Nano-zirconia dispersion, its preparation method, and resulting monomer dispersion and optical film

By modifying zirconia particles with organic acids and dispersion aids, the method addresses the dispersibility and preparation complexity issues of zirconia dispersions in organic solvents, resulting in high-refractive index nanozirconia dispersions for improved optical film performance.

JP2024536747AActive Publication Date: 2024-10-08SHANDONG SINOCERA FUNCTIONAL MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024515833
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-13
Filing Date
2022-08-04
Publication Date
2024-10-08
Estimated Expiration
2042-08-04

AI Technical Summary

Technical Problem

Conventional zirconia particle dispersions in organic solvents face challenges with poor dispersibility and complex, costly preparation processes, particularly when transitioning from an alcohol solvent phase, limiting their application in optical materials.

Method used

A method involving the use of organic acids, modifiers, and oil-based dispersion aids to modify zirconia particles, followed by rotary evaporation, results in a nanozirconia dispersion with improved dispersibility and high refractive index, eliminating the need for intermediate alcohol solvent phases.

Benefits of technology

The method achieves a simple, cost-effective preparation of nanozirconia dispersions with high uniformity and refractive index, enhancing the performance of optical films by improving compatibility with photocurable monomers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536747000001_ABST
    Figure 2024536747000001_ABST
Patent Text Reader

Abstract

The present application provides a nano-zirconia dispersion in the fine chemical field, a method for preparing the same, and a monomer dispersion and an optical film obtained thereby. The nano-zirconia dispersion provided herein contains nano-zirconia particles in an amount of 45-75 wt % and has a refractive index of 1.420-1.565. Here, when the nano-zirconia particles were characterized by infrared spectroscopy, the following functional groups in the peak-out range were found on the surface of the nano-zirconia particles: hydroxyl group: 3200 cm -1 ~3600cm -1 , Zr-O-Zr: 480 cm -1 ~850cm -1 , saturated carbon-hydrogen bond: 2850 cm -1 ~2960cm -1 , ester carbonyl group: 1700cm -1 ~1750cm -1 , delocalized conjugated ester group: 1460cm -1 ~1580cm -1 , Si-O-Zr: 800 cm -1 ~1200cm -1 and CO ether bond: 1000 cm -1 ~1200cm -1 It has been found that the nano-zirconia dispersion provided in the present application has a high dispersion content, and the dispersion content of the nano-zirconia monomer dispersion obtained thereon can reach 55-85wt%, and the refractive index can reach 1.620-1.720, which can then greatly improve the refractive index of the high refractive coating layer in the process of producing, for example, a brightness enhancement film or an anti-reflection film, thereby improving the performance of the film.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] <Related Applications> This application claims priority to a Chinese patent application filed with the China Patent Office on September 13, 2021, bearing application number 202111067304.6 and entitled "Nano zirconia dispersion, its preparation method, and resulting monomer dispersion and optical film", the entire contents of which are incorporated herein by reference.

[0002] The present application is in the field of fine chemicals, and in particular relates to nano-zirconia dispersions, methods for their preparation, and the resulting monomer dispersions and optical films. [Background technology]

[0003] In recent years, zirconia particle dispersions have been increasingly used in the optical field by combining them with transparent resins and thin films, taking advantage of their high refractive index. For example, zirconia dispersions with high refractive index are used in the manufacture of optical films such as brightness enhancement films and anti-reflection films, which can increase the brightness and clarity of LCD display screens, and can also improve the refractive index of LED encapsulation resins, further improving the brightness of LEDs. In conclusion, their high refractive index properties can be used in coating layers with high refractive indexes, and are applied in a variety of fields.

[0004] Conventionally, the above-mentioned zirconia particle dispersions have used dispersions in which the dispersion medium is water, and in many applications of optical materials such as the production of optical thin films, it has been common to mix an aqueous dispersion with a resin composition for use, but since aqueous dispersions have particularly poor kneadability with water-insoluble resin compositions, in recent years, there has been a strong demand for dispersions in which the dispersion medium is an organic solvent. Zirconia particles are usually fairly well dispersed in aqueous solvents, but are usually poorly dispersible in organic solvents.

[0005] The performance of the zirconia dispersion is closely related to the crystal structure of nano-zirconia in the system, the dispersion state of the particles, and the preparation process of the dispersion. CN107001066B discloses a method for preparing highly dispersed zirconia nanoparticles and their transparent dispersion. In the preparation method, zirconia particles are directly prepared by reacting zirconium salt with alkali under the condition of 170°C, and then the water of the dispersion medium of the aqueous dispersion of the zirconia particles is replaced with at least one alcohol solvent selected from methanol and ethanol, and then the zirconia particles in the alcohol dispersion are surface-treated with a silane coupling agent and a 12-hydroxystearic acid surface treatment agent, and finally the alcohol solvent of the alcohol dispersion of the zirconia particles is replaced with the desired organic solvent by a distillation replacement method or an ultrafiltration concentration replacement method. The organic solvent dispersion of zirconia dispersion prepared by this method has a transmittance of 10% or more at a wavelength of 400 nm, a transmittance of 80% or more at a wavelength of 800 nm, and a viscosity of 10 mPa·s or less immediately after preparation at 25°C. However, this process requires an alcohol solvent as an intermediate phase to obtain a dispersion of the target phase, which makes the preparation process complicated and expensive, and also causes problems such as insufficient modification due to the limited modification temperature caused by the low boiling point of the alcohol solvent.

[0006] Therefore, how to prepare zirconia dispersions with stable system, uniform dispersion, and high refractive index is particularly important to better meet the performance needs of transparent organic-inorganic composites. Summary of the Invention [Problem to be solved by the invention]

[0007] The present application provides a nano-zirconia dispersion, a preparation method thereof, and the resulting monomer dispersion and optical film, and the resulting nano-zirconia dispersion has characteristics such as good dispersion uniformity and a high refractive index. [Means for solving the problem]

[0008] To achieve the above objectives, the present application adopts the following technical solutions: A first aspect of the present invention provides a nano-zirconia dispersion, the nano-zirconia particles contained in the nano-zirconia dispersion are in an amount of 45 to 75 wt % and the refractive index of the nano-zirconia dispersion is 1.420 to 1.565, and the nano-zirconia particles are characterized by infrared spectroscopy, and the nano-zirconia particles are found to have functional groups on their surfaces in the following peak-out range: Hydroxy group: 3200cm -1 ~3600cm -1 , Zr-O-Zr: 480 cm -1 ~850cm -1 , saturated carbon-hydrogen bond: 2850 cm -1 ~2960cm -1 , ester carbonyl group: 1700cm -1 ~1750cm -1 , delocalized conjugated ester group: 1460cm -1 ~1580cm -1 , Si-O-Zr: 800 cm -1 ~1200cm -1 and CO ether bond: 1000 cm -1 ~1200cm -1 was found to be grafted.

[0009] In some embodiments of the present application, the refractive index of the nano-zirconia dispersion is 1.420 to 1.535 when the zirconia content is 45% to 65%, and is 1.498 to 1.565 when the zirconia content is 65% to 75%.

[0010] In some embodiments of the present application, the refractive index of the nano-zirconia particles in the nano-zirconia dispersion is 2.20 to 2.60, and the proportion of the tetragonal phase grain structure in the nano-zirconia particles is 60 to 95%.

[0011] A second aspect of the present embodiment provides a method for preparing a nano-zirconia dispersion, the method comprising: The method includes the steps of adding an organic solvent to an aqueous zirconia solution, mixing the solution uniformly, adding an organic acid and a modifier to the system to modify the zirconia particles, and then adding an oil-based dispersion aid and removing water by rotary evaporation to obtain a nano-zirconia dispersion; Here, the organic acid is added in an amount of 3 to 20 wt% based on the content of nano-zirconia, the modifier is added in an amount of 5 to 20 wt% based on the content of nano-zirconia, and the oil-based dispersion aid is added in an amount of 5 to 20 wt% based on the content of nano-zirconia.

[0012] In some embodiments of the present application, modifying the zirconia particles by adding an organic acid and a modifier to the system specifically includes: Adding an organic acid and a modifier to the system at atmospheric pressure and 50 to 150°C to modify the zirconia particles; or The organic acid and the modifier are dissolved in the organic solvent, and the solution is added to a dispersion liquid in which an aqueous zirconia solution and an organic solvent are mixed under conditions of atmospheric pressure and 50 to 150° C., to modify the zirconia particles.

[0013] In some embodiments of the present application, the organic solvent is at least one of butanone, methyl isobutyl ketone, propylene glycol methyl ether, and ethylene glycol methyl ether, and the volume ratio of the added organic solvent to the zirconia aqueous solution is (3-5):1.

[0014] In some embodiments of the present application, the organic acid is selected from at least one of saturated or unsaturated monocarboxylic acids, polycarboxylic acids, and hydroxycarboxylic acids.

[0015] In some embodiments of the present application, the monocarboxylic acid is selected from at least one of formic acid, acetic acid, propionic acid, butyric acid, isooctanoic acid, acrylic acid, and methacrylic acid, the polycarboxylic acid is selected from at least one of oxalic acid, malonic acid, succinic acid, phthalic acid, fumaric acid, and maleic acid, and the hydroxycarboxylic acid is selected from at least one of lactic acid, malic acid, tartaric acid, and citric acid.

[0016] In some embodiments of the present application, the modifier is at least one of 3-(methacryloyl oxy)propyl trimethoxy silane, 3-glycidyl ether oxypropyl trimethoxy silane.

[0017] In some embodiments of the present application, the oil-based dispersing aid is selected from at least one of an anionic dispersant, a cationic dispersant, a non-ionic dispersant, and a polymeric dispersant.

[0018] In some embodiments of the present application, the oil-based dispersing aid is selected from BYK-9076 or BYK-9077.

[0019] A third aspect of the present invention provides a nano-zirconia monomer dispersion, which is prepared by adding a photocurable resin to any one of the nano-zirconia dispersions described above, and removing the organic solvent from the dispersion by distillation under reduced pressure.

[0020] In some embodiments of the present application, the nano-zirconia content in the nano-zirconia monomer dispersion is 55 to 85 wt %, and the refractive index of the nano-zirconia monomer dispersion is 1.620 to 1.720.

[0021] In some embodiments of the present application, the photocurable resin is selected from acrylic or methacrylic acid monomers or oligomers thereof having ester, urethane, ether, silicon, halogen and / or phosphorus-containing groups, and the photocurable resin is added in an amount of 15 to 45 wt % based on the total mass of the zirconia and the photocurable resin.

[0022] In some embodiments of the present application, the photocurable resin is at least one of phenoxybenzyl acrylate, methyl acrylate, and methyl methacrylate.

[0023] A fourth aspect of the present invention provides an optical film prepared using any one of the nano-zirconia dispersions described above, or any one of the nano-zirconia monomer dispersions described above. Effect of the Invention

[0024] Compared with the prior art, the present application has the following advantages and positive effects: 1. The method for preparing nano-zirconia dispersion provided in at least one embodiment of the present application is simple in operation. The simplest distillation replacement method can be directly used to obtain an organic solvent dispersion by phase inversion of an aqueous zirconia dispersion, and the organic solvent dispersion can be further replaced to obtain a monomer dispersion, without the need for an intermediate phase. 2. The method for preparing nano-zirconia dispersion provided in at least one embodiment of the present application uses an organic acid, a modifier and an oil-based dispersion aid to act on zirconia particles simultaneously, fully utilizing their synergistic effect to achieve the best dispersion effect, and effectively improve the compatibility of the subsequent organic solvent dispersion with the photocurable monomer. 3. In the preparation method of nano-zirconia dispersion provided in at least one embodiment of the present application, when adding the raw material components, it is necessary to add the organic acid and modifier to the dispersion system before adding the oil-based dispersion aid, so as to ensure that there are enough active sites on the zirconia surface for the organic acid and modifier to interact with each other to achieve the best modification and dispersion effect. 4. In the preparation method of nano-zirconia dispersion provided in at least one embodiment of the present application, the contents of the added organic acid, modifier and oil-based dispersion aid need to be controlled within the ranges limited in the present application. If the contents are too low, the expected modification effect will not be obtained, and if the contents are too high, the opposite effect will occur and unnecessary economic losses may also occur. 5. The nano-zirconia dispersion provided in at least one embodiment of the present application has a high dispersion content of nano-zirconia particles, which can reach 45-75 wt%, and a refractive index, which can reach 1.420-1.565, and the nano-zirconia monomer dispersion obtained therefrom has a dispersion content of 55-85 wt%, and a refractive index, which can reach 1.620-1.720. [Brief description of the drawings]

[0025] [Figure 1] FIG. 2 is an infrared spectrum diagram of the nano-zirconia dispersion provided in Example 1 of the present invention. [Diagram 2] FIG. 2 is an infrared spectrum diagram of the nano-zirconia dispersion provided in Example 5 of the present invention. [Diagram 3] FIG. 2 is an infrared spectrum diagram of the nano-zirconia dispersion provided in Example 6 of the present invention. [Figure 4] FIG. 1 is an infrared spectrum diagram of the nano-zirconia dispersion provided in Example 7 of the present invention. [Diagram 5] FIG. 2 is an infrared spectrum diagram after adding BYK-9076 used in the examples of the present invention to zirconia (addition amount 40%). [Figure 6] FIG. 2 is an infrared spectrum diagram after adding BYK-9076 (addition amount 5%) used in the examples of the present invention to zirconia. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The technical solutions of the embodiments of the present application are described below clearly and completely, but it is clear that the described embodiments are only some of the embodiments of the present application, and are not all of the embodiments. Based on the embodiments of the present application, all other embodiments that can be obtained by those skilled in the art without creative labor fall within the scope of protection of the present application.

[0027] In the description of the present application, unless otherwise specified, all contents whose units are not clearly specified are mass contents, and in order to obtain a nano-zirconia dispersion, the above-mentioned aqueous zirconia solutions in the raw materials of the present application are all understood to refer to aqueous nano-zirconia solutions.

[0028] In order to achieve the above object, the present application provides a nano-zirconia dispersion, the amount of nano-zirconia particles contained in the nano-zirconia dispersion is 45 to 75 wt %, and the nano-zirconia particles are characterized by infrared spectroscopy, and the surface of the nano-zirconia particles contains the following functional groups in the peak-out range: Hydroxy group: 3200cm -1 ~3600cm -1 , Zr-O-Zr: 480 cm -1 ~850cm -1 , saturated carbon-hydrogen bond: 2850 cm -1 ~2960cm -1 , ester carbonyl group: 1700cm -1 ~1750cm -1 , delocalized conjugated ester group: 1460cm -1 ~1580cm -1 , Si-O-Zr: 800 cm -1 ~1200cm -1 and CO ether bond: 1000 cm -1 ~1200cm -1 It has been found that the successful introduction of these functional groups can significantly improve the oleophilicity of the zirconia particles, offering possibilities for the subsequent manufacture of various dispersions and films thereof, as well as positively influencing the improvement of the solids content and refractive index of solvent- and monomer-based dispersions.

[0029] In some embodiments, the refractive index of the nano-zirconia dispersion is 1.420-1.535 when the zirconia content is 45%-65%, and 1.498-1.565 when the zirconia content is 65%-75%.

[0030] In some embodiments, the refractive index of the nano-zirconia particles in the nano-zirconia dispersion is between 2.20 and 2.60.

[0031] In some embodiments, the ratio of the tetragonal phase crystal grain structure in the nano-zirconia particles is 60 to 95%. The crystal type of zirconia is divided into monoclinic phase, tetragonal phase, and cubic phase, and it is understood that in the nano-zirconia dispersion of the embodiments of the present application, the zirconia nanoparticles having the tetragonal crystal type are the mass ratio of all the crystal types of zirconia.

[0032] The present application also provides a method for preparing a nano-zirconia dispersion, the method comprising: The method includes the steps of adding an organic solvent to an aqueous zirconia solution, mixing uniformly, adding an organic acid and a modifier to the system to modify the zirconia particles, then adding an oil-based dispersion aid, and removing water by rotary evaporation to obtain a nano-zirconia dispersion.

[0033] The method for preparing nano-zirconia dispersion provided in the above examples is to add an organic acid and a modifier to a dispersion of zirconia particles mixed with water and an organic solvent, which is then subjected to lipophilic modification treatment, and then remove water while obtaining a zirconia dispersion of pure organic solvent phase, and then add an oil-based dispersion aid, thereby enhancing the stability and dispersibility of the dispersion. The above solution does not require complicated operations or dispersion equipment, is simple, and processing based on this method has significant advantages over the dispersions in the prior art that have undergone dispersion medium replacement.

[0034] In some embodiments, modifying the zirconia particles by adding an organic acid and a modifier to the system specifically includes: Adding an organic acid and a modifier to the system at atmospheric pressure and 50 to 150°C to modify the zirconia particles; or The organic acid and the modifier are dissolved in the organic solvent, and the solution is added to a dispersion liquid in which an aqueous zirconia solution and an organic solvent are mixed under conditions of atmospheric pressure and 50 to 150° C., to modify the zirconia particles.

[0035] In some embodiments, the volume ratio of the added organic solvent to the aqueous zirconia solution is (3-5:1).

[0036] In some embodiments, the organic solvent is at least one of butanone, methyl isobutyl ketone, propylene glycol methyl ether, and ethylene glycol methyl ether.

[0037] In some embodiments, the organic acid is selected from at least one of saturated or unsaturated monocarboxylic acids, polycarboxylic acids, and hydroxycarboxylic acids, and the organic acid is added in an amount of 3 to 20 wt% based on the content of nano-zirconia.

[0038] In some embodiments, the monocarboxylic acid is selected from at least one of formic acid, acetic acid, propionic acid, butyric acid, isooctanoic acid, acrylic acid, and methacrylic acid, the polycarboxylic acid is selected from at least one of oxalic acid, malonic acid, succinic acid, phthalic acid, fumaric acid, and maleic acid, and the hydroxycarboxylic acid is selected from at least one of lactic acid, malic acid, tartaric acid, and citric acid.

[0039] In some embodiments, the modifier is at least one of 3-(methacryloyloxy)propyl trimethoxy silane and 3-glycidyl ether oxypropyl trimethoxy silane, and the modifier is added in an amount of 5 to 20 wt% based on the content of the nano-zirconia.

[0040] In the preparation method of nano-zirconia dispersion provided in the embodiment of the present application, organic acid and modifier are added to treat the surface of zirconia. This improves the lipophilicity of zirconia particles on the one hand, and disperses zirconia particles uniformly on the other hand, and can more fully bond modifier and zirconia. In addition, the presence of organic acid promotes hydrolysis and grafting of modifier, and the presence of modifier promotes grafting of organic acid and zirconia, and the two promote each other, and oil-based dispersion aid also plays a positive effect of promoting grafting of organic acid and modifier with zirconia. The amount of organic acid added may be 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 wt% of the nano-zirconia content or any point value within the above range, and the amount of modifier added may be 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 wt% of the nano-zirconia content or any point value within the above range.

[0041] In some embodiments, the oil-based dispersion aid is selected from at least one of anionic dispersants, cationic dispersants, nonionic dispersants, and polymeric dispersants, and is preferably a phosphate ester-based dispersion aid. The oil-based dispersion aid is added in an amount of 5 to 20 wt% based on the content of nano-zirconia.

[0042] It is understood that in the above step, an oil-based dispersion aid is added to further improve the stability and dispersibility of the dispersion. In particular, the oil-based dispersion aid should be added after the organic acid and modifier are added to the dispersion, which ensures that the organic acid and modifier provide sufficient active sites on the surface of the zirconia particles for surface treatment. The amount of the oil-based dispersion aid added can be 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19wt% of the nano-zirconia content or any point value within the above range.

[0043] In some embodiments, the oil-based dispersing aid may be selected from dispersants BYK-9076 and BYK-90777, among others, manufactured by BYK, Germany.

[0044] In the above examples, BYK-9076 is a high molecular weight copolymer silyl ammonium salt, and FIG. 5 shows the infrared spectrum of zirconia after adding BYK-9076 (40%). -2 The hydroxyl group peak at 2926 cm corresponds to the hydroxyl group remaining on the zirconia surface. -2 is the saturated hydrocarbon peak of BYK9076, and 1633 cm -2 is the peak of water adsorbed on the zirconia inorganic powder, and 1060 cm -2 is Si-O-Zr produced by grafting BYK9076 onto zirconia, and has a peak at 565cm -2 is Zr-O-Zr of zirconia. The appearance of the Si-O-Zr peak in the product in FIG. 5 explains that BYK-9076 can be grafted to zirconia to form Si-O-Zr functional groups. FIG. 6 is an infrared spectrum diagram of zirconia after adding BYK-9076 (5%). From FIG. 5 and FIG. 6, it can be seen that if BYK9076 is added, a Si-O-Zr peak appears regardless of the amount of BYK9076 added. BYK9077 is a high molecular weight copolymer with a pigment affinity group. Therefore, when BYK9076 is used as an oil-based dispersion aid, it can provide Si-O-Zr functional groups together with the modifier, further increase the number of Si-O-Zr functional groups in the prepared nano-zirconia dispersion, and improve the refractive index of the nano-zirconia dispersion. The structure of BYK9077 is similar to that of BYK9076, but due to greater steric hindrance and less grafting with zirconia, its infrared spectrum shows hydroxyl group peaks, water peaks, and Zr-O-Zr of zirconia.

[0045] The present application also provides a nano-zirconia-monomer dispersion prepared by adding a photocurable resin to the nano-zirconia dispersion based on any one of the above technical solutions, and removing the organic solvent in the dispersion by vacuum distillation. Here, it should be noted that the monomer dispersion in the present application refers to a dispersion to which a single component is added, and does not specifically refer to the monomer or its oligomer contained in the photocurable component.

[0046] In some embodiments, the nano-zirconia content of the nano-zirconia monomer dispersion is 55-85 wt% and the refractive index of the nano-zirconia monomer dispersion is 1.620-1.720. It is understood that the nano-zirconia content of the monomer dispersion can also be 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84 wt%, or any point value within the above range.

[0047] In some embodiments, the photocurable resin is selected from acrylic or methacrylic monomers or oligomers containing ester, urethane, ether, silicon, halogen and / or phosphorus groups, any of which may be commercially available.

[0048] In some embodiments, the photocurable resin is added in an amount of 15-45 wt% based on the total mass of zirconia and photocurable resin. It is understood that the content of the photocurable resin may be 20, 25, 30, 35 wt% or any point value within the above range.

[0049] In some embodiments, the photocurable resin is at least one of phenoxybenzyl acrylate, methyl acrylate, and methyl methacrylate.

[0050] The present application also provides an optical film, characterized in that it is prepared using a nano-zirconia dispersion prepared by a preparation method based on any one of the above technical solutions, or a nano-zirconia monomer dispersion prepared by any one of the above technical solutions.

[0051] In some embodiments, the optical film is one of a brightness enhancing film, an anti-reflective film, and other optical films having a highly refractive coating layer.

[0052] In order to more clearly and in detail describe the nano-zirconia dispersion provided in the examples of the present application, the preparation method thereof and the resulting monomer dispersion, specific examples are provided below in conjunction with the examples.

[0053] Example 1 Propylene glycol methyl ether (PGME) solvent was added to the zirconia aqueous solution and mixed uniformly. Isooctanoic acid (addition amount: 5% of zirconium content) and 3-(methacryloyloxy)propyl trimethoxysilane (addition amount: 10% of zirconium content) were then added to the above system in order to modify the zirconia particles. Then, oil-based dispersion aid BYK-9076 (addition amount: 5%) was added and the water was removed by rotary evaporation to obtain a nano-zirconia organic PGME-type dispersion.

[0054] In the nano-zirconia organic PGME dispersion, when the nano-zirconia concentration was 45 wt%, the refractive index was 1.475, when the concentration was 65%, the refractive index was 1.535, and when the concentration was 75 wt%, the refractive index was 1.565.

[0055] FIG. 1 attached herewith shows an infrared spectrum of Example 1. Here, 3418 cm -1 The absorption peak is the characteristic absorption peak of the hydroxyl group on the surface of the zirconia particles, and is at 589 cm -1 and 496 cm -1 is a characteristic absorption peak of Zr-O-Zr. Also, 2950cm -1 is a characteristic peak of saturated carbon-hydrogen bonds, and 1718 cm-1 is a characteristic peak of the ester carbonyl group, and 1561 cm -1 and 1463 cm -1 is the characteristic absorption peak of the delocalized conjugated ester group, and 1170 cm -1 is a characteristic absorption peak of Si-O-Zr, and 1025 cm -1 is the characteristic absorption peak of the CO ether bond, which indicates that isooctanoic acid and 3-(methacryloyloxy)propyltrimethoxysilane were successfully grafted onto the surface of zirconia particles. Example 2

[0056] The preparation method was the same as in Example 1, except that the amount of isooctanoic acid added was 3% of the zirconium content, the amount of 3-glycidyl ether oxypropyl trimethoxy silane added was 5% of the zirconium content, and the amount of oil-based dispersion aid BYK-9076 added was 10% of the zirconium content to obtain a nano-zirconia organic PGME-type dispersion liquid.

[0057] In the nano-zirconia organic PGME dispersion, when the nano-zirconia concentration was 45 wt%, the refractive index was 1.470, when the concentration was 65%, the refractive index was 1.529, and when the concentration was 75 wt%, the refractive index was 1.558. Example 3

[0058] The preparation method was the same as in Example 1, with the difference being that the amount of isooctanoic acid added was 12% of the zirconium content, the amount of modifier 3-(methacryloyloxy)propyl trimethoxysilane added was 15% of the zirconium content, and the amount of oil-based dispersion aid BYK-9077 added was 15% of the zirconium content to obtain a nano-zirconia organic PGME-type dispersion liquid.

[0059] In the nano-zirconia organic PGME dispersion, when the nano-zirconia concentration was 45 wt%, the refractive index was 1.461, when the concentration was 65%, the refractive index was 1.522, and when the concentration was 75 wt%, the refractive index was 1.552. Example 4

[0060] The preparation method was the same as in Example 1, with the difference being that the amount of isooctanoic acid added was 20% of the zirconium content, the amount of modifier 3-glycidyl ether oxypropyl trimethoxy silane added was 20% of the zirconium content, and the amount of oil-based dispersion aid BYK-9077 added was 20% of the zirconium content to obtain a nano-zirconia organic PGME-type dispersion liquid.

[0061] In the nano-zirconia organic PGME dispersion, when the concentration of nano-zirconia was 45 wt%, the refractive index was 1.449, when the concentration was 65%, the refractive index was 1.509, and when the concentration was 75 wt%, the refractive index was 1.540. Example 5

[0062] The preparation method was the same as in Example 1, with the difference being that the organic acid was 12-hydroxystearic acid, and the amount of acid added was 5% of the zirconium content, to obtain a nano-zirconia organic PGME-type dispersion liquid.

[0063] In the nano-zirconia organic PGME dispersion, when the nano-zirconia concentration was 45 wt%, the refractive index was 1.467, when the concentration was 65%, the refractive index was 1.525, and when the concentration was 75 wt%, the refractive index was 1.554.

[0064] FIG. 2 attached herewith shows the infrared spectrum of Example 5. Here, 3427 cm -1 The absorption peak at 586 cm is a characteristic peak of the surface hydroxyl group of zirconia particles. -1 and 483 cm -1 is a characteristic absorption peak of Zr-O-Zr. Also, 2925 cm -1 is a characteristic peak of saturated carbon-hydrogen bonds, and 1715 cm -1 is the characteristic peak of the ester carbonyl group, and 1562 cm -1 and 1463 cm -1 is the characteristic absorption peak of the delocalized conjugated ester group, and 1169 cm -1is a characteristic absorption peak of Si-O-Zr, and 1032 cm -1 is the characteristic absorption peak of the CO ether bond, which indicates that 12-hydroxystearic acid and 3-(methacryloyloxy)propyltrimethoxysilane were successfully grafted onto the surface of zirconia particles. Example 6

[0065] The preparation method was the same as in Example 1, with the difference being that the organic acid added was acetic acid, and the amount of acid added was 5% of the zirconium content, to obtain a nano-zirconia organic PGME-type dispersion liquid.

[0066] In the nano-zirconia organic PGME dispersion, when the nano-zirconia concentration was 45 wt%, the refractive index was 1.420, when the concentration was 65%, the refractive index was 1.498, and when the concentration was 75 wt%, the refractive index was 1.530.

[0067] FIG. 3 attached herewith shows the infrared spectrum of Example 6. Here, 3427 cm -1 The absorption peak is a characteristic peak of the surface hydroxyl group of zirconia particles, and is at 589 cm -1 and 496 cm -1 is a characteristic absorption peak of Zr-O-Zr. Also, 2934cm -1 is a characteristic peak of saturated carbon-hydrogen bonds, and 1711 cm -1 is a characteristic peak of the ester carbonyl group, and 1558 cm -1 and 1465 cm -1 is the characteristic absorption peak of the delocalized conjugated ester group, and 1167 cm -1 is a characteristic absorption peak of Si-O-Zr, and 1031 cm -1 is the characteristic absorption peak of the CO ether bond, which indicates that acetic acid and 3-(methacryloyloxy)propyl trimethoxysilane were successfully grafted onto the surface of zirconia particles. Example 7

[0068] The preparation method was the same as in Example 1, with the difference being that the organic acid added was propionic acid, and the amount of acid added was 5% of the zirconium content, to obtain a nano-zirconia organic PGME-type dispersion liquid.

[0069] In the nano-zirconia organic PGME dispersion, when the concentration of nano-zirconia was 45 wt%, the refractive index was 1.457, when the concentration was 65%, the refractive index was 1.513, and when the concentration was 75 wt%, the refractive index was 1.548.

[0070] FIG. 4 attached herewith shows the infrared spectrum of Example 7. Here, 3434 cm -1 The absorption peak is a characteristic peak of the surface hydroxyl group of zirconia particles, and is at 580 cm -1 and 490cm -1 is a characteristic absorption peak of Zr-O-Zr. Also, 2932 cm -1 is a characteristic peak of saturated carbon-hydrogen bonds, and 1714 cm -1 is a characteristic peak of the ester carbonyl group, and 1563 cm -1 and 1467 cm -1 is the characteristic absorption peak of the delocalized conjugated ester group, and 1109 cm -1 is a characteristic absorption peak of Si-O-Zr, and 1027 cm -1 is the characteristic absorption peak of the CO ether bond, which indicates that propionic acid and 3-(methacryloyloxy)propyl trimethoxysilane were successfully grafted onto the zirconia particle surface. Example 8

[0071] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid obtained in Example 1, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0072] In the dispersion, when the content of nano-zirconia was 55 wt%, the refractive index was 1.675, when the content was 75 wt%, the refractive index was 1.700, and when the content was 85 wt%, the refractive index was 1.720. Example 9

[0073] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid obtained in Example 2, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0074] In the dispersion, when the content of nano-zirconia was 55 wt%, the refractive index was 1.660, when the content was 75 wt%, the refractive index was 1.687, and when the content was 85 wt%, the refractive index was 1.706. Example 10

[0075] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid obtained in Example 3, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0076] In the dispersion, when the content of nano-zirconia was 55 wt%, the refractive index was 1.644, when the content was 75 wt%, the refractive index was 1.667, and when the content was 85 wt%, the refractive index was 1.687. Example 11

[0077] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid obtained in Example 4, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0078] In the dispersion, when the content of nano-zirconia was 55 wt%, the refractive index was 1.620, when the content was 75 wt%, the refractive index was 1.643, and when the content was 85 wt%, the refractive index was 1.662. Example 12

[0079] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid obtained in Example 5, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0080] In the dispersion, when the content of nano-zirconia was 55 wt%, the refractive index was 1.650, when the content was 75 wt%, the refractive index was 1.676, and when the content was 85 wt%, the refractive index was 1.695. Example 13

[0081] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid obtained in Example 6, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0082] In the dispersion, when the content of nano-zirconia was 55 wt%, the refractive index was 1.621, when the content was 75 wt%, the refractive index was 1.641, and when the content was 85 wt%, the refractive index was 1.656. Example 14

[0083] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid obtained in Example 7, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0084] In the dispersion, when the content of nano-zirconia was 55 wt%, the refractive index was 1.631, when the content was 75 wt%, the refractive index was 1.657, and when the content was 85 wt%, the refractive index was 1.678. Comparative Example 1

[0085] The preparation method was the same as in Example 1, with the difference being that the content of isooctanoic acid added was 0 to obtain a nano-zirconia organic PGME-type dispersion. The zirconia particles had hydroxyl groups, Zr-O-Zr, and Si-O-Zr on the surface, but did not have ester carbonyl groups, CO ether bonds, conjugated ester groups, or saturated carbon-hydrogen bond groups.

[0086] In the nano-zirconia organic PGME dispersion, when the nano-zirconia concentration was 45 wt%, the refractive index was 1.395, when the concentration was 65%, the refractive index was 1.434, and when the concentration was 75 wt%, the refractive index was 1.472. Comparative Example 2

[0087] When phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid prepared in Comparative Example 1 and the mixture was distilled under reduced pressure to remove the organic solvent, the final product, zirconia, was precipitated, and a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate was not obtained. Comparative Example 3

[0088] Propylene glycol methyl ether (PGME) solvent was added to the zirconia aqueous solution and mixed uniformly. Then, oil-based dispersion aid BYK-9076 (addition amount 5%) was added to the above system, followed by isooctanoic acid (addition amount 5% of zirconium content) and 3-(methacryloyloxy)propyl trimethoxysilane (addition amount 10% of zirconium content) to modify the zirconia particles, and water was removed by rotary evaporation to obtain nano-zirconia organic PGME type dispersion. The zirconia particles had hydroxyl groups, Zr-O-Zr, Si-O-Zr groups, conjugated ester groups, ester carbonyl groups and CO ether bond groups on the surface, but no saturated carbon-hydrogen bond groups.

[0089] In the nano-zirconia organic PGME dispersion, when the concentration of nano-zirconia was 45 wt%, the refractive index was 1.398, when the concentration was 65%, the refractive index was 1.445, and when the concentration was 75 wt%, the refractive index was 1.484. Comparative Example 4

[0090] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid prepared in Comparative Example 3, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0091] In the dispersion, when the content of nano-zirconia was 55 wt%, the refractive index was 1.575, and when the content was 75 wt%, the refractive index was 1.598. Comparative Example 5

[0092] The preparation method was the same as in Comparative Example 3, with the difference being that the oil-based dispersion aid BYK-9076 (addition amount 5%) was added to the system, and then 12-hydroxystearic acid (addition amount 5% of the zirconium content) and 3-(methacryloyloxy)propyl trimethoxysilane (addition amount 10% of the zirconium content) were added to modify the zirconia particles to obtain a nano-zirconia organic PGME-type dispersion. The zirconia particles had hydroxyl groups, Zr-O-Zr, Si-O-Zr groups, conjugated ester groups, ester carbonyl groups and CO ether bond groups on the surface, but did not have saturated carbon-hydrogen bond groups.

[0093] In the nano-zirconia organic PGME dispersion, when the concentration of nano-zirconia was 45 wt%, the refractive index was 1.396, when the concentration was 65%, the refractive index was 1.442, and when the concentration was 75 wt%, the refractive index was 1.480. Comparative Example 6

[0094] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid prepared in Comparative Example 5, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0095] In the dispersion, when the content of nano-zirconia was 55 wt%, the refractive index was 1.570, and when the content was 75 wt%, the refractive index was 1.594. Comparative Example 7

[0096] The preparation method was the same as in Example 5, except that the amount of 12-hydroxystearic acid, 3-(methacryloyloxy)propyl trimethoxysilane and oil-based dispersion aid BYK-9076 added was 25% of the zirconium content, respectively, to obtain a nano-zirconia organic PGME-type dispersion. The zirconia particles have hydroxyl groups, Zr-O-Zr, Si-O-Zr groups, CO ether bonds, ester carbonyl groups and saturated carbon-hydrogen bond groups on the surface, but no conjugated ester groups.

[0097] In the nano-zirconia organic PGME dispersion, when the nano-zirconia concentration was 45 wt%, the refractive index was 1.398, when the concentration was 65%, the refractive index was 1.447, and when the concentration was 75 wt%, the refractive index was 1.481. Comparative Example 8

[0098] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid prepared in Comparative Example 7, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0099] In the dispersion, when the content of nano-zirconia was 55 wt%, the refractive index was 1.567, and when the content was 75 wt%, the refractive index was 1.591. Comparative Example 9

[0100] The preparation method was the same as in Example 1, except that the amount of isooctanoic acid, 3-glycidyl ether oxypropyl trimethoxy silane and oil-based dispersion aid BYK-9076 added was 30% of the zirconium content to obtain a nano-zirconia organic PGME-type dispersion. The zirconia particles had hydroxyl groups, Zr-O-Zr, Si-O-Zr groups, CO ether bonds, ester carbonyl groups and saturated carbon-hydrogen bond groups on the surface, but no conjugated ester groups.

[0101] In the nano-zirconia organic PGME dispersion, when the nano-zirconia concentration was 45 wt%, the refractive index was 1.389, when the concentration was 65%, the refractive index was 1.446, and when the concentration was 75 wt%, the refractive index was 1.485. Comparative Example 10

[0102] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid prepared in Comparative Example 9, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0103] In the dispersion, when the content of nano-zirconia was 55 wt%, the refractive index was 1.557, and when the content was 75 wt%, the refractive index was 1.582. Comparative Example 11

[0104] The preparation method was the same as in Example 1, except that the content of 3-(methacryloyloxy)propyltrimethoxysilane was set to 0 to obtain nano-zirconia organic PGME-type dispersion. The zirconia particles had hydroxyl groups, Zr-O-Zr and Si-O-Zr on the surface, but did not have ester carbonyl groups, CO ether bonds, conjugated ester groups or saturated carbon-hydrogen bond groups.

[0105] In the nano-zirconia organic PGME dispersion, when the nano-zirconia concentration was 45 wt%, the refractive index was 1.399, when the concentration was 65%, the refractive index was 1.439, and when the concentration was 75 wt%, the refractive index was 1.477. Comparative Example 12

[0106] When phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid prepared in Comparative Example 11 and the mixture was distilled under reduced pressure to remove the organic solvent, the final product zirconia was precipitated, and no nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate was obtained. Comparative Example 13

[0107] The preparation method was the same as in Example 1, with the difference being that the oil-based dispersion aid added was DISPERBYK-111 (addition amount was 5% of the zirconium content), and a nano-zirconia organic PGME-type dispersion was obtained. The zirconia particles had hydroxyl groups, Zr-O-Zr, COOH, saturated carbon-hydrogen bond groups, ester carbonyl groups and CO ether bonds on the surface, but did not have Si-O-Zr or conjugated ester groups.

[0108] In the nano-zirconia organic PGME dispersion, when the nano-zirconia concentration was 45 wt%, the refractive index was 1.391, when the concentration was 65%, the refractive index was 1.443, and when the concentration was 75 wt%, the refractive index was 1.481. Comparative Example 14

[0109] Phenoxybenzyl acrylate was added to the nano-zirconia organic PGME-type dispersion liquid prepared in Comparative Example 13, and the mixture was distilled under reduced pressure to remove the organic solvent, thereby obtaining a nano-zirconia dispersion liquid containing photocurable phenoxybenzyl acrylate.

[0110] In the dispersion, when the content of nano-zirconia was 55 wt %, the refractive index was 1.560, and when the content was 75 wt %, the refractive index was 1.587.

[0111] Table 1. Summary of differences between Examples 1-14 and Comparative Examples 1-14 and the product data obtained JPEG2024536747000002.jpg176170

[0112] The examples of the present application and comparative examples will be compared and analyzed below. When no organic acid (Comparative Example 1) or modifier (Comparative Example 11) was added, there was no mutual promotion effect between the organic acid and the modifier, so the zirconia of Comparative Examples 1 and 11 only had Si-O-Zr provided by the oil-based dispersion aid on the surface, and as a result, the preparation of the monomer-type dispersion of Comparative Examples 2 and 12 failed. This explains that the actions of the organic acid, modifier, and oil-based dispersion aid on the zirconia particles are mutually promoted, and such changes in promotion effect lead to differences in the surface graft groups of the zirconia particles, which further affect whether the dispersion can be successfully prepared or not.

[0113] In Comparative Examples 3 and 5, 5% of the oil-based dispersion aid BYK9076 was added first, which resulted in a shortage of surface active sites of zirconia, and isooctanoic acid and 12-hydroxystearic acid, which have long carbon chains, have large steric hindrance and are difficult to graft to the few active sites on the zirconia surface, so there are no saturated hydrocarbons in Comparative Examples 3 and 5. The content of nano-zirconia in the monomer-type dispersion is at most 75 wt%, and the refractive index is 1.598 and 1.594, which is much lower than the refractive index of 1.641 to 1.700 of the 75 wt% monomer-type dispersion in Examples 8 to 14, not to mention the higher refractive index of 85 wt% in Examples 8 to 14. In Examples 1 to 7 of the present application, when the zirconia particles are modified by first adding a modifier and an organic acid, the zirconia has sufficient active sites on the surface for the organic acid and modifier to act, so that a better modification effect and dispersion effect can be obtained.

[0114] In Comparative Examples 7 and 9, 12-hydroxystearic acid and isooctanoic acid have long electron-donating carbon chains and are added in large amounts (25% and 30%), so the grafting of such a large amount of electron-donating groups directly weakens or eliminates the electron deficiency of the zirconia center. Therefore, no conjugated ester groups appear, and the content of nanozirconia in the monomer-type dispersion is at most 75 wt%, and the refractive index is only 1.591 and 1.582. In the examples of this application, the amount of organic acid added is small and insufficient to offset the electron deficiency of the zirconia center, so the conjugated ester groups exist.

[0115] In Example 1, a different oil-based dispersion aid from that in Comparative Example 13 is used, and in Comparative Example 13, there is a COOH peak on the surface of the zirconia particles, and no Si-O-Zr and conjugated ester group peaks appear, which explains that the organic acid and modifier in Comparative Example 13 do not interact with zirconia by the way of grafting, but are simply coated on the surface of zirconia. Furthermore, in Comparative Example 13, the refractive index of the solvent-based dispersion at each concentration is lower than that of Example 1, and at the same time, the content of nano-zirconia in the monomer-based dispersion of Comparative Example 14 is at most 75wt%, and the refractive index is 1.587, which is much lower than the refractive index of the 75wt% monomer-based dispersion in Example 8, which is 1.700, not to mention the higher refractive index of 85wt% in Example 8. This explains that the oil-based dispersion aid BYK9076 has an important effect on promoting the grafting of organic acid and modifier to zirconia particles, and further affects the number and type of graft groups on the surface of zirconia particles, thereby significantly improving the refractive index of the dispersion.

[0116] From the above, the preparation method provided in Examples 1 to 7 of the present application utilizes the mutual promotion effect of organic acid, modifier and oil-based dispersion aid on zirconia particles at the same time, and controls the content of each reagent within the range provided in the Examples of the present application to graft each expected functional group onto the surface of nano-zirconia particles, and finally obtains a nano-zirconia dispersion with good dispersion uniformity and high refractive index. The nano-zirconia dispersion can greatly improve the refractive index of the high refractive coating layer in the subsequent preparation of brightness enhancement film or anti-reflection film, etc., thereby improving the performance of the film. From the refractive index data in Table 1, it can be seen that in the case of a solvent-based dispersion, under the same 75wt% condition, the refractive index of Examples 1 to 7 is 1.530 to 1.565, and the refractive index of Comparative Examples 1, 3, 5, 7, 9, 11 and 13 is 1.472 to 1.485, with a difference of 0.058 to 0.08. Numerically, the difference in refractive index is not large, but from the perspective of the refractive index of the dispersion, the difference is like night and day. For example, when brightness enhancement films are manufactured using dispersions with a refractive index difference of 0.01 and applied to displays, the light transmittance is 89% and 93%, which is the difference between a B-class screen and an A-class screen.

Claims

1. A nano-zirconia dispersion, comprising: The amount of nano-zirconia particles contained in the nano-zirconia dispersion is 45 to 75 wt %, and the refractive index of the nano-zirconia dispersion is 1.420 to 1.

565. When the nano-zirconia particles were characterized by infrared spectroscopy, the following functional groups in the peak-out range were present on the surface of the nano-zirconia particles: Hydroxy group: 3200 cm -1 ~3600cm -1 , Zr-O-Zr: 480cm -1 ~850cm -1 , saturated carbon-hydrogen bond: 2850 cm -1 ~2960cm -1 , ester carbonyl group: 1700 cm -1 ~1750cm -1 , delocalized conjugated ester group: 1460 cm -1 ~1580cm -1 , Si-O-Zr: 800cm -1 ~1200cm -1 and C—O ether bond: 1000 cm -1 ~1200cm -1 A nano-zirconia dispersion, characterized in that it has been found that a nano-zirconia dispersion having a grafted thereon is

2. The nano-zirconia dispersion according to claim 1, characterized in that the refractive index of the nano-zirconia dispersion is 1.420 to 1.535 when the zirconia content is 45% to 65%, and is 1.498 to 1.565 when the zirconia content is 65% to 75%.

3. The nano-zirconia dispersion according to claim 1 or 2, characterized in that the refractive index of the nano-zirconia particles in the nano-zirconia dispersion is 2.20 to 2.60, and the proportion of the tetragonal phase crystal grain structure in the nano-zirconia particles is 60 to 95%.

4. 2. A method for preparing the nano-zirconia dispersion according to claim 1, comprising the steps of: The preparation method comprises the steps of: The method includes the steps of adding an organic solvent to an aqueous zirconia solution, mixing the solution uniformly, adding an organic acid and a modifier to the system to modify the zirconia particles, and then adding an oil-based dispersion aid and removing water by rotary evaporation to obtain a nano-zirconia dispersion; The preparation method is characterized in that the organic acid is added in an amount of 3 to 20 wt % based on the content of nano-zirconia, the modifier is added in an amount of 5 to 20 wt % based on the content of nano-zirconia, and the oil-based dispersion aid is added in an amount of 5 to 20 wt % based on the content of nano-zirconia.

5. The modification of the zirconia particles by adding an organic acid and a modifier to the system specifically includes: Adding an organic acid and a modifier to the system at atmospheric pressure and 50 to 150° C. to modify the zirconia particles; or The preparation method according to claim 4, characterized in that an organic acid and a modifier are dissolved in the organic solvent, and the solution is added to a dispersion of an aqueous zirconia solution and an organic solvent under atmospheric pressure and at 50 to 150°C to modify the zirconia particles.

6. The preparation method according to claim 4, characterized in that the organic solvent is at least one of butanone, methyl isobutyl ketone, propylene glycol methyl ether and ethylene glycol methyl ether, and the volume ratio of the added organic solvent to the zirconia aqueous solution is (3-5):

1.

7. 5. The process according to claim 4, characterized in that the organic acid is selected from at least one of the following: saturated or unsaturated monocarboxylic acids, polycarboxylic acids and hydroxycarboxylic acids.

8. 8. The method according to claim 7, characterized in that the monocarboxylic acid is selected from at least one of the following: formic acid, acetic acid, propionic acid, butyric acid, isooctanoic acid, acrylic acid, methacrylic acid, the polycarboxylic acid is selected from at least one of the following: oxalic acid, malonic acid, succinic acid, phthalic acid, fumaric acid, maleic acid, and the hydroxycarboxylic acid is selected from at least one of the following: lactic acid, malic acid, tartaric acid, citric acid.

9. The preparation method according to claim 4, characterized in that the modifier is at least one of 3-(methacryloyl oxy)propyl trimethoxy silane, 3-glycidyl ether oxypropyl trimethoxy silane.

10. 5. The method according to claim 4, characterized in that the oil-based dispersing aid is selected from at least one of anionic dispersants, cationic dispersants, non-ionic dispersants and polymeric dispersants.

11. The preparation method according to claim 4, characterized in that the oil-based dispersing aid is selected from BYK-9076 or BYK-9077.

12. A nano-zirconia monomer dispersion comprising: A nano-zirconia monomer dispersion liquid, which is obtained by adding a photocurable resin to the nano-zirconia dispersion liquid according to any one of claims 1 to 3, and removing the organic solvent from the dispersion liquid by distillation under reduced pressure.

13. The nano-zirconia monomer dispersion according to claim 12, characterized in that in the nano-zirconia monomer dispersion, the content of nano-zirconia is 55 to 85 wt %, and the refractive index of the nano-zirconia monomer dispersion is 1.620 to 1.

720.

14. The nano-zirconia monomer dispersion according to claim 12, characterized in that the photocurable resin is selected from acrylic or methacrylic acid monomers or oligomers thereof having ester, urethane, ether, silicon, halogen and / or phosphorus-containing groups, and the photocurable resin is added in an amount of 15 to 45 wt % based on the total mass of zirconia and the photocurable resin.

15. The nano-zirconia monomer dispersion according to claim 14, wherein the photocurable resin is at least one of phenoxybenzyl acrylic acid ester, methyl acrylate, and methyl methacrylate.

16. An optical film, An optical film, characterized by being prepared using the nano-zirconia dispersion according to any one of claims 1 to 3, or the nano-zirconia monomer dispersion according to any one of claims 12 to 15.

Citation Information

Patent Citations

  • Dispersant for non-aqueous dispersion media

    JP2015000970A

  • Polymerizable composition containing inorganic oxide particle or siloxane compound, manufacturing method of layer using the polymerizable composition, and layer containing inorganic oxide particle or siloxane compound

    JP2019183137A

  • Surface-modified zirconia nanoparticles

    US20110288215A1

  • Dispersion containing metal oxide particles

    WO2015111664A1