Laminate having excellent barrier properties and method for preparing same
A laminate structure with a metallized polyethylene film and PET/PP films, using a specific adhesive composition, addresses the oxygen barrier challenge in packaging, achieving an OTR of less than 2.0 cc/m²/24 hours for enhanced shelf life.
Patent Information
- Application Number
- JP2024526600
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-11-08
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2041-11-08
AI Technical Summary
Existing packaging materials, such as PET, PP, and PE films, struggle to provide high oxygen barrier performance, which is crucial for extending the shelf life of sensitive contents like meats, candies, and snacks, despite their mechanical and optical properties.
A laminate structure comprising a metallized polyethylene-based film bonded with a PET-based or PP-based film using a two-component solvent-based polyurethane adhesive composition, where the metallized film has low fatty acid content and specific polyester polyol component with 40-60% aromatic rings, and a weight ratio of 100:5 to 100:30 for polyester polyol to polyisocyanate components.
The laminate achieves an oxygen transmission rate (OTR) of less than 2.0 cc/m²/24 hours, significantly improving barrier performance and ensuring extended shelf life for packaged foods.
Smart Images

Figure 2024539382000001 
Figure 2024539382000002 
Figure 2024539382000003
Abstract
Description
[Technical field]
[0001] LAMINATES, ARTICLES COMPRISING THE LAMINATES, AND METHODS OF PREPARING THE LAMINATES FIELD OF THE DISCLOSURE The present disclosure relates to laminates, articles including the laminates, and methods of preparing the laminates. The laminates exhibit excellent barrier performance. [Background technology]
[0002] Today, market trends such as consumer, food safety, and e-commerce are increasing the demands on packaging functions that require higher performance packaging structures with extended shelf life and / or improved package integrity. These changes are therefore driving a rapidly growing market for high barrier films that provide critical protection of the contents from the external environment to ensure a longer shelf life.
[0003] In the flexible packaging industry, polyethylene terephthalate (PET), polyethylene (PE), and polypropylene (PP) are typical materials for substrate films to provide desired mechanical and barrier properties. PET or PP films, which have high stiffness, good optical properties, and heat resistance, are widely used for the skin layer of laminate films as printing substrates. Meanwhile, PE films usually have better toughness and heat seal properties than PET or PP, and are very common as the inner heat seal layer of laminate films. However, based on the polymer properties, PET, PP, and PE films typically cannot provide the desired high oxygen barrier, which is important for the protection of delicate contents such as some meats, candies, snacks, or cookies. Therefore, although there are various approaches to obtain barrier performance in the industry, such as the incorporation of polymer barrier resins by coextrusion, vacuum metallization onto film substrates, or coating of barrier materials onto the film surface, achieving high barrier performance of laminates in terms of oxygen transmission rate (OTR) remains a challenge in the packaging industry.
[0004] For the above reasons, there remains a need in the packaging industry to develop packaging materials with excellent barrier performance. Summary of the Invention
[0005] The present disclosure provides unique laminates that exhibit superior barrier performance, articles including the laminates, and methods for preparing the laminates.
[0006] In a first aspect, the present disclosure provides a laminate comprising: A first substrate including a metallized polyethylene-based (PE-based) film; A second substrate including a polyethylene terephthalate (PET) film or a polypropylene (PP) film; an adhesive layer that adheres the first substrate to the second substrate, the adhesive layer being derived from a two-component solvent-based polyurethane adhesive composition; The concentration of fatty acid or fatty acid derivative in the metallized PE-based film is less than 300 ppm, based on the total weight of the metallized PE-based film; A two-component solvent-based polyurethane adhesive composition comprising a polyester polyol component and a polyisocyanate component, The polyester polyol component has about 40% by weight to 60% by weight of aromatic rings in the main chain based on the total weight of the polyester polyol, and has a molecular weight (Mw) of 5,000 to 50,000; A laminate is provided in which the weight ratio of the polyester polyol component to the polyisocyanate component is 100:5 to 100:30.
[0007] In a second aspect, the present disclosure provides an article comprising a laminate of the present disclosure.
[0008] In a third aspect, the present disclosure provides a method for preparing a laminate of the present disclosure, comprising: 1) providing a first substrate comprising a metallized PE-based film and a second substrate comprising a PET-based film or a PP-based film; 2) adhering the first substrate to the second substrate by using a two-component solvent-based polyurethane adhesive composition; The concentration of fatty acid or fatty acid derivative in the metallized PE-based film is less than 300 ppm based on the total weight of the metallized PE-based film; A two-component solvent-based polyurethane adhesive composition comprising a polyester polyol component and a polyisocyanate component, The polyester polyol component has 40% by weight to 60% by weight of aromatic rings in the main chain based on the total weight of the polyester polyol, and has a Mw of 5,000 to 50,000; The weight ratio of the polyester polyol component to the polyisocyanate component is from 100:5 to 100:30. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs, and all publications, patent applications, patents, and other references mentioned herein are incorporated by reference.
[0010] As disclosed herein, all ranges include the endpoints unless otherwise indicated.
[0011] According to one embodiment of the present disclosure, the adhesive composition is a "two-component" or "two-part" composition comprising a polyester polyol component and a polyisocyanate component. According to another embodiment, the polyester polyol component and the polyisocyanate component are packaged, shipped, and stored separately and are combined immediately or immediately prior to use to produce a laminate.
[0012] "Polyethylene polymer", "polyethylene-based polymer", "PE-based polymer", "polyethylene", or "ethylene-based polymer" is intended to mean a polymer that contains a majority of units derived from ethylene monomer (>50 mol%, or >60 mol%, or >70 mol%, or >80 mol%, or >90 mol%, or >95 mol%, or >97 mol%). This includes polyethylene homopolymers or copolymers (meaning units derived from two or more comonomers). Common forms of polyethylene known in the art include, but are not limited to, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), ultra low density polyethylene (ULDPE), very low density polyethylene (VLDPE), single-site catalyzed linear low density polyethylene (m-LLDPE), which includes both linear and substantially linear low density resins, medium density polyethylene (MDPE), and high density polyethylene (HDPE). These polyethylene materials are generally well known in the art. However, the following description may be helpful in understanding the differences between some of these different polyethylene resins.
[0013] The term "LDPE", which may also be referred to as "high pressure ethylene polymer", or "highly branched polyethylene", is defined to mean that the polymer is partially or fully homopolymerized or copolymerized in an autoclave or tubular reactor at pressures in excess of 14,500 psi (100 MPa) using a free radical initiator, such as a peroxide (see, for example, U.S. Pat. No. 4,599,392, incorporated herein by reference). LDPE resins typically have a density in the range of 0.916 to 0.935 g / cm3.
[0014] The term "LLDPE" includes both resins made using traditional Ziegler-Natta and chromium-based catalysts, as well as single-site catalysts, including, but not limited to, bis-metallocene catalysts (sometimes referred to as "m-LLDPE") and constrained geometry catalysts, and includes linear, substantially linear, or heterogeneous polyethylene copolymers or homopolymers. LLDPE contains less long chain branching than LDPE and includes substantially linear ethylene polymers, as further defined in U.S. Patents 5,272,236, 5,278,272, 5,582,923, and 5,733,155; homogeneously branched linear ethylene polymer compositions, such as those in U.S. Patent 3,645,992, heterogeneously branched ethylene polymers, such as those prepared according to the process disclosed in U.S. Patent 4,076,698, and / or blends thereof, such as those disclosed in U.S. Patents 3,914,342 or 5,854,045. LLDPE can be made via gas phase, solution phase, or slurry polymerization, or any combination thereof, using any type of reactor or reactor configuration known in the art.
[0015] The term "MDPE" refers to polyethylene having a density of 0.926 to 0.935 g / cm3. "MDPE" is typically made using chromium or Ziegler-Natta catalysts, or using single-site catalysts, including but not limited to bis-metallocene catalysts and constrained geometry catalysts, and typically has a molecular weight distribution ("MWD") greater than 2.5.
[0016] The term "HDPE" refers to polyethylene having a density greater than about 0.935 g / cm3 to about 0.970 g / cm3 that is generally prepared using a single-site catalyst, including, but not limited to, Ziegler-Natta, chromium, or bis-metallocene and constrained geometry catalysts.
[0017] The term "ULDPE" generally refers to polyethylene having a density between 0.880 and 0.912 g / cm3 that is prepared with a single-site catalyst, including but not limited to Ziegler-Natta, chromium, or bis-metallocene and constrained geometry catalysts.
[0018] "Polypropylene-based polymer", "PP-based polymer", or "polypyrene-based polymer" is intended to mean a polymer that contains a majority (>50 mol%, or >60 mol%, or >70 mol%, or >80 mol%, or >90 mol%, or >95 mol%) of units derived from polypyrene monomers.
[0019] "Polyethylene terephthalate-based polymer" or "PET-based polymer" is intended to mean a polymer that contains a majority amount (>50% by weight, or >60% by weight, or >70% by weight, or >80% by weight, or >90% by weight, or >95% by weight) of ethylene terephthalate.
[0020] A "polyolefin plastomer" can be a polyethylene plastomer or a polypropylene plastomer. Polyolefin plastomers include, for example, polymers made using single-site catalysts, such as metallocene and constrained geometry catalysts. Polyolefin plastomers have a viscosity of 0.885 to 0.915 g / cm 3 It has a density of 0.885g / cm 3 ~0.915g / cm 3 All individual values and subranges are included herein and disclosed herein. For example, the density of the plastomer may be 0.895, 0.900, or 0.905 g / cm 3 0.905, 0.910, or 0.915 g / cm 3 In some embodiments, the polyolefin elastomer may have a viscosity of from 0.890 to 0.910 g / cm 3 has a density of
[0021] The "polyolefin elastomer" may be a polyethylene elastomer or a polypropylene elastomer. The polyolefin elastomer has a modulus of 0.857 to 0.885 g / cm 3 It has a density of 0.857g / cm 3 ~0.885g / cm 3 All individual values and subranges are included herein and disclosed herein. For example, low density polyethylene has a density of 0.857, 0.860, 0.865, 0.870, or 0.875 g / cm 3 From the lower limit of 0.870, 0.875, 0.880, or 0.885 g / cm 3 In some embodiments, the polyolefin elastomer has a viscosity of 0.860 to 0.880 g / cm 3 has a density of
[0022] "Polyethylene-based film" or "PE-based film" refers to a film that contains at least 90 weight percent polyethylene, at least 95 weight percent polyethylene, or at least 97 weight percent polyethylene, based on the total weight of the film.
[0023] "Polypropylene-based film" or "PP-based film" refers to a film that contains at least 90 weight percent polypropylene, at least 95 weight percent polypropylene, or at least 97 weight percent polypropylene, based on the total weight of the film.
[0024] "Polyethylene terephthalate-based film" or "PET-based film" refers to a film that contains at least 90 weight percent polyethylene terephthalate, at least 95 weight percent polyethylene terephthalate, or at least 97 weight percent polyethylene terephthalate, based on the total weight of the film.
[0025] First Substrate The first substrate includes a metallized PE-based film. The metallized PE-based film includes a PE-based film and a metal layer.
[0026] The PE-based film in the metallized PE-based film has at least one layer containing polyethylene. There may be one layer containing polyethylene. Alternatively, there may be two or more layers containing polyethylene. These two or more layers may be extruded together to form the PE-based film. There may be three (or more) layers containing polyethylene. When there are three (or more) layers containing polyethylene, the layer adjacent to the metal layer is referred to herein as a skin layer, the layer opposite the metal layer on the outside of the PE-based film is referred to as a sealant layer, and the layer or layers between the skin layer and the sealant layer are one or more core layers. When only one layer containing polyethylene is provided, any of the polyethylene compositions described herein as a skin layer, a core layer, or a sealant layer may be used. When only two layers containing polyethylene are provided, any combination of a skin layer and a core layer, a skin layer and a sealant layer, or a core layer and a sealant layer may be used. When two or more polyethylene-containing layers are provided, each polyethylene-containing layer may be directly adjacent to at least one other polyethylene-containing layer, or an adhesive layer or other intermediate layer may be used between the two or more polyethylene-containing layers. In one embodiment, the PE-based film in the metallized PE-based film includes a sealant layer. In one embodiment, the PE-based film in the metallized PE-based film includes a skin layer, a core layer, and a sealant layer.
[0027] The PE-based film in the metallized PE-based film can include linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), low density polyethylene (LDPE), as well as combinations of two or more of the foregoing. Preferably, the PE-based film in the metallized PE-based film can include Ziegler-Natta catalyzed, single-site catalyzed (including but not limited to metallocene), or chromium catalyzed linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), autoclave-produced or tubular-produced low density polyethylene (LDPE), as well as combinations of two or more of the foregoing.
[0028] The PE-based film in the metallized PE-based film can further comprise at least one of very low density polyethylene, polyolefin plastomer, polyolefin elastomer, ethylene vinyl acetate copolymer, ethylene ethyl acrylate copolymer, ethylene vinyl alcohol, and any polymer comprising at least 50% ethylene monomer, and combinations thereof.
[0029] The skin layer may comprise linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), low density polyethylene (LDPE), and combinations of two or more of the foregoing, preferably linear low density polyethylene (LLDPE), low density polyethylene (LDPE), or combinations thereof. The LLDPE may be single-site catalyzed polyethylene (such as, but not limited to, m-LLDPE). The skin layer may further comprise additives such as, for example, antioxidants, UV stabilizers, heat stabilizers, slip agents, antiblock agents, pigments or colorants, processing aids, crosslinking catalysts, flame retardants, fillers, and foaming agents. When used in combination with a core layer or a sealant layer, the skin layer is metallized, and in that case is a layer that advantageously does not contain a slip agent, but may contain an antiblock agent (e.g., talc, silicon dioxide, etc.), antioxidants, and processing aids. In one embodiment, additives such as slip agents and antiblock agents are typically not used in the skin layer.
[0030] The core layer may comprise linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), low density polyethylene (LDPE), and combinations of two or more of the foregoing. The core layer may preferably comprise medium density polyethylene (MDPE), high density polyethylene (HDPE), or combinations thereof. The core layer may also comprise additives as described for the skin layers. Preferably, additives such as slip agents and antiblock agents are typically not used in the core layer. This layer may be adjacent to the skin layer on the side of the skin layer opposite the metal layer.
[0031] The sealant layer may comprise linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), low density polyethylene (LDPE), polyolefin elastomers or plastomers, as well as combinations of two or more of the foregoing. Preferably, the sealant layer may comprise Ziegler-Natta catalyzed, single-site catalyzed (including metallocene), or chromium catalyzed linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), autoclave-produced or tubular-produced low density polyethylene (LDPE), as well as combinations of two or more of the foregoing, preferably linear low density polyethylene (LLDPE), low density polyethylene (LDPE), or combinations thereof. The LLDPE may be a single-site catalyzed polyethylene (such as mLLDPE). It may be an outer layer of the film. The sealant layer may advantageously comprise an antiblocking agent. For example, the anti-blocking agent may be present in the sealant layer in an amount of at least about 200 ppm, at least about 1000 ppm, or at least about 1500 ppm, preferably about 6000 ppm or less, or about 5000 ppm or less.In addition, slipping agents (e.g., erucamide) may be useful.For example, the slipping agent may be present in the sealant layer in an amount of less than 500 ppm, or less than 300 ppm, or less than 200 ppm, or less than 100 ppm, preferably less than 50 ppm, or equal to 0 ppm, based on the total weight of the sealant layer.
[0032] The PE-based film of the metallized PE-based film can be a blown film, a cast film, a longitudinally stretched film, or a biaxially stretched film. The PE-based film of the metallized PE-based film layer can be produced by blown, cast, water-cooled, double bubble, or other techniques known to those skilled in the art, such as those described in Film Processing Advances, Toshitaka Kanai and Gregory A. Campbell (eds.), Chapter 7 (Biaxial Oriented Film Technology), pp. 194-229. In some embodiments, after production, the film may be subjected to a machine direction orientation (MDO) or biaxial stretching process to provide a machine direction stretched film or a biaxially stretched film, respectively.
[0033] The PE-based film of the metallized PE-based film layer can be metallized by any known method for metallizing polyethylene films. For example, the metal layer can be applied using vacuum metallization. This may involve providing a metal source and evaporating it in a vacuum environment to condense on the surface of the film. The metal is deposited on the skin layer of the PE-based film.
[0034] Suitable metals include Al, Zn, Au, Ag, Cu, Ni, Cr, Ge, Se, Ti, Sn, or oxides thereof. In some embodiments, the metal layer is aluminum or aluminum oxide (Al 2 O 3 ) can be formed.
[0035] After metallization, the metallized PE-based film can be conveniently stored in rolls, with the metallized surface layer in contact with the polyethylene layer on the opposite side of the film.
[0036] The total thickness of the metallized film can be at least 10 microns, at least 20 microns, or at least 30 microns. The total thickness of the metallized film according to certain embodiments is no more than 200 microns, no more than 150 microns, no more than 120 microns, no more than 100 microns, no more than 80 microns, no more than 70 microns, or no more than 60 microns.
[0037] The metallized PE-based film can have an optical density (OD) of at least 1.5, or at least 1.8, and no more than 4.0, no more than 3.5, or no more than 3.0. In some embodiments, the OD is 2.0. The optical density of the metallized PE-based film (e.g., a multi-layer structure comprising a polyethylene film having a metal layer deposited thereon) can be measured using an optical density meter (model number LS177 manufactured by Shenzhen Linshang Technology).
[0038] The metallized PE-based film can retain a surface energy of the metallized surface of at least 34 dynes / cm, at least 38 dynes / cm, at least 40 dynes / cm, at least 42 dynes / cm, or at least 46 dynes / cm for at least one week or at least two weeks after metallization.
[0039] The metallized PE-based film can be characterized by the absence (0 ppm) or substantial absence of fatty acids or derivatives thereof. Such absence or substantial absence of fatty acids or derivatives thereof includes saturated fatty acids having an even number of carbon atoms from 4 to 28, such as stearic acid (18 carbon atoms) and palmitic acid (16 carbon atoms), and the metal salts of the respective fatty acids, such as calcium stearate, zinc stearate, calcium palmitate, etc. Specifically, the concentration of fatty acids or derivatives thereof in the metallized PE-based film can be 300 ppm or less, 250 ppm or less, 200 ppm or less, 100 ppm or less, or 50 ppm or less, or equal to 0 ppm, based on the total weight of the metallized PE-based film.
[0040] The concentration of the antioxidant in the metallized PE-based film layer is less than 3000 ppm, or less than 2000 ppm, or less than 1500 ppm, or less than 1300 ppm, based on the total weight of the metallized PE-based film.
[0041] Additives Antioxidants are compounds that are included in polymer films to stabilize the polymer(s) or prevent oxidative degradation of the polymer(s). Antioxidants are well known to those skilled in the art.
[0042] Anti-blocking agents are compounds that minimize or prevent sticking (i.e., adhesion) between two adjacent layers of a film. Sticking can cause problems, for example, during unwinding of a film roll. The use of anti-blocking agents is well known to those skilled in the art. Examples of suitable anti-blocking agents include, but are not limited to, silica, talc, calcium carbonate, and combinations thereof.
[0043] Slip agents are compounds added to films to reduce friction between films and / or between the film and equipment. Typical slip agents include migratory and non-migratory slip agents and are well known to those skilled in the art.
[0044] adhesive layer The adhesive layer is derived from a two-component solvent-based polyurethane adhesive composition, which includes a polyester polyol component and a polyisocyanate component.
[0045] A. Polyester polyol component Polyester polyols are typically obtained by reacting a polyfunctional alcohol having 2 to 12 carbon atoms, preferably 2 to 10 carbon atoms, with a polyfunctional carboxylic acid having 2 to 12 carbon atoms, preferably 2 to 10 carbon atoms, or anhydride / ester thereof. Typical polyfunctional alcohols for preparing polyester polyols are preferably diols, triols, tetraols, and may include ethylene glycol, butylene glycol, diethylene glycol, triethylene glycol, polyalkylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, trimethylolpropane, glycerol, erythritol, pentaerythritol, trimethylolbenzene, and any combination thereof. Typical polyfunctional carboxylic acids for preparing polyester polyols may be aliphatic, cycloaliphatic, araliphatic, aromatic, or heterocyclic, may be substituted, for example, with halogen atoms, and / or may be saturated or unsaturated. Preferably, the polyfunctional carboxylic acid is selected from the group consisting of adipic acid, suberic acid, azelaic acid, sebacic acid, phthalic acid, isophthalic acid, glutaric acid, tetrachlorophthalic acid, maleic acid, fumaric acid, itaconic acid, malonic acid, 2-methylsuccinic acid, 3,3-diethylglutaric acid, 2,2-dimethylsuccinic acid, trimellitic acid, their anhydrides, and any combination thereof. Adipic acid or a mixture of adipic acid and isophthalic acid is preferred. In another embodiment, the polyester polyol has an OH value of 2 to 30 mg KOH / g, preferably 5 to 25 mg KOH / g, more preferably 8 to 20 mg KOH / g.
[0046] According to one embodiment of the present disclosure, the polyester polyol has a hydroxyl functionality of at least 1.8, or at least 1.9, or at least 2.0, or at least 2.1, or at least 2.2, or up to 2.3, or up to 2.4, or up to 2.5, or up to 2.6, or up to 2.7, or up to 2.8, or up to 2.9, or up to 3.0, or within a range obtained by combining any two of the above endpoints. The polyester polyol may have a molecular weight of 5,000 to 50,000 g / mol, or 5,500 to 30,000 g / mol, or 6,000 to 25,000 g / mol, or 10,000 to 15,000 g / mol, or within a range obtained by combining any two of the above endpoints. The above explanations regarding the origin, production method, category, molecular structure, and various parameters of polyester polyols also apply to this second polyester polyol.
[0047] According to one embodiment of the present disclosure, the polyester polyol has an aromatic ring content of about 40% to about 60% by weight, or about 45% to about 55% by weight, or about 47% to about 55% by weight, based on the dry weight of the polyester polyol.
[0048] For example, in one exemplary embodiment, the content of the polyester polyol can be 40% by weight to 85% by weight, or 50% by weight to 80% by weight, or 60% by weight to 77% by weight, or 65% by weight to 75% by weight, based on the total weight of the polyurethane composition.
[0049] The solids content of the polyester polyol component can be 40-85 wt%, preferably 50-80 wt%, more preferably 55-75 wt%, and the solvent used for the polyester polyol can be ethyl acetate or MEK, or a combination, preferably ethyl acetate.
[0050] B. Polyisocyanate component Polyisocyanates may include any molecule having two or more isocyanate groups and mixtures thereof. Such polyisocyanates may be aliphatic, cycloaliphatic, aromatic, or mixtures thereof. The polyisocyanates may have an average functionality of >2 or from 2.5 to 10. Examples of suitable polyisocyanates include C 2 -C 12 Aliphatic diisocyanates and their dimers and trimers, such as tetramethylene diisocyanate and hexamethylene diisocyanate (HDI), 1,12-dodecane diisocyanate, 2,2,4-trimethyl-hexamethylene diisocyanate, 2,4,4-trimethyl-hexamethylene diisocyanate, 2-methyl-1,5-pentamethylene diisocyanate, etc. 2 -C 8 Alkylene diisocyanate; C 6 -C 15 Cycloaliphatic diisocyanates and their dimers and trimers, such as isophorone diisocyanate (IPDI) and dicyclohexyl methane diisocyanate (HMDI), 1,4-cyclohexane diisocyanate, and 1,3-bis-(isocyanatomethyl)cyclohexane; 6 -C 12 Aromatic diisocyanates and their dimers and trimers, such as toluene diisocyanate (TDI) and diphenyl methane diisocyanate (MDI); 7 -C 15 Aromatic aliphatic diisocyanates and their dimers and trimers are included.
[0051] Preferably, the polyisocyanate comprises an aliphatic or aromatic polyisocyanate, more preferably the polyisocyanate is a hexamethylene diisocyanate homopolymer, a hexamethylene diisocyanate adduct, an isophorone diisocyanate homopolymer, an isophorone diisocyanate adduct, a toluene diisocyanate (TDI), a toluene diisocyanate (TDI) adduct, a diphenylmethane diisocyanate (MDI), a diphenylmethane diisocyanate (MDI) adduct, or a mixture thereof. Trimers (or isocyanurates) in polyisocyanates can be prepared by methods known in the art, for example, as disclosed in US Patent Publication No. 2006 / 0155095(A1), by trimerizing cycloaliphatic diisocyanates (e.g., isophorone diisocyanate) in the presence of one or more trimerization catalysts, such as tertiary amines or phosphines, or heterogeneous catalysts, and optionally in the presence of solvents and / or auxiliaries, such as cocatalysts, conveniently at elevated temperatures, until the desired NCO content is reached, followed by deactivation of the catalyst using inorganic and organic acids, the corresponding acid halides and alkylating agents, and preferably heating. Similarly, isocyanurate compositions containing isocyanurates from aliphatic diisocyanates can be formed by cyclizing aliphatic diisocyanates in the presence of one or more trimerization catalysts, followed by deactivation of the catalyst. Any of the isocyanurates can be further modified by conventional methods to contain urethane, urea, imino-s-triazine, uretonimine, or carbodiimide moieties.Preferably, the polyisocyanates useful in the present invention are selected from the group consisting of aromatic diisocyanates, their dimers and trimers, or mixtures thereof.
[0052] The polyisocyanates useful in the present invention may include one or more polyisocyanate prepolymers, which may be formed by reaction with monols, diols, diamines, or monoamines, which are then modified by reaction with additional isocyanates to form allophanate or biuret modified prepolymers. Such prepolymers may further include polyalkoxy or polyether chains. Alternatively, such prepolymers may then be mixed with a trimerization catalyst to obtain allophanate or biuret modified polyisocyanate compositions. The preparation of such allophanate or biuret prepolymers and subsequent trimerization are known in the art, see, for example, U.S. Pat. Nos. 5,663,272 and 6,028,158. Still further, suitable polyisocyanates may be modified with ionic compounds, such as aminosulfonic acids.
[0053] Commercially available polyisocyanates include, for example, Desmodur L75, N3300, N3600, and N3900 polyisocyanates, and Bayhydur XP 2655, 401-60, and 401-70 polyisocyanates (Covestro); Tolonate HDT, HDT-LV, and HDT-LV2, and Easaqua L 600 polyisocyanates (Vencorex Chemicals); DURANATE TLA-100 and TMA-100 polyisocyanates (AsahiKASEI); and Aquolin 268, 269, and 270 polyisocyanates (Wanhua Chemicals).
[0054] The polyisocyanates useful in the present invention can be used alone or diluted with one or more solvents to form a polyisocyanate solution before mixing with the polyol component. Such solvents (also referred to as "diluting solvents") can reduce the viscosity of the polyisocyanate and are not reactive with the polyisocyanate. The solvents can be used in amounts of 5% to 150%, 15% to 130%, 20% to 120%, or 30% to 100% by weight based on the weight of the polyisocyanate. Suitable diluting solvents can include, for example, ethyl acetate, butyl acetate, MEK, or mixtures thereof. The solids content of the polyisocyanate component can be 40 to 100% by weight, preferably 50 to 90% by weight, and more preferably 55 to 80%. The polyurethane adhesive composition of the present invention may have an equivalent ratio of the total number of isocyanate group equivalents in the polyisocyanate, which may contain several different polyisocyanates, to the total number of hydroxyl group equivalents in the polyester polyol component, which may be, for example, in the range of 1:1 to 2.0:1, or 1:1 to 1.8:1, or 1:1 to 1.5:1, or 1:1 to 1.2:1. According to a preferred embodiment of the present disclosure, the amount of the polyisocyanate compound is appropriately selected so that the isocyanate groups are present in a stoichiometric molar amount relative to the total molar amount of hydroxyl groups contained in the polyester polyol component.
[0055] The polyurethane adhesive composition of the present invention may further include conventional additives such as, for example, catalysts to accelerate cure, pigments, light stabilizers, ultraviolet (UV) absorbing compounds, leveling agents, wetting agents, dispersants, neutralizing agents, defoamers, or rheology modifiers, or mixtures thereof. These additives may be present in amounts of 0 to 20% by weight, 1 to 10% by weight, based on the weight of the polyurethane composition.
[0056] According to one embodiment of the present disclosure, the weight ratio of the polyester polyol component to the polyisocyanate component is from about 100:5 to about 100:30, preferably from about 100:8 to about 100:25, and more preferably from about 100:10 to about 100:20.
[0057] The polyurethane adhesive can be prepared by mixing the polyester polyol component and the polyisocyanate component to homogeneity and adding an amount of solvent to achieve the desired solids content.
[0058] Second Substrate The second substrate includes a polyethylene terephthalate (PET) film or a polypropylene (PP) film.
[0059] There are three general types of PP polymers: homopolymer, random copolymer, and block copolymer. Comonomers are typically used with ethylene or butylene. Suitable suppliers / products for PP include Sinopec Chemicals.
[0060] The PP-based film may comprise 50% to 100% by weight of the PP component. Preferably, the PP-based film comprises 70% to 99% by weight of the PP component, preferably 80% to 95% by weight, or alternatively 90% to 98% by weight of the PP component. The PP component comprises at least one PP polymer, optionally two or more PP polymers (i.e., different grades of PP).
[0061] Preferably, the PP-based film comprises 50% to 100% by weight of a PP component of homopolymer PP or random copolymer PP or a combination thereof. Preferably, the PP-based film comprises 100% by weight of a PP component of either homopolymer PP or random PP copolymer.
[0062] An example of a PP grade is homopolymer PP. Preferably, the homopolymer PP has a melt flow rate (230°C / 2.16Kg) ("MFR") of 2.6-3.0g / 10min, preferably 2.7-2.9g / 10min, more preferably about 2.8g / 10min. Preferably, the homopolymer PP has a tensile strength at yield of 26-36MPa, preferably 28-35MPa, more preferably about 30MPa or more. Preferably, the homopolymer PP has an isotactic index of 93% or more, more preferably 94% or more, even more preferably 95% or more, or even less than 98%.
[0063] An example of a PP grade is random copolymer PP (RCPP). Preferably, the RCPP has a melt flow rate (230°C / 2.16Kg) ("MFR") of 2.6-3.0g / 10min, preferably 2.7-2.9g / 10min, more preferably 2.8g / 10min. Preferably, the random copolymer PP has a tensile strength at yield of 27-37MPa, preferably 29-36MPa, more preferably 31MPa or more. Preferably, the random copolymer PP comprises an isotactic index of 96% or more, more preferably 97% or more, even more preferably 98% or more.
[0064] The PP-based film in the second substrate can be a blown film, a cast film, a machine-direction stretched film, or a biaxially stretched film. The PP-based film in the second substrate can be produced by blown, cast, water-cooled, double bubble, or other techniques known to those skilled in the art, such as those described in Film Processing Advances, Toshitaka Kanai and Gregory A. Campbell (eds.), Chapter 7 (Biaxial Oriented Film Technology), pp.194-229. In some embodiments, after production, the film may be subjected to machine-direction stretching (MDO) or biaxial stretching process to provide a machine-direction stretched film or a biaxially stretched film, respectively.
[0065] PET stands for polyethylene terephthalate. Polyethylene terephthalate can be obtained by a conventionally known method of polycondensing a diol component (i.e., ethylene glycol) and a dicarboxylic acid component (i.e., terephthalic acid). Specifically, it can be produced by a general melt polymerization method in which the diol component and the dicarboxylic acid component are esterified and / or transesterified, and then polycondensed under reduced pressure, or by a known solution heating dehydration condensation method using an organic solvent.
[0066] The manufacturing process for PET can include longitudinally stretching or biaxially stretching the film.
[0067] The amount of the diol component used in producing PET is substantially equimolar to 100 moles of the dicarboxylic acid or its derivative, but is usually in excess of 0.1 mol % to 20 mol % due to distillation occurring during esterification and / or transesterification and / or polycondensation.
[0068] The polycondensation is preferably carried out in the presence of a polymerization catalyst. The timing of adding the polymerization catalyst is not particularly limited as long as it is added before the polycondensation, and the catalyst may be added when the raw materials are charged or when the pressure reduction is started.
[0069] The PET-based film or PP-based film in the second substrate may include 1 to 10 layers, or 1 to 8 layers, or 1 to 5 layers.
[0070] Laminate The laminate is 1) providing a first substrate comprising a metallized PE-based film (as described above) and a second substrate comprising a polyethylene terephthalate-based film or a polypropylene-based film (as described above); 2) adhering together a first substrate to a second substrate by using a two-component solvent-based polyurethane adhesive composition, The concentration of fatty acid or fatty acid derivative in the metallized PE-based film is less than 300 ppm based on the total weight of the metallized PE-based film; A two-component solvent-based polyurethane adhesive composition comprising a polyester polyol component and a polyisocyanate component, The polyester polyol component has 40% by weight to 60% by weight of aromatic rings in the main chain based on the total weight of the polyester polyol, and has a Mw of 5,000 to 50,000; The weight ratio of the polyester polyol component to the polyisocyanate component is from 100:5 to 100:30.
[0071] The laminate of the present disclosure has a viscosity of 2.3 cc / m2 measured for 24 hours at 23° C. and 0% relative humidity, when measured using the test method described herein. 2 An OTR of less than 2.0 cc / m2 in 24 hours when measured using the test method described herein. 2 Less than or equal to 1.9cc / m in 24 hours 2 Less than or equal to 1.8cc / m in 24 hours 2 It has the following OTR:
[0072] The laminates can be used to form articles such as packaging. Examples of packaging that can be formed from the laminates of the present invention can include flexible packaging, pouches, stand-alone pouches, and pre-made packages or pouches. The laminates of the present invention can be used in food packaging. Examples of food products that can be included in such packaging include meat, cheese, cereal, nuts, juice, sauces, and the like. Such packaging can be formed using techniques known to those skilled in the art based on the teachings herein and based on the particular application of the packaging (e.g., type of food, amount of food, and the like). EXAMPLES
[0073] Some embodiments of the present invention will now be described in the following examples. However, the scope of the present disclosure is of course not limited to the formulations shown in these examples. Rather, the examples simply relate to the invention of the present disclosure.
[0074] Information on the raw materials used in the examples is listed in Table 1 below.
[0075] [Table 1]
[0076] * IPA stands for isophthalic acid, PA stands for phthalic acid, AdA stands for adipic acid, EG stands for ethylene glycol, DEG stands for diethylene glycol, SA stands for sebacic acid, and NPG stands for neopentyl glycol.
[0077] All PE-based films were produced by blowing process. The formulations are listed in Table 2. The thickness of film-1 and film-2 was 50 μm. Vacuum metallization was carried out on an industrial metallizer (Machine type K5 EXPERT, BOBST Company) with OD=2.0. MET-1 and MET-2 are the symbols for metallized film-1 and film-2, respectively. Before adhesive lamination, the produced vacuum deposited films were stored in the form of film rolls under an environment of 23°C and 50% humidity for 2 weeks. The surface energy of the metal layer of metallized film-1 (MET-1) was reduced to less than 34 dynes, and the surface energy of the metal layer of metallized film-2 (MET-2) is still more than 46 dynes / cm. Then, adhesive lamination was carried out on a Labo-Combi 400 machine manufactured by Nordmeccanica.
[0078] [Table 2]
[0079] Prior to adhesive lamination, the prepared VMPE films were stored in the form of film rolls under an environment of 23°C and 50% humidity for 2 weeks. The surface energy of the metal layer of MET-1 was reduced to less than 34 dynes, and the surface energy of the metal layer of MET-2 was still greater than 46 dynes / cm. Then, all VMPE films were laminated with PET film (thickness=12μm, product type: PET flat film, Anhui Guofeng Plastic Industry Co.,Ltd.) or BOPP film (thickness=18μm, product type: PP, Guangdong Weifu Packaging Material Co., Ltd.) using the adhesives listed in Tables 3 and 4. In addition, a three-layer laminate structure containing VMPET (thickness=12μm, product type: P11, Jiaxing Pengxiang Packaging Materials CO.) was prepared for comparison, as shown in Table 3.
[0080] As shown in Tables 3 and 4, all of the inventive samples have a lower OTR than the comparative samples. The results demonstrate a good synergy between the adhesive with the chemical composition of the present invention and the VMPE film of the present invention with good surface energy of the metal layer in enhancing the oxygen barrier of the laminate structure.
[0081] Example 1
[0082] [Table 3] All coating weights are 3.0 gsm.
[0083] Examples 1-1, 1-2, 1-3, and 1-4 used a two-component SB (solvent-based) PU adhesive of the present invention and a metallized PE-based film of the present invention (MET-2), which showed good OTR results.
[0084] Examples 1-1, 1-2, and 1-4 used the same inventive metallized PE-based film (MET-2), but used a two-component SB PU adhesive that was polyester polyol-based but had either a lower aromatic ring backbone or too high a Mw, which were outside the scope of the present invention, and they showed inferior OTR relative to the inventive examples.
[0085] Comparative Examples 1-3 used the same inventive metallized PE-based film (MET-2), but used a two-component SB PU adhesive with a polyether polyol backbone rather than a polyester polyol backbone, and the OTR was not as good as the inventive examples.
[0086] Comparative Examples 1-5 were pure PET films with no adhesive lamination and showed very high OTR results relative to the inventive examples, indicating that both metallization and adhesive are important to achieve good OTR.
[0087] Comparative Examples 1-6 were pure metallized PE films with no adhesive lamination and showed very high OTR results for the inventive examples, indicating that the adhesive is important to achieve good OTR.
[0088] Comparative Examples 1-7 were PE films without adhesive lamination and showed very high OTR results for the inventive examples, indicating that both metallization and adhesive are important to achieve good OTR.
[0089] Example 2
[0090] [Table 4] All coating weights are 3.0 gsm.
[0091] Examples 2-1 and 2-2 used a two-component SB (solvent-based) PU adhesive of the present invention and a metallized PE-based film of the present invention (MET-2), which showed good OTR results.
[0092] Comparative Examples 2-1 and 2-2 used the adhesive of the present invention, but with a different metallized PE film (MET-1), and showed poor OTR results.
[0093] Comparative Example 2-3 used the same inventive metallized PE-based film (MET-2), but used a two-component SB PU adhesive with a polyether polyol backbone rather than a polyester polyol backbone, and its OTR was not as good as the inventive examples.
[0094] Comparative Examples 2-4 used the same metallized PE-based film of the present invention (MET-2), but used a polyacrylic WB adhesive rather than the adhesive of the present invention, and they showed poor OTR results.
[0095] Comparative Examples 2-5 used OPP / / VMPET / / PE and polyacrylic based WB adhesives, which showed poor OTR results.
[0096] Comparative Examples 2-6 used PET / / VMPET / / PE and a polyacrylic WB adhesive, which showed poor OTR results.
[0097] Comparative Example 2-7 was a PET film with no adhesive lamination and showed significantly higher OTR results relative to the inventive examples.
[0098] Comparative Example 2-8 was an OPP film with no adhesive lamination and showed significantly higher OTR results relative to the inventive examples.
[0099] Comparative Example 2-9 was a pure metallized PE film (MET-1) with no adhesive lamination and showed very high OTR results relative to the inventive examples.
[0100] Comparative Example 2-10 was a pure metallized PE film with no adhesive lamination (MET-2) and showed very high OTR results relative to the inventive examples.
[0101] Comparative Example 2-11 was a PE film with no adhesive lamination and showed very high OTR results relative to the inventive examples.
[0102] Standard process for preparing the inventive example polyester (IE-PES) and the comparative example polyester (CE-PES): All raw materials (IPA, AdA, EG and DEG etc.) are charged to the reactor, heated at 100°C and held at this temperature for 30 minutes, then heated to 175°C and held for another 45 minutes, then the temperature is increased to 225°C and held until the acid number is less than 25 mg KOH / g. Vacuum (about 500mmHg) is then applied and held for 15-30 minutes. The temperature is then maintained and the vacuum gradually reduced to about 200mmHg. If the acid number is less than 10 KOH / g, the vacuum is reduced to about 50mmHg, if the acid number is less than 2 KOH / g, the vacuum is reduced to about 10mmHg, then cooling to 160°C begins with N 2 Break the vacuum at and when the temperature is below 160°C, then begin adding ethyl acetate to achieve the desired solids content, continue cooling to 70°C and charge.
[0103] Preparation of Polyurethane Adhesive Compositions Solvent-based (SB) adhesives were prepared according to the following procedure: weigh out a certain amount of polyester polyol and co-reactant F, mix them together according to the designed mix ratio, then start stirring and add a calculated amount of ethyl acetate to achieve 30% solids, and continue stirring to ensure the adhesive is homogeneous. The prepared SB adhesives were subjected to lamination process on a Labo-Combi 400 machine manufactured by Nordmeccanica to ensure the dry coating weight was 3.0-3.5 gsm.
[0104] Solvent-free (SL) adhesives: weigh out a certain amount of NCO prepolymer and polyol co-reactant and mix them together to get a homogenous adhesive, then pour the adhesive onto a coating roller on a Labo-Combi 400 machine from Nordmeccanica and perform lamination, ensuring that the dry coating weight is 1.8-2.0 gsm coating weight.
[0105] Water-Based (WB) Adhesive: The WB adhesive was directly laminated on a Labo-Combi 400 machine from Nordmeccanica to ensure a dry coating weight of 2.0-2.5 gsm.
[0106] Test Method Oxygen transmission rate (OTR) Oxygen transmission rates were measured using purified oxygen in accordance with ASTM D-3985 at a temperature of 23°C and 0% relative humidity using a MOCON OX-TRAN model 2 / 21 measuring device. Samples with a barrier data of 200cc / m 2 / day or more, the test area is expanded to 50cm 2 From 5cm 2 A mask was applied to reduce the chromatic aberration to obtain data over a wider test range.
[0107] Optical Density (OD) Testing The OD test was carried out using a spectrophotometer (Type LS117, Shenzhen Linshang Technology Co., Ltd.). The metallized film was placed between the light emitter and the receptor, with the metallized surface facing the emitter. The OD was read and recorded.
[0108] Surface Energy Test The test was based on the use of an ACCU DYNE TEST™ marker pen based on a valve tip applicator. The principle was to keep the test portion of the pen separate from the fluid storage portion of the pen.
[0109] The dyne level test procedure using the pen was as follows.
[0110] A piece of metallized film sample is placed on a flat glass plate.
[0111] Record the ambient temperature and relative humidity. If the sample temperature is different from the ambient temperature, allow it to stabilize.
[0112] At least three points are tested across the sample; 1 / 4, 1 / 2, and 3 / 4 points across the film section.
[0113] Wetness determination 1. Select a marker pen with a dyne level that is likely to be slightly lower than the dyne level of the test sample.
[0114] 2. Press the applicator tip firmly down onto the target material until the tip is saturated with ink.
[0115] 3. With a light touch, draw the pen across the test sample in two or three parallel passes. Ignore the first pass. Evaluate only the last pass to wash contaminants from the tip and to ensure that the test fluid layer is thin enough for accurate measurements.
[0116] 4. If the last ink swath remains wet on the test specimen for more than 3 seconds, repeat steps 2 and 3 with the next higher dyne level marker. If the last ink swath beaded, tears, or shrinks into a thin line within 1 second, repeat steps 2 and 3 with the next lower dyne level marker.
[0117] 5. When the ink swath is held for 1-3 seconds before losing its integrity, the dyne level of the marker closely matches the dyne level of the sample, and the corresponding pen value is recorded.
[0118] Determination of fatty acid content The fatty acid content is CH 2 CI 2The additives were analyzed by extracting them from the films using HCl followed by filtration and analysis by LC-MS (liquid chromatography mass spectrometry). Standard solutions were made with fatty acids at appropriate concentration ranges.
[0119] Determination of anti-adhesive agent content The antiblocking agent was analyzed by thermogravimetric (TGA) analysis. The TGA was performed on a TA Q500 instrument. The film samples were N 2 The test protocol was as follows: -Heating from 25°C to 800°C at 10°C / min Isothermal at -800 °C for 3 min
[0120] The weight of the residue was recorded as the amount of antiblock additive.
[0121] Determination of slip agent content and antioxidant content The slip agent and antioxidant content were analyzed by total dissolution method. Film samples were dissolved with 0.075% triethyl phosphite in o-xylene at 130°C. The solution was cooled and methanol was added followed by stirring. After the solids settled, the solution was injected into a liquid chromatography (LC) autosampler for antioxidant analysis and a gas chromatography (GC) for slip additive analysis.
Claims
1. A laminate comprising: A first substrate comprising a metallized polyethylene-based (PE-based) film; A second substrate comprising a polyethylene terephthalate-based film or a polypropylene-based film; an adhesive layer adhering the first substrate to the second substrate, the adhesive layer being derived from a two-component solvent-based polyurethane adhesive composition; the concentration of fatty acid or fatty acid derivative in the metallized PE-based film is less than 300 ppm, based on the total weight of the metallized PE-based film; the two-component solvent-based polyurethane adhesive composition comprises a polyester polyol component and a polyisocyanate component; the polyester polyol component has about 40% by weight to 60% by weight of aromatic rings in the main chain, based on the total weight of the polyester polyol, and has a molecular weight (Mw) of 5,000 to 50,000; A laminate, wherein the weight ratio of said polyester polyol component to said polyisocyanate component is from 100:5 to 100:
30.
2. The laminate of claim 1, wherein the weight ratio of said polyester polyol component to said polyisocyanate component is from 100:10 to 100:
20.
3. 2. The laminate of claim 1, wherein the metallized PE-based film comprises a PE-based film and a metal layer.
4. 2. The laminate of claim 1, wherein the PE-based film in the metallized PE-based film comprises a skin layer, a core layer, and a sealant layer.
5. 5. The laminate of claim 4, wherein the antiblocking agent is present in the sealant layer in an amount of at least 200 ppm based on the total weight of the sealant layer.
6. 5. The laminate of claim 4, wherein a slip agent is present in the sealant layer in an amount less than 500 ppm based on the total weight of the sealant layer.
7. 10. The laminate of claim 1, wherein the metallized PE-based film has an optical density (OD) of at least 1.5 and no greater than 4.
0.
8. 10. The laminate of claim 1, wherein the concentration of antioxidant in the metallized PE-based film layer is less than 3000 ppm based on the total weight of the metallized PE-based film.
9. 2. The laminate of claim 1, wherein the PE-based film of the metallized PE-based film layer is a blown film, a cast film, a longitudinally stretched film, or a biaxially stretched film.
10. 4. The stack of claim 3, wherein the metal layer comprises Al, Zn, Au, Ag, Cu, Ni, Cr, Ge, Se, Ti, Sn, or an oxide thereof.
11. The laminate according to claim 1 , wherein the PP-based film comprises 50% to 100% by weight of a PP component of the PP-based film.
12. An article comprising the laminate according to any one of claims 1 to 11.
13. A method for preparing a laminate according to any one of claims 1 to 11, comprising the steps of: 1) providing a first substrate comprising a metallized PE-based film and a second substrate comprising a PET-based film or a PP-based film; 2) adhering the first substrate to the second substrate by using a two-component solvent-based polyurethane adhesive composition; the concentration of fatty acid or fatty acid derivative in the metallized PE-based film is less than 300 ppm based on the total weight of the metallized PE-based film; the two-component solvent-based polyurethane adhesive composition comprises a polyester polyol component and a polyisocyanate component; the polyester polyol component has 40% by weight to 60% by weight of aromatic rings in its main chain based on the total weight of the polyester polyol, and has a Mw of 5,000 to 50,000; The method wherein the weight ratio of said polyester polyol component to said polyisocyanate component is from 100:5 to 100:30.
Citation Information
Patent Citations
Adhesive composition
JP2004285183A
Metallized polyethylene film with improved metal adhesion
JP2016523193A
Reactive adhesive, laminate film, and package
JP2020094154A
Gas barrier laminating adhesive, laminate and packaging
JP6915728B1
Metallized polyethylene films and related structures
WO2020155795A1