porous membrane after filtration using the 2.5 mm 2 filter and after backwashing after filtration [mg / 1962.5 mm 2 Backwashing is the process of washing the filtering elements in the filter by flowing a cleaning solution in the opposite direction to the solution flow during filtration. In general, in external pressure filtration modules, backwashing is used after the raw solution is treated. By calculating the amount of turbidity that adheres after backwashing, it is possible to confirm the amount of turbidity that remains on the surface of each porous membrane even after washing. The evaluation conditions and procedures are as follows. (1) Amount of turbidity adhered after filtration Surface area is Φ50:1962.5mm 2 200 mL of 10,000 ppm sodium humate solution was filtered through each of the porous membranes at a supply pressure of 100 KPa. After filtration, each porous membrane was left in a 40°C thermostatic chamber for 24 hours to dry, and then the mass of each porous membrane was measured. The amount of turbidity adhered after filtration was calculated using the following formula. Amount of turbidity adhered after filtration [mg / 1962.5mm 2 ] = Mass of porous membrane after filtration - Mass of porous membrane before filtration (unused) (2) Amount of adhered turbidity after backwashing Each porous membrane after filtration was backwashed with 200 mL of pure water as a cleaning solution at a supply pressure of 100 KPa. After backwashing, each porous membrane was left in a 40°C thermostatic chamber for 24 hours to dry, and then the mass of each porous membrane was measured. The amount of adhered turbidity after backwashing was calculated by the following formula. Amount of adhered turbidity after backwashing [mg / 1962.5mm 2 ] = Mass of porous membrane after backwashing - Mass of porous membrane before filtration (unused)

[0045] (Evaluation of filtration efficiency based on pure water flow rate decrease rate) For each porous membrane with a surface area of ​​Φ50, the amount of pure water permeated was measured for both the unused membrane before filtration and the membrane after filtering 200 mL of 10,000 ppm sodium humate solution at a supply pressure of 100 KPa. The amount of pure water permeated was determined by measuring the amount of pure water permeated for 1 minute at a supply pressure of 100 kP. The pure water flow rate reduction rate [%] was calculated using the following formula. Pure water flow rate decrease rate [%] = {1-(pure water flow rate after filtration of sodium humate solution / pure water flow rate through porous membrane before filtration)} x 100 Furthermore, when the cross section of a porous membrane sample was observed with an electron microscope, it was confirmed that the majority of the sodium humate was layered on the surface of the porous membrane, with very little present within the pores of the porous membrane, and it was therefore believed that the thickness of the porous membrane had almost no effect on the rate of decrease in pure water flow rate.

[0046] Table 1 shows the evaluation results of the average thickness, arithmetic mean roughness Ra, IPA bubble point, porosity, amount of adhered suspended matter, and pure water flow rate reduction rate of the porous membranes of Tests No. 1 to No. 6.

[0047] [Table 1]

[0048] As shown in Table 1, the No. 1 porous membrane, which has a surface arithmetic mean roughness Ra of 70 nm or less and an isopropanol bubble point of 180 kPa or more and 250 kPa or less, had a small amount of turbidity adhered after filtration and backwashing, and the rate of decrease in the pure water flow rate was suppressed.

[0049] On the other hand, porous membranes No. 2 to No. 5, which have an isopropanol bubble point of 180 kPa or more and 250 kPa or less but a surface arithmetic mean roughness Ra of more than 70 nm, and porous membrane No. 6, which has an isopropanol bubble point of less than 180 kPa and a surface arithmetic mean roughness Ra of more than 70 nm, had a greater amount of turbidity adhered after filtration and backwashing than porous membrane No. 1, and had a higher rate of decrease in pure water flow rate.

[0050] As described above, it has been shown that the porous membrane can suppress the decrease in filtration efficiency caused by adhesion of turbidity during filtration. Therefore, the porous membrane can be suitably used in filtration devices for wastewater treatment and the like. [Explanation of symbols]

[0051] 1 Porous membrane

Claims

1. The main component is polytetrafluoroethylene or modified polytetrafluoroethylene, The arithmetic mean roughness Ra of the surface is 70 nm or less, A porous membrane having an isopropanol bubble point of 180 kPa or more and 250 kPa or less.

2. The porous membrane according to claim 1, having a porosity of 40 volume % or more and 80 volume % or less.

Citation Information

Patent Citations

  • Method of manufacturing porous fluororesin thin film and porous fluororesin thin film

    JP2010094579A