Method for producing glass substrates and method for producing magnetic disks
Patent Information
- Application Number
- LAP756
- Authority / Receiving Office
- LA · LA
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-07-27
- Filing Date
- 2019-07-26
- Publication Date
- 2026-01-09
AI Technical Summary
Existing methods for manufacturing glass substrates for magnetic disks face challenges in achieving low surface roughness on both main and end surfaces, particularly with thin substrates, as they often result in unreliable separation due to re-fixation issues and increased likelihood of cracks during processing.
A method involving laser processing to form defects and separate glass substrates by thermally expanding the outer portion relative to the inner portion, creating a gap and ensuring reliable separation, while maintaining low surface roughness and preventing re-fixation of cracks, using techniques such as irradiating laser beams along concentric circles or annular shapes to form through holes and control heating to achieve precise separation.
This method enables the reliable separation and extraction of glass substrates with reduced surface roughness, preventing re-fixation of cracks and ensuring efficient production of thin glass substrates suitable for magnetic disks, thereby improving the manufacturing efficiency and quality of glass substrates for magnetic disks.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Method for manufacturing a glass substrate and a method for manufacturing a magnetic disk
[0001] This invention relates to a method for manufacturing a glass substrate and a magnetic disk, both of which involve shaping the glass substrate using laser light.
[0002] Today, hard disk drives are used for data storage in personal computers, notebook computers, DVD (Digital Versatile Disc) recording devices, and data centers for cloud computing. Hard disk drives use magnetic disks, which consist of a magnetic layer on a disc-shaped, non-magnetic glass substrate for magnetic disks. The magnetic disk is incorporated into a DFH (Disk Flying Height) type magnetic head, for example, with a levitation distance of about 5 nm.
[0003] In this type of DFH magnetic head, the short levitation distance means that the adhesion of fine particles to the main surface of the magnetic disk must be avoided. To suppress this adhesion of fine particles, it is desirable that the surface roughness of the glass substrate is small not only on the main surface but also on the edge surfaces.
[0004] To satisfy the requirements of such magnetic disks, a technique is known for efficiently manufacturing glass substrates with reduced surface roughness on the inner edge of the glass substrate for magnetic disks (Patent Document 1). Specifically, the focal line of a pulsed laser beam is directed to multiple positions within the substrate, and the beam is absorbed by the glass substrate at multiple positions to create through-hole defect lines on a predetermined first path. Furthermore, the glass substrate is heated along the first path to propagate cracks and separate the portion inside the first path from the glass substrate, and this inner portion is further heated and extracted from the glass substrate.
[0005] Japanese Patent Publication No. 2015-083320
[0006] However, with the above technology, while it was possible to heat the glass substrate along the first path to propagate cracks and separate the inner portion from the glass substrate relative to the first path, it was not possible to reliably extract this inner portion from the glass substrate by heating it. For example, when separating the inner portion from the glass substrate relative to the first path by heating the glass substrate along the first path to propagate cracks after forming a defect using a laser, it was found that the separation due to the crack may re-solidify due to heat, making reliable separation impossible. In this case, even if the inner portion is heated, the re-solidified portion cannot be separated. For this reason, it was difficult to efficiently manufacture glass substrates with reduced surface roughness on the inner edge face using laser light. Furthermore, in recent years, the thickness of glass substrates has decreased, making them more susceptible to cracking during processing including separation by laser irradiation and heating. In this respect as well, it is desirable to be able to reliably manufacture thin glass substrates.
[0007] Therefore, the present invention aims to provide a method for manufacturing a glass substrate that can reliably separate and extract a glass substrate of a predetermined shape from a glass sheet when shaping the glass sheet that will become the basis of the glass substrate using laser light in order to reduce the surface roughness of the edge face of the glass substrate, and a method for manufacturing a magnetic disk using this method.
[0008] One aspect of the present invention is a method for manufacturing a glass substrate having an opening. The manufacturing method comprises the steps of: forming an inner circular portion and an outer circular portion on the surface of a glass sheet that will be the basis of the glass substrate by irradiating it with laser light in substantially concentric circles; heating the outer portion of the outer circular portion to cause the outer portion of the glass sheet to expand relative to the inner portion of the outer circular portion, thereby forming a gap in the outer circular portion and separating the inner portion and the outer portion of the outer circular portion; and heating the outer portion of the inner circular portion to cause the outer portion of the glass sheet to expand relative to the inner circular portion, thereby forming a gap in the inner circular portion and separating the inner portion and the outer portion of the inner circular portion.
[0009] Another aspect of the present invention is a method for manufacturing a glass substrate. This manufacturing method comprises the steps of: irradiating the surface of a glass sheet that will become the glass substrate with laser light on a predetermined ring-shaped line to form a defect on the line; and separating the outer portion and the inner portion of the glass sheet by heating the outer portion of the glass sheet with the defect formed on it at a greater temperature than the inner portion at a boundary with the line.
[0010] The glass substrate has an annular shape with an opening, and in the step of forming the defect, the laser light is used to form the defect so that the shape of the outer edge of the annular shape is the predetermined shape, and in the step of separating the outer portion and the inner portion, it is preferable to perform a first heat treatment in which the first outer portion of the glass substrate, separated by the outer edge of the annular shape, is heated to a higher temperature than the first inner portion of the glass substrate, separated by the outer edge of the annular shape.
[0011] In the step of separating the outer portion and the inner portion, it is preferable that the first outer portion and the first inner portion are separated while leaving a margin of 0.1% to 5% of the outer diameter of the ring shape of the glass substrate.
[0012] In the step of forming the defect, the laser light is used to form the defect so that the shape of the inner edge of the ring shape having the opening is the predetermined shape. In the step of separating the outer portion and the inner portion, it is preferable to perform a second heating treatment in which the heating of the second outer portion of the glass substrate, separated by the inner edge of the ring shape having the opening, is higher than that of the second inner portion of the glass substrate, separated by the inner edge of the ring shape.
[0013] In the step of separating the portion that will become the glass substrate from the glass base plate, it is preferable to perform the second heat treatment after the first heat treatment.
[0014] Another aspect of the present invention is a method for manufacturing a glass substrate. The manufacturing method comprises the steps of: irradiating the surface of a glass sheet that will become the glass substrate with laser light on a predetermined ring-shaped line to form a defect on the line; and separating the outer portion and the inner portion of the glass sheet by heating the outer portion of the glass sheet with the defect formed on it at an outer portion and an inner portion
[0015] In the step of separating the outer portion and the inner portion, it is preferable to raise the temperature of the outer portion compared to the inner temperature, causing the outer portion to thermally expand relative to the inner portion, thereby forming a gap along the line and separating the outer portion and the inner portion.
[0016] The irradiation of the surface of the glass substrate with the laser light preferably includes, first, forming point-like through holes at a plurality of discrete points on the line with pulsed laser light, and then, with non-pulsed laser light, the irradiation position moving continuously along the line to connect the discrete points on the line. The non-pulsed laser light is, for example, non-pulsed CO 2 A laser is preferred.
[0017] Preferably, the heating includes heating the main surfaces on both sides of the glass substrate by radiant heat from heating sources provided on both sides of the main surface of the glass substrate.
[0018] The area ratio of the main surface area of the glass blank to the main surface area of the glass substrate is 101% to 160%, and in the step of separating the outer portion and the inner portion, it is preferable to remove one glass substrate from one glass blank.
[0019] The thickness of the glass substrate is preferably 0.6 mm or less.
[0020] Still another aspect of the present invention is a method for manufacturing a magnetic disk, further comprising a step of forming at least a magnetic layer on the glass substrate produced by the method for manufacturing the glass substrate to produce a magnetic disk.
[0021] According to the above-described method for manufacturing a glass substrate and the method for manufacturing a magnetic disk, a glass substrate having a predetermined shape can be reliably separated and extracted from a glass substrate blank.
[0022] It is a diagram for explaining heating of an outer portion in the method for manufacturing a glass substrate according to one embodiment. It is a diagram for explaining heating of an outer portion in the method for manufacturing a glass substrate according to another embodiment. (a) is a perspective view of an example of a glass substrate for a magnetic disk manufactured in one embodiment, and (b) is a diagram showing an example of a cross section of an outer end face of the glass substrate for a magnetic disk shown in FIG. 3(a). It is a diagram for explaining irradiation of a laser beam in the method for manufacturing a glass substrate according to one embodiment. It is a diagram for specifically explaining heating of a glass substrate blank in the method for manufacturing a glass substrate according to one embodiment. It is a diagram for explaining irradiation of a laser beam in the method for manufacturing a glass substrate according to one embodiment.
[0023] Hereinafter, the method for manufacturing a glass substrate and the method for manufacturing a magnetic disk will be described in detail. As the material of the glass substrate, aluminosilicate glass, soda lime glass, borosilicate glass, or the like can be used. In particular, amorphous aluminosilicate glass can be preferably used in that chemical strengthening can be performed as necessary, and a glass substrate for a magnetic disk excellent in the flatness of the main surface and the strength of the substrate can be produced.
[0024] (Schematic Explanation of Method for Manufacturing Glass Substrate) The method for manufacturing a glass substrate according to one embodiment includes: (A) a step of irradiating a laser beam onto a line forming a predetermined annular shape on the surface of a glass blank serving as the glass substrate to form a defect on the line; and (B) a step of separating an outer portion and an inner portion of the glass blank having the defect formed thereon by heating the outer portion to a higher temperature than the inner portion with the line as a boundary. Forming a defect includes making a hole in the glass blank or forming a crack that extends from the hole. The defect may be formed over the entire area of the line, that is, formed linearly, or may be formed discretely at spaced locations on the line. That is, in the method for manufacturing a glass substrate according to one embodiment, the outer portion and the inner portion of the glass blank are separated by heating the outer portion of the portion where the defect is formed along the line to a higher temperature than the heating of the inner portion with respect to the line. The hole formed by irradiating the laser beam is preferably a through-hole that penetrates the glass blank (in the thickness direction of the glass blank) by ablation. By forming the through-hole, the outer portion and the inner portion of the glass blank can be easily separated when the outer portion of the glass blank is heated. The through-hole extends substantially perpendicular (at an angle of 85 to 95 degrees) to the main surface of the glass blank. Therefore, the separation surface of the separated outer portion and inner portion is a wall surface substantially perpendicular to the main surface of the glass blank, different from a wall surface inclined with respect to the main surface such as a cross-sectional surface formed using a conventional scriber.
[0025] Figure 1 illustrates the heating of the outer portion in a manufacturing method for a glass substrate according to one embodiment. The glass plate 20 is a glass plate that is substantially circular or substantially elliptical in shape and has a certain thickness. A defect is formed on the surface of the glass plate 20 by irradiating it with laser light along a ring-shaped line 22. Furthermore, the glass plate 20 is heated in order to extract the portion that will become the glass substrate from the glass plate 20 on which the defect has been formed. At this time, the heating of the outer portion 24 is made higher than that of the inner portion 26, so that the amount of thermal expansion of the outer portion 24 is greater than that of the inner portion 26. As a result, the outer portion 24 expands outward due to thermal expansion as shown in Figure 1. Therefore, a gap can be reliably formed at the interface between the outer portion 24 and the inner portion 26. Thus, the separation of the outer portion 24 and the inner portion 26 can be reliably achieved. Specifically, because the outer portion 24 is heated to a higher degree than the inner portion 26, the inner diameter of the outer portion 24 expands relatively larger than the outer diameter of the inner portion 26 due to thermal expansion, forming a gap. Therefore, the formed gap allows for reliable separation of the outer portion 24 and the inner portion 26. Note that heating the outer portion 24 to a higher degree than heating the inner portion 26 includes not only cases where the outer portion 24 and the inner portion 26 are heated to different degrees, but also cases where the outer portion 24 is selectively heated, but the inner portion 26 is not heated as intended. Even if the outer portion 24 is selectively heated, the inner portion 26 is also heated indirectly by heat conduction through the space or through the glass plate 20. In this case, it can be said that the heating of the outer portion 24 is higher than that of the inner portion 26. In this specification, the "gap" between the inner and outer parts described refers not only to the formation of a measurable space at any point between the inner and outer parts, but also to the absence of physical or chemical bonding between opposing surfaces of the inner and outer parts, even if a measurable space is not available. In other words, the "gap" also includes the formation of a microscopic space at least in part of the boundary between the inner and outer parts.
[0026] When the inner portion 26 is heated instead of the outer portion 24, the thermal expansion of the inner portion 26 is greater than that of the outer portion 24. As a result, the inner portion 26 pushes the interface between the inner portion 26 and the outer portion 24 outward, propagating the cracks formed by the laser irradiation and generating new cracks at the interface. However, since these cracks are pushed outward from the inner portion 26, it is difficult to create a gap at the interface between the inner portion 26 and the outer portion 24. Therefore, the heat from the heated inner portion 26 can be transferred to the interface, re-fixing the formed cracks and preventing reliable separation. In this embodiment, by increasing the heating of the outer portion 24 relative to the wire 22 compared to the heating of the inner portion 26, a gap can be reliably formed, preventing the separation caused by cracks formed using the laser from being re-fixed by heat.
[0027] Another embodiment is a method for manufacturing a glass substrate having an opening. This method for manufacturing a glass substrate comprises: (C) forming an inner circular portion and an outer circular portion on the surface of a glass sheet that will become the glass substrate by irradiating it with laser light in a substantially concentric manner; (D) heating the outer portion of the outer circular portion to cause the outer portion of the outer circular portion of the glass sheet to expand relatively with respect to the inner portion of the outer circular portion, thereby forming a gap in the outer circular portion and separating the inner portion and the outer portion of the outer circular portion; and (E) heating the outer portion of the inner circular portion to cause the outer portion of the inner circular portion of the glass sheet to expand relatively with respect to the outer portion of the inner circular portion, thereby forming a gap in the inner circular portion and separating the inner portion and the outer portion of the inner circular portion.
[0028] Another embodiment is a method for manufacturing a glass substrate having an opening. This method for manufacturing a glass substrate includes: (F) irradiating the surface of a glass sheet that will become the glass substrate with laser light on a predetermined ring-shaped line to form a defect on the line; and (G) separating the outer and inner parts of the glass sheet by heating the outer part of the glass sheet with the defect formed on it at a boundary with the line, wherein the outer part is heated at a higher temperature than the inner part, and the outer part of the glass sheet is heated at a higher temperature than the inner part, thereby separating the outer and inner parts of the glass sheet and removing the inner part as an opening.
[0029] Figure 2 illustrates the heating of the outer portion in a manufacturing method for a glass substrate according to one embodiment. Figure 2 illustrates the process of forming an inner circular portion as described in (C) above on the surface of a circular glass substrate 30, or forming a defect on a predetermined ring-shaped line as described in (F) above by irradiating it with laser light, and then separating it by heating as described in (E) or (G). The glass substrate 30 is a plate obtained by forming an outer circular portion on the surface of the glass substrate as described in (C) above, and then separating and removing the inner portion and the outer portion of the outer circular portion by performing the steps described in (D) above. In the embodiment shown in Figure 1, the inner circular portion and the outer circular portion refer to the defective portion formed on the line 22. Therefore, the shape of the outer circular portion described in (D) above corresponds to the outer shape of the glass substrate 30 shown in Figure 2. By heating the outer portion 34 of the inner circumferential portion 32 formed by laser irradiation, the outer portion 34 of the inner circumferential portion 32 of the glass substrate 30 undergoes relative thermal expansion, creating a gap in the inner circumferential portion 32 and separating the inner portion 36 from the outer portion 34. In (G) above, the separated inner portion 36 is removed. As in (G) above, by simultaneously heating the outer portion 34 from both sides of the main surface of the glass substrate 30, the amount of thermal expansion of the outer portion of the inner circumferential portion 32, which is smaller than the amount of thermal expansion of the outer portion of the outer circumferential portion during heating as described in (D) above, can be made substantially uniform in the thickness direction of the glass substrate 30, and a uniform gap can be formed in the thickness direction. As a result, even if the gap is small, the inner portion 36 can be extracted from the outer portion 34. The inner circumferential portion 32 corresponds to a defect formed along the line 22 in the embodiment shown in Figure 1.
[0030] In the embodiments having steps (C) to (E) above, as well as in the embodiments having steps (F) and (G) above, heating the outer portion causes the outer portion of the outer or inner circumference to expand thermally relative to the inner portion, forming a gap between the outer and inner circumferences. This prevents the interface formed by cracks created using a laser from re-solidifying due to heat. As a result, a glass substrate with openings can be efficiently formed. The above-mentioned "approximately concentric circles" means that the difference between the center position of the outer circumference and the center position of the inner circumference is 20 μm or less, and preferably 5 μm or less.
[0031] (Specific description of the manufacturing method of the glass substrate) The manufacturing method of the glass substrate and the manufacturing method of the magnetic disk according to one embodiment will be described in detail below. Figure 3(a) is a perspective view of an example of a glass substrate for a magnetic disk manufactured according to one embodiment. Figure 3(b) is a diagram showing an example of a cross-section of the outer end face of the glass substrate for a magnetic disk shown in Figure 3(a).
[0032] The glass substrate 1 shown in Figure 3(a) is a glass substrate for magnetic disks. The glass substrate 1 is a thin, annular glass substrate. The size of the glass substrate for magnetic disks is not specified, but a typical glass substrate for magnetic disks is, for example, a nominal diameter of 2.5 inches or 3.5 inches. For a glass substrate for magnetic disks with a nominal diameter of 2.5 inches, for example, the outer diameter is 65 mm, the diameter of the center hole is 20 mm to 25 mm, and the thickness is 0.3 to 0.8 mm. For a glass substrate for magnetic disks with a nominal diameter of 3.5 inches, for example, the outer diameter is 95 mm, the diameter of the center hole is 20 mm to 25 mm, and the thickness is 0.3 to 0.8 mm. A magnetic layer is formed on the main surface of this glass substrate 1 to create a magnetic disk.
[0033] The glass substrate 1 comprises a pair of main surfaces 11p and 12p, a side wall surface 11w formed on the outer peripheral end face, chamfered surfaces 11c and 12c interposed between the side wall surface 11w and the main surfaces 11p and 12p, a side wall surface (not shown) formed on the inner peripheral end face in the same manner as the outer peripheral end face, and a chamfered surface (not shown) interposed between this side wall surface and the main surfaces 11p and 12p. The glass substrate 1 has a circular hole in its center. The side wall surface 11w includes the center position in the thickness direction of the glass substrate 1. The inclination angle of the chamfered surfaces 11c and 12c with respect to the main surfaces 11p and 12p is not particularly limited, and is, for example, 45°. Furthermore, the boundary between the side wall surface 11w and the chamfered surfaces 11c and 12c is not limited to a shape having an edge as shown, but may be a smoothly continuous curved surface.
[0034] As shown in Figure 1 or Figure 2, such a glass substrate 1 is extracted from pre-fabricated glass blanks 20 and 30 using laser light. Figure 4 is a diagram illustrating the irradiation of laser light in a glass substrate manufacturing method according to one embodiment.
[0035] The glass substrate 60 irradiated by the laser beam L shown in Figure 4 is, for example, a glass plate of a certain thickness manufactured using the floating method or the down-draw method. Alternatively, it may be a glass plate formed by press-molding a block of glass using a mold. The thickness of the glass substrate 60 is thicker than the target thickness when it becomes the final product, a glass substrate for a magnetic disk, by the amount of material removed by grinding and polishing, for example, by several micrometers.
[0036] The laser light source 40 is a device that emits laser light L, and for example, a solid-state laser such as a YAG laser or an ND:YAG laser is used. Therefore, according to one embodiment, the wavelength of the laser light is preferably in the range of 1030 nm to 1070 nm. The laser light L is a pulsed laser, and in one embodiment, the pulse width of the laser light L is 10 -12A pulse duration of less than 1 picosecond is preferable because it can suppress excessive deterioration of the glass at the focal point of the laser beam L. Furthermore, the optical energy of the laser beam L can be appropriately adjusted according to the pulse width and the repetition frequency of the pulse width. Providing excessive optical energy relative to the pulse width and repetition frequency makes the glass more susceptible to excessive deterioration, and residue is more likely to be present at the focal point.
[0037] In one embodiment, the laser light source 40 divides the emitted laser light into two beams, and irradiates the glass substrate 60 with the laser light L tilted with respect to the direction normal to the main surface of the glass substrate 60 so that these two beams intersect on the surface of the glass substrate 60 or inside the glass substrate 60. By irradiating with the laser light L in this way, the intersection of the beams is formed continuously along the thickness direction at a point on the line 62 of the glass substrate 60, so that at this point, the light energy is concentrated linearly along the depth direction, and a part of the glass substrate 60 is plasma-generated, forming a hole or through hole. In one embodiment, it is preferable to irradiate the glass substrate 60 with the laser light L in a burst pulse method, in which multiple groups of light pulses are intermittently generated, with each group of light pulses being configured to continuously generate pulsed light pulses at regular time intervals. In this case, it is also preferable to make the light energy of one pulse within one group of light pulses variable. An example of such irradiation with laser light L is disclosed in Japanese Patent Publication No. 5959597.
[0038] In the irradiation of the laser light source 40 with laser light L, the laser light L is moved relative to the glass substrate 60 and irradiated onto a predetermined ring-shaped line. This forms a defect on the line. For example, an inner or outer circular portion can be formed on the glass substrate 60. In the irradiation of the laser light L, the laser light L may be moved without moving the glass substrate 60, or the glass substrate 60 may be moved without moving the laser light L.
[0039] When holes are intermittently formed at discrete positions along line 62 by irradiation with laser light L, for example, cracks are easily formed that propagate from these holes toward adjacent holes. Therefore, the outer and inner parts can be easily separated by heating the outer part of the inner or outer circular portion without having to irradiate the line again with a different type of laser light. In other words, the outer and inner parts can be easily separated by heating the outer part of the glass substrate 60 while maintaining the defects formed by irradiation with laser light L. In particular, the outer and inner parts can be separated more easily by heating the outer part from both sides of the main surface of the glass substrate 60 simultaneously.
[0040] Next, the outer and inner portions of the glass substrate 60 are separated by heating the outer portion more intensely than the inner portion, or by heating the outer portion, with respect to the line separating the outer and inner portions of the glass substrate 60. Figure 5 is a diagram illustrating the heating of the glass substrate 60 in a manufacturing method of a glass substrate according to one embodiment. When heating the glass substrate 60, for example, the outer portion 64 is placed in the heating space between heaters 50 and 52 with respect to the line 62 on which the defect is formed in the glass substrate 60, and the inner portion 66 is placed outside the heating space. This allows the outer portion 64 to be heated. At this time, the degree of heating of the outer portion 64 is higher than that of the inner portion 66, so the amount of thermal expansion of the outer portion 64 can be made greater than the amount of thermal expansion of the inner portion 66. As a result, the outer portion 64 expands outward as shown in Figure 5. Therefore, a gap can be reliably formed at the interface between the outer portion 64 and the inner portion 66. Thus, the separation of the outer portion 64 and the inner portion 66 can be reliably achieved.
[0041] In the example shown in Figures 4 and 5, the laser beam L is irradiated along a ring-shaped line to form a defect, and then the outer portion 64 of the line is heated. However, as shown in Figure 6, the laser beam L can also be irradiated onto the glass substrate 60 along two different substantially concentric circular arcs to form two defect portions, the outer circular portion 62a and the inner circular portion 62b, and then the outer portion of the outer circular portion 62a and the outer portion of the inner circular portion 62b are heated. Figure 6 is a diagram illustrating the irradiation of laser beam in a manufacturing method of a glass substrate according to one embodiment.
[0042] In this way, when separating the outer portion 64 and the inner portion 66, the temperature of the outer portion 64 is made higher than that of the inner portion 66, causing the outer portion 64 to expand relatively with respect to the inner portion 64, thereby forming a gap along the line 62 and separating the outer portion 64 and the inner portion 66. This ensures that the portion that will become the glass substrate is reliably extracted from the glass sheet. In particular, after forming the inner circumferential portion 62b, by simultaneously heating the outer portion of the inner circumferential portion 62b from both sides of the main surface of the glass sheet 60, the amount of thermal expansion can be made uniform along the thickness direction of the glass sheet 60, thus forming a uniform gap. In particular, since the inner circumferential portion 62b is close to the center of the glass sheet 60, even if heated to the same extent as the outer portion of the outer circumferential portion 62a, the amount of thermal expansion is smaller than that of the outer circumferential portion 62a. For this reason, it is preferable to accurately form a gap for reliably extracting the portion that will become the glass substrate from the glass sheet. From this perspective, it is preferable to heat the outer portion of the inner circumferential part 62b simultaneously from both sides of the main surface of the glass plate 60 to equalize the amount of thermal expansion in the thickness direction.
[0043] Furthermore, the glass substrate 1 has an annular shape with an opening. When manufacturing such a glass substrate 1, it is preferable to form a defect by irradiating the outer edge of the annular shape with an opening with a line 62 (see Figure 4) using laser light L, and then perform a first heat treatment in which the outer portion 64 (first outer portion) is heated at a higher temperature than the inner portion 66 (first inner portion). The surface roughness of the outer peripheral end face that constitutes the outer edge of the glass substrate 1 formed by the laser light L is smaller than that of the outer peripheral end face that is mechanically cut using a conventional scriber, and satisfies the surface roughness required for the outer cross-section required for, for example, a glass substrate for a magnetic disk in a hard disk drive device, so there is no need to polish the end face, or if polishing is required, the polishing time is short. For this reason, the outer edge shape of the glass substrate 1 can be formed efficiently. In this case, it is preferable that the glass substrate 60 is separated into an outer portion 64 (first outer portion) and an inner portion 66 (first inner portion) with a margin of 0.1% to 5% of the outer diameter of the ring shape remaining relative to the ring shape of the glass substrate 1. If the margin is large, the amount of glass substrate 60 to be discarded increases, resulting in waste. In addition, the heat during heating is more easily diffused by thermal conduction, so the heating time required to cause a predetermined amount of thermal expansion becomes longer, which is undesirable in terms of productivity.
[0044] When forming an opening (internal hole) in the glass substrate 1, it is preferable to form a defect by irradiating the ring-shaped inner edge having the opening with laser light L, using the shape of line 62, and then performing a second heat treatment in which the outer portion 64 (second outer portion) is heated at a higher temperature than the inner portion 66 (second inner portion). The surface roughness of the inner circumferential end face constituting the inner edge of the glass substrate 1 formed by laser light L is smaller than that of the outer circumferential end face mechanically cut using a conventional scriber, and satisfies the surface roughness required for the inner cross-section of a glass substrate for magnetic disks that come into contact with the rotating shaft in a hard disk drive, for example. Therefore, there is no need to polish the end face, or if polishing is required, the polishing time is short. For this reason, an opening in the glass substrate 1 can be formed efficiently.
[0045] In this case, it is preferable to perform the second heat treatment after the first heat treatment. The inner portion 66 during the first heat treatment becomes the outer portion 64 during the second heat treatment. In the first heat treatment, the inner portion 66 is not heated, or if it is heated, the degree of heating is lower than that of the outer portion 64. However, the inner portion 66 is heated by heat conduction from the heated outer portion 64. Therefore, when heating the heated inner portion 66 as the outer portion 64 in the second heat treatment, the heating time required to induce a predetermined amount of thermal expansion can be shortened. In this way, the glass substrate 1 can be manufactured efficiently.
[0046] The irradiation of the glass substrate 60 with laser light L may include, after forming point-like through-holes at multiple discrete points along a line with pulsed laser light, continuously moving the irradiation position along the line to connect the discrete points along the line with a different type of laser light. In this case, among the multiple through-holes formed with pulsed laser light, cracks or potential cracks can be formed between adjacent through-holes, and then the cracks or manifested cracks can be connected between the through-holes with a different type of laser light, so that the shape of the glass substrate can be processed efficiently in a short time. For example, as the different type of laser light, CO 2 A laser can be used. This laser light can be used to form linear defects that connect intermittently formed defects. That is, after intermittently forming defects at discrete positions of line 62 by irradiation with laser light L, a different type of laser light, CO, can be used. 2 Using a laser, it is also possible to reliably form cracks by creating linear defects that connect intermittently formed defects. This ensures reliable separation of the outer and inner parts by heating, as described later.
[0047] Furthermore, the heating of the glass substrate 60 after irradiation with laser light L preferably includes heating the main surfaces of the glass substrate 60 on both sides by radiant heat from heating sources provided on both sides of the main surface of the glass substrate 60. With radiant heating, heat is transferred from the main surface of the glass substrate 60 by thermal conduction, causing the glass substrate 60 to rise in temperature, so the interface between the outer portion 64 and the inner portion 66 does not reach a temperature high enough to re-bond. Therefore, a gap can be formed at the interface by thermal expansion of the outer portion 64.
[0048] The area ratio of the main surface area of the glass sheet 60 to the main surface area of the glass substrate 1 is 101% to 160%, and when separating the outer portion 64 and the inner portion 66, it is preferable to extract one glass substrate 1 from one glass sheet 60. If multiple glass substrates 1 are extracted from a large glass sheet 60, the variation in thickness of the glass sheet 60 from place to place will result in large differences in the thickness of the glass substrates 1 between individual sheets. In particular, for glass substrates for magnetic disks, it is preferable to have a uniform thickness, which makes it complicated to adjust the degree of grinding and polishing of the main surface of the glass substrates between glass substrates. Furthermore, it is possible to irradiate the glass sheet 60 with laser light with high precision while rotating the glass sheet 60, and the handling of the glass sheet 60 for separating the outer portion from the inner portion by heating the outer portion is improved. Thus, using a small-sized glass sheet 60 that ensures a uniform thickness and extracting one inner portion from one glass sheet 60 is preferable from the viewpoint of the efficiency of glass substrate 1 production. Furthermore, when removing one glass plate from a large glass substrate 60, the entire outer portion of the large glass substrate 60 is heated, and when removing the glass plate from this heated portion, the temperature of both the outer and inner portions remains high. Therefore, the temperature required to heat the outer portion to achieve a predetermined amount of thermal expansion becomes high, which is undesirable.
[0049] In one embodiment, the thickness of the glass substrate 60 is 0.6 mm or less. A glass substrate 1 made from a glass substrate 60 of such thickness can be effectively used as a glass substrate for magnetic disks. By reducing the thickness of the glass substrate for magnetic disks, the number of magnetic disks installed in the hard disk drive can be increased to increase storage capacity. Furthermore, a glass substrate 60 with a thickness of 0.6 mm or less is extremely thin and prone to cracking during the process of separating the outer and inner parts by laser irradiation and heating. Therefore, the effect of this embodiment, which allows for reliable separation and removal of the glass substrate from the glass substrate, becomes even greater with thin glass substrates.
[0050] The glass substrates, shaped in this manner, undergo various treatments to acquire properties suitable for the final product.
[0051] In this way, chamfering is performed on the corners formed between the outer and inner periphery ends (end faces which are the interface between the outer portion 64 and the inner portion 66) of the glass substrate extracted from the glass blank 60 and the main surface. According to one embodiment, the corners are chamfered with a laser beam of a different type than the laser beam L. This laser beam is irradiated onto the corners from a direction with an inclination angle of 30 to 60 degrees relative to the main surface, and the corners can be chamfered by heating, softening, and evaporating them. For example, CO 2 A laser can be suitably used. This type of chamfering can form a chamfered surface with low surface roughness and high roundness. Thus, the corners formed by the inner or outer edge surface and the main surface can be chamfered using laser light. Since the corners are chamfered with laser light, production efficiency is higher compared to when chamfering is done with a grinding wheel or the like. Production efficiency is improved because edge polishing is not performed from the process of extracting a glass substrate of a predetermined shape from the glass blank 60 to the chamfering of the corners of the glass substrate.
[0052] The obtained glass substrate 1 is subjected to grinding and polishing of its main surface. In the grinding and polishing process, the glass substrate 1 is ground and then polished. In the grinding process, a double-sided grinding device equipped with a planetary gear mechanism is used to grind the main surface of the glass substrate 1. Specifically, the outer peripheral end face of the glass substrate 1 is held in a holding hole provided in the holding member of the double-sided grinding device, and the main surfaces on both sides of the glass substrate 1 are ground. The double-sided grinding device has a pair of upper and lower grinding plates (upper plate and lower plate), and the glass substrate 1 is sandwiched between the upper and lower plates. Then, by moving either the upper plate or the lower plate, or both, and supplying coolant, the glass substrate 1 and each plate move relative to each other, both main surfaces of the glass substrate 1 can be ground. For example, a grinding member formed by fixing abrasive grains of diamond fixed in resin into a sheet shape can be attached to the grinding plate and the grinding process can be performed.
[0053] Next, the main surface of the glass substrate 1 after grinding is subjected to a first polishing process. Specifically, the outer edge of the glass substrate 1 is held in a holding hole provided in the polishing carrier of the double-sided polishing device, while the main surfaces on both sides of the glass substrate are polished. The purpose of the first polishing is to remove scratches and distortions remaining on the main surface after grinding, or to adjust minute surface irregularities (microwaveness, roughness).
[0054] In the first polishing process, the glass substrate 1 is polished using a double-sided polishing apparatus, which has the same configuration as the double-sided grinding apparatus used in the above-mentioned grinding process using fixed abrasive grains, while applying polishing slurry. In the first polishing process, polishing slurry containing free abrasive grains is used. As free abrasive grains used in the first polishing, for example, cerium oxide or zirconia abrasive grains are used. In the double-sided polishing apparatus, as in the double-sided grinding apparatus, the glass substrate 1 is sandwiched between a pair of upper and lower platens. Flat polishing pads (for example, resin polishers) that are annular in shape overall are attached to the upper surface of the lower platen and the bottom surface of the upper platen. Then, by moving either the upper platen or the lower platen, or both, the glass substrate 1 is moved relative to each platen, thereby polishing both main surfaces of the glass substrate 1. The size of the polishing abrasive grains is preferably in the range of 0.5 to 3 μm in average particle size (D50).
[0055] After the first polishing, the glass substrate 1 may be chemically strengthened. In this case, a mixed molten solution of potassium nitrate and sodium sulfate is used as the chemical strengthening solution, and the glass substrate 1 is immersed in the chemical strengthening solution. This allows a compressive stress layer to be formed on the surface of the glass substrate 1 by ion exchange.
[0056] Next, the glass substrate 1 is subjected to a second polishing process. The purpose of the second polishing process is to achieve a mirror finish on the main surface. In the second polishing process, a double-sided polishing apparatus having the same configuration as the double-sided polishing apparatus used in the first polishing process is used. Specifically, the outer peripheral end face of the glass substrate 1 is held in a holding hole provided in the polishing carrier of the double-sided polishing apparatus, while the main surfaces on both sides of the glass substrate 1 are polished. In the second polishing process, the type and particle size of the free abrasive particles and the hardness of the resin polisher differ from those in the first polishing process. It is preferable that the hardness of the resin polisher is lower than that of the first polishing process. For example, a polishing solution containing colloidal silica as free abrasive particles is supplied between the polishing pad of the double-sided polishing apparatus and the main surface of the glass substrate 1, and the main surface of the glass substrate 1 is polished. It is preferable that the size of the polishing abrasive particles used in the second polishing process is in the range of 5 to 50 nm in average particle size (d50). Whether or not chemical strengthening treatment is necessary should be appropriately selected considering the glass composition and its necessity. In addition to the first and second polishing processes, further polishing processes may be added, or the polishing of the two main surfaces may be completed with a single polishing process. The order of the above processes may also be changed as appropriate. In this way, the main surface of the glass substrate 1 is polished to obtain a glass substrate for magnetic disks that satisfies the conditions required for a glass substrate for magnetic disks. After this, at least a magnetic layer is formed on the glass substrate 1 prepared by polishing the main surface to produce a magnetic disk.
[0057] Note that before performing the first polishing, the end face of the glass substrate 1 may be polished by an end face polishing process, for example, after the first grinding, before the first polishing, or before the first grinding. Even when such an end face polishing process is performed, the arithmetic mean roughness Ra of the end face of the glass substrate 1 extracted from the glass blank 60 using laser light is less than 0.01 μm, and the roundness is 15 μm or less, so the time required for the end face polishing process is short. The end face polishing process may use a polishing brush method in which a polishing brush is used for polishing while supplying free abrasive grains to the end face, or a polishing method using a magnetic functional fluid. The polishing method using a magnetic functional fluid is, for example, a method in which a slurry containing abrasive grains in a magnetorheological fluid is formed into a mass by a magnetic field, the end face of the glass substrate 1 is inserted into the mass, and the mass and the glass substrate are rotated relative to each other to polish the end face.
[0058] However, in order to improve production efficiency, it is preferable not to perform the end face polishing process. In this case, in the grinding and polishing process of the main surface, while maintaining the roundness of the glass substrate 1 extracted from the glass blank 60 and further maintaining the surface roughness of at least a part of the cut surface, the main surface of the glass substrate 1 is ground or polished.
[0059] Regarding the composition of such a glass substrate 1, although it is not limited, the following composition is preferable. Specifically, in terms of oxide standard and expressed in mol%, SiO 2 is 50 to 75%, Al 2 O 3 is 1 to 15%, at least one component selected from Li 2 O, Na 2 O and K 2 O is 5 to 35% in total, at least one component selected from MgO, CaO, SrO, BaO and ZnO is 0 to 20% in total, and ZrO 2 , TiO 2 , La 2 O 3 , Y 2 O 3 , Ta 2 O 5 , Nb 2 O 5 and HfO 2This is an amorphous aluminosilicate glass having a composition containing at least one component selected from the above in a total amount of 0-10%.
[0060] Furthermore, the glass substrate 1 is preferably, for example, SiO2 expressed in mass %. 2 57-75%, Al 2 O 3 5-20%, (however, SiO 2 and Al 2 O 3 The total amount is 74% or more), ZrO 2 , HfO 2 , Nb 2 O 5 Ta 2 O 5 La 2 O 3 , Y 2 O 3 and TiO 2 If the total exceeds 0% and is 6% or less, Li 2 O is more than 1% and 9% or less, Na 2 O is 5-28% (however, by mass ratio Li 2 O / Na 2 O is 0.5 or less), K 2 It may also be an amorphous aluminosilicate glass having a composition of 0-6% O, 0-4% MgO, more than 0% but 5% or less CaO (provided that the total amount of MgO and CaO is 5% or less, and the CaO content is greater than the MgO content), and 0-3% SrO + BaO.
[0061] The composition of glass substrate 1 is, as an essential component, SiO 2 Li 2 O, Na 2 The glass substrate 1 contains 0 and one or more alkaline earth metal oxides selected from the group consisting of MgO, CaO, SrO, and BaO, and the molar ratio of the content of CaO to the total content of MgO, CaO, SrO, and BaO (CaO / (MgO + CaO + SrO + BaO)) is 0.20 or less, and the glass transition temperature may be 650°C or higher. A glass substrate 1 with such a composition is suitable for use as a glass substrate for magnetic disks used in energy-assisted magnetic recording disks.
[0062] Although the methods for manufacturing a glass substrate and a magnetic disk of the present invention have been described in detail above, the methods for manufacturing a glass substrate and a magnetic disk of the present invention are not limited to the above embodiments, and various improvements and modifications may be made without departing from the spirit of the present invention.
[0063] 1. Glass substrate 11p, 12p Main surface 11c, 12c Chamfered surface 11w Side wall surface 20, 30, 60 Glass plate 22, 62 Line 24, 34, 64 Outer part 26, 36, 66 Inner part 32, 62b Inner circumference 40 Laser light source 50, 52 Heater 62a Outer circumference
Claims
1. A method for manufacturing a glass substrate having an opening, comprising: a step of irradiating a surface of a raw glass plate that is the basis for the glass substrate with laser light in a substantially concentric pattern to form an inner circular portion and an outer circular portion; a step of heating the outer portion of the outer circular portion to thermally expand the outer portion of the outer circular portion of the glass plate relative to the inner portion of the outer circular portion, thereby forming a gap in the outer circular portion and separating the inner portion of the outer circular portion from the outer portion of the outer circular portion; and a step of heating the outer portion of the inner circular portion to thermally expand the outer portion of the inner circular portion of the glass plate relative to the inner portion of the inner circular portion, thereby forming a gap in the inner circular portion and separating the inner portion of the inner circular portion from the outer portion of the inner circular portion.
2. A method for manufacturing a glass substrate, comprising the steps of: irradiating a laser beam along a line forming a predetermined ring shape on the surface of a raw glass plate that is the base of the glass substrate, thereby forming a defect along the line; and separating the outer and inner parts of the raw glass plate, with the defect formed in the outer part separated by the line, by heating the outer part more than the inner part.
3. The method for manufacturing a glass substrate according to claim 2, wherein the glass substrate has an annular shape with an opening, the defect forming step uses the laser light to form the defect with an outer edge of the annular shape as the annular shape, and the step of separating the outer portion and the inner portion performs a first heating process in which a first outer portion of the glass plate, bounded by the outer edge of the annular shape, is heated to a higher temperature than a first inner portion of the glass plate, bounded by the outer edge of the annular shape.
4. The method for manufacturing a glass substrate according to claim 3, wherein in the step of separating the outer portion and the inner portion, the first outer portion and the first inner portion are separated, leaving a length of 0.1% to 5% of the outer diameter of the annular shape as a margin for the annular shape of the glass substrate.
5. A method for manufacturing a glass substrate as described in claim 3 or 4, wherein in the step of forming the defect, the defect is formed by using the laser light to set the shape of the inner edge of the ring shape having the opening to the predetermined shape, and in the step of separating the outer portion and the inner portion, a second heating process is performed in which a second outer portion of the glass plate, which is separated by the inner edge of the ring shape having the opening, is heated to a higher temperature than a second inner portion of the glass plate, which is separated by the inner edge of the ring shape.
6. The method for manufacturing a glass substrate according to claim 5, wherein in the step of separating the portion that will become the glass substrate from the raw glass plate, the second heating treatment is performed after the first heating treatment.
7. A method for manufacturing a glass substrate having an opening, comprising: a step of irradiating a laser beam along a line forming a predetermined ring shape on the surface of a raw glass plate that is to become the glass substrate, thereby forming a defect along the line; and a step of separating the outer and inner portions of the glass plate, of which the defect has been formed, by heating the outer portion more highly than the inner portion, the step including the steps of simultaneously heating the outer portion from both sides of the main surface of the glass plate and heating the outer portion more highly than the inner portion, thereby separating the outer and inner portions of the glass plate and removing the inner portion as the portion that will become the opening.
8. A method for manufacturing a glass substrate according to any one of claims 1 to 7, wherein in the step of separating the outer portion from the inner portion, the temperature of the outer portion is made higher than the temperature of the inner portion, causing the outer portion to thermally expand relative to the inner portion, and forming a gap along the line, thereby separating the outer portion from the inner portion.
9. A method for manufacturing a glass substrate according to any one of claims 1 to 8, wherein the irradiation of the surface of the glass plate with the laser light includes forming point-like through holes at a plurality of discrete points on the line with a pulsed laser light, and then continuously moving the irradiation position along the line with a laser light different from the pulsed laser light so as to connect the discrete points on the line.
10. A method for manufacturing a glass substrate according to any one of claims 1 to 9, wherein the heating includes heating both main surfaces of the glass plate by radiant heat from heating sources provided on both sides of the main surfaces of the glass plate.
11. A method for manufacturing a glass substrate according to any one of claims 1 to 10, wherein the area ratio of the main surface of the glass plate to the main surface of the glass substrate is 101% to 160%, and in the step of separating the outer portion and the inner portion, one glass substrate is extracted from one glass plate.
12. The method for manufacturing a glass substrate according to any one of claims 1 to 11, wherein the thickness of the raw glass plate is 0.6 mm or less.