Semiconductor nanoparticle complex, semiconductor nanoparticle complex dispersion liquid, semiconductor nanoparticle complex composition, and semiconductor nanoparticle complex cured film

A core/shell structured semiconductor nanoparticle composite with specific ligands allows dispersion in polar media at high mass fractions, maintaining high fluorescence quantum efficiency and heat resistance, addressing dispersion challenges in display technology.

JP2024180509AActive Publication Date: 2024-12-26SHOEI CHEM IND CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024177848
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-06-13
Filing Date
2024-10-10
Publication Date
2024-12-26
Estimated Expiration
2039-08-01

AI Technical Summary

Technical Problem

Semiconductor nanoparticles face challenges in being dispersed in polar dispersion media at high mass fractions while maintaining high fluorescence quantum efficiency, heat resistance, and low viscosity, which are essential for applications like display technology.

Method used

A semiconductor nanoparticle composite with a core/shell structure containing In and P, coated with a ligand having a mercapto fatty acid ester with specific molecular weight and SP value, allowing dispersion in polar media with high mass fraction and maintaining high fluorescence quantum efficiency.

Benefits of technology

The composite achieves high fluorescence quantum efficiency, heat resistance, and low viscosity, enabling efficient dispersion and application in display technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024180509000005
    Figure 2024180509000005
  • Figure 2024180509000006
    Figure 2024180509000006
  • Figure 2024180509000001
    Figure 2024180509000001
Patent Text Reader

Abstract

To provide a semiconductor nanoparticle complex that is dispersible at a high mass fraction in a polar dispersion medium while maintaining high fluorescence quantum yield (QY) in semiconductor nanoparticles.SOLUTION: Provided is a semiconductor nanoparticle complex in which a ligand is coordinated to a surface of a semiconductor nanoparticle. The semiconductor nanoparticle is a core-shell type semiconductor nanoparticle including a core containing In and P and one or more layers of shells. The semiconductor nanoparticle further includes halogen and the molar ratio of halogen to In is 0.80 to 15.00 in terms of atoms. The ligand includes one or more mercapto fatty acid esters represented by the following general formula: HS-R1-COO-R2 (1). The mercapto fatty acid ester has an SP value of 9.20 or more. The mercapto fatty acid ester has a molecular weight of 700 or less, and the average SP value of the entire ligand is 9.10 to 11.00.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to semiconductor nanoparticle composites. [Background technology]

[0002] Semiconductor nanoparticles (quantum dots, QDs) are so small that the quantum confinement effect is manifested. The band gap depends on the photoexcitation and charge injection of semiconductor nanoparticles. The excitons formed in the nuclei recombine to emit photons with an energy depending on the band gap. Therefore, by appropriately selecting the composition and particle size of semiconductor nanoparticles, it is possible to obtain a desired wavelength. It is possible to obtain light emission of

[0003] In the early stages of research into semiconductor nanoparticles, the focus was on elements including Cd and Pb. Since Cd and Pb are regulated substances such as those subject to the Restriction of Use of Certain Hazardous Substances, in recent years, Research on Pb-based and non-Pb-based semiconductor nanoparticles has been conducted.

[0004] Semiconductor nanoparticles are used in a variety of applications, including displays, biolabeling, and solar cells. Applications to display applications include QD films and QD patterning. It is expected that this technology will be applied to self-luminous devices (QLEDs) and other applications.

[0005] FIG. 2 shows a schematic diagram of the device configuration for converting the wavelength from a light source in a conventional display. As shown in Figure 2, a blue LED 101 is used as the light source. Blue light is converted into white light. To convert blue light into white light, a semiconductor A QD film is made by dispersing nanoparticles in a resin and forming it into a film with a thickness of about 100 μm. A wavelength conversion layer such as the QD film 102 is preferably used. The obtained white light is further filtered through a color filter (R) 104 and a color filter (G) 10 5, and a color filter (B) 106 respectively transmit red light, green light, and blue light. The polarizing plate is omitted in Figure 2.

[0006] Recently, as shown in Figure 1, QD patterning has been used as a wavelength conversion layer without using a QD film. The type of display shown in Figure 1 (polarizers not shown) is currently under development. In this display, the blue light from the blue LED1 light source is not converted into white light, Direct blue-to-red or blue-to-green light generation using QD patterning (7, 8) QD patterning (7, 8) is a technique for patterning semiconductor nanoparticles dispersed in a resin. The thickness is limited to 5μm to 10μm due to the display structure. The blue light from the blue LED 1, which is the light source, is diffused. The light is used after passing through a diffusion layer 9 containing an agent. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2013-136498 A [Non-patent literature]

[0008] [Non-Patent Document 1] Takashi Jin, "Semiconductor Quantum Dots, Their Synthesis and Applications to Life Sciences," Production and Technology, Vol. 63, No. 2, pp. 58-63, 2011 [Non-Patent Document 2] Fabien Dubois et al, “A Versatile Strategy for Quantum Dot Ligand Exchange” J.AM.CHEM.SOC Vol.129, No.3, p.482-483, 2007 [Non-Patent Document 3] Boon-Kin Pong et al, “Modified Ligand-Exchange for Efficient Solubilization of CdSe / ZnS Quantum Dots in Water: A Procedure Guided by Computational Studies” Langmuir Vol.24, No.10, p.5270-5276, 2008 [Non-Patent Document 4] Samsulida Abd. Rahman et al, “Thiolate-Capped CdSe / ZnS Core-Shell Quantum Dots for the Sensitive Detection of Glucose” Sensors Vol.17, No.7, p.1537, 2017 [Non-Patent Document 5] Whitney Nowak Wenger et al, “Functionalization of Cadmium Selenide Quantum Dots with Poly(ethylene glycol): Ligand Exchange, Surface Coverage, and Dispersion Stability” Langmuir, Vol.33, No.33, pp8239-8245, 2017 Summary of the Invention [Problem to be solved by the invention]

[0009] Semiconductor nanoparticles and semiconductor nanoparticle composites are generally dispersed in a dispersion medium to form a dispersion liquid. In particular, for display applications, glycol ether is used. Dispersion liquids in polar organic dispersion media such as esters and glycol ether esters By using and curing the dispersion, QD films and QD patterning can be performed. A cured film is formed. Then, in order to increase the wavelength conversion efficiency, the semiconductor nanoparticles in the cured film are A high mass fraction of particles is desired.

[0010] However, semiconductor nanoparticles and semiconductor nanoparticle composites synthesized in non-polar dispersion media Because of its high hydrophobicity, it is easy to disperse in non-polar dispersion media, but difficult to disperse in polar dispersion media. It was.

[0011] Semiconductor nanoparticles and semiconductor nanoparticle composites synthesized in non-polar dispersion media have dipole-dipole interactions. Therefore, it is considered that the molecular weight is small in organic solvents, even among polar dispersion media. Like the semiconductor nanoparticles formed, toluene and chloroform, which have small dipole-dipole forces and hydrogen bonding forces, However, these polar dispersion media are highly toxic. Therefore, it has no practical use.

[0012] The ligand exchange method is known as a method for making semiconductor nanoparticles dispersible in polar dispersion media. The ligand exchange method is a method for bonding ligands to the surface of semiconductor nanoparticles. This method involves replacing the ligand contained in the nanoparticle complex with a ligand having a hydrophilic group. The semiconductor nanoparticle composite thus obtained can be dispersed in a polar dispersion medium. However, the semiconductor nanoparticles disclosed in Non-Patent Documents 1 to 5 and Patent Document 1 Although the particle complex enables dispersion of semiconductor nanoparticles in a polar dispersion medium, the luminescence efficiency decreases. There was a problem.

[0013] Another method for making semiconductor nanoparticles dispersible in a polar dispersion medium is encapsulation. The encapsulation method is known, but the encapsulation method is obtained by binding a ligand to the surface of semiconductor nanoparticles. Since the method further coats the semiconductor nanoparticle composite with an amphiphilic polymer, The amount of dispersant relative to the nanoparticles increases, making it difficult to achieve a high mass fraction of semiconductor nanoparticles. This makes it difficult to apply.

[0014] For these reasons, the semiconductor nanoparticle composite has a high fluorescence quantum efficiency of semiconductor nanoparticles. There is a demand for a material that can be dispersed at a high mass fraction in a polar dispersion medium while maintaining its QY. There are.

[0015] In addition, when forming a cured film such as a QD film or QD patterning, the dispersion liquid Any hardening method can be used to harden the resin, but when the hardening method is thermal hardening, In the case of the semiconductor nanoparticle composite, heat is applied to the dispersion liquid, so that the semiconductor nanoparticles and the semiconductor nanoparticles are heated. The composite material must be heat resistant.

[0016] In addition, when forming a cured film such as a QD film or QD patterning, the dispersion liquid Any hardening method can be used to harden the resin. However, some hardening methods (e.g., In some cases, such as for ink jet printing, the dispersion may be required to have a low viscosity.

[0017] Therefore, an object of the present invention is to provide a method for producing semiconductor nanoparticles having a high fluorescence quantum efficiency (QY) while maintaining the high fluorescence quantum efficiency (QY). To provide a semiconductor nanoparticle composite that can be dispersed at a high mass fraction in a polar dispersion medium. Another object of the present invention is to provide a method for producing semiconductor nanoparticles having a high fluorescence quantum efficiency (QY), In addition to being dispersible in polar dispersion media at a high mass fraction, it has high heat resistance and is suitable for applications where heat resistance is required. The present invention also aims to provide a semiconductor nanoparticle composite that is useful in a desired application. The purpose of this study is to develop a polar dispersion of semiconductor nanoparticles while maintaining their high fluorescence quantum efficiency (QY). In addition to being able to disperse in a medium at a high mass fraction, the viscosity of the dispersion when dispersed in the dispersion medium is low. To provide a semiconductor nanoparticle composite that is useful in applications requiring a low viscosity dispersion. The point is... [Means for solving the problem]

[0018] The above problems are solved by the present invention described below. That is, the semiconductor nanoparticle composite (1) of the present invention has ligands on the surface of the semiconductor nanoparticles. A semiconductor nanoparticle composite having a coordinating group, The semiconductor nanoparticles have a core containing In and P and one or more shell layers. Core / shell type semiconductor nanoparticles, The semiconductor nanoparticles further contain a halogen, and in the semiconductor nanoparticles, In the calculation, the molar ratio of halogen to In is 0.80 to 15.00; The ligand has the following general formula (1): HS-R1-COO-R2(1) (In general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group.) The composition contains one or more mercapto fatty acid esters represented by the formula: The SP value of the mercapto fatty acid ester is 9.20 or more, and the mercapto fatty acid The molecular weight of the ester is 700 or less, and the average SP value of the entire ligand is 9.10 to 11.00; The present invention provides a semiconductor nanoparticle composite characterized by the above.

[0019] The present invention (2) also relates to a molecule of a mercapto fatty acid ester represented by the general formula (1). The semiconductor nanoparticle composite according to claim 1, wherein the amount of the cations is 300 or more and 700 or less. This is what we do.

[0020] The present invention (3) also relates to a mercapto fatty acid ester molecule represented by the general formula (1): The amount of the semiconductor nanoparticle composite is 300 or more and 600 or less. This is what we do.

[0021] In addition, the present invention (4) is characterized in that the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) The semiconductor nanoparticle composite according to (2) or (3), characterized in that the ratio of the particle diameter to the particle diameter is 1.00 or less. It provides the body.

[0022] In addition, the present invention (5) is characterized in that the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) The semiconductor nanoparticle composite according to (2) or (3), characterized in that the particle size distribution (particle size) is 0.70 or less. It provides the body.

[0023] In addition, the present invention (6) is characterized in that the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) Any one of (2) to (5) semiconductor nanoparticles, characterized in that the ratio of nanoparticles to nanoparticles is 0.40 or more. It provides a child complex.

[0024] The present invention (7) also relates to a mercapto fatty acid ester molecule represented by the general formula (1): The semiconductor nanoparticle composite according to claim 1, wherein the amount of the nanoparticles is less than 300. be.

[0025] In addition, the present invention (8) is characterized in that the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) The present invention provides a semiconductor nanoparticle composite according to the above (7), characterized in that the ratio of the particle diameter to the particle diameter is 0.40 or less. This is what we have in mind.

[0026] The present invention (9) also relates to a method for producing a mercapto group represented by the general formula (1) which is contained in the entire ligand. The content of the butyric acid fatty acid ester is 40 mol % or more (1) to (8). Any semiconductor nanoparticle composite is provided.

[0027] The present invention (10) also relates to a method for producing a mercapto group represented by the general formula (1) that accounts for a large proportion of the ligand as a whole. The content of caproic fatty acid ester is 50 mol % or more. ) a semiconductor nanoparticle composite.

[0028] The present invention (11) also relates to a mercapto group represented by the general formula (1) that accounts for the entire ligand. The content of capryloyl fatty acid ester is 60 mol% or more. ) a semiconductor nanoparticle composite.

[0029] In addition, the present invention (12) is characterized in that at least one of the shells is formed of ZnSe. The present invention provides a semiconductor nanoparticle composite according to any one of (1) to (11), characterized by: .

[0030] In addition, the present invention (13) is characterized in that the shell has two or more layers, and the outermost layer of the shell is ZnS. A semiconductor nanoparticle composite according to any one of (1) to (12), characterized in that the semiconductor nanoparticle composite is formed of It is what we provide.

[0031] The present invention (14) also provides a semiconductor device comprising: a core having a shell made of at least ZnSe; a first shell covering the outer surface of the first shell, the second shell being made of ZnS; and a shell. This provides:

[0032] The present invention (15) also relates to the compound according to the above general formula (1), wherein R2 is an oligoethylene glycol group, It is any one selected from the group consisting of a polyethylene glycol group and an alkoxy group. The present invention provides a semiconductor nanoparticle composite according to any one of (1) to (14), characterized in that:

[0033] The present invention (16) also relates to a terminal group that is not bonded to the carboxyl group of R2 in the general formula (1). The terminal group is any one selected from the group consisting of an alkyl group, an alkenyl group, and an alkynyl group. The present invention provides a semiconductor nanoparticle composite according to any one of (1) to (15), It is.

[0034] In addition, the present invention (17) is characterized in that the ligand further includes an aliphatic ligand. The present invention provides a semiconductor nanoparticle conjugate according to any one of (1) to (16).

[0035] In addition, the present invention (18) is characterized in that the aliphatic ligand is an aliphatic thiol, an aliphatic carboxylic acid, or the like. and aliphatic phosphines (17). The present invention provides a semiconductor nanoparticle composite.

[0036] In addition, the present invention (19) provides a semiconductor nanoparticle composite having a quantum efficiency of 80% or more after purification. The present invention provides a semiconductor nanoparticle composite according to any one of (1) to (18), which is characterized in that That is why.

[0037] In addition, the present invention (20) is a semiconductor nanoparticle composite having an emission spectrum half width of 38 The present invention provides a semiconductor nanoparticle composite according to any one of (1) to (19), characterized in that the nanoparticle diameter is 0.01 nm or less. This is to provide.

[0038] The present invention (21) further provides a semiconductor nanoparticle composite according to any one of (1) to (20), The present invention provides a dispersion liquid of semiconductor nanoparticle composites dispersed in a dispersion medium.

[0039] The present invention (22) also relates to a semiconductor nanoparticle composite according to any one of (1) to (20), The present invention provides a composite composition of semiconductor nanoparticles dispersed in a polymer or prepolymer.

[0040] The present invention (23) also relates to a semiconductor nanoparticle composite having a high molecular weight. The present invention provides a cured film of a semiconductor nanoparticle composite dispersed in a polymer matrix.

[0041] The present invention (24) also relates to a polymer having a core containing In and P and one or more shell layers. These are core / shell type semiconductor nanoparticles that further contain halogens and have a ratio of 1:1 to In on an atomic basis. The molar ratio of halogen to semiconductor nanoparticles is 0.80 to 15.00. A surface modifying compound having a binding group capable of binding to nanoparticles is contacted with the surface modifying compound. A semiconductor nanoparticle composite, The surface modifying compound is represented by the following general formula (1): HS-R1-COO-R2(1) (In general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group.) The composition contains one or more mercapto fatty acid esters represented by the formula: The SP value of the mercapto fatty acid ester is 9.20 or more, and the mercapto fatty acid The molecular weight of the ester is 700 or less, and the average SP value of the entire surface modifying compound is 9.10 to 11.00; The present invention provides a semiconductor nanoparticle composite characterized by the above.

[0042] In addition, the present invention (25) provides a method for preparing a surface modifying compound, the surface modifying compound being bonded to one end of a semiconductor nanoparticle. The surface modification compound further includes an aliphatic group-containing surface modifying compound having an aliphatic group at one end and a bonding group at the other end. The present invention provides a semiconductor nanoparticle composite according to (24), characterized in that

[0043] In this application, the range indicated by "~" is the range including the numbers on both ends. Effect of the Invention

[0044] According to the present invention, it is possible to obtain a polar semiconductor nanoparticle while maintaining a high fluorescence quantum efficiency (QY). It is possible to provide a semiconductor nanoparticle composite that can be dispersed at a high mass fraction in a dispersion medium. In addition, according to the present invention, the polarity of the semiconductor nanoparticles can be controlled while maintaining the high fluorescence quantum efficiency (QY). In addition to being dispersible at a high mass fraction in a dispersion medium having the above properties, it also has high heat resistance and is used in applications where heat resistance is required. In addition, the present invention provides a semiconductor nanoparticle composite that is useful in the above-mentioned applications. By using this method, it is possible to obtain a highly transparent semiconductor nanoparticle that can be dispersed in a polar dispersion medium while maintaining its high fluorescence quantum efficiency (QY). In addition to being dispersible at a high mass fraction, the viscosity of the dispersion when dispersed in a dispersion medium is low, To provide a semiconductor nanoparticle composite useful for applications requiring a low viscosity dispersion can be done. [Brief description of the drawings]

[0045] [Figure 1] FIG. 1 is a schematic diagram showing a QD device. [Diagram 2] FIG. 1 is a schematic diagram showing a QD device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0046] (Semiconductor nanoparticle composite) The semiconductor nanoparticle composite (A) of the present invention is a semiconductor nanoparticle having a ligand coordinated to the surface thereof. A semiconductor nanoparticle composite comprising: The semiconductor nanoparticles have a core containing In and P and one or more shell layers. Core / shell type semiconductor nanoparticles, The semiconductor nanoparticles further contain a halogen, The molar ratio of the halogen is 0.80 to 15.00 in atomic terms, The ligand has the following general formula (1): HS-R1-COO-R2(1) (In general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group.) The composition contains one or more mercapto fatty acid esters represented by the formula: The SP value of the mercapto fatty acid ester is 9.20 or more, and the mercapto fatty acid The molecular weight of the ester is 700 or less, and the average SP value of the entire ligand is 9.10 to 11.00; The semiconductor nanoparticle composite is characterized by the following:

[0047] The semiconductor nanoparticle composite of the present invention is a semiconductor nanoparticle having a ligand coordinated to the surface thereof. The semiconductor nanoparticle composite of the present invention is a composite of a semiconductor nanoparticle and a ligand. The molecule is obtained by contacting the molecule with a ligand.

[0048] In the present invention, the semiconductor nanoparticle composite is a semiconductor nanoparticle composite having a light-emitting property. The semiconductor nanoparticle composite of the present invention absorbs light of 340 nm to 480 nm and emits light. These particles emit light with a peak wavelength of 400 nm to 750 nm.

[0049] The full width at half maximum (FWHM) of the emission spectrum of the semiconductor nanoparticle composite of the present invention is 38 nm or less. It is preferable that the wavelength of the emission spectrum is 35 nm or less. When the half-value width is in the above range, the semiconductor nanoparticle composite is applied to a display or the like. Color mixing can be reduced.

[0050] The semiconductor nanoparticle composite of the present invention preferably has a fluorescence quantum efficiency (QY) of 80% or more. It is preferable that the fluorescence quantum efficiency of the semiconductor nanoparticle composite is 8% or more, and more preferably 85% or more. 0% or more, more efficient color conversion is possible when semiconductor nanoparticles are used in applications. .

[0051] In the present invention, the optical properties of the semiconductor nanoparticle composite are measured using a quantum efficiency measurement system. The semiconductor nanoparticle composite is dispersed in a dispersion liquid, and the emission spectrum is measured by applying excitation light. From the emission spectrum obtained here, the amount of re-excited fluorescence is calculated. Fluorescence quantum efficiency (QY) is calculated from the emission spectrum after re-excitation correction excluding the induced fluorescence emission spectrum. The dispersion liquid is, for example, normal hexane, PGMEA, or chloroform. Roholm, etc.

[0052] (Semiconductor nanoparticles) The semiconductor nanoparticles constituting the semiconductor nanoparticle composite of the present invention contain In and P. A core / shell type semiconductor nanoparticle has a core and one or more shell layers. The particle may have at least one shell layer. For example, the semiconductor nanoparticle may have Core / shell type semiconductor nanoparticles consisting of a core and one shell layer, and core and two shell layers Core / shell type semiconductor nanoparticles consisting of a core and three or more shell layers In particular, the shell is made up of two or more layers, making it possible to obtain semiconductor nanoparticles with The fluorescent quantum efficiency of the particles can be maintained, and the semiconductor nanoparticle composite also has a high fluorescent quantum efficiency. In addition, the structure of the semiconductor nanoparticles is such that the shell is Although it is sufficient if the shell covers at least a portion of the surface, a structure in which the shell covers the entire surface of the core is preferable, and a structure in which the shell uniformly covers the entire surface of the core is particularly preferable.

[0053] The shell preferably includes a shell having a composition containing Zn and Se. At least one of the semiconductor nanoparticles is preferably made of ZnSe. In the case where the outermost layer has a shell of the above-mentioned composition, it is preferable that the shell has a composition containing Zn and S. It is preferable that the metal is ZnS.

[0054] In particular, the shell is formed of at least ZnSe and covers the outer surface of the core particle. The first shell and the second shell, which is made of ZnS and covers the outer surface of the first shell, In this case, the fluorescence quantum efficiency can be increased.

[0055] The composition in the shell does not necessarily have to be a stoichiometric composition as long as the effect of the present invention is not impaired. Each shell may contain elements other than Zn, Se, and S, or elements constituting the shell may be different from those constituting the shell. The nanotube may have one or more gradient shells in which the ratio of the elements present varies.

[0056] In the present invention, it is important to determine whether the shell covers at least a part of the core, and whether the shell is a shell. The element distribution inside the well can be measured, for example, by using an energy dispersive X-ray microscope (EDX) with a transmission electron microscope. This can be confirmed by composition analysis using line spectroscopy (TEM-EDX). .

[0057] The semiconductor nanoparticles in the semiconductor nanoparticle composite of the present invention contain a halogen. The molar ratio of halogen to In in the particles is 0.80 to 15.00 in atomic terms, and preferably The halogen contained in the semiconductor nanoparticles is F, Cl, Br is preferred. When the semiconductor nanoparticles contain halogen in the above range, they have a high fluorescence quantum yield. Furthermore, during the synthesis of the semiconductor nanoparticle composite described below, The halogens are not necessarily essential for the core and shell of semiconductor nanoparticles. The presence of the fluorine-containing compound at the interface and / or in the shell of the semiconductor nanoparticles enhances the aforementioned effects. It can be done.

[0058] In the semiconductor nanoparticles of the semiconductor nanoparticle composite of the present invention, the molar ratio of P to In is In terms of atoms, it is preferable that the molar ratio of Zn to In is 0.20 to 0.95. The mole ratio is preferably 10.00 to 60.00 in atomic terms.

[0059] The elements that compose semiconductor nanoparticles were analyzed using a high-frequency inductively coupled plasma emission spectrometer. This can be done using an inductively coupled plasma (ICP) analyzer or an X-ray fluorescence analyzer (XRF).

[0060] An example of a method for producing semiconductor nanoparticles will be disclosed below. A precursor obtained by mixing an In precursor, a P precursor, and, if necessary, an additive in a solvent. By heating the mixture, the core of the semiconductor nanoparticle can be formed. Coordinating and non-coordinating solvents are used. Examples of solvents include 1-octadecene, hexadecane, squalane, oleylamine, Examples include trioctylphosphine and trioctylphosphine oxide. The precursor of In includes acetates, carboxylates, halides, etc., containing In. These include, but are not limited to: Examples of precursors of P include, but are not limited to, organic compounds and gases containing the above-mentioned P. In the case where the precursor is a gas, the gas is added to a precursor mixture that contains gases other than the above gas. The core can be formed by reacting while injecting.

[0061] The semiconductor nanoparticles may contain one or more elements other than In and P as long as the effect of the present invention is not impaired. The amount of the element may be more than 1000, and in that case, the precursor of the element may be added during the formation of the core. Additives include, for example, carboxylic acids, amines, thiols, and phosphides as dispersants. phosphine oxides, phosphinic acids, and phosphonic acids. However, the dispersant is not limited to these. The dispersant may also serve as a solvent.

[0062] After the core of the semiconductor nanoparticle is formed, a halide is added as necessary to form the semiconductor nanoparticle. The luminescence characteristics of the nanoparticles can be improved.

[0063] In one embodiment, the In precursor and optionally the precursor with a dispersing agent in a solvent are The solutions are mixed under vacuum, heated at 100°C to 300°C for 6 to 24 hours, and then Add the P precursor, heat at 200°C to 400°C for 3 to 60 minutes, and then cool. A precursor of the amine is added, and the mixture is heated at 25° C. to 300° C., preferably at 100° C. to 300° C., more preferably at 100° C. to 300° C. By heat treating at 150℃ to 280℃, a core particle dispersion liquid containing core particles can be obtained. can.

[0064] By adding a shell-forming precursor to the synthesized core particle dispersion, semiconductor nanoparticles are formed. The molecules have a core / shell structure, which can enhance the fluorescence quantum efficiency (QY) and stability. .

[0065] The elements that make up the shell form alloys, heterostructures, or amorphous structures on the surface of the core particles. However, some of the particles seem to have moved to the inside of the core particle by diffusion. It can also be considered that.

[0066] The added shell-forming elements are mainly present near the surface of the core particles and surround the semiconductor nanoparticles. The core / shell structure of semiconductor nanoparticles is characterized by the shell acting as a protective layer against environmental factors. It is preferable that the surface of the core particle is covered with the fluorine-containing compound. It is preferable that the surface area is uniformly covered.

[0067] In one embodiment, after adding a Zn precursor and a Se precursor to the aforementioned core particle dispersion liquid, Heat at 0°C to 300°C, preferably 180°C to 250°C, and then mix the Zn precursor and the S precursor. and heating at 200°C to 400°C, preferably 250°C to 350°C. Core / shell type semiconductor nanoparticles can be obtained.

[0068] Here, the Zn precursor is not particularly limited, but may be zinc acetate, propionic acid, etc. Zinc and carboxylates such as zinc myristate, and halogens such as zinc chloride and zinc bromide. For example, an organic salt such as zinc chloride or diethyl zinc can be used. The Se precursors are tributylphosphine selenide, trioctylphosphine selenide, phosphine selenides such as phosphine selenide and tris(trimethylsilyl)phosphine selenide; Selenols such as benzeneselenol and selenocysteine, and selenium / octa A decene solution or the like can be used. The S precursors are tributylphosphine sulfide and trioctylphosphine sulfide. phosphine sulfides such as phosphine sulfide and tris(trimethylsilyl)phosphine sulfide Thiols such as thiols, octanethiol, dodecanethiol, and octadecanethiol and sulfur / octadecene solutions can be used.

[0069] The shell precursors may be premixed and added in one or multiple portions. The shell precursor may be added in a single portion or in multiple portions. If the shell precursor is added in several portions, it is possible to heat the shell precursor at different temperatures after each addition. good.

[0070] In the present invention, the method for producing semiconductor nanoparticles is not particularly limited. In addition to the above-mentioned methods, Conventional methods include the hot injection method, the homogeneous solvent method, the reverse micelle method, and the CVD method. The method for producing the film may be any method.

[0071] (Ligand) The semiconductor nanoparticle composite of the present invention is a semiconductor nanoparticle having a ligand coordinated to the surface thereof. The coordination mentioned here means that the ligands chemically affect the surface of the semiconductor nanoparticles. The surface of the semiconductor nanoparticles is bonded to the semiconductor nanoparticles by coordinate bonds or any other bonding method (e.g., covalent bonds). , ionic bonds, hydrogen bonds, etc.) or on the surface of the semiconductor nanoparticles. When at least a part of the molecule has a ligand, it is not necessary to form a bond. .

[0072] In the semiconductor nanoparticle composite of the present invention, the ligand coordinated to the semiconductor nanoparticle is The mercapto fatty acid ester includes a mercapto fatty acid ester represented by the general formula (1). HS-R1-COO-R2(1)

[0073] In the general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group. In other words, in the mercapto fatty acid ester represented by the general formula (1), -SH is bonded to one of R1. The semiconductor nanoparticle composite of the present invention is a compound having -COO-R2 bonded to the other end. In the present invention, the ligand coordinated to the semiconductor nanoparticle is a mercaptolipid represented by the general formula (1). The mercapto fatty acid ester represented by the general formula (1) may be included. It may contain two or more types of sterols.

[0074] The mercapto fatty acid ester represented by the general formula (1) is coordinated to the semiconductor nanoparticles, In this way, a semiconductor nanoparticle composite having a high fluorescence quantum efficiency and a narrow half-value width can be obtained.

[0075] In the general formula (1), R1 is a methylene group (-CH2-), an ethylene group (-CH2C H2-), propylene group (-CH2CH2CH2-), methylethylene group (-CH(CH 3)-), and the dimethylmethylene group (-C(CH3)2-).

[0076] In the general formula (1), R2 is not particularly limited as long as it is a hydrophilic group, and may be, for example, an alkyl group, Alkynyl group, alkenyl group, alkoxy group, hydroxy group, aldehyde group, carboxy aryl group, amino group, imino group, nitro group, cyano group, vinyl group, aryl group, halogeno group, Examples of hydrophilic groups include those containing a ketone group, an ether bond, an ester bond, a siloxane bond, and the like. R2 is an oligoethylene glycol group, a polyethylene glycol group or an alkoxy group. A hydrophilic group having a silyl group is preferred, and an oligoethylene glycol group or a polyethylene glycol group is preferred. It is particularly preferred that R2 is an oligoethylene glycol group, a polyethylene glycol group, The hydrophilic group having a carboxyl group or an alkoxy group allows the semiconductor nanoparticles to be dissolved in a polar solvent. Furthermore, in the general formula (1), the carboxyl group of R2 can be dispersed at a high concentration. The terminal group not bonded to the alkyl group is a group consisting of an alkyl group, an alkenyl group, and an alkynyl group. It is preferable that the side of R2 that is not bonded to the carboxyl group is selected from the following. Any one of the terminal groups selected from the group consisting of an alkyl group, an alkenyl group, and an alkynyl group. This suppresses the interactions between the semiconductor nanoparticle complexes and dissolves the semiconductor nanoparticles in a polar solvent. It can be dispersed in a medium at a high concentration.

[0077] The molecular weight of the mercapto fatty acid ester represented by the general formula (1) is 700 or less. The molecular weight of the mercapto fatty acid ester represented by the general formula (1) is 700 or less, It becomes possible to disperse conductive nanoparticles in a polar solvent at a high concentration.

[0078] In the present invention, the molecular weight of the mercapto fatty acid ester represented by the general formula (1) is refers to the average molecular weight of the mercapto fatty acid ester represented by the general formula (1). The average molecular weight of mercapto fatty acid esters represented by the formula (1) was measured by GPC (gel permeation chromatography). The number average of the obtained values ​​was calculated as the average molecular weight (number average molecular weight Mn )

[0079] Furthermore, the SP value of the mercapto fatty acid ester represented by the general formula (1) is 9.20 or more. When the SP value is in the above range, the semiconductor nanoparticles can be It is possible to disperse particles in a polar solvent. Here, the SP value is calculated by the Y-MB method. In the present invention, the ligand is represented by two or more general formula (1). When using mercapto fatty acid esters, the SP of each mercapto fatty acid ester is The SP value is calculated by multiplying the value by the volume fraction of each mercapto fatty acid ester and then adding them together. is the SP value of the mercapto fatty acid ester. For example, Mercapto fatty acid ester is P1 volume %, and mercapto fatty acid ester with SP value A2 is P2 When the mercapto fatty acid ester is coordinated with vol.%, the SP value is expressed by the following formula (2): It is expressed as: SP value of mercapto fatty acid ester = Σ(Ai × Pi / 100) (2)

[0080] In the semiconductor nanoparticle composite of the present invention, the ligand is a mercapto group represented by general formula (1) The compound of the general formula (1) may contain ligands other than the aryl fatty acid ester. As a ligand other than the mercapto fatty acid ester shown in the above, a semiconductor nanoparticle is attached to one end. There are no particular limitations on the compound as long as it has a bonding group that can be coordinated to the semiconductor nanoparticles. The mercapto fatty acid ester represented by the general formula (1) can be used as a compound having a function of positioning the mercapto fatty acid ester. When used in combination with Stell, the average SP value of the entire ligand is 9.20 to 11.00, preferably It is fine as long as it can be adjusted between 9.20 and 10.00.

[0081] The SP value of the ligand other than the mercapto fatty acid ester represented by the general formula (1) is not particularly limited. Although not limited thereto, it is preferably 7.50 to 15.00, and particularly preferably 7.50 to 15.00. It is.

[0082] The average SP value of all the ligands coordinated to the semiconductor nanoparticles is 9.20 to 11.00. The average of all the ligands coordinated to the semiconductor nanoparticles is preferably 9.20 to 10.00. When the SP value is within the above range, it becomes possible to disperse the semiconductor nanoparticles in a polar solvent. The SP value of the ligand can be calculated from the structural formula using the Y-MB method. When multiple types of ligands are coordinated to the nanoparticle, the SP value of each ligand is multiplied by the volume fraction of the ligand. After multiplying by the number of ligands, the sum of the average SP value of all ligands is the SP value of the ligand. Example For example, in a semiconductor nanoparticle, the ligand with SP value A1 is P1 volume % and the ligand with SP value A2 is P1 volume %. When P is coordinated with 2% by volume, the average SP value of all ligands is calculated by the following formula (3): Represented. Average SP value of all ligands = Σ(Ai × Pi / 100) (3)

[0083] As the ligand other than the mercapto fatty acid ester represented by the general formula (1), aliphatic ligands By including an aliphatic ligand as the ligand, the semiconductor nanoparticles can be made extremely It can be dispersed at high concentration in organic solvents with a wider range of SP values. In addition, when the composition and dispersion liquid described later are applied, the dispersion medium This makes it possible to expand your options.

[0084] Aliphatic ligands include aliphatic thiols, aliphatic carboxylic acids, aliphatic phosphines, Aliphatic phosphine oxides and aliphatic amines are examples of these, and they have strong coordination power with semiconductor nanoparticles. Therefore, the compound is selected from the group consisting of an aliphatic thiol, an aliphatic carboxylic acid, and an aliphatic phosphine. It is preferable to use at least one of them. The aliphatic group of the aliphatic ligand may contain a substituent or a heteroatom. Good too.

[0085] The content of the mercapto fatty acid ester represented by the general formula (1) in the entire ligand is It is preferably 40 mol % or more, more preferably 50 mol % or more, and even more preferably The proportion of mercapto groups represented by general formula (1) in the total ligands is 60 mol % or more. By setting the content of the fatty acid ester in the above range, it is possible to highly concentrate the semiconductor nanoparticles in the polar solvent. It is possible to achieve high dispersion and high quantum efficiency.

[0086] The semiconductor nanoparticle composite (A) of the present invention may be in the following first form. The first embodiment of the semiconductor nanoparticle composite (A) of the present invention is The molecular weight of the mercapto fatty acid ester represented by the general formula (1) is 300 or more and 700 or less. and preferably 300 or more and 600 or less.

[0087] That is, the first embodiment of the semiconductor nanoparticle composite (A) of the present invention is a semiconductor nanoparticle having a surface a semiconductor nanoparticle complex having a ligand coordinated thereto, The semiconductor nanoparticles have a core containing In and P and one or more shell layers. Core / shell type semiconductor nanoparticles, The semiconductor nanoparticles further contain a halogen, and in the semiconductor nanoparticles, In the calculation, the molar ratio of halogen to In is 0.80 to 15.00; The ligand has the following general formula (1): HS-R1-COO-R2(1) (In general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group.) The composition contains one or more mercapto fatty acid esters represented by the formula: The SP value of the mercapto fatty acid ester is 9.20 or more, and the mercapto fatty acid The molecular weight of the ester is 300 or more and 700 or less, preferably 300 or more and 600 or less, and the average SP value of the entire ligand is 9.10 to 11.00; The semiconductor nanoparticle composite is characterized by the following: By having the molecular weight of the ester in the above range, the semiconductor nanoparticles can be dispersed in an organic solvent. This ensures sufficient steric hindrance, making it possible to disperse the material at a higher concentration. In the present invention, the heat resistance of the semiconductor nanoparticle composite is improved. When the particle composite is heat-treated at a certain temperature, the particles are re-dispersed in the solvent before the heat treatment. This means that it is distributable.

[0088] As one embodiment of the evaluation of heat resistance, the semiconductor nanoparticle composite was heated at 180 After treating at ℃ for 1 hour, judge whether the semiconductor nanoparticle composite can be redispersed in a good solvent. Semiconductor nanoparticle composites that do not have sufficient heat resistance may deteriorate due to denaturation or elimination of the ligands. Dispersibility in a good solvent decreases significantly after heating.

[0089] In the first embodiment of the semiconductor nanoparticle complex (A) of the present invention, the quality of the ligand and the semiconductor nanoparticles is The ratio (ligand / semiconductor nanoparticle) is preferably 1.00 or less, and more preferably 0.70 or less. The mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor) is preferably less than 1. By keeping the content of nanoparticles within the above range, the heat resistance of the semiconductor nanoparticle composite can be maintained. This makes it possible to disperse semiconductor nanoparticles in a polar solvent at a high concentration.

[0090] In the first embodiment of the semiconductor nanoparticle composite (A) of the present invention, the ligand and the semiconductor nanoparticle It is preferable that the mass ratio of the ligand to the semiconductor nanoparticles is 0.40 or more. The mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is within the above range. This allows the semiconductor nanoparticles to be concentrated in a polar solvent while maintaining the heat resistance of the semiconductor nanoparticle composite. It is possible to distribute the

[0091] The semiconductor nanoparticle composite (A) of the present invention may be of the following second embodiment. The second form of the semiconductor nanoparticle composite (A) of the present invention is Among them, the molecular weight of the mercapto fatty acid ester represented by the general formula (1) is less than 300. A conductive nanoparticle composite.

[0092] That is, the second form of the semiconductor nanoparticle composite (A) of the present invention is a semiconductor nanoparticle having a surface a semiconductor nanoparticle complex having a ligand coordinated thereto, The semiconductor nanoparticles have a core containing In and P and one or more shell layers. Core / shell type semiconductor nanoparticles, The semiconductor nanoparticles further contain a halogen, and in the semiconductor nanoparticles, In the calculation, the molar ratio of halogen to In is 0.80 to 15.00; The ligand has the following general formula (1): HS-R1-COO-R2(1) (In general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group.) The composition contains one or more mercapto fatty acid esters represented by the formula: The SP value of the mercapto fatty acid ester is 9.20 or more, and the mercapto fatty acid The molecular weight of the ester is less than 300, preferably 100 or more and less than 300; and the average SP value of the entire ligand is 9.10 to 11.00; The semiconductor nanoparticle composite is characterized by the following: By having the molecular weight of the ster be within the above range, the semiconductor nanoparticle composite can be dispersed at a high mass fraction. In the present invention, the viscosity of the dispersion can be reduced by using a semiconductor nanoparticle complex. The viscosity of the dispersion liquid when the composite is dispersed at a high mass fraction is low when the semiconductor nanoparticle composite is The semiconductor nanoparticles were dispersed in isobornyl acrylate so that the mass ratio of the semiconductor nanoparticles was 30.0 mass%. This means that when dispersed, the viscosity at 25°C is 30 cp or less.

[0093] In the second embodiment of the semiconductor nanoparticle complex (A) of the present invention, the quality of the ligand and the semiconductor nanoparticles is The ratio of the ligand to the semiconductor nanoparticles is preferably 0.40 or less. When the mass ratio of the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is within the above range, The present invention provides a method for dispersing semiconductor nanoparticles while suppressing an increase in the viscosity of a dispersion in which the semiconductor nanoparticle composite is dispersed. It is possible to disperse it at a high concentration in a polar solvent.

[0094] The semiconductor nanoparticle composite (B) of the present invention comprises a core containing In and P and one or more layers of and a shell, and the core / shell type semiconductor nanoparticles further contain halogen and are capable of being substituted with an atomic group. In calculation, the molar ratio of halogen to In is 0.80 to 15.00. contacting one end of the semiconductor nanoparticle with a surface modifying compound having a binding group capable of binding to the semiconductor nanoparticle; A semiconductor nanoparticle composite obtained by The surface modifying compound is represented by the following general formula (1): HS-R1-COO-R2(1) (In general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group.) The composition contains one or more mercapto fatty acid esters represented by the formula: The SP value of the mercapto fatty acid ester is 9.20 or more, and the mercapto fatty acid The molecular weight of the ester is 700 or less, and the average SP value of the entire surface modifying compound is 9.10 to 11.00; The semiconductor nanoparticle composite is characterized by the following:

[0095] The semiconductor nanoparticle composite (B) of the present invention is a semiconductor nanoparticle having a semiconductor nanoparticle on one end side. A semiconductor nanotube obtained by contacting a surface modifying compound having a bonding group that bonds to The method for contacting the semiconductor nanoparticles with the surface modifying compound is not particularly limited. Although it is not known how to do this, one method is to add a surface modifying compound to a dispersion of semiconductor nanoparticles. Depending on the binding strength of the surface modifying compound to the semiconductor nanoparticles, The addition may be accompanied by heating or stirring.

[0096] The semiconductor nanoparticles according to the semiconductor nanoparticle composite (B) of the present invention are The same applies to the semiconductor nanoparticles related to the child complex (A).

[0097] Binding group related to a surface modification compound having a binding group at one end thereof that binds to semiconductor nanoparticles Examples of the aryl group include a thiol group, a carboxylic acid group, a phosphine group, a phosphine oxide group, and an amine group. Examples of surface modification compounds having a group capable of binding to semiconductor nanoparticles on one end include and the ligand related to the semiconductor nanoparticle composite (A) of the present invention.

[0098] In the semiconductor nanoparticle composite (B) of the present invention, a bonding property that bonds to a semiconductor nanoparticle at one end is As a surface modifying compound having a group, a mercapto fatty acid ester represented by the following general formula (1) is used. Includes Tell. HS-R1-COO-R2(1)

[0099] In the semiconductor nanoparticle composite (B) of the present invention, the surface modifying compound represented by general formula (1) The mercapto fatty acid ester represented by the following formula (1) is The same applies to the mercapto fatty acid ester represented by the general formula (1).

[0100] In the semiconductor nanoparticle composite (B) of the present invention, a mercapto lipid represented by general formula (1) is By using fatty acid esters as surface modification compounds, the fluorescence quantum efficiency is high and the half-value Narrow semiconductor nanoparticle composites can be obtained.

[0101] In the semiconductor nanoparticle composite (B) of the present invention, a mercapto lipid represented by general formula (1) is The molecular weight of the fatty acid ester is 700 or less. The molecular weight of the ester is 700 or less, so semiconductor nanoparticles can be dispersed in polar solvents at high concentrations. It is possible to do so.

[0102] In the semiconductor nanoparticle composite (B) of the present invention, a mer represented by general formula (1) The SP value of the caprylic fatty acid ester is 9.20 or more, preferably 9.20 to 12.00. When the SP value is within the above range, the semiconductor nanoparticles can be dispersed in a polar solvent. It becomes Noh.

[0103] In the semiconductor nanoparticle composite (B) of the present invention, a bond that is bonded to a semiconductor nanoparticle at one end is As a surface modifying compound having a synthetic group, a mercapto fatty acid ester represented by the general formula (1) is used. The surface modification compound represented by the general formula (1) can be used. As a surface modification compound other than the rucapto fatty acid ester, There are no particular limitations on the compound, so long as it has a bonding group that bonds to the surface of the semiconductor nanoparticle. A mercapto fatty acid that can be used as a modifying compound and is represented by the general formula (1): When used in combination with esters, the average SP value of all surface modification compounds is 9.20 to 11.00. Preferably, it is possible to adjust the range to 9.20 to 10.00.

[0104] The SP value of a surface modifying compound other than the mercapto fatty acid ester represented by the general formula (1) is Although not particularly limited, it is preferably 7.00 to 15.00, and particularly preferably 7.50 to 1 It is 5.00.

[0105] The average S of all surface modification compounds having a bonding group on one end that bonds to semiconductor nanoparticles The P value is 9.20 to 11.00, preferably 9.20 to 10.00. The average SP value of all surface modifying compounds having a binding group that binds to the body nanoparticles is within the above range. This allows the semiconductor nanoparticles to be dispersed in a polar solvent.

[0106] Examples of surface modifying compounds other than the mercapto fatty acid ester represented by the general formula (1) include: An aliphatic group having a bonding group at one end that bonds to a semiconductor nanoparticle and an aliphatic group at the other end As the surface modifying compound, an aliphatic group-containing surface modifying compound is preferred. By including the compound, the semiconductor nanoparticles can be dispersed in a polar solvent at a high concentration. In addition, it is possible to disperse the composition in an organic solvent having a wider range of SP values. In addition, when applied to dispersion liquids, it becomes possible to expand the options for dispersion media.

[0107] Examples of the aliphatic group-containing surface modification compound include aliphatic thiols, aliphatic carboxylic acids, and aliphatic Examples include phosphine, aliphatic phosphine oxide, and aliphatic amine. Due to the strong coordination power with aliphatic thiols, aliphatic carboxylic acids, and aliphatic phosphines, It is preferable that the aliphatic group of the aliphatic group-containing surface modification compound is one or more selected from the group consisting of , may contain substituents and heteroatoms.

[0108] A surface modification compound having a bonding group at one end thereof that bonds to a semiconductor nanoparticle is The content of the mercapto fatty acid ester represented by the general formula (1) is 40 mol % or more. It is preferable that the content of the fluorine-containing compound is 50 mol % or more, more preferably 60 mol % or more. The proportion of all surface modification compounds having a bonding group on one end that bonds to semiconductor nanoparticles is By setting the content of the mercapto fatty acid ester represented by the general formula (1) in the above range, Semiconductor nanoparticles can be dispersed in polar solvents at high concentrations and have high quantum efficiency.

[0109] The semiconductor nanoparticle composite (B) of the present invention may be in the following first form: The first embodiment of the semiconductor nanoparticle composite (B) of the present invention is The molecular weight of the mercapto fatty acid ester represented by the general formula (1) is 300 or more and 700 or less. and preferably 300 or more and 600 or less.

[0110] That is, the first form of the semiconductor nanoparticle composite (B) of the present invention contains In and P. The core / shell type semiconductor nanoparticles have a core and one or more shell layers, and further have a halo. The molar ratio of halogen to In is 0.80 to 15.00 in atomic terms. A surface modification compound having a bonding group on one end side capable of bonding to the semiconductor nanoparticles is provided. a semiconductor nanoparticle composite obtained by contacting a The surface modifying compound is represented by the following general formula (1): HS-R1-COO-R2(1) (In general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group.) The composition contains one or more mercapto fatty acid esters represented by the formula: The SP value of the mercapto fatty acid ester is 9.20 or more, and the mercapto fatty acid The molecular weight of the ester is 300 or more and 700 or less, preferably 300 or more and 600 or less, and the average SP value of the entire surface modifying compound is 9.10 to 11.00; The semiconductor nanoparticle composite is characterized by the following: By having the molecular weight of the ester in the above range, the semiconductor nanoparticles can be dispersed in an organic solvent. This ensures sufficient steric hindrance, making it possible to disperse the material at a higher concentration. The heat resistance of the nanoparticle composite is improved.

[0111] In the first embodiment of the semiconductor nanoparticle composite (B) of the present invention, a surface modifying compound and a semiconductor nanoparticle are The mass ratio of the particles (surface modifying compound / semiconductor nanoparticles) is preferably 1.00 or less. The surface modification compound and the semiconductor nanoparticles are preferably 0.70 or less. By having the mass ratio (surface modifying compound / semiconductor nanoparticles) in the above range, To disperse semiconductor nanoparticles in a polar solvent at a high concentration while maintaining the heat resistance of the particle complex This becomes possible.

[0112] In the first embodiment of the semiconductor nanoparticle composite (B) of the present invention, a surface modifying compound and a semiconductor The mass ratio of the semiconductor nanoparticles (surface modification compound / semiconductor nanoparticles) is 0.40 or more. The mass ratio of the surface modifying compound to the semiconductor nanoparticles (surface modifying compound / semiconductor nanoparticles) is preferably By the fact that the particle size is within the above range, the heat resistance of the semiconductor nanoparticle composite is maintained, It becomes possible to disperse semiconductor nanoparticles in a polar solvent at a high concentration.

[0113] The semiconductor nanoparticle composite (B) of the present invention may be of the following second embodiment. The second form of the semiconductor nanoparticle composite (B) of the present invention is Among them, the molecular weight of the mercapto fatty acid ester represented by the general formula (1) is less than 300. A conductive nanoparticle composite.

[0114] That is, the second type of the semiconductor nanoparticle composite (B) of the present invention contains In and P. The core / shell type semiconductor nanoparticles have a core and one or more shell layers, and further have a halo. The molar ratio of halogen to In is 0.80 to 15.00 in atomic terms. A surface modification compound having a bonding group on one end thereof that can be bonded to the semiconductor nanoparticles is provided. a semiconductor nanoparticle composite obtained by contacting a The surface modifying compound is represented by the following general formula (1): HS-R1-COO-R2(1) (In general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group.) The composition contains one or more mercapto fatty acid esters represented by the formula: The SP value of the mercapto fatty acid ester is 9.20 or more, and the mercapto fatty acid The molecular weight of the ester is less than 300, preferably 100 or more and less than 300; and the average SP value of the entire surface modifying compound is 9.10 to 11.00; The semiconductor nanoparticle composite is characterized by the following: By having the molecular weight of the ester in the above range, the dispersion liquid in which the semiconductor nanoparticle composite is dispersed can be The viscosity can be reduced.

[0115] In the second embodiment of the semiconductor nanoparticle composite (B) of the present invention, a surface modifying compound and a semiconductor nanoparticle are The mass ratio of the particles (surface modifying compound / semiconductor nanoparticles) is preferably 0.40 or less. The mass ratio of the surface modification compound to the semiconductor nanoparticles (surface modification compound / semiconductor nanoparticles) ) is within the above range, the viscosity of the dispersion in which the semiconductor nanoparticle composite is dispersed is increased. It is possible to disperse semiconductor nanoparticles in a polar solvent at a high concentration while suppressing the addition of the nanoparticles.

[0116] (Regarding purification) The semiconductor nanoparticle composite of the present invention can be separated and purified from the reaction solution, if necessary. As a purification method, the semiconductor nanoparticle composite is aggregated using a poor solvent, and then the semiconductor nanoparticle composite is A method for isolating the body-nanoparticle complex is used.

[0117] In one embodiment, the semiconductor nanoparticles are dissolved in a polarity-reversing solvent such as acetone. The nanoparticle complex can be precipitated from the dispersion. The precipitated nanoparticle complex can be filtered or The reaction mixture can be recovered by centrifugation or by other methods, while the remaining fraction contains unreacted starting materials and other impurities. The supernatant containing the semiconductor nanoparticle composite can be discarded or reused. The mixture can be washed with additional dispersion medium and dispersed again. This purification process can be carried out, for example, by This can be repeated 2-4 times or until the desired purity is reached.

[0118] In the present invention, in addition to the above-mentioned methods, the semiconductor nanoparticle composite can be purified by the following methods. For example, flocculation, liquid-liquid extraction, distillation, electrodeposition, size exclusion chromatography and / or ultrafiltration. Any of the methods may be used alone or in combination.

[0119] (Semiconductor nanoparticle composite dispersion) The semiconductor nanoparticle composite of the present invention is dispersed in a polar dispersion medium. In the present invention, the semiconductor nanoparticle composite is dispersed in a dispersion medium. The state where the semiconductor nanoparticle composite is in a ... The complex does not precipitate or remain as a visible turbidity (cloudiness) The semiconductor nanoparticle composite dispersed in a dispersion medium is called a semiconductor nanoparticle. This is referred to as a composite dispersion.

[0120] The semiconductor nanoparticle composite of the present invention is an organic dispersion medium having an SP value of 8.50 or more, and further an SP It also disperses in organic dispersion media with an SP value of 9.00 or more and organic dispersion media with an SP value of 10.00 or more. A dispersion of the solid nanoparticle complex is formed.

[0121] The SP value here is determined by the Hansen Solubility Plot, similar to the method for determining the SP value of the polar ligand. The Hansen solubility parameters are calculated from the Hansen parameters in the Handbook, e.g. "Hansen Solubility Parameters: A User's Handbook”, 2nd ed., C. M. Hansen (2007), Practice provided by Hanson and Abbot et al. The HSPiP program (2nd edition) can be used to determine the HSPiP score. For organic dispersion media not listed in the above, the content can be determined by calculation using the Y-MB method.

[0122] In the present invention, the organic dispersion medium of the semiconductor nanoparticle composite dispersion liquid of the present invention is methanol, Alcohols such as ethanol, isopropyl alcohol, and normal propyl alcohol , acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclo Ketones such as hexanone, methyl acetate, ethyl acetate, isopropyl acetate, normal acetate Esters such as propyl, n-butyl acetate, and ethyl lactate, diethyl ether, dipropyl Ethers such as propyl ether, dibutyl ether, and tetrahydrofuran; Recol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol Cholesterol monomethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, propylene glycol monomethyl ether (PGME), Glycol monoethyl ether, propylene glycol monopropyl ether, propylene Propylene glycol monobutyl ether, propylene glycol dimethyl ether, dipropylene Dimethyl ether, propylene glycol, diethyl ether, dipropylene glycol Glycol ethers such as ethylene glycol diethyl ether, ethylene glycol acetate Ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate Diethylene glycol monobutyl ether acetate, propyl Propylene glycol monomethyl ether acetate (PGMEA), dipropylene glycol Glycol ether esters such as monoethyl ether acetate are preferred. By dispersing the semiconductor nanoparticle composite of the present invention in these organic dispersion media, the hardened nanoparticles described below can be obtained. When applying it to dispersion in a synthetic film or resin, the semiconductor nanoparticle composite can be used while maintaining its dispersibility. It is possible.

[0123] In particular, in the semiconductor nanoparticle composite of the present invention, the organic dispersion medium is preferably an alcohol, Select polar organic dispersion media such as glycol ethers and glycol ether esters It becomes possible to disperse the semiconductor nanoparticle composite of the present invention in these organic dispersion media. This makes it possible to improve the dispersion of the semiconductor nanoparticle composite when applying it to dispersion in cured films and resins, which will be described later. In particular, in the field of photoresists, PGMEA and PGME is commonly used as a diluent, and semiconductor nanoparticle composites are If the semiconductor nanoparticle complex can be dispersed in A and PGME, it can be widely used in the photoresist field. It can be widely applied.

[0124] The semiconductor nanoparticle composite of the present invention has the above-mentioned configuration. can be dispersed in an organic dispersion medium at a high mass fraction, resulting in a semiconductor nanoparticle composite particle. The mass fraction of the semiconductor nanoparticles in the dispersion is 20 mass% or more, and further 30 mass% or more; Furthermore, it can be set to 35 mass % or more.

[0125] Furthermore, in the present invention, a monomer is used as a dispersion medium for the semiconductor nanoparticle composite dispersion liquid of the present invention. The monomer is not particularly limited, but may be selected from the group consisting of the following monomers, depending on the application of the semiconductor nanoparticles: It is preferable that the (meth)acrylic monomer is one that can be selected from a wide range of options. Depending on the application of the semiconductor nanoparticle composite dispersion, the monomer is selected from methyl (meth)acrylate, ethylenediaminetetraacetate ... Cetyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate Isobutyl (meth)acrylate, Isoamyl (meth)acrylate, Octyl (meth)acrylate meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (Meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate Acrylate, 3,5,5-trimethylcyclohexanol (meth)acrylate, disil Ropentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, methoxy Diethyl (meth)acrylate, Ethyl carbitol (meth)acrylate, Methoxy Triethylene glycol acrylate, 2-ethylhexyl diglycol acrylate, Toxic polyethylene glycol acrylate, methoxydipropylene glycol acrylate acrylate, phenoxyethyl (meth)acrylate, 2-phenoxydiethylene glycol ( meth)acrylate, 2-phenoxypolyethylene glycol (meth)acrylate (n ≒2), Tetrahydrofurfuryl (meth)acrylate, 2-hydroxyethyl acrylate acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate Acrylate, 2-hydroxybutyl (meth)acrylate, dicyclopentanyloxyl Ethyl (meth)acrylate, isobornyloxyethyl (meth)acrylate, ada Manthyl (meth)acrylate, Dimethyl adamantyl (meth)acrylate, Dicyclo Pentenyloxyethyl (meth)acrylate, benzyl (meth)acrylate, ω-capryloxyethyl (meth)acrylate Polycaprolactone (n≒2) monoacrylate, 2-hydroxy-3-phenyl Phenoxypropyl acrylate, 2-hydroxy-3-phenoxyethyl (meth)acrylate ate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl(meth)ate Acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, o-F Phenylphenol ethoxy (meth)acrylate, dimethylamino (meth)acrylate , diethylamino(meth)acrylate, 2-(meth)acryloyloxyethyl phthalate Acid, 2-(meth)acryloyloxyethylhexahydrophthalate, glycidyl (meth) Acrylates, 2-(meth)acryloyloxyethyl phosphate, acryloylmorpholine , dimethylacrylamide, dimethylaminopropylacrylamide, isopropylacrylamide acrylamide, diethylacrylamide, hydroxyethylacrylamide, and N- From (meth)acrylic monomers such as acryloyloxyethylhexahydrophthalimide These can be used alone or in combination of two or more. In particular, acrylic monomers can be used in combination with Laurie depending on the application of the semiconductor nanoparticle composite dispersion liquid. 1,6-hexadiol di(meth)acrylate and 1,6-hexadiol di(meth)acrylate It is preferable to use one or a mixture of two or more of the above-mentioned compounds.

[0126] In the present invention, a prepolymer is used as a dispersion medium for the semiconductor nanoparticle composite dispersion of the present invention. The prepolymer is not particularly limited, but an acrylic resin prepolymer can be selected. Examples of suitable resins include silicone resin prepolymers, silicone resin prepolymers, and epoxy resin prepolymers.

[0127] (Semiconductor nanoparticle composite composition) In the present invention, a monomer or a polymer is used as a dispersion medium for the semiconductor nanoparticle composite dispersion of the present invention. The copolymer can be selected to form a semiconductor nanoparticle composite composition. The semiconductor nanoparticle composite composition of the present invention is a semiconductor nanoparticle composite of the present invention. The present invention relates to a semiconductor nanoparticle composite composition dispersed in a prepolymer. The polymer is not particularly limited, but may be a radical polymerizable compound containing an ethylenically unsaturated bond, oxane compounds, epoxy compounds, isocyanate compounds, and phenol derivatives, etc. Examples of the monomer include the monomers used as the dispersion medium described above. In addition, the prepolymer may be the prepolymer used as the dispersion medium described above. - are some examples.

[0128] Furthermore, the semiconductor nanoparticle composite composition of the present invention can contain a crosslinking agent. Depending on the type of monomer in the semiconductor nanoparticle composite composition of the present invention, Acrylates, polyfunctional silane compounds, polyfunctional amines, polyfunctional carboxylic acids, polyfunctional thiols , polyfunctional alcohols, and polyfunctional isocyanates.

[0129] Furthermore, the semiconductor nanoparticle composite composition of the present invention can be used in a wide range of solvents, including pentane, hexane, cyclohexanone, aliphatic hydrocarbons such as hexane, isohexane, heptane, octane and petroleum ether; Coals, ketones, esters, glycol ethers, glycol ether esters aromatic hydrocarbons such as benzene, toluene, xylene and mineral spirits; and alkyl halides such as dichloromethane and chloroform, which do not affect curing. The organic solvent may further contain various organic solvents. It can be used not only for diluting the composition but also as an organic dispersion medium. The semiconductor nanoparticle composite of the present invention is dispersed in the organic solvent, It is also possible to prepare a dispersion.

[0130] In addition, the semiconductor nanoparticle composite composition of the present invention is Depending on the type of mer, appropriate initiators, scattering agents, catalysts, binders, surfactants, adhesion promoters, etc. The additives may include additives, antioxidants, UV absorbers, anti-agglomerating agents, and dispersants.

[0131] Furthermore, the semiconductor nanoparticle composite composition of the present invention or the semiconductor nanoparticle of the present invention described later In order to improve the optical properties of the particle composite cured film, the semiconductor nanoparticle composite composition is The scattering agent may be a metal oxide such as titanium oxide or zinc oxide. From the viewpoint of scattering effect, the particle diameter of the scattering agent is preferably 100 nm to 500 nm. It is more preferable that the diameter is 200 nm to 400 nm. The luminous intensity is increased by about two times. The content of the composition is preferably 2% by mass to 30% by mass, and the composition is more preferably 2% by mass to 30% by mass in order to maintain the patternability of the composition. From this viewpoint, it is more preferable that the content is 5% by mass to 20% by mass.

[0132] Due to the configuration of the semiconductor nanoparticle composite of the present invention, The mass fraction of the semiconductor nanoparticles can be 30 mass % or more. By setting the mass fraction of the semiconductor nanoparticles in the body composition to 30 mass % to 95 mass %, The present invention also provides a method for dispersing semiconductor nanoparticle composites and semiconductor nanoparticles at a high mass fraction in a cured film formed by the above-mentioned method. can be done.

[0133] When the semiconductor nanoparticle composite composition of the present invention is formed into a 10 μm film, the normal direction of the film The absorbance of the light having a wavelength of 450 nm from the More preferably, the ratio is 1.5 or more, and even more preferably, 1.5 or more. Because it can efficiently absorb black light, it can reduce the thickness of the cured film described below. The device to which it is applied can be made smaller.

[0134] (Diluted Composition) The diluted composition is the semiconductor nanoparticle composite composition of the present invention that is diluted with an organic solvent. This is what we have in mind.

[0135] The organic solvent for diluting the semiconductor nanoparticle composite composition is not particularly limited, and examples thereof include For example, pentane, hexane, cyclohexane, isohexane, heptane, octane and cyclohexane. Aliphatic hydrocarbons such as oil ethers, alcohols, ketones, esters, glycol ethers, etc. ethers, glycol ether esters, benzene, toluene, xylene and minerals Aromatic hydrocarbons such as dichloromethane and chloroform, and halogenated hydrocarbons such as dichloromethane and chloroform. Among these, alkyl esters that have a wide range of solubility in resins and can be used to coat films are From the viewpoint of film uniformity, glycol ethers and glycol ether esters are preferred. I wish.

[0136] (Cured film of semiconductor nanoparticle composite) The semiconductor nanoparticle composite cured film of the present invention is a film containing the semiconductor nanoparticle composite of the present invention. The cured film of the semiconductor nanoparticle composite of the present invention is a film that is cured. The conductive nanoparticle composite composition or the diluted composition is cured to form a film.

[0137] The semiconductor nanoparticle composite cured film of the present invention is a cured film of the semiconductor nanoparticle composite of the present invention. The nanoparticles and the ligands coordinated to the surface of the semiconductor nanoparticles and the polymer matrix are included. In other words, the semiconductor nanoparticle composite cured film of the present invention is The body is a hardened membrane dispersed in a polymer matrix.

[0138] The polymer matrix is ​​not particularly limited, but may be (meth)acrylic resin, silicone, etc. Resin, epoxy resin, silicone resin, maleic acid resin, butyral resin, polyester Resin, melamine resin, phenolic resin, polyurethane resin, etc. The semiconductor nanoparticle composite composition of the present invention is cured to obtain the semiconductor nanoparticles of the present invention. A cured film of the semiconductor nanoparticle composite of the present invention may be obtained. That's fine.

[0139] The method for hardening the film is not particularly limited, but may be a heat treatment, an ultraviolet treatment, or the like. The film can be cured by a curing method suitable for the material.

[0140] The semiconductor nanoparticles and the semiconductor nanoparticles contained in the semiconductor nanoparticle composite cured film of the present invention The ligands coordinated to the surface of the nanoparticles constitute the semiconductor nanoparticle composite of the present invention. The semiconductor nanoparticle composite contained in the cured film of the semiconductor nanoparticle composite of the present invention is preferably By configuring as described above, the semiconductor nanoparticle composite can be contained in the cured film at a higher mass fraction. The mass of the semiconductor nanoparticles in the cured film of the semiconductor nanoparticle composite can be The fraction is preferably 30% by mass or more, and more preferably 40% by mass or more. However, if the content is more than 70% by mass, the composition constituting the film becomes small, and the film becomes hard. It becomes difficult to form a solid.

[0141] The semiconductor nanoparticle composite cured film of the present invention contains semiconductor nanoparticle composites at a high mass fraction. Therefore, the absorbance of the cured film of the semiconductor nanoparticle composite can be increased. When the thickness of the cured film of the semiconductor nanoparticle composite is 10 μm, the normal line of the cured film of the semiconductor nanoparticle composite is For light with a wavelength of 450 nm coming from the direction, the absorbance should be 1.0 or more, and 1.3 or more is preferable. It is more preferable that the ratio is 1.5 or more, and further preferably 1.5 or more.

[0142] Furthermore, the semiconductor nanoparticle composite cured film of the present invention contains semiconductor nanoparticles having high light-emitting properties. Because it contains a particle composite, it is possible to provide a cured film of a semiconductor nanoparticle composite with high luminescence properties. The fluorescence quantum efficiency of the cured film of the semiconductor nanoparticle composite of the present invention is preferably 70% or more. It is preferable that the content is 80% or more.

[0143] The thickness of the semiconductor nanoparticle composite cured film of the present invention is determined based on the thickness of the cured film to be applied. In order to miniaturize the device, the thickness is preferably 50 μm or less, and more preferably 20 μm or less. It is more preferable that the thickness is 10 μm or less, and further more preferable that the thickness is 10 μm or less.

[0144] (Semiconductor nanoparticle composite patterned film and display element) The semiconductor nanoparticle composite patterned film is formed by the above-mentioned semiconductor nanoparticle composite composition or The semiconductor nanoparticle composite composition can be obtained by forming a film pattern from the solution composition. The method for forming a pattern from the product and the diluted composition is not particularly limited, and may be, for example, spin coating, These include bar coating, inkjet, screen printing, and photolithography. do.

[0145] The display element uses the above-mentioned semiconductor nanoparticle composite patterned film. For example, By using a semiconductor nanoparticle composite patterned film as a wavelength conversion layer, it is possible to obtain an excellent fluorescence intensity. It is possible to provide a display device having high pixel efficiency.

[0146] The compositions and / or methods described herein are presented as examples and are susceptible to numerous variations. Therefore, it should be understood that these specific examples or examples should not be construed in a limiting sense. It will be understood that the particular procedure or method described herein represents one of many possible processing methods. Accordingly, the various acts described and / or described may be Similarly, the steps of the method described above may be performed in the order listed or may be omitted. is mutable.

[0147] The subject matter of the present disclosure relates to various methods, systems, and configurations disclosed herein, as well as other Any novel and non-obvious combination of features, functions, acts, and / or properties of This includes all combinations and subcombinations, and all equivalents thereof. EXAMPLES

[0148] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited thereto. It is not something that is done.

[0149] (Ligand) The ligands used in the examples and comparative examples were prepared as follows. PEG refers to a polyethylene glycol chain, and is represented by the formula -(CH2CH2O) n -CH3" This is the structure represented by the following formula: <Preparation of single ligand> (Method for preparing 1,1-dimethyl-3-oxobutyl mercaptopropionate) A flask was charged with 4.2 g of 3-mercaptopropionic acid (40 mmol) and 4.7 g of di Cetone alcohol (40 mmol), 5.4 g of 1-hydroxybenzotriazole (4 0 mmol), 100 mL of methylene chloride and 7.7 g of 1-ethyl-3-(3- Dimethylaminopropyl)carbodiimide (40 mmol) was mixed under a nitrogen atmosphere. After the solution was reacted at room temperature for 60 minutes, the reaction solution was transferred to a separatory funnel and separated with saturated sodium bicarbonate water, water, The organic phase was washed with saturated saline in sequence, and then dried over magnesium sulfate. The concentrate was then filtered and concentrated by evaporation. The desired ligand (mercaptocarbamate) was purified by column chromatography using the developing solvent. The compound was obtained by eluting the 1,1-dimethyl-3-oxobutyl butyrate.

[0150] (Preparation method of thioglycolic acid PEG ester (molecular weight 470)) A flask was charged with 3.7 g of thioglycolic acid (40 mmol) and 19.2 g of methoxy PE. G-OH (molecular weight 400, 48 mmol) and 0.2 g of concentrated sulfuric acid were mixed under a nitrogen atmosphere. The solution was stirred at 60°C, the pressure was reduced to 30 mmHg or less, and the reaction was carried out for 24 hours. After cooling the reaction solution to room temperature, it was dissolved in toluene and washed in turn with saturated sodium bicarbonate water, water, and saturated saline. The organic phase was dried over magnesium sulfate, filtered, and then eluted. The desired ligand (thioglycolic acid PEG ester, molecular Amount 470) was obtained.

[0151] (Preparation method of thioglycolic acid PEG ester (molecular weight 760)) Methoxy PEG-OH (molecular weight 400, 48 mmol) was dissolved in methoxy PEG-OH (molecular weight The amount was changed to 690, 48 mmol) and the preparation was carried out in the same manner as above to obtain a thiol with a molecular weight of 760. Glycolic acid PEG ester was obtained.

[0152] (Preparation method of 3-mercaptopropionic acid PEG ester (molecular weight 550)) A flask was charged with 4.2 g of 3-mercaptopropionic acid (40 mmol) and 21.6 g of methionine. Toxo-PEG-OH (molecular weight 450, 48 mmol) and 0.2 g of concentrated sulfuric acid were The solution was stirred at 60°C under reduced pressure of 30 mmHg or less and reacted for 24 hours. The reaction solution was cooled to room temperature, dissolved in toluene, and then extracted with saturated sodium bicarbonate water, water, and saturated saline. The organic phase was dried over magnesium sulfate and then washed with water. The mixture was filtered and concentrated by evaporation to obtain the desired ligand (3-mercaptopropionic acid PEG ester, molecular weight 550) was obtained.

[0153] (Preparation method of 3-mercaptopropionic acid PEG ester (molecular weight 640)) Methoxy PEG-OH (molecular weight 450, 48 mmol) was dissolved in methoxy PEG-OH (molecular weight The amount was changed to 550, 48 mmol) and the preparation was carried out in the same manner as above to obtain 3- Mercaptopropionic acid PEG ester was obtained.

[0154] (3-Mercaptopropionic acid 2-[2-(2-acetoxyethoxy)ethoxy]ethyl ester (How to adjust) In a flask, add 2.1 g of 3-mercaptopropionic acid (20 mmol) and 1.2 g of acetic acid. (20 mmol), 7.2 g triethylene glycol (48 mmol), 100 mL Toluene and 0.2 g of concentrated sulfuric acid were mixed under a nitrogen atmosphere. The flask was fitted with a Dean star. The solution was stirred at 110°C for 24 hours in a flask equipped with a thermocouple. After cooling at 40°C, the mixture was washed with saturated sodium bicarbonate water, water, and saturated saline in that order. After drying over magnesium, it was filtered and concentrated by evaporation. The product was purified by column chromatography using hexane and ethyl acetate as developing solvents. The desired ligand (2-[2-(acetoxyethoxy)-3-mercaptopropionic acid) )Ethoxy]ethyl) was obtained.

[0155] (Method for preparing 6-mercaptohexanoic acid PEG ester) A flask was charged with 5.9 g of 6-mercaptohexanoic acid (40 mmol) and 19.2 g of meth 100 g of dimethyl ether (PEG-OH) (molecular weight 400, 48 mmol) and 0.2 g of concentrated sulfuric acid were placed in a nitrogen atmosphere. The solution was stirred at 60°C, the pressure was reduced to 30 mmHg or less, and the mixture was reacted for 24 hours. The reaction solution was cooled to room temperature, dissolved in toluene, and then extracted with saturated sodium bicarbonate water, water, and saturated saline. The organic phase was dried over magnesium sulfate, and then filtered. The desired ligand (6-mercaptohexanoic acid PE) was obtained by filtration and concentration by evaporation. G ester, molecular weight 530) was obtained.

[0156] (3-Mercaptopropionic acid 2-[2-(2-levulinoxyethoxy)ethoxy]ethyl) (How to adjust the A flask was filled with 2.1 g of 3-mercaptopropionic acid (20 mmol), 2.3 g of Lev. Phosphoric acid (20 mmol), 6.0 g triethylene glycol (40 mmol), 5.4 g of 1-hydroxybenzotriazole (40 mmol), 100 mL of methylene chloride and and 7.7 g of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride ( The solution was reacted at room temperature for 60 minutes, and then the reaction The solution was transferred to a separatory funnel and washed successively with saturated sodium bicarbonate water, water, and saturated saline. The organic phase was dried over magnesium sulfate, filtered and concentrated by evaporation. The concentrate was subjected to column chromatography using hexane and ethyl acetate as developing solvents. The desired ligand (3-mercaptopropionic acid 2-[2-(2-reductase) The resulting mixture was linoxy (ethoxy)ethoxy)ethyl.

[0157] (3-Mercaptopropionic acid 2-[2-[2-(2-hexyloxyethoxy)ethoxy] Preparation of ]ethoxy]ethyl A flask was filled with 4.2 g of 3-mercaptopropionic acid (40 mmol) and 13.4 g of tetrahydrofuran. Triethylene glycol monohexyl ether (48 mmol), 100 mL of toluene and 0.2 g of concentrated sulfuric acid were mixed under a nitrogen atmosphere. A Dean-Stark apparatus was attached to the flask. The solution was reacted for 24 hours while stirring at 110°C. After cooling the reaction solution to room temperature, The organic phase was washed with saturated sodium bicarbonate water, water, and saturated saline in that order. The concentrate was dried using a gel, filtered and concentrated by evaporation. The desired product was obtained by purifying it by column chromatography using ethyl acetate as a developing solvent. The ligand (2-[2-[2-(hexyloxyethoxy)-3-mercaptopropionic acid) )ethoxy]ethoxy]ethyl) was obtained.

[0158] [Example 1] An InP-based semiconductor nanoparticle composite was prepared according to the following method. (Preparation of core particles) Indium acetate (0.3 mmol) and zinc oleate (0.6 mmol) were dissolved in oleic acid. Acid (0.9 mmol), 1-dodecanethiol (0.1 mmol), and octadecene (10 mL), heated to about 120°C under vacuum (<20 Pa), and reacted for 1 hour. The mixture was reacted under vacuum, and then cooled to 25°C under a nitrogen atmosphere to obtain tris(trimethylsilyl) After adding phosphine (0.2 mmol), the mixture was heated to about 300°C and reacted for 10 minutes. The reaction mixture was cooled to 25°C, and octanoic acid chloride (1.1 mmol) was added. After heating at 0° C. for 30 minutes, the mixture was cooled to 25° C. to obtain a dispersion of InP-based semiconductor nanoparticles.

[0159] (Precursor for shell formation) In preparing the shell, the following precursors were first prepared. (Preparation of Zn precursor solution) 40 mmol of zinc oleate was mixed with 75 mL of octadecene and heated at 110°C in a vacuum. The mixture was heated at RT for 1 hour to prepare a Zn precursor with [Zn] = 0.4 M. (Preparation of Se precursor (trioctylphosphine selenide)) 22 mmol of selenium powder and 10 mL of trioctylphosphine were mixed in nitrogen. The mixture was stirred until dissolved to obtain trioctylphosphine selenide ([Se] = 2.2 M). (Preparation of S precursor (trioctylphosphine sulfide)) 22 mmol of sulfur powder and 10 mL of trioctylphosphine were mixed under nitrogen. The mixture was stirred until dissolved to give trioctylphosphine sulfide ([S] = 2.2 M).

[0160] Using each of the precursors obtained as described above, the InP-based semiconductor nanoparticles (cores) were A shell was formed on the surface as follows. (Shell formation) The core dispersion was heated to 200° C. At 250° C., 6.0 mL of Zn precursor solution was added. and 2.0 mL of trioctylphosphine selenide were added and reacted for 30 minutes to form an InP-based semiconductor. A ZnSe shell was formed on the surface of the nanoparticles. 1.8 mL of trioctylphosphine sulfide was added, the temperature was raised to 280°C, and the reaction was carried out for 1 hour. A ZnS shell was formed. The obtained semiconductor nanoparticles were observed by STEM-EDS, and the core / shell structure was confirmed. It was confirmed that the structure The solution in which the synthesized core / shell-type semiconductor nanoparticles were dispersed was mixed with dehydrated acetonitrile. The mixture was then centrifuged (4000 rpm, 10 min) to aggregate the semiconductor nanoparticles. ) After that, the supernatant was removed and the semiconductor nanoparticles were redispersed in hexane. This was repeated to Purified semiconductor nanoparticles were obtained.

[0161] (composition analysis) Elemental analysis of semiconductor nanoparticles was performed using a high-frequency inductively coupled plasma emission spectrometer (ICP) and The ICP measurement was performed using an X-ray fluorescence analyzer (XRF). After dissolving in nitric acid and heating, it was diluted with water and analyzed by an ICP emission spectrometer (Shimadzu Corporation, ICPS-81 00) was used for the calibration curve method. The specimen was placed in a pull holder and quantitative analysis was performed using an X-ray fluorescence analyzer (Rigaku, ZSX100e). The molar ratio of halogen to In in the semiconductor nanoparticles is shown in Table 1.

[0162] (Preparation of semiconductor nanoparticle composites) The purified semiconductor nanoparticles were placed in a flask at a mass ratio of 10% by mass. A 1-octadecene dispersion of semiconductor nanoparticles was prepared. 10.0 g of the 1-octadecene particle dispersion was placed in a flask, and the mercapto fatty acid ester was added. 3.6 g of thioglycolic acid PEG ester (molecular weight 470) was used as a non-polar ligand. Then, 0.4 g of dodecanethiol was added, and the mixture was stirred at 110°C for 60 minutes under a nitrogen atmosphere. The mixture was cooled to 5° C. to obtain a semiconductor nanoparticle composite. The reaction mixture was transferred to a centrifuge tube and centrifuged at 4000G for 20 minutes to obtain a clear 1-octadecameric peptide. The 1-octadecene phase was removed, and the remaining semiconducting nanoparticle composite phase was The conductor nanoparticle composite phase was recovered. 5.0 mL of acetone was added to the obtained semiconductor nanoparticle composite phase to prepare a dispersion liquid. 50 mL of normal hexane was added to the dispersion and centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was collected. This procedure was repeated several times. A purified semiconductor nanoparticle composite was obtained.

[0163] <Analysis> (Measurement of molecular weight of ligand) The molecular weight of the ligand was measured using a liquid chromatograph (LC-20: Shimadzu Corporation). This was done by GPC. First, the ligand was dissolved in THF (tetrahydrofuran) and The solution was dissolved in a column (KF-801, KF-803, KF-805: Shodex). The syneresis liquid was poured into the sample, and the number average molecular weight was calculated from the molecular weight distribution curve obtained. Polyethylene glycol (PGE) with a known average molecular weight is used. col READY_CAL SET Mp 102-40,000: Aldrich) Used.

[0164] (Fluorescence quantum efficiency measurement) The optical properties of the semiconductor nanoparticle composite were measured using a fluorescence quantum efficiency measurement system (Otsuka Electronics, QE-2 100) was used for the measurement. The semiconductor nanoparticle composite obtained by synthesis was dispersed in a dispersion medium. The emission spectrum was obtained by applying a single light of 450 nm as excitation light. The reexcitation compensation spectrum is the spectrum that excludes the reexcitation fluorescence emission spectrum of the reexcitation fluorescence emission spectrum. The fluorescence quantum efficiency (QY) and full width at half maximum (FWHM) were calculated from the emission spectrum after irradiation. The catalyst used was propylene glycol monomethyl ether acetate (PGMEA). The results are shown in Table 2.

[0165] ( 1 H-NMR measurement) The purified semiconductor nanoparticle complex was subjected to the purification of the ligands coordinated to the semiconductor nanoparticles. The results were analyzed using a nuclear magnetic resonance (NMR) spectrometer (JNM-LA400 manufactured by JEOL Ltd.). In all measurements, deuterated chloroform was used as the solvent and tetrahydrofuran was used as the internal standard for chemical shifts. Using tetramethylsilane, 1 The H-NMR was measured. From the complex, sigma due to the alkyl group of dodecanethiol was observed around 0.8 to 1.6 ppm. and a signal due to the polyethylene glycol skeleton at around 3.5 to 4.0 ppm. The abundance ratio of each ligand was calculated from the area ratio of these signals. Based on the abundance ratio of each ligand, the average SP value of all ligands and the mercapto group for all ligands were calculated. The ratio of fatty acid esters was calculated. The results are shown in Tables 1 and 3.

[0166] (Thermogravimetric analysis) The purified semiconductor nanoparticle complex was heated to 550℃ by differential thermogravimetry (DTA-TG). After heating, the sample was held for 10 minutes and then cooled. The residual mass after analysis was taken as the mass of the semiconductor nanoparticles. The mass ratio of the ligand to the semiconductor nanoparticles in the semiconductor nanoparticle complex (ligand / semiconductor nanoparticle) was calculated from The results are shown in Tables 1 and 3.

[0167] (Dispersibility test) With reference to the above mass ratio, the semiconductor nanoparticle composite is mixed with a semiconductor nanoparticle having a concentration of 20 The organic dispersion medium was added so that the concentration was 0.0 mass%, 30.0 mass%, and 35.0 mass%. The dispersion state of the powder was checked. Those that were dispersed were marked with a "○", and those that showed precipitation or turbidity were marked with a "○". The following are marked with "X" in Tables 2 and 4. PGMEA was used.

[0168] (Filterability test) A semiconductor nanoparticle composite PGMEA dispersion with a semiconductor nanoparticle concentration of 20.0 mass% was prepared. Filterability tests were conducted on samples that could be prepared. 1 mL of the composite PGMEA solution was weighed into a syringe and inserted into a PTFE syringe with a 0.45 μm aperture. The solution was filtered using a syringe filter (filter diameter 13 mm). Those that could be filtered were marked with a "〇", and those that became clogged were marked with an "×" in Tables 2 and 3. This is described in 4.

[0169] (Heat resistance test) 50 mg of the semiconductor nanoparticle composite was weighed into a sample tube and heated at 180°C in air. The samples were then cooled to room temperature and 1 mL of chloroform was added. The dispersion state of the powder was checked. Those that were dispersed were marked with a "○", and those that showed precipitation or turbidity were marked with a "○". Those that were not satisfactory are marked with an "X" in Tables 2 and 4.

[0170] (Viscosity measurement) The semiconductor nanoparticle composite was mixed with isopropanol so that the concentration of the semiconductor nanoparticles was 30.0 mass %. The resulting dispersion was then dispersed in 25% ethyl acrylate. Viscosity was measured using a TA Instruments AR-2000 rheometer at ℃ Measurement takes 0.1 seconds. -1 After pre-shearing for 1 minute, -1 From 1000s -1 The shear rate was changed from 100s to 100s. -1 The viscosity at is 30 cp or less. If it is more than 30cp and less than 60cp, it is marked with "◎", if it is more than 60cp, it is marked with "〇", if it is more than 60cp, it is marked with "〇". The results are shown in Tables 2 and 4. Samples for which the sobornyl acrylate dispersion could not be prepared are marked with a hyphen. Ta.

[0171] Example 2 In the process of preparing the semiconductor nanoparticle composite, 3-mercapto fatty acid ester is used. 3.2 g of PEG ester of butyropropionic acid (molecular weight 550) was used as an aliphatic ligand. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 0.8 g of leic acid was used.

[0172] Example 3 In the process of preparing a semiconductor nanoparticle composite, thioglycol is used as a mercapto fatty acid ester. 3.2 g of PEG ester of carboxylic acid (molecular weight 470) was used instead of the aliphatic ligand. A semiconductor was prepared in the same manner as in Example 1, except that 0.8 g of ethylhexyl caproate was used. The body-nanoparticle complexes were obtained.

[0173] Example 4 In the process of preparing the semiconductor nanoparticle composite, 3-mercapto fatty acid ester is used. 6.4 g of butyl propionate PEG ester (molecular weight 640) was used as an aliphatic ligand. A semiconductor nanoparticle composite was prepared in the same manner as in Example 1, except that 0.8 g of decanethiol was used. Got it.

[0174] Example 5 In the process of preparing a semiconductor nanoparticle composite, thioglycol is used as a mercapto fatty acid ester. 2.8 g of PEG ester of carboxylic acid (molecular weight 470) and dodecanethiol as an aliphatic ligand. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 1.2 g of the ruthenium oxide was used.

[0175] Example 6 In the process of preparing a semiconductor nanoparticle composite, thioglycol is used as a mercapto fatty acid ester. 2.4 g of PEG ester of carboxylic acid (molecular weight 470) and dodecanethiol as an aliphatic ligand. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 1.6 g of the ruthenium oxide was used.

[0176] Example 7 When preparing the dispersion of the core particles, 0.45 mmol of octanoic acid chloride was added to the semiconductor nanoparticles. When preparing the polymer complex, 3-mercaptopropionic acid PEG was used as the mercapto fatty acid ester. 3.6 g of ester (molecular weight 550) and 0.4 g of dodecanethiol as an aliphatic ligand A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that g was used.

[0177] Example 8 When preparing the dispersion of the core particles, 2.5 mmol of octanoic acid chloride was added to the semiconductor nanoparticle complex. When preparing the composite, 3-mercaptopropionic acid PEG ester is used as the mercapto fatty acid ester. The same procedure was carried out except that 3.8 g of tert-butyl ether and 0.2 g of dodecanethiol were used as the aliphatic ligand. In the same manner as in Example 1, a semiconductor nanoparticle composite was obtained.

[0178] Example 9 In the process of preparing the semiconductor nanoparticle composite, 3-mercapto fatty acid ester is used. 2-[2-[2-(2-hexyloxyethoxy)ethoxy]ethoxy]butyropropionic acid The same procedure was carried out except that 3.6 g of ethyl was used and 0.4 g of dodecanethiol was used as the aliphatic ligand. In the same manner as in Example 1, a semiconductor nanoparticle composite was obtained.

[0179] Example 10 In the process of preparing the semiconductor nanoparticle composite, 3-mercapto fatty acid ester is used. 3.8g 2-[2-(2-levulinoxyethoxy)ethoxy]ethyl butyl propionate The same method as in Example 1 was used except that 0.2 g of dodecanethiol was used as the aliphatic ligand. A semiconductor nanoparticle composite was obtained.

[0180] Example 11 In the process of preparing the semiconductor nanoparticle composite, 3-mercapto fatty acid ester is used. 3.6 g of 1,1-dimethyl-3-oxobutyl butyrate as an aliphatic ligand The same procedure as in Example 1 was repeated except that 0.4 g of trioctylphosphine was used. A child complex was obtained.

[0181] Example 12 When preparing the dispersion of the core particles, 0.45 mmol of octanoic acid chloride was added to the semiconductor nanoparticles. When preparing the molecular complex, 3-mercaptopropionic acid 3-mercapto fatty acid ester was used. The other compounds used were 3.2 g of butyl ether and 0.8 g of dodecanethiol as an aliphatic ligand. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1.

[0182] Example 13 When preparing the dispersion of the core particles, 2.5 mmol of octanoic acid chloride was added to the semiconductor nanoparticles. When preparing the complex, 1,1-3-mercaptopropionic acid was used as the mercapto fatty acid ester. 3.2 g of dimethyl-3-oxobutyl and 0.5 g of dodecanethiol as an aliphatic ligand. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 8 g was used.

[0183] Example 14 In the process of preparing the semiconductor nanoparticle composite, 3-mercapto fatty acid ester is used. 2.8 g of 3-methoxybutyl butyrate and 2.8 g of dodecanethiol as an aliphatic ligand. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 1.2 g of ruthenium was used.

[0184] Example 15 In the process of preparing the semiconductor nanoparticle composite, 3-mercapto fatty acid ester is used. 3.8 g of 2-[2-(2-acetoxyethoxy)ethoxy]ethyl butadiene The same method as in Example 1 was used except that 0.05 g of dodecanethiol was used as the aliphatic ligand. A semiconductor nanoparticle composite was obtained.

[0185] (Example 16) In the process of preparing the semiconductor nanoparticle composite, 3-mercapto fatty acid ester is used. 2.8 g of 3-methoxybutyl butyrate was used, and benzenethiol was used instead of the aliphatic ligand. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 1.2 g of ol was used.

[0186] (Example 17) In the shell formation reaction, after the ZnSe shell was formed, the Zn precursor solution and trisulfide were The mixture was cooled to room temperature without adding octylphosphine. In the process, 1,1-dimethyl 3-mercaptopropionate is used as the mercapto fatty acid ester. 3.2 g of ethyl-3-oxobutyl and 0.8 g of dodecanethiol as an aliphatic ligand A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that the above-mentioned compound was used.

[0187] Comparative Example 1 In the process of preparing the semiconductor nanoparticle composite, thioglycol is used as the mercapto fatty acid ester. 9.6 g of PEG ester of carboxylic acid (molecular weight 760) and dodecanethiol as an aliphatic ligand. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 0.8 g of the ruthenium oxide was used.

[0188] Comparative Example 2 When preparing the dispersion of the core particles, 4.5 mmol of octanoic acid chloride was added to the semiconductor nanoparticles. When preparing the complex, thioglycolic acid PEG ester (mol.) was used as the mercapto fatty acid ester. The molecular weight of the compound was 3.6 g, and 0.4 g of dodecanethiol was used as the aliphatic ligand. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1.

[0189] Comparative Example 3 In the process of preparing the semiconductor nanoparticle composite, 6-mercapto fatty acid ester is used. 3.2 g of butyrohexanoic acid PEG ester and 0 g of dodecanethiol as an aliphatic ligand were used. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 0.8 g was used.

[0190] Comparative Example 4 In the process of preparing the semiconductor nanoparticle composite, thioglycol is used as the mercapto fatty acid ester. 2.0 g of PEG ester of carboxylic acid (molecular weight 470) and dodecanethiol as an aliphatic ligand A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 2.0 g of the ethanol was used. Chloroform was used as a solvent for measuring the fluorescence quantum yield.

[0191] Comparative Example 5 In the process of producing semiconductor nanoparticle composites, no mercapto fatty acid ester is added, and fatty Using 4.0 g of dodecanethiol as an aromatic ligand, the reaction was carried out at 110°C for 60 minutes under a nitrogen atmosphere. The mixture was stirred and cooled to 25° C. to obtain a semiconductor nanoparticle composite. The reaction solution containing the complex was transferred to a centrifuge tube, 100 mL of acetone was added, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation for a short time, the mixture was separated into a clear supernatant and a semiconductor nanoparticle composite phase. The remaining semiconductor nanoparticle composite phase was collected. 5.0 mL of normal hexane was added to prepare a dispersion. Seton was added and centrifuged at 4000G for 20 minutes. After centrifugation, the clear supernatant was removed. The procedure was repeated several times. The rest of the procedure was the same as in Example 1. A semiconductor nanoparticle composite was obtained. For the measurement of the fluorescence quantum yield, normal hexane was used as the solvent. was used.

[0192] Comparative Example 6 When preparing the dispersion of the core particles, 0.2 mmol of octanoic acid chloride was added to the semiconductor nanoparticles. When preparing the complex, 3-mercaptopropionic acid 3-methionine was used as the mercapto fatty acid ester. Except for the use of 3.2 g of xybutyl as an aliphatic ligand and 0.8 g of dodecanethiol as an aliphatic ligand, A semiconductor nanoparticle composite was obtained in the same manner as in Example 1.

[0193] Comparative Example 7 In the process of preparing semiconductor nanoparticle composites, 3-mercapto fatty acid ester is used. 3.2 g of ethylhexyl isopropionate and 0.0 g of dodecanethiol as an aliphatic ligand. 0.8g, stirred at 110℃ for 60 minutes under nitrogen atmosphere, and cooled to 25℃. A semiconductor nanoparticle composite was obtained. The reaction solution containing the semiconductor nanoparticle composite was transferred to a centrifuge tube. Add 100 mL of acetone and centrifuge at 4000G for 20 minutes to obtain a clear supernatant. The semiconductor nanoparticle composite phase was separated. The supernatant was removed, and the remaining semiconductor nanoparticle composite was The phase was collected. 5.0 mL of normal hexane was added to the obtained semiconductor nanoparticle composite phase, A dispersion was prepared. 50 mL of acetone was added to the obtained dispersion, and the mixture was stirred at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was collected. The procedure was otherwise the same as in Example 1 to obtain a semiconductor nanoparticle composite. Chloroform was used as a solvent for measuring the fluorescence quantum yield.

[0194] Comparative Example 8 In the process of preparing the semiconductor nanoparticle composite, 3-mercapto fatty acid ester is used. 3.2 g of 2-hydroxyethyl butyrate and trioctyl as an aliphatic ligand A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 0.8 g of phosphine was used. This semiconductor nanoparticle complex was not dispersed in chloroform or PGMEA, and the fluorescence intensity was It was not possible to measure the molecular yield.

[0195] Comparative Example 9 When preparing the dispersion of the core particles, 4.5 mmol of octanoic acid chloride was added to the semiconductor nanoparticles. When preparing the complex, 3-mercaptopropionic acid-3-mercapto fatty acid ester was used. The other compounds were used: 3.6 g of butyl acetate and 0.4 g of dodecanethiol as an aliphatic ligand. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1.

[0196] Comparative Example 10 The same procedure as in Example 1 was repeated except that octanoic acid chloride was not added when preparing the dispersion of the core particles. A semiconductor nanoparticle composite was obtained in the same manner as described above.

[0197] Comparative Example 11 When preparing the dispersion of core particles, 0.3 mm of indium chloride was used instead of indium acetate. The same procedure as in Example 1 was repeated except that 100 ml of octanoic acid chloride was added and no octanoic acid chloride was added. The body-nanoparticle complexes were obtained. The indium chloride added during the preparation of the core particle dispersion produces hydrogen chloride as a by-product during the synthesis. Therefore, in the final semiconductor nanoparticles, the halogen precursor is generated. Compared with the case where a halogen precursor was added during the preparation of the core particle dispersion, It was found that the halogen content of

[0198] The meanings of the abbreviations shown in Tables 1 to 4 are as follows: MPAE: Mercapto fatty acid ester QD: Semiconductor nanoparticles DDT: Dodecanethiol TOP: Trioctylphosphine EHMP: Ethylhexyl 3-mercaptopropionate PGMEA: Propylene glycol monomethyl ether acetate

[0199] [Table 1]

[0200] [Table 2]

[0201] [Table 3]

[0202] [Table 4]

[0203] As can be seen from the above results, in Examples 1 to 17, the semiconductor nanoparticle composites had high fluorescence. It has high quantum efficiency (QY) and excellent dispersibility in polar dispersion media, and has a high mass fraction. It is possible to distribute the amount by a factor of 10. On the other hand, Comparative Example 5, which does not use mercapto fatty acid ester, Comparative Example 1 in which the molecular weight was too large, Comparative Example 3 in which the SP value of the mercapto fatty acid ester was too low, and Comparative Example 7: The average SP of the entire ligand is too low. Comparative Example 4: The average SP of the entire ligand is too low. In Comparative Example 8, which was too high, the dispersibility in a polar dispersion medium was poor, and the dispersion at a high mass fraction Dispersion is difficult. In addition, Comparative Examples 2, 6, 9, 10, and 11 However, the halogen / In ratio of the semiconductor nanoparticles is outside the range specified in the present invention, so the amount of fluorescence The molecular efficiency was low and the filterability was also low.

[0204] The molecular weight of the mercapto fatty acid ester represented by the general formula (1) is 300 to 700. Examples 1 to 10 in the following ranges are excellent in heat resistance, and are represented by the general formula (1) of the present invention. The mercapto fatty acid ester represented by the formula (1) is a mercapto fatty acid ester having a molecular weight of 300 or more and 700 or less. The semiconductor nanoparticle composites we developed are particularly suitable for applications where heat resistance is important. In Examples 1 to 10, the viscosity of the dispersion liquid when dispersed in a dispersion medium was Examples 11 to 17 using mercapto fatty acid esters represented by general formula (1) Although it is more expensive than , it can be used unless the application requires a low viscosity dispersion medium. It is.

[0205] In addition, the molecular weight of the mercapto fatty acid ester represented by the general formula (1) is in the range of 300 or less. In Examples 11 to 17 given above, the viscosity of the dispersion liquid when dispersed in the dispersion medium is low. In the present invention, as shown in Examples 11 to 17, a mercapto fatty acid represented by the general formula (1) is used. The semiconductor nanoparticle composite using an acid ester having a molecular weight of less than 300 has a molecular weight of A mercapto fatty acid ester represented by the general formula (1) having a molecular weight of 300 or more and 700 or less is used. Although it does not have the heat resistance of Examples 1 to 10, it is more important to reduce the viscosity of the dispersion than to improve heat resistance. It was found that the above-mentioned composition is suitable for the above-mentioned applications. [Explanation of symbols]

[0206] 1, 101 Blue LED 3, 103 LCD 7, 8 QD patterning 9 Diffusion Layer 11 cores 12. Shell 102 QD Film 104 Color Filter(R) 105 Color Filter (G) 106 Color Filter (B)

Claims

1. A semiconductor nanoparticle composite in which a ligand is coordinated to a surface of a semiconductor nanoparticle, The semiconductor nanoparticles have a core containing In and P and one or more shell layers. Core / shell semiconductor nanoparticles, The semiconductor nanoparticles further contain a halogen, and in the semiconductor nanoparticles, In calculation, the molar ratio of halogen to In is 0.80 to 15.00, The ligand has the following general formula (1): HS-R 1 -COO-R 2 (1) (In general formula (1), R 1 represents an alkylene group having 1 to 3 carbon atoms; R 2 represents a hydrophilic group.) The composition contains one or more mercapto fatty acid esters represented by the formula: The SP value of the mercapto fatty acid ester is 9.20 or more, and the mercapto fatty acid The molecular weight of the ester is 700 or less, and the average SP value of the entire ligand is 9.10 to 11.00; A semiconductor nanoparticle composite comprising:

2. The molecular weight of the mercapto fatty acid ester represented by the general formula (1) is 300 to 700. The semiconductor nanoparticle composite according to claim 1,

3. The molecular weight of the mercapto fatty acid ester represented by the general formula (1) is 300 to 600.

2. The semiconductor nanoparticle composite according to claim 1, wherein

4. The mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is 1.00 or less.

4. The semiconductor nanoparticle composite according to claim 2, wherein

5. The mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is 0.70 or less.

4. The semiconductor nanoparticle composite according to claim 2, wherein

6. The mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is 0.40 or more. The semiconductor nanoparticle composite according to any one of claims 2 to 5, wherein

7. The molecular weight of the mercapto fatty acid ester represented by the general formula (1) is less than 300. The semiconductor nanoparticle composite according to claim 1 .

8. The mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is 0.40 or less.

8. The semiconductor nanoparticle composite according to claim 7,

9. The content of the mercapto fatty acid ester represented by the general formula (1) in the entire ligand The semiconductor according to any one of claims 1 to 8, characterized in that the content is 40 mol % or more. Nanoparticle conjugates.

10. The content of the mercapto fatty acid ester represented by the general formula (1) in the entire ligand The semiconductor according to any one of claims 1 to 8, characterized in that the content is 50 mol % or more. Nanoparticle conjugates.

11. The content of the mercapto fatty acid ester represented by the general formula (1) in the entire ligand The semiconductor according to any one of claims 1 to 8, characterized in that the content is 60 mol % or more. Nanoparticle conjugates.

12. At least one of the shells is formed of ZnSe.

12. The semiconductor nanoparticle composite according to any one of claims 11 to 11.

13. The shell has two or more layers, and the outermost layer of the shell is formed of ZnS. The semiconductor nanoparticle composite according to any one of claims 1 to 12.

14. The shell comprises at least a first shell covering an outer surface of the core formed of ZnSe. and a second shell covering the outer surface of the first shell formed of ZnS. The semiconductor nanoparticle composite according to any one of claims 1 to 13.

15. R in the general formula (1) 2 is an oligoethylene glycol group, a polyethylene glycol group and an alkoxy group.

4. The semiconductor nanoparticle composite according to any one of claims 1 to 4.

16. R in the general formula (1) 2 The terminal group that is not bonded to the carboxyl group of the The compound according to claim 1, wherein the aryl group is an aryl group and an alkynyl group. Item 16. The semiconductor nanoparticle composite according to any one of items 1 to 15.

17. 17. The method according to claim 1, wherein the ligand further comprises an aliphatic ligand.

2. The semiconductor nanoparticle composite according to claim 1.

18. The aliphatic ligands are selected from the group consisting of aliphatic thiols, aliphatic carboxylic acids and aliphatic phosphines. The semiconductor nanoparticle complex according to claim 17, characterized in that the semiconductor nanoparticle complex is one or more selected from the group consisting of Merge.

19. The semiconductor nanoparticle composite is characterized in that the quantum efficiency after purification is 80% or more. The semiconductor nanoparticle composite according to any one of claims 1 to 18.

20. The semiconductor nanoparticle composite has an emission spectrum with a half-width of 38 nm or less. The semiconductor nanoparticle composite according to any one of claims 1 to 19.

21. The semiconductor nanoparticle composite according to any one of claims 1 to 20 is dispersed in an organic dispersion medium. Conductor nanoparticle composite dispersion.

22. The semiconductor nanoparticle composite according to any one of claims 1 to 20, A composite composition of semiconductor nanoparticles dispersed in a polymer.

23. The semiconductor nanoparticle composite according to any one of claims 1 to 20 is dispersed in a polymer matrix. A cured film of dispersed semiconductor nanoparticle composite.

24. A core / shell type semiconductor nanoparticle having a core containing In and P and one or more shell layers. The particle further contains halogen, and the molar ratio of halogen to In is 0. .80 to 15.00, a bonding property of bonding to the semiconductor nanoparticles on one end side The semiconductor nanoparticle composite is obtained by contacting a surface modifying compound having a group with the the law of nature, The surface modifying compound is represented by the following general formula (1): HS-R 1 -COO-R 2 (1) (In general formula (1), R 1 represents an alkylene group having 1 to 3 carbon atoms; R 2 represents a hydrophilic group.) The composition contains one or more mercapto fatty acid esters represented by the formula: The SP value of the mercapto fatty acid ester is 9.20 or more, and the mercapto fatty acid The molecular weight of the ester is 700 or less, and the average SP value of the entire surface modifying compound is 9.10 to 11.00; A semiconductor nanoparticle composite comprising:

25. The surface modifying compound has a bonding group on one end that bonds to the semiconductor nanoparticles and a lipid on the other end.

25. The method according to claim 24, further comprising the step of: providing an aliphatic group-containing surface modifying compound having an aliphatic group. The semiconductor nanoparticle composite described herein.

Citation Information

Patent Citations

  • Quantum dot solid film and preparation method thereof

    CN106479503A

  • Quantum dots, a composition or composite including the same, and an electronic device including the same

    EP3327814A1

  • Ultrafine semiconductor particle

    JP2002121549A

  • Thin film-like molding containing semiconductor crystal grain, and its use

    JP2002162501A

  • Quantum dot material and method for manufacturing same

    WO2017188300A1