Reinforcement-Inserted Noncombustible Board and its manufacturing method
A semi-noncombustible expanded polystyrene insulation material with molded grooves and GFRP reinforcement addresses environmental and health issues of existing materials, offering enhanced fire resistance, thermal insulation, and durability for building applications.
Patent Information
- Application Number
- KR1020240087709
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-07-03
AI Technical Summary
Existing building materials, such as styrofoam and gypsum boards, pose environmental pollution and health risks due to non-decomposability and asbestos content, while lacking adequate fire resistance and moisture resistance, necessitating a non-combustible, eco-friendly alternative with improved rigidity and thermal management.
A semi-noncombustible expanded polystyrene insulation material is manufactured with molded grooves and reinforced with GFRP, processed to form grooves, and bonded with asbestos-free boards to enhance rigidity and fire resistance, featuring a manufacturing process that includes adding flame retardants and reinforcing materials.
The solution provides a non-combustible board with delayed combustion, reduced toxic gas generation, excellent thermal insulation, sound absorption, and improved durability, suitable for floors, walls, and roofs, while being eco-friendly and resistant to moisture.
Smart Images

Figure 112024072325807-PAT00006_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a non-combustible board using an insulating material and a method for manufacturing the same. More specifically, the invention relates to a non-combustible board using an insulating material that is resistant to moisture and does not easily rust, and can be used as a floor, wall, and roof material, and a method for manufacturing the same, by manufacturing an insulating material made of semi-non-combustible expanded polystyrene, processing a plurality of molding grooves on the surface, inserting a reinforcing material to improve rigidity, and bonding asbestos-free boards to both sides of the insulating material with the inserted reinforcing material. Background Technology
[0003] Generally, styrofoam, which is produced by mechanically injecting butane and nitrogen gases into polymer polystyrene and expanding it into a molten state, is a synthetic resin product with a very wide range of uses and applications, such as cushioning packaging for electrical products, building insulation, and disposable food containers, as it is extremely lightweight due to its low specific gravity and has excellent resilience, cushioning, thermal insulation, processability, and economic efficiency.
[0004] As such, although styrofoam is utilized as an essential item in daily life due to its various good physical properties, most products made from styrofoam are disposable, so it was common for them to be buried in landfills or incinerated after a single use.
[0005] However, the quantity and volume of waste styrofoam products being disposed of are vast, requiring enormous manpower and expense for collection and transportation. Furthermore, since landfilled waste styrofoam products do not decompose easily, they cause serious pollution, and when incinerated, they become a major cause of global warming.
[0006] To resolve this problem, Korean registered patent No. 10-0710044 proposed a method for manufacturing insulation material by mixing stone powder and a non-combustible adhesive with waste styrofoam and pressure molding the mixture.
[0007] In addition, Korean registered patent No. 10-1943853 proposed a method for manufacturing a non-combustible insulation board by immersing waste styrofoam in a nano-zinc mica loess solution, mixing it with calcium sulfate, and then molding it.
[0008] However, these prior art documents had disadvantages such as insufficient non-flammability or high manufacturing costs, making commercialization difficult.
[0009] Meanwhile, gypsum board is widely used as a non-combustible board for conventional building interiors. This is because the aforementioned gypsum board is inexpensive and non-combustible. However, gypsum board contains small amounts of asbestos, a carcinogen, and is vulnerable to moisture, which generates fine dust due to weathering during long-term use that is harmful to the human body. Consequently, its use is restricted in principle, but the reality is that its use cannot be curbed due to the lack of suitable substitutes.
[0010] Therefore, there is a demand for a board that can be used as a finishing material for interior walls, ceilings, etc., is non-combustible, is harmless to the human body, guarantees sufficient rigidity, and has an aesthetic appearance. Prior art literature
[0012] [Patent Document 0001] Korean Registered Patent No. 10-2590374 (Registered Oct. 12, 2023) [Patent Document 0002] Korean Registered Patent No. 10-2558934 (Registered Jul. 19, 2023) [Patent Document 0003] Korean Registered Patent No. 10-2484574 (Registered Dec. 30, 2022) [Patent Document 0004] Korean Registered Patent No. 10-2415013 (Registered Jun. 27, 2022) The problem to be solved
[0013] The objective of the present invention is to provide a semi-noncombustible expanded polystyrene insulation material that imparts noncombustible or semi-noncombustible performance during the production process of board panels used as interior and exterior building materials, thereby preventing gas generation, building collapse, and damage caused by fire, and possessing excellent thermal management performance for building materials.
[0014] Another objective of the present invention is to improve stiffness by processing a molded groove on one or both sides of the insulation material and inserting a reinforcing material made of GFRP, which is suitable for permanent structures as a substitute for rebar, having excellent specific strength and mechanical performance and high strength and elastic modulus.
[0015] Another objective of the present invention is to provide a panel applicable to floors, walls, and roofs by providing an eco-friendly non-combustible finishing material for CRC boards on both sides of an insulating material with inserted reinforcing material. means of solving the problem
[0017] The present invention relates to an insulating material having a plurality of molded grooves formed at regular intervals, and
[0018] A reinforcing material inserted into the above-mentioned molding groove to improve rigidity, and
[0019] It is characterized by applying adhesive to the upper and lower sides of the insulation material and joining the upper finishing material and the lower finishing material.
[0021] The above insulation material is characterized by the fact that the reinforcing material inserted into the molding groove formed on the upper side is GFRP that has been cut and inserted.
[0023] The present invention comprises the step of molding semi-flammable expanded polystyrene;
[0024] Step of forming the reinforcing material;
[0025] Insulation material cutting step of processing insulation material by cutting foam-molded semi-noncombustible expanded polystyrene in a cutting device;
[0026] A groove forming step in which the cut insulation material is supplied to a groove forming device and a carbide blade connected to a drill shaft is rotated at high speed to form grooves at regular intervals on the upper side of the insulation material;
[0027] A dust discharge step in which dust generated while processing molding grooves in the insulation material is collected in a dust collection tank and discharged to the outside through a discharge duct via a discharge pipe;
[0028] A reinforcement insertion step in which a reinforcement is inserted into and fixed in a molded groove of the insulation material;
[0029] A bonding agent application step of applying adhesive to the upper and lower sides of the insulation material fixed by inserting reinforcing materials;
[0030] A finishing material joining step in which an upper finishing material is supplied to the upper side and a lower finishing material to the lower side of an insulation material coated with an adhesive on the upper and lower sides, so as to join them to form an integrated unit;
[0031] It is characterized by a board completion stage in which a board panel is completed by joining finishing materials.
[0033] The above-mentioned molding groove forming step is characterized by allowing a drill shaft to rotate from a drill drive unit installed at regular intervals on a drill mounting base, and enabling the depth of the molding groove to be freely adjusted.
[0035] The above-mentioned molding groove forming step is characterized by allowing a drill shaft to rotate from a drill drive unit installed at regular intervals on a drill mounting base, enabling the depth of the molding groove to be freely adjusted, and simultaneously forming a lower molding groove on the lower side while forming the molding groove. Effects of the invention
[0039] The non-combustible expanded polystyrene according to the present invention has the advantage of significantly delaying the combustion speed in the event of a fire and suppressing the generation of toxic gases, thereby minimizing casualties and logistical damage, by imparting non-combustible or semi-non-combustible performance to the insulation material, and providing excellent flame retardancy, thermal insulation, sound absorption, and bonding properties.
[0040] According to the present invention, a processing device is provided for automatically processing a molded groove using carbide on one or both sides of an insulating material, thereby improving rigidity by inserting a reinforcing material made of GFRP, which is suitable for permanent structures as a substitute for rebar and has excellent specific strength and mechanical performance and high strength and elastic modulus, and contributing to resource circulation as a recycled material.
[0041] The present invention provides an eco-friendly, non-combustible finishing material for CRC boards that is resistant to fire and moisture and has excellent durability on both sides of an insulating material with inserted reinforcing material, as well as sound insulation, thermal insulation and heat resistance, temperature and humidity control, a high acoustic coefficient, and no shrinkage or expansion, thereby providing a panel applicable to floors, walls, and roofs. Brief explanation of the drawing
[0043] FIG. 1 is a plan view of an insulation material molding groove processing device according to one embodiment of the present invention. FIG. 2 is a front view of an insulation material molding groove processing device according to an embodiment of the present invention. FIG. 3 is a front view of another embodiment of a thermal insulation material molding groove processing device according to one embodiment of the present invention. FIG. 4 is an enlarged front view of a major part of the insulation material molding groove processing device of the present invention. FIG. 5 is a perspective view of an insulating material processed through the insulating material molding groove processing device of the present invention. FIG. 6 is a perspective view of a state in which a reinforcing material is inserted into a molded groove of the insulation material of the present invention and a finishing material is bonded. FIG. 7 is a front view of the insulation material cut from the non-combustible expanded polystyrene of the present invention. FIG. 8 is a front view of the processing state of the insulation material molding groove of the present invention. FIG. 9 is a front view of the state in which a reinforcing material is inserted into the molding groove of the insulation material of the present invention. FIG. 10 is a front view of the state in which finishing materials are bonded to both sides of the insulation material of the present invention. FIG. 11 is an enlarged cross-sectional view of a key part of the board panel of the present invention in a formed state. FIG. 12 is a front view of the insulation material processed according to FIG. 2 of the present invention, with a reinforcing material inserted and the insulation material joined. FIG. 13 is an enlarged cross-sectional view of the main part of FIG. 12 of the present invention. FIG. 14 is a block diagram showing the process of manufacturing expanded polystyrene of the present invention. FIG. 15 is a block diagram showing the most preferred embodiment of the present invention. Specific details for implementing the invention
[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by a skilled expert in the art to which this invention pertains. In general, the nomenclature used herein is well known and commonly used in the art.
[0046] The present invention relates to a method for manufacturing semi-flammable expanded polystyrene, wherein
[0047] When adding a non-combustible composition to expanded polystyrene particles, composition A containing chlorinated paraffin, chlorinated phosphate ester, a composite flame retardant, and an inorganic flame retardant,
[0048] Composition B containing polyhydric alcohol and inorganic phosphorus-based flame retardant, fly ash, quicklime, sodium silicate, magnesium hydroxide, non-combustible agent, and non-combustible agent-2,
[0049] Add expanded graphite and stir,
[0050] Composition C comprising acetic acid, polyethylene terephthalate, polyurethane, polyisocyanurate, ethylene-vinyl acetate copolymer, carbamate compound, and foaming agent,
[0051] It was confirmed that when semi-noncombustible expanded polystyrene is produced by sequentially adding and stirring diphenylmethaneisocyanate (MDI), excellent noncombustibility is imparted to the insulation material, thereby significantly delaying the combustion speed in the event of a fire and greatly suppressing the generation of toxic gases, thereby minimizing casualties and logistical damage, while also providing excellent flame retardancy, thermal insulation, sound absorption, and adhesion.
[0052] Accordingly, in one aspect, the present invention relates to a method for manufacturing semi-flammable expanded polystyrene comprising the steps of: adding a non-flammable composition to expanded polystyrene particles and stirring; and molding, pressing, and drying, wherein the step of adding a non-flammable composition to the expanded polystyrene particles and stirring comprises
[0053] (a) A first step of adding and stirring a composition of A containing chlorinated paraffin, chlorinated phosphate ester, a composite flame retardant, and an inorganic flame retardant;
[0054] (b) A second step of adding and stirring a composition B containing polyhydric alcohol, an inorganic phosphorus-based flame retardant, fly ash, quicklime, sodium silicate, magnesium hydroxide, a non-combustible agent, and non-combustible agent-2;
[0055] (c) A third step of adding expanded graphite and stirring;
[0056] (d) a fourth step of adding and stirring a composition of C comprising acetic acid, polyethylene terephthalate, polyurethane, polyisocyanurate, ethylene-vinyl acetate copolymer, a carbamate compound, and a foaming agent; and
[0057] (e) a fifth step of adding and stirring diphenylmethaneisocyanate (MDI); the present invention relates to a method for manufacturing semi-flammable expanded polystyrene comprising: (e) a fifth step of adding and stirring diphenylmethaneisocyanate (MDI).
[0059] In addition, the present invention relates to a method for manufacturing semi-flammable expanded polystyrene comprising the steps of: adding a non-combustible composition to expanded polystyrene particles and stirring; and molding, pressing, and drying, wherein the step of adding a non-combustible composition to the expanded polystyrene particles and stirring comprises: (a) a first step of adding and stirring a composition C comprising acetic acid, polyurea-polyethylene terephthalate, polyisocyanurate, ethylene-vinyl acetate copolymer, carbamate compound, and blowing agent to the expanded polystyrene particles; (b) a second step of adding and stirring a composition A containing chlorinated paraffin, chlorinated phosphate ester, composite flame retardant, inorganic flame retardant, polyhydric alcohol and inorganic phosphorus-based flame retardant, fly ash, quicklime, magnesium hydroxide, non-combustible agent, and non-combustible agent-2; and (c) a third step of adding and stirring expanded graphite. (d) a fourth step of adding and stirring diphenylmethaneisocyanate (MDI); the present invention relates to a method for manufacturing semi-flammable expanded polystyrene comprising: (d) a fourth step of adding and stirring diphenylmethaneisocyanate (MDI).
[0061] The present invention will be described in detail below.
[0062] The present invention relates to a method for manufacturing semi-noncombustible expanded polystyrene, wherein a noncombustible material having noncombustibility is added and stirred to expanded polystyrene particles that easily burn in fire in the order of composition A, composition B, expanded graphite, composition C, and MDI, compressed in a molding die to produce an EPS composition, and a drying process is performed to continuously manufacture expanded polystyrene for noncombustible interior and exterior building materials.
[0063] In the present invention, the process of adding and stirring a non-combustible composition to the expanded polystyrene particles is as follows, in the order of adding the non-combustible composition.
[0065] Step 1 (Composition of Agent A, KS-1000)
[0066] In the non-combustible composition of the present invention, composition A comprises chlorinated paraffin, chlorinated phosphate ester, composite flame retardant, and inorganic flame retardant.
[0067] In the present invention, the amount of A composition added may be 45 to 65 parts by weight, preferably 50 to 60 parts by weight, and more preferably 50 to 55 parts by weight, per 100 parts by weight of expanded polystyrene particles. When stirring with less than 45 parts by weight of A composition added during coating of expanded polystyrene, molding and curing do not occur during press molding, resulting in an unmolded defect. When stirring with more than 65 parts by weight of A composition added during coating of expanded polystyrene, the expanded polystyrene particles are not coated with a non-flammable agent, resulting in deformation and curing during press stirring, which leads to a defective product. Furthermore, even if a product is formed, it cannot be used due to deformation and whitening occurring over time.
[0069] Step 2 (Composition of Part B, KS-1000)
[0070] In the non-combustible composition of the present invention, the B-component composition comprises polyhydric alcohol, fly ash, quicklime, sodium silicate, magnesium hydroxide, non-combustible agent, non-combustible agent-2, and an inorganic phosphorus-based flame retardant.
[0071] In the present invention, the amount of the B composition added may be 45 to 65 parts by weight, preferably 50 to 60 parts by weight, and more preferably 50 to 55 parts by weight, per 100 parts by weight of expanded polystyrene particles. When stirring with less than 45 parts by weight of the B composition added during coating of expanded polystyrene, molding and curing do not occur during press molding, resulting in an unmolded defect. When stirring with more than 65 parts by weight of the B composition added during coating of expanded polystyrene, the expanded polystyrene particles are not coated with a non-flammable agent, resulting in deformation and curing during press stirring, which leads to a defective product. Furthermore, even if a product is formed, it cannot be used due to deformation and whitening occurring over time.
[0072] The A composition and B composition of the first and second steps contain KS-1000, and since mixing and stirring the A composition and B composition at once may result in abnormal coating and defects, the first and second steps are separated for addition and stirring.
[0074] Phase 3 (KSG)
[0075] Add expanded graphite (KSG) and stir.
[0076] In the present invention, the amount of expanded graphite added is 15 to 30 parts by weight, preferably 15 to 20 parts by weight, and more preferably 18 to 25 parts by weight, per 100 parts by weight of expanded polystyrene, and at this time, a significant effect on flame retardancy is observed. If less than 15 parts by weight of expanded graphite is added, a sufficient flame retardant effect cannot be obtained relative to the amount of expanded graphite used, and if it exceeds 30 parts by weight, cracks occur in the coated film, and the coating strength decreases, which may reduce flame retardancy.
[0078] Step 4 (Composition of C, KSP-2000)
[0079] In the non-combustible composition of the present invention, the C composition comprises acetic acid, polyethylene terephthalate, polyurethane, polyisocyanurate, ethylene-vinyl acetate copolymer, carbamate compound, and a foaming agent.
[0080] In the present invention, the amount of C composition added may be 45 to 65 parts by weight, preferably 50 to 60 parts by weight, and more preferably 50 to 55 parts by weight, per 100 parts by weight of expanded polystyrene particles. When stirring with less than 45 parts by weight of the C composition added during coating of expanded polystyrene, molding and curing do not occur during press molding, resulting in an unmolded defect. When stirring with more than 65 parts by weight of the C composition added during coating of expanded polystyrene, the expanded polystyrene particles are not coated with a non-flammable agent, resulting in deformation and curing during press stirring, which leads to a defective product. Furthermore, even if a product is formed, it cannot be used due to deformation and whitening occurring over time.
[0082] Stage 5 (KSM)
[0083] Diphenylmethaneisocyanate (MDI) is added and stirred.
[0084] In the present invention, the amount of MDI added is 100 to 120 parts by weight, preferably 100 to 110 parts by weight, per 100 parts by weight of expanded polystyrene, and at this time, a significant effect on flame retardancy is observed. If less than 100 parts by weight of MDI is added, a sufficient flame retardant effect cannot be obtained relative to the amount of MDI used, and if it exceeds 120 parts by weight, cracks occur in the coated film, and the coating strength decreases, which may reduce flame retardancy.
[0086] As shown in FIG. 1, the present invention can manufacture a semi-fireproof foam board (B) by adding EPS and stirring, adding composition A and composition B of KS-1000 and stirring first and second times, adding powdered KSG and stirring third time to coat the powder, adding composition C of KSP-2000 and stirring fourth time (each stirring time at room temperature is about 4 to 6 minutes), adding KSM and stirring fifth time (stirring time at room temperature is about 1 to 2 minutes), then introducing into a molding die, and performing a press process, a molding die drying process, a molding die discharge process, and a cutting process.
[0088] In the method for manufacturing semi-flammable expanded polystyrene of the present invention, the constituent components are described in detail.
[0089] Expanded polystyrene
[0090] The expanded polystyrene powder used in the present invention is a raw material that is widely available on the market. Polystyrene is a widely used plastic and is a polymer of styrene. It is a colorless, transparent thermoplastic material that softens at temperatures above 100°C and becomes a viscous liquid at around 185°C, and has properties that are resistant to acids, alkalis, oils, alcohols, etc.
[0091] Expanded polystyrene is a foamed product produced by injecting hydrocarbon gases, such as pentane or butane, into polystyrene resin and then expanding it with steam; it is a resource-saving material in which 98% of the volume is air and the remaining 2% is resin. The manufacturing process of expanded polystyrene involves injecting a blowing agent, such as pentane or butane gas, into styrene and polymerizing it with water, followed by heating until a predetermined molecular weight is achieved. The resulting beads, which are spherical particles of expanded polystyrene, are then washed and dried, and after wastewater treatment and sorting, the finished product is expanded polystyrene powder.
[0092] The raw material, expanded polystyrene powder, is first expanded at 100–110°C and 0.2–0.3 atmospheres. When heated to the above temperature at a pressure lower than atmospheric pressure, the raw material, expanded polystyrene particles, expand and foam.
[0094] Composition of A and B (KS-1000)
[0095] In the present invention, composition A comprises chlorinated paraffin, chlorinated phosphate ester, composite flame retardant, and inorganic flame retardant, and composition B comprises polyhydric alcohol and inorganic phosphorus-based flame retardant, fly ash, quicklime, sodium silicate, magnesium hydroxide, non-combustible agent, and non-combustible agent-2.
[0096] The above-described composition A of the present invention is characterized by containing 8-16% by weight of chlorinated paraffin, 20-60% by weight of chlorinated phosphate ester, 22-4% by weight of a composite flame retardant, 8-16% by weight of an inorganic flame retardant, and the remainder being additives.
[0097] The above B composition is characterized by containing 10 to 34 weight% polyhydric alcohol, 6 to 16 weight% inorganic phosphorus-based flame retardant, 1 to 6 weight% fly ash, 0.5 to 4 weight% quicklime, 6 to 18 weight% sodium silicate, 0.5 to 4 weight% magnesium hydroxide, 10 to 30 weight% non-combustible agent, 3 to 15 weight% non-combustible agent-2, and the remainder being additives.
[0098] Generally, flame retardants are classified into organic flame retardants and inorganic flame retardants. Organic flame retardants are flame retardants whose main components are halogen compounds such as bromine and chlorine compounds, and phosphorus compounds such as phosphate ester compounds. Inorganic flame retardants are flame retardants whose main components are antimony oxide compounds such as antimony trioxide and antimony pentoxide, hydroxide compounds such as aluminum hydroxide, heavy metal compounds, calcium carbonate (CaCO3), magnesium carbonate (MgHCO3), clay, talc, etc. Inorganic flame retardants are mainly used as auxiliary flame retardants.
[0099] First, the organic flame retardant of the present invention may be a halogenated hydrocarbon or a phosphate ester. Specifically, chlorinated paraffin or a chlorinated phosphate ester, or tris(1-chloro-2-propyl)phosphate (TCP) is used.
[0100] The composite flame retardant of the present invention may be a mixture of a phosphate, a halogenated hydrocarbon, and antimony oxide.
[0101] The inorganic flame retardant of the present invention uses aluminum hydroxide (Al(OH)3), magnesium hydroxide (Mg(OH)2), calcium carbonate (CaCO3), etc., and preferably aluminum hydroxide is used. Such inorganic flame retardants function to reduce the heat of combustion caused by an endothermic reaction. It is advantageous in terms of dispersibility and workability to use aluminum hydroxide with an average particle size of 1 to 10 μm, preferably 2 to 4 μm. If the aluminum hydroxide content is less than 6 weight%, the flame retardant effect cannot be properly obtained, and if it exceeds 14 weight%, cracks occur in the coating layer and strength decreases, which can reduce the flame retardant performance.
[0102] In addition, the inorganic phosphorus flame retardant of the present invention may be a single substance or a mixture thereof selected from the group consisting of red phosphorus, ammonium phosphate, and ammonium polyphosphate (APP). The inorganic phosphorus flame retardant is a representative substance for flame retardant action by promoting carbonization, and is produced into phosphoric acid, metaphosphoric acid, and polymetaphosphoric acid by thermal decomposition as shown in the reaction equation below. The main effects are the protective layer provided by the phosphoric acid layer and the blocking effect provided by the char produced by the dehydration of polymetaphosphoric acid.
[0104] R-OP → R + HOP → HO-P-OH → HOP-P… … … OP-OH+H2O
[0106] The polyalcohol of the present invention has a higher boiling point than water, which can improve the water resistance of the non-combustible board. As the polyalcohol, one or more types such as glycerin, ethylene glycol, and diethylene glycol may be used. The polyalcohol may be included in an amount of 10 to 30 weight%, preferably 15 to 25 weight%. At this time, if the content of the polyalcohol is less than 10 weight%, water resistance may decrease, and if it exceeds 30 weight%, the adhesion between the non-combustible material and the expanded polystyrene may decrease.
[0108] The additive of the present invention may be sodium silicate or sodium chloride, but is not limited thereto.
[0110] Expandable Graphite (KSG)
[0111] The expanded graphite used in the present invention may be commercially available expanded graphite. Generally, graphite is a crystalline form of carbon, having a structure in which carbon atoms are bonded in the form of planar hexagons and stacked in layers. The carbon-carbon bonds between the hexagonal planes are strong bonds, such as those in diamond, but the overlap of the sheets is a weak van der Waals bond, making them easy to exfoliate. It is known that graphite interlayer compounds are formed by the insertion of ions or molecules between the sheets.
[0112] Expanded graphite is made from this interlayer compound; that is, when a graphite interlayer compound in which a material is inserted between sheets using a chemical reaction is rapidly heated, the material inserted between the layers may become combustion gas. The release of the gas generated at that time explosively expands the space between the layers, causing the graphite to expand in a stacked, layer-by-layer direction. In some cases, it swells up to hundreds of times the size of the graphite. Such a material is called expanded graphite.
[0113] Expanded graphite is produced by acid-treating graphite, in which nitric acid or sulfuric acid is added to the crystal structure of the acid-treated graphite. The added substances increase in volume when heated, allowing the expanded graphite to expand vertically. As the vertically expanded graphite increases in volume, it blocks flames, and the pores created during expansion improve thermal insulation performance. Expanded graphite is an alternative material that imparts flame retardancy; when heated, the water and oxide compounds contained within it generate gas, and as a result, the scale-shaped graphite expands to form a layer (carbide) that is stable against heat or chemicals, thereby exhibiting a flame retardant effect in a solid-state char manner.
[0114] The present invention forms flame-retardant expanded polystyrene by bonding the expanded polystyrenes together through a process of spraying and coating with the aforementioned expanded graphite and drying.
[0116] C composition (KSP-2000)
[0117] In the present invention, the C composition contains acetic acid, polyethylene terephthalate, polyurethane, polyisocyanurate, ethylene-vinyl acetate copolymer, carbamate compound, and a foaming agent.
[0118] The C composition of the present invention may contain 20-30% by weight of acetic acid, 1-5% by weight of polyethylene terephthalate, 20-40% by weight of polyurethane, 15-30% by weight of polyisocyanurate, 7-15% by weight of ethylene-vinyl acetate copolymer, 3-12% by weight of a carbamate compound, and 1-5% by weight of a foaming agent.
[0120] Polyurethane (PUR) and polyisocyanurate (PIR) refer to urethane foam used as raw materials for foamed urethane. PUR is a polymer generally bonded by carbamate (urethane) bonds; it is an abbreviation for polyurethane, which is referred to as rigid urethane insulation, and is a product produced by foam molding using isocyanates and polyols as main ingredients. PIR is an abbreviation for polyisocyanurate, and it is a product produced by foam molding isocyanurate formed by the self-reaction of three isocyanate molecules. Although PUR and PIR are referred to by the same general term and belong to the same PU family, they are materials with different molecular structures. Furthermore, PIR is a product developed to enhance the flame retardancy of existing PUR properties.
[0122]
[0123] [PIR Chemical Equation]
[0124]
[0125] [Chemical reaction equation of PUR]
[0127] Ethylene-vinyl acetate copolymer, carbamate compounds, and blowing agents are used as raw materials that primarily act as adhesives in making EPS compositions. Partial chemical reactions occur during the mixing process of the C composition.
[0128] The above carbamate compound may be a tertiary amine carbamate selected from the group consisting of dimethylaminoethoxyethyl carbamate, bis(dimethylaminopropyl)amino-2-propyl carbamate, dimethylaminoethyl carbamate, and mixtures thereof.
[0129] The above foaming agent may use physical foaming agents and chemical foaming agents.
[0130] Chemical blowing agents are compounds that form gaseous products upon reaction with isocyanates, and physical blowing agents are compounds that are dissolved or emulsified in the starting materials for polyurethane production and vaporize under polyurethane formation conditions. Possible chemical blowing agents are, in particular, water, and, carboxylic acids, for example, formic acid may also be used. Examples of physical blowing agents include chlorofluorocarbons, hydrofluorocarbons, hydrocarbons, and liquid CO2.
[0132] MDI (diphenylmethane diisocyanate, KSM)
[0133] The present invention performs a process of adding and stirring MDI (diphenyl methane diisocyanate) to expanded polystyrene. The MDI functions as a foaming agent to enhance flame retardancy.
[0134] Since the aforementioned expanded graphite is a foamable graphite, there is no issue with the mixing order during the formulation process; however, since MDI is used as a curing foaming agent, it must be added at the end of the process.
[0135] Polystyrene particles are first foamed according to the user at a constant temperature and pressure, and the expanded polystyrene raw material is stored in a silo and dried, then transferred to a stirrer and stirred in the order of A composition - B composition - expanded graphite - C composition - MDI simultaneously with stirring in the stirrer, discharged to a molding jig (600X1050X3670) of expanded polystyrene, and a pressure of 500T is applied to the molding jig at the press position to form a molded product and manufacture a product molded product.
[0137] The semi-noncombustible expanded polystyrene of the present invention can be applied without limitation to the type, shape, or location of materials vulnerable to heat and flames, and when burned with high-temperature heat, only the surface directly in contact with the applied substrate burns locally while the substrate does not burn, thereby protecting lives and property from fire.
[0139] The expanded polystyrene fireproof board for construction according to one embodiment of the present invention satisfies the semi-fireproof performance in the standards for flame retardant performance and fire spread prevention structure of building finishing materials as stipulated in Ministry of Land, Infrastructure and Transport Notification No. 2020-1053.
[0140] In the above notice, semi-noncombustible materials are defined as materials for which the total heat released during the first 10 minutes after the start of the heating test according to Korean Industrial Standard KS F ISO 5660-1 [Combustion Performance Test - Heat Release, Smoke Generation, Mass Loss Rate Part 1: Heat Release Rate (Cone Calorimeter Method)] is 8 MJ / ㎡ or less, the maximum heat release rate during the first 10 minutes does not exceed 200 kW / ㎡ for 10 seconds or more continuously, and there are no fire-hazardous cracks, holes, or melting (including the complete melting or disappearance of the core material in the case of composite materials) penetrating the test specimen after heating for 10 minutes, and in the case of composite materials, while satisfying the above conditions, there is no partial melting or shrinkage of the core material (referring to cases where the core material of the test specimen melts or shrinks, causing the steel plate on the bottom surface of the test specimen to be visible).
[0141] In addition, according to the gas toxicity test results of Korean Industrial Standard KS F 2271, the average time to stop activity of experimental mice must be 9 minutes or more.
[0143] The semi-flammable expanded polystyrene produced in this manner is not limited to the technical details described above, but includes those produced through various compositions and steps.
[0144] After molding the above-mentioned semi-flammable expanded polystyrene, it is moved to a conventional cutting device not shown to be cut to a desired size and thickness and supplied as an insulating material (110).
[0145] The above-mentioned insulating material (110) is formed by forming a molded groove (111) on the upper side or on both the upper and lower sides through a groove forming device (200) as shown in FIGS. 1 to 4.
[0146] The above-mentioned home forming device (200) is installed such that a supply belt (212) is installed horizontally along a frame (210) that is installed at a certain height from the floor, and power from a motor not shown is supplied to rotate it clockwise.
[0147] A dust collection tank (310) is installed in the upper central part of the above frame (210), and a dust discharge device (300) is installed in which a discharge duct (330) for discharging dust to the outside is connected to the upper side of the dust collection tank (310) through a plurality of discharge pipes (320).
[0148] The above-mentioned home forming device (200) is configured such that supply guide rollers (213) are installed at regular intervals on both sides of the frame (210) to allow the insulation material (110) to be placed on top and supplied while moving along a regular trajectory on the upper side of the supply belt (212), and is installed in two places at regular intervals inside the dust collection tank (310), or a drill mounting stand (210) is installed on one side.
[0149] On the above drill mounting base (210), drill drive units (220, 240) are installed on one side or facing each other at regular intervals in the direction in which the insulation material (110) is supplied, and a drill shaft (221) is connected to the drill drive units (220, 240) to rotate at high speed, and a carbide blade (222) is installed at the tip of the drill shaft (221) to independently form the molding groove (111) or to simultaneously process the molding groove (111) and the lower molding groove (112).
[0150] The above drill shaft (221) is rotated at a high speed of about 55,000 to 75,000 rpm per minute through the drill drive unit (220, 240), and the carbide blade (222) continuously processes the supplied insulating material (110) by selecting the molding groove (111) and the lower molding groove (112).
[0151] The molding groove (111) and lower molding groove (112) processed in the above insulation material (110) are formed only in one direction, either the upper side and the lower side or the upper side and the lower side. The molding groove (111) and lower molding groove (112) are processed at regular intervals along the direction in which the insulation material (110) is supplied, and the number and depth of the molding groove (111) and lower molding groove (112) can be varied by adjusting the position of the carbide blade (222).
[0152] As the above insulation material (110) is supplied, the drill shaft (221) is driven by the driving unit (220, 240) installed at regular intervals, and the molding groove (111) is simultaneously formed at regular intervals through the carbide blade (222) that rotates together.
[0153] By installing a drill drive unit (220) on one side through the above drill mounting stand (211), a molding groove (111) can be formed on one side, and by installing drill drive units (220, 240) on both the upper and lower sides, a molding groove (111) and a lower molding groove (112) can be formed simultaneously on both the upper and lower sides.
[0154] By further installing a drive roller (225) in the direction in which the insulation material (110) is supplied from the above drill mounting stand (211) to support and guide the insulation material (110), it is guided to move along the direction of forming the molding groove (111) and the lower molding groove (112) while maintaining it accurately without lifting or shifting its position.
[0155] The dust generated as the molding groove (111) and lower molding groove (112) are processed in the insulation material (110) is collected inside the dust collection tank (310), and is discharged to the outside through the discharge duct (330) via the discharge pipe (320) installed at regular intervals on the upper side of the dust collection tank (310), thereby preventing dust from being generated in the groove molding device (200) and allowing it to be discharged to a desired location from the dust discharge device (300), thus improving the working environment.
[0156] The above-mentioned groove forming device (200) can further install a height adjustment device (230) on one or both sides of the outer side of the frame (210) to perform height adjustment of the dust collection tank (310) as needed, and the height (position) of the drill mounting stand (211) can be adjusted according to the height adjustment of the dust collection tank (310), thereby allowing the depth of the forming groove (111) and the lower forming groove (112) of the carbide blade (222) through the drill shaft (221) to be adjusted.
[0158] The present invention is described according to the illustrations in FIGS. 5 to 11. Insulating material (110), which is cut from semi-flammable expanded polystyrene to have a predetermined size and thickness in a cutting device, is processed to have molding grooves (111) at regular intervals on the upper side, and after processing the molding grooves (111), reinforcing material (120) is inserted and fixed.
[0159] One of the above reinforcing materials (120) includes installing GFRP that can improve rigidity after being molded by extrusion and injection using various synthetic resins and recycled materials.
[0160] The above reinforcing material (120) is an FRP structure that is suitable for pultrusion molding, which is formed by coating a PET polyol obtained by reacting a polyhydric acid and a polyhydric alcohol, an unsaturated basic acid and an acrylate monomer, and an epoxy resin modified acrylate resin at a high temperature with recycled PET and isophthalic acid, and then coating it with various materials such as resin and a low shrinkage agent. The structure has excellent corrosion resistance, a high molecular weight molecular structure and a high content of double bonds, fast curing reactivity, and high toughness. It is made of a polymer resin utilizing recycled PET, is eco-friendly, and has excellent material price competitiveness, allowing it to be widely used in the marine industry, civil engineering, and construction markets. The coated pultrusion molded FRP structure is made of FRP with excellent mechanical strength on the inside and a thermoplastic material with excellent corrosion resistance, weather resistance, and water resistance on the outside, thereby providing a pultrusion molded FRP structure that is strong against corrosion and corrosion caused by the environment and has strength of the structure.
[0161] The above reinforcing material (120) and lower reinforcing material (121) may be made of a wider variety of materials for increasing rigidity in addition to the GFRP described above, inserted from the outside and fixed integrally in the molding groove (111) and lower molding groove (112), and an adhesive may be used as needed.
[0163] In addition, as shown in FIGS. 12 and 13, the present invention includes forming a molding groove (111) on the upper side of an insulating material (110) and a lower molding groove (112) on the lower side, and inserting a reinforcing material (120) into the molding groove (111) and a lower reinforcing material (121) into the lower molding groove (112) so that reinforcement can be provided from both sides.
[0164] In this way, after inserting a reinforcing material (120) into the molding groove (111) of the insulation material (110) or inserting a lower reinforcing material (121) into the lower molding groove (112), an adhesive is supplied to the upper and lower sides of the insulation material (110) so as to be evenly distributed, and then the upper finishing material (130) and the lower finishing material (140) are joined together to complete a board panel (100) that is fixed as an integral unit.
[0165] The upper finishing material (130) and lower finishing material (140) are asbestos-free, eco-friendly, non-combustible finishing materials (CRC board) made of compressed coconut, which have the advantage of being resistant to moisture, fire, and humidity and having excellent durability. They also have excellent sound insulation and heat insulation / cooling functions, and at the same time have excellent temperature and humidity control and have an acoustic coefficient of 35.5 to 57.2 dB, so they have excellent air-transmitted sound blocking performance, have minimal changes in shrinkage and expansion, are suitable for humid areas, and have excellent insect resistance so there is no damage from pests.
[0167] Hereinafter, preferred embodiments are presented to aid in understanding the present invention; however, the following embodiments are merely illustrative of the invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and spirit of the invention, and that such variations and modifications fall within the scope of the appended claims.
[0169] [Example]
[0170] Example 1: Preparation of semi-flammable expanded polystyrene
[0171] 100 parts by weight of expanded polystyrene raw material were transferred to a mixer, and composition A of KSP-2000 of Table 1 was added and stirred, and composition B of KSP-2000 of Table 2 was added and stirred, with 55 parts by weight of composition A and composition B added and stirred in the range of 20 to 80 parts by weight of composition A : 20 to 80 parts by weight of composition B, 15 parts by weight of expanded graphite were added and stirred, and 55 parts by weight of composition C of SP-1000 of Table 3 were added and stirred, and then 110 parts by weight of MDI were added and stirred (stirred for 4 to 6 minutes at 100 to 300 rpm each). After being fed into a mold and undergoing a press process at 0.5 to 0.7 atmospheres, the mixture underwent a drying process at a temperature of 40 to 50°C in the mold and was cut after discharge.
[0173] Ingredients Content (weight%) Chlorinated paraffin 10 TCPP 50 Composite flame retardant (phosphate, halogenated hydrocarbon, and antimony oxide) 30 Inorganic flame retardant 10
[0175] Ingredients Content (weight%) alcohol 26 Inorganic transfer of pyrotechnics 15 Fly ash (SiO2Al2O3) 4 Quicklime (CaCO3) 2 Sodium silicate 15 magnesium hydroxide 2 Non-combustible agent (Ihx-999) 25 Non-combustible material-2 (DBPE) 11
[0177] Ingredients Content (weight%) Acetic acid 25 PET 3 PUR 30 PIR 22 EVA 10 Memory (Carbamate) 7 blowing agent 3
[0179] Comparative Example 1
[0180] The procedure was carried out in the same manner as Example 1, except that KSP-2000 and KS-1000 were prepared as a one-component type in the non-combustible material composition in Example 1, added, and stirred.
[0182] [Experimental Example]
[0183] The non-flammability of the non-flammable expanded polystyrene prepared according to Example 1 and Comparative Example 1 was measured and compared.
[0184] Experimental Example 1: Heat Release Rate Test
[0185] KS F ISO 5660-1 (Combustion Performance Test - Heat Release, Smoke Generation, Mass Loss Rate - Part 1: Measurement of Heat Release Rate (Cone Calorimeter Method) and Smoke Generation Rate (Dynamic Measurement)
[0187] (i) Maintain the radiant heat and exhaust flow rate of the cone heater of the cone calorimeter test apparatus at (50±1) kW / m² and (0.024±0.002) m³ / s, respectively.
[0188] (ii) Place the holder with the test specimen installed on the mass measuring device under the cone heater.
[0189] (iii) After removing the radiant heat shield, heat the test specimen for 10 minutes.
[0190] (iv) Measure the total heat released by the test specimen and the maximum heat release rate.
[0191] (v) After heating is finished, remove the specimen holder from the mass measuring device and observe for fire-hazardous cracks, holes, and melting penetrating the specimen.
[0192] The total heat released during the 10 min period after the start of the heating test must be 8 MJ / m² or less, and the maximum heat release rate during the 10 min period must not exceed 200 kW / m² continuously for 10 s or more.
[0193] After heating for 10 minutes, there should be no fire-hazardous cracks, holes, or melting penetrating the test specimen (including the core material in the case of composite materials).
[0195] The results of the emission rate experiment are shown in Table 4.
[0196] Test specimen No. Example 1 Comparative Example 1 Total heat released (MJ / ㎡) 5.7 8 200 KW / ㎡ excess time(s) 0 10 Ignition time (sin) 12.5 9 Presence of cracks, holes, and melting radish you Whether or not fire-hazardous factors occurred in the test specimen radish radish
[0198] As shown in Table 4, the total heat released during the 10 min after the start of the heating test is 5.7 MJ / m², which is 8 MJ / m² or less, according to the KS F ISO 5660-1 (cone calorimeter method) test results.
[0199] Example 1 describes the average value of the results obtained by examining three specimens.
[0200] The maximum heat release rate during 10 min is less than 10s, which is the judgment criterion.
[0201] In this regard, the present invention has confirmed that there are no cases where the temperature exceeds 200 kW / m², and that no fire-hazardous cracks, holes, or melting penetrate the test specimen after heating for 10 minutes occur.
[0202] In addition, in the embodiment of the present invention, it was found that there was no occurrence of fire-hazardous factors in the test specimen, as per the judgment criteria.
[0203] Example 1 describes the average value of the results obtained by examining three specimens.
[0205] Experimental Example 2: Gas Toxicity Test
[0206] KS F 2271 (Test Method for Gas Toxicity of Building Finishing Materials)
[0207] (i) Maintain the temperature inside the test box of the gas toxicity test device at 30℃.
[0208] (ii) Install eight rotating baskets, each containing one experimental white rat (ICR female, 5 weeks old, (20 ± 2) g), inside the test box.
[0209] (iii) After installing the test specimen in the furnace, heat it for 6 min (secondary heat source; LPG 0-6 min, primary heat source; electric heat 3-6 min).
[0210] (iv) Measure the time of cessation of activity of each experimental white rat for 15 minutes after the start of heating.
[0211] (v) Calculate the average value and standard deviation of the behavioral cessation time of 8 experimental white rats after the test ends.
[0212] (vi) The average behavioral cessation time (x) of experimental white rats is calculated using the following formula.
[0213]
[0214] x: Average time to behavior cessation of experimental white rats (unit - min : s)
[0215] X: Average value of behavior cessation time of 8 laboratory white rats (Unit - min : s)
[0216] σ: Standard deviation of behavior cessation time of 8 experimental white rats (unit - min : s)
[0218] According to the results of the gas toxicity test in Korean Industrial Standard KS F 2271, as shown in the ignition times in Figure 2 and Table 4, the time taken to collect the gas generated during the ignition time of 14 minutes 46 seconds and 10 minutes 28 seconds to determine the average time of cessation of activity of the test white rats was confirmed to be 9 minutes or more.
[0219] Therefore, it was confirmed that the building interior and exterior insulation material with semi-noncombustible performance according to the present invention satisfies semi-noncombustible performance.
[0221] It was confirmed that the expanded polystyrene of Example 1 has excellent non-flammability compared to conventional general styrofoam as well as the expanded polystyrene of Comparative Example 1.
[0222] As in Comparative Example 1, when KSP-2000 and KS-1000 are mixed together, the non-combustible agent undergoes a chemical reaction and hardens, which is disadvantageous to the performance of non-combustible properties and causes product defects. Therefore, KSP-2000 is separated into composition A and composition B and stirred, and expanded graphite (KSG) powder is supplied to composition B so that coating is performed normally, thereby preventing defects and satisfying semi-non-combustible performance through coating.
[0224] Example 2: Preparation of reinforcing material
[0225] Step 1: preparing a PET polyol by glycol-cisification of recycled PET and isophthalic acid at high temperature, preparing an isotype PET unsaturated polyester oligomer by reacting a polyhydric basic acid and a polyhydric alcohol, then diluting the unsaturated polyester oligomer with an acrylate monomer at low temperature and reacting the unsaturated polyester oligomer with an epoxy resin to prepare an epoxy resin-modified acrylate resin;
[0226] A second method for preparing a suitable compound by mixing a low-shrinkage agent, an interfacial adhesion and strength reinforcing agent, a filler, and a curing agent with an epoxy resin-modified acrylate resin prepared in the first step;
[0227] A third step of producing an FRP of a structure by impregnating the compound produced in the second step with a reinforcing material such as glass fiber, carbon fiber, aramid fiber, or basalt fiber, and then curing it at a high temperature using a mold in a pultrusion process;
[0228] The method comprises a fourth step of coating the pultrusion-molded FRP structure manufactured in the third step with a thermoplastic material such as polyester, nylon, PVC (polyvinyl chloride), polyethylene, polypropylene, CAB (cellulose acetate butyrate), or ABS (acrylonitrile butadiene styrene).
[0231] The above first step is a 1-1 step of producing PET-isophthalic acid polyol by manufacturing recycled PET, glycol, and isophthalic acid at a high temperature in the presence of a catalyst;
[0232] Step 1-2, which involves preparing the PET-isophthalic acid polyol prepared in Step 1-1, adding a polybasic acid and a polyglycol, and then reacting the PET-isotype unsaturated polyester oligomer prepared at high temperature with an acrylic monomer and maleic anhydride at low temperature to prepare an isotype unsaturated polyester monobasic acid;
[0233] Step 1-3, which involves mixing an epoxy resin and a catalyst with the isotype unsaturated polyester oligomer prepared in Step 1-2 and reacting the mixture at a low temperature to produce a PET-epoxy resin modified acrylate oligomer;
[0234] The method includes a first-4 step of manufacturing a PET-epoxy resin-modified acrylate resin by diluting the PET-epoxy resin-modified oligomer manufactured in the first-3 step with a reactive monomer and adjusting it to a resin specification suitable for pultrusion.
[0236] The above 1-1 step comprises preparing a PET-isophthalic acid polyol with reduced viscosity by adding 500 to 600 parts by weight of recycled PET, 100 to 200 parts by weight of neopentyl glycol (NPG), 100 to 200 parts by weight of diethylene glycol (DEG), 80 to 160 parts by weight of isophthalic acid, 1 to 2 parts by weight of a metal salt catalyst for PET depolymerization, and 0.1 to 0.3 parts by weight of a metal salt catalyst for the isophthalic acid reaction, mixing them by raising the temperature in a nitrogen atmosphere, reacting at 215 to 225°C to perform glycolysis, and additionally adding 4 to 6 parts by weight of propylene glycol (PG).
[0239] The unsaturated polyester oligomer acid of the above 1-2 steps is prepared by mixing 50-70 parts by weight of glycol, 340-390 parts by weight of PET-polyol, and 165-195 parts by weight of polyvalent basic acid and reacting them to produce an unsaturated polyester oligomer with an acid value of 40 or less, diluting it with 175-195 parts by weight of acrylate monomer and 210-230 parts by weight of maleic anhydride, adding 0.5-0.8 parts by weight of an amine-based catalyst and 0.10-0.3 parts by weight of a polymerization inhibitor, and reacting the mixture to produce an acid value of 150-200.
[0241] The above 1-3 steps are steps for preparing an epoxy resin-modified acrylate resin oligomer by reacting an epoxy resin with the PET-isophthalic acid unsaturated polyester base acid prepared in the 1-2 steps, and include preparing an epoxy resin-modified vinyl ester resin oligomer by adding 300-350 parts by weight of PET-isophthalic acid unsaturated polyester base acid, 200-300 parts by weight of epoxy resin, 0.5-0.9 parts by weight of catalyst, and 0.15-0.30 parts by weight of polymerization inhibitor and reacting them.
[0243] The above Step 1-4 is a step of preparing a vinyl ester resin by diluting the epoxy resin-modified acrylate resin oligomer prepared in Step 1-3 with a vinyl monomer. Specifically, it includes preparing a vinyl ester resin by adding 0.09 to 0.12 parts by weight of a room temperature stable polymerization retardant and 0.4 to 0.6 parts by weight of a triphenylantimony-based storage stabilizer to the epoxy resin-modified acrylate oligomer prepared in Step 1-3, and then diluting it with 380 to 430 parts by weight of a vinyl monomer.
[0245] The method includes manufacturing a PET-unsaturated polyester epoxy resin modified acrylate resin, which is a thermosetting resin for glass fiber pultrusion molding, using a PET-isophthalic acid unsaturated polyester oligomer having a resin viscosity of 400-800 cps, an acid value of 25 or less, a non-volatile content of 57-62%, a medium-temperature curing agent benzoperoxide (BPO) 1%, and a gel time of 8-15 minutes at 82°C, while undergoing the process of the first step above.
[0247] The above second step is a step of preparing a resin compound suitable for pultrusion by mixing additives such as a thermoplastic low-shrinkage agent, a curing agent, a strength reinforcing agent, and an antifoaming agent with the PET-epoxy resin-modified acrylate resin prepared in the first step suitable for lintel molding.
[0248] The method comprises preparing a compound mixed with 90 parts by weight of PET-epoxy resin modified acrylate resin and 10 parts by weight of a polyvinyl acetate-based low-shrinkage agent, 1 part by weight of a curing agent, 0.7 parts by weight of an additive for interfacial adhesion and strength reinforcement, 0.3 parts by weight of an antifoaming agent, 0.7 parts by weight of a viscosity reducing agent, 3 parts by weight of an internal release agent, and 40 parts by weight of a filler consisting of calcium carbonate, aluminum hydroxide, talc, alumina, or a mixture thereof.
[0249] The reinforcing material described above is made of GFRP that serves as a substitute for steel bars, and is molded using recycled raw materials.
[0251] Example 3; Manufacturing of a board panel
[0252] As described in Example 1, the step (S100) of molding semi-flammable expanded polystyrene is performed.
[0253] As described in Example 2, the step (S200) of forming the reinforcing material (120) is performed.
[0254] A step (S300) of cutting the insulation material (110) by cutting the semi-noncombustible expanded polystyrene that has been foamed and molded in a cutting device is performed.
[0255] A molding groove forming step (S400) is performed in which the cut insulation material (110) is supplied to a groove forming device (200) and a carbide blade (222) connected to a drill shaft (221) is rotated at high speed to form molding grooves (111) at regular intervals on the upper side of the insulation material (110).
[0256] The above drill shaft (221) is rotated from drill drive units (220, 240) installed at regular intervals on the drill mounting base (211), and the depth of the molding groove (111) can be freely adjusted, and only the molding groove (111) can be molded on the upper side, or the molding groove (111) can be molded while simultaneously forming the lower molding groove (112) on the lower side.
[0257] A dust discharge step (S500) is performed in which dust generated while processing the molding groove (111) or the lower molding groove (112) in the insulation material (110) is collected in a dust collection tank (310) and discharged to the outside through the discharge duct (330) via the discharge pipe (320).
[0258] A reinforcing material insertion step (S600) is performed in which a reinforcing material (120) is inserted and fixed into the molding groove (111) or lower molding groove (112) of the insulating material (110).
[0259] A bonding agent application step (S700) is performed, in which an adhesive is applied to the upper and lower sides of the insulation material (110) that has been fixed by inserting a reinforcing material (120).
[0260] A finishing material joining step (S800) is performed by supplying an upper finishing material (130) to the upper side and a lower finishing material (140) to the lower side of an insulating material (110) that has an adhesive applied to the upper and lower sides, so that they are joined to form an integrated structure.
[0261] The board completion step (S900) is performed by joining the finishing materials (130, 140) to complete the board panel (100).
[0263] Foregoing, specific parts of the present invention have been described in detail. It will be apparent to those skilled in the art that such specific descriptions are merely preferred embodiments and do not limit the scope of the invention. Accordingly, the actual scope of the invention is defined by the claims and their equivalents. Explanation of the symbols
[0265] 100: Board panel 110: Insulation material 111 : Molding groove 112 : Lower molding groove 120 : Reinforcement 121 : Lower reinforcement 130 : Upper finishing material 140 : Lower finishing material 200 : Home forming device 210 : Frame 211: Drill stand 212: Supply belt 213: Supply Guide Roller 220, 240: Drill Drive Unit 221 : Drill shaft 222 : Carbide blade 225 : Drive roller 230 : Height adjuster 300: Dust discharge device 310: Dust collection tank 320 : Exhaust pipe 330 : Exhaust duct
Claims
Claim 1 In a non-combustible board with reinforcing inserts comprising an insulating material (110), a reinforcing material (120) with a circular cross section, an upper finishing material (130), and a lower finishing material (140), the insulating material (110) is composed of semi-non-combustible expanded polystyrene formed by mixing a composition A containing chlorinated paraffin, chlorinated phosphate ester, a composite flame retardant, and an inorganic flame retardant in expanded polystyrene particles; a composition B containing a polyhydric alcohol, an inorganic phosphorus-based flame retardant, fly ash, quicklime, sodium silicate, magnesium hydroxide, a non-combustible agent, and a non-combustible agent-2; a composition C containing expanded graphite, acetic acid, polyethylene terephthalate, polyurethane, polyisocyanurate, ethylene-vinyl acetate copolymer, a carbamate compound, and a foaming agent; and diphenylmethane diisocyanate (MDI). A plurality of molding grooves (111) with a circular cross section are formed in the upper longitudinal direction of the insulating material (110). A reinforcing material insertion fireproof board characterized by fixing a reinforcing material (120) with a circular cross-section that improves rigidity in a molding groove (111), applying adhesive to the upper and lower sides of the insulating material (110), and joining the upper finishing material (130) and the lower finishing material (140). Claim 2 A non-combustible board with reinforcing material insert according to claim 1, characterized in that the composition A comprises 8-16% by weight of chlorinated paraffin, 20-60% by weight of chlorinated phosphate ester, 22-42% by weight of a composite flame retardant, and 8-16% by weight of an inorganic flame retardant, based on 100 parts by weight of expanded polystyrene particles. Claim 3 A non-combustible board with reinforcing material insert according to claim 2, wherein the above-mentioned composition B comprises 10-34% by weight of polyhydric alcohol, 6-16% by weight of inorganic phosphorus-based flame retardant, 1-6% by weight of fly ash, 0.54% by weight of quicklime, 618% by weight of sodium silicate, 0.5-4% by weight of magnesium hydroxide, 10-30% by weight of non-combustible agent, and 3-15% by weight of non-combustible agent-2, based on 100 parts by weight of expanded polystyrene particles. Claim 4 A non-combustible board with reinforcing material insert according to claim 3, wherein the above C composition comprises 20-30% by weight of acetic acid, 1-5% by weight of polyethylene terephthalate, 20-40% by weight of polyurethane, 15-30% by weight of polyisocyanurate, 7-15% by weight of ethylene-vinyl acetate copolymer, 3-12% by weight of carbamate compound, and 1-5% by weight of foaming agent, based on 100 parts by weight of expanded polystyrene particles. Claim 5 A non-combustible board with reinforcing material insert according to claim 4, characterized in that the diphenylmethane diisocyanate (MDI) comprises 100 to 120 parts by weight based on 100 parts by weight of expanded polystyrene particles. Claim 6 A non-combustible board with reinforcing material insertion, characterized in that, in any one of claims 1 to 5, the reinforcing material (120) inserted into the molding groove (111) formed on the upper side of the insulating material (100) is cut and inserted from GFRP. Claim 7 A method for manufacturing a non-combustible board of claim 1 by molding semi-non-combustible expanded polystyrene to produce an insulating material, and by inserting a circular reinforcing material and bonding a finishing material, comprising: ① a molding step (S100) of preparing an expanded polystyrene resin containing graphite and then injecting it into a mold under certain pressure and temperature conditions to perform foam molding; ② an insulating material cutting step (S300) of cutting the foamed polystyrene to form an insulating material (110); ③ a step of forming a circular molding groove with an open top (S400) of processing a plurality of molding grooves (111) at regular intervals on the upper side of the insulating material (110); ④ a reinforcing material insertion step (S600) of inserting and fixing a reinforcing material (120) with a circular cross-section into the processed molding grooves (111); and ⑤ a finishing material of bonding an upper finishing material (130) and a lower finishing material (140) by applying an adhesive to the upper and lower sides of the insulating material (110) into which the reinforcing material (120) is inserted. A method for manufacturing a non-combustible board with reinforcing material inserted, comprising a bonding step (S800); wherein the polystyrene foamed in the molding step (S100) is molded to satisfy semi-non-combustible performance with a total heat output of 600 MJ / m² or less according to KS F ISO 5660-1 standards. Claim 8 In claim 7, the molding groove molding step (S400) is configured such that a drill shaft (221) having a spherical end is rotated by a drill driving unit (220) installed at regular intervals on a drill mounting base (211), and the depth of the molding groove (111) can be freely adjusted, characterized in that a method for manufacturing a non-combustible board with a reinforcing material inserted therein. Claim 9 In claim 7, the molding groove forming step (S400) is configured such that a drill shaft (221) having a spherical end is rotated by a plurality of drill driving units (220, 240) installed at regular intervals on a drill mounting base (211), thereby allowing the depth of the molding groove (111) to be freely adjusted, and simultaneously forming the molding groove (111) and forming a lower molding groove (112) on the lower side of the insulation material (110). This describes a method for manufacturing a non-combustible board with a reinforcing material inserted.
Citation Information
Patent Citations
Method of producing reinforced EPS heat insulator, and reinforced EPS heat insulator and reinforcement-attached heat insulator panel using thereof
KR1020160117229A
A insulation composite panel for construction and the method for manufacturing the same
KR1020210097586A
Dust removal device with air paddle
KR102562603B1