Sidewall wetting barrier for conductive pillars
Patent Information
- Application Number
- TW111102866
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-25
- Filing Date
- 2022-01-24
- Publication Date
- 2026-11-01
- Estimated Expiration
- 2042-01-23
AI Technical Summary
Conventional IC packages face issues with sidewall wetting during solder reflow, leading to unwanted electrical shorts, low solder clearances, and increased risk of intermetallic compound bridging and mechanical stress due to insufficient solder gap height.
The introduction of a wetting barrier with a width greater than the solder post, formed on the second surface of the solder pillar, which acts as a physical and chemical barrier to prevent sidewall wetting, and can be made of a material with lower solderability than the solder post to enhance solder joint formation.
This solution prevents sidewall wetting, maintains adequate solder gap height, reduces the risk of electrical shorts and mechanical failure, and is compatible with existing bumping processes without requiring passivation cleaning, enabling smaller solder caps for fine-pitch applications.
Smart Images

Figure TWG2TB001918193_001 
Figure TWG2TB001918193_002 
Figure TWG2TB001918193_003
Abstract
Description
Technical Field
[0001] This case generally relates to integrated circuit (IC) packages and structures, and particularly, but not exclusively, to sidewall wetting barriers for conductive pillars (for example, copper (Cu) pillar bumps). Prior Technology
[0002] Integrated circuit technology has made significant progress in improving computing power through the miniaturization of active components. Packaged devices can be found in many electronic devices, including processors, servers, and radio frequency (RF) integrated circuits. Packaging technology has become more economical in high-pin-count devices and / or high-volume components.
[0003] An example of IC packaging typically includes an IC structure and a substrate. The IC structure includes a die and one or more die interconnects for electrically coupling the die to the substrate. Each die interconnect includes a solder cap on a copper (Cu) pillar. Solder reflow is performed to electrically connect the solder cap to conductive pads on the substrate.
[0004] When performing solder reflow, solder may adhere to the sidewalls of the copper pillars. This can cause problems such as unwanted electrical short circuits due to solder bridging. It can also lead to low solder gaps, resulting in intermetallic compound (IMC) bridging and bulk stress on the IC package.
[0005] Accordingly, there is a need for systems, apparatuses, and methods (including those provided herein) to overcome the deficiencies of conventional IC packaging and structures. Summary of the Invention
[0006] The following provides a simplified overview of one or more variations and / or examples associated with the various apparatuses and methods disclosed herein. Thus, this overview should not be considered an exhaustive overview of all conceived variations and / or examples, nor should it be considered to identify key or defining elements or illustrations associated with all conceived variations and / or examples and to define the scope of any particular variation and / or example. Accordingly, the following overview serves only to present, in a simplified form, certain concepts related to one or more variations and / or examples of the apparatuses and methods disclosed herein before the detailed descriptions provided below.
[0007] An exemplary integrated circuit (IC) structure is disclosed. The IC structure may include a die. The IC structure may also include solder posts on the die. A first surface of the solder post may face the die. The IC structure may further include a wetting barrier on a second surface of the solder post. The width of the wetting barrier may be greater than the width of the solder post. The IC structure may also include a solder cap on the wetting barrier such that the die is electrically coupled to the solder cap at least via the solder post and the wetting barrier.
[0008] An exemplary method for manufacturing an integrated circuit (IC) structure is disclosed. The method may include forming a solder pillar on a die. A first surface of the solder pillar may face the die. The method may also include forming a wetting barrier on a second surface of the solder pillar. The width of the wetting barrier may be greater than the width of the solder pillar. The method may further include forming a solder cap on the wetting barrier such that the die is electrically coupled to the solder cap at least via the solder pillar and the wetting barrier.
[0009] An exemplary integrated circuit (IC) package is disclosed. The IC package may include a substrate having conductive pads. The IC package may also include an IC structure disposed on the substrate. The IC structure may include a die. The IC structure may also include solder pillars on the die. A first surface of the solder pillar may face the die. The IC structure may further include a wetting barrier on a second surface of the solder pillar. The width of the wetting barrier may be greater than the width of the solder pillar. The IC structure may also include a solder cap on the wetting barrier such that the die is electrically coupled to the conductive pads of the substrate at least via the solder cap, the solder pillar, and the wetting barrier.
[0010] Based on the accompanying drawings and detailed description, other features and advantages associated with the various apparatuses and methods disclosed herein will be apparent to those skilled in the art to which this invention pertains. Simple Explanation of the Diagram
[0011] A more complete understanding of the various aspects of this case and its many accompanying advantages will be readily available when considered in conjunction with the following detailed description, which is provided for illustrative purposes only and does not constitute any limitation on this case.
[0012] Figure 1 illustrates an example of an ideal IC package with a corresponding integrated circuit (IC) structure.
[0013] Figure 2 illustrates a typical IC package with an IC structure, which suffers from sidewall wetting issues.
[0014] Figure 3 illustrates a typical IC structure that mitigates sidewall wetting issues.
[0015] Figure 4 illustrates an example IC structure for mitigating sidewall wetting problems according to one or more of the present invention.
[0016] Figures 5A-5G illustrate examples of the various stages of manufacturing an IC structure according to one or more of the present invention.
[0017] Figures 6A-6G illustrate examples of the various stages of manufacturing another IC structure according to one or more of the present invention.
[0018] Figures 7A-7G illustrate examples of the various stages of manufacturing another IC structure according to one or more of the present invention.
[0019] Figures 8A-8G illustrate examples of the various stages of manufacturing a re-IC structure according to one or more of the present invention.
[0020] Figures 9A-9E illustrate examples of one or more types of IC packages according to this invention.
[0021] Figure 10-18 illustrates a flowchart of an example method for manufacturing an IC structure according to one or more of the present invention.
[0022] Figure 19 illustrates various electronic devices that can utilize one or more of the forms described in this case.
[0023] Based on the accompanying drawings and detailed description, other objects and advantages associated with the various embodiments disclosed herein will be apparent to those skilled in the art to which this invention pertains. By convention, the features illustrated in the drawings may not be drawn to scale. Accordingly, for clarity, the dimensions of the illustrated features may be arbitrarily enlarged or reduced. By convention, some drawings are simplified for clarity. Therefore, the drawings may not depict all parts of a particular apparatus or method. Furthermore, similar element symbols are used throughout the specification and accompanying drawings to indicate similar features. Implementation
[0024] The various embodiments illustrated in this document are disclosed in the following description and related drawings with reference to specific embodiments. Alternative embodiments or examples may be designed without departing from the scope of this teaching. Additionally, well-known elements of the illustrative embodiments herein will not be described in detail or will be omitted so as not to obscure the relevant details of the teachings herein.
[0025] In some of the described implementation examples, instances are identified where various parts of the component structures and operations are available from known general techniques and are subsequently arranged according to one or more exemplary embodiments. In such instances, internal details of known conventional component structures and / or operations may be omitted to help avoid potential confusion with the concepts illustrated in the illustrative embodiments disclosed herein.
[0026] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting. As used herein, the singular forms “a,” “some,” and “the” are intended to include the plural forms as well, unless the context clearly indicates otherwise. It will be further understood that the terms “comprising,” “having,” “including,” and / or “containing” as used herein specify the presence of the stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof.
[0027] Based on the various aspects presented in this paper, solutions are proposed to address issues associated with conventional IC packages and structures. For context, Figure 1 illustrates an example of an idealized IC package, and Figure 2 illustrates a conventional IC package with associated issues.
[0028] An ideal IC package 100 includes a die 110 and a substrate 120 having conductive pads 125. One or more die interconnects 130 electrically couple the die 110 to the substrate 120, and more particularly, electrically couple the die 110 to the pads 125. Each die interconnect 130 includes a conductive pillar 140 (e.g., a copper pillar) and a solder cap 150 connected to the pad 125. In this context, it can be said that the ideal IC package 100 includes the substrate 120 and the idealized IC structure. That is, it can be said that the idealized IC structure includes the die 110 and the die interconnects 130.
[0029] A conventional IC package 200 includes a die 210 and a substrate 220 having conductive pads 225. One or more die interconnects 230 electrically couple the die 210 to the substrate 220, and more particularly, electrically couple the die 210 to the pads 225. Each die interconnect 230 includes a pillar 240 (e.g., a copper pillar) and a solder cap 250 connected to the pad 225. In this context, it can be said that a conventional IC package 100 includes a substrate 220 and a conventional IC structure. That is, it can be said that a conventional IC structure includes the die 210 and the die interconnects 230.
[0030] In the ideal IC package 100, there is no sidewall wetting. That is, no solder forms on the sidewalls of the copper pillars 140. Note that in Figure 1, there is no solder material on the sidewalls of the solder pillars 140. However, sidewall wetting exists on the copper pillars 240 of the conventional IC package 200. Sidewall wetting typically occurs during solder reflow. When sidewall wetting occurs, solder material is pushed to the side. As can be seen in Figure 2, the sidewalls of the solder pillars 240 are wetted with solder material.
[0031] In an ideal IC package 100 without sidewall wetting, a good solder gap height exists. In this context, the solder gap height is defined as the distance between the lower and upper surfaces of the solder cap 150, as highlighted in the dashed circle in Figure 1. A good solder gap height can also be considered sufficient to prevent intermetallic compound (IMC) bridging. A good solder gap height also prevents solid stress, which minimizes mechanical failure.
[0032] However, in the conventional IC package 200 with sidewall wetting, the solder gap height is significantly smaller, as highlighted in the larger dashed circle in Figure 2. During solder reflow, less solder remains between the solder post 240 and the substrate 220 as the solder material of the solder cap 250 is pushed to the side, resulting in a shorter solder gap height. A small solder gap height can lead to IMC bridging and increase the likelihood of mechanical failure.
[0033] Furthermore, in the ideal IC package 100 without sidewall wetting, there is no solder bridging that could lead to unwanted electrical short circuits because the solder material remains below the solder pillars 140. However, in the conventional IC package 200 with solder wetting, solder bridging can occur—two solder caps 250 come into contact with each other, as highlighted in the smaller dashed circle in Figure 2. Solder bridging becomes more likely as the spacing between adjacent die interconnects 230 becomes narrower.
[0034] There are indeed some methods to mitigate solder wetting problems. Figure 3 illustrates a conventional IC structure 300 that mitigates sidewall wetting problems. The IC structure 300 includes a die 310 and several die interconnects 330. Each die interconnect 330 includes a copper pillar 340 and a solder cap 350. Each die interconnect 330 also includes a sidewall passivation 332.
[0035] During the fabrication of IC structure 300, the entire die interconnect 330 is covered with a passivation layer. That is, the sidewalls of the solder pillars 340 and the corresponding solder caps 350 are passivated. Subsequently, the solder caps 350 undergo passivation cleaning (e.g., plasma etching), leaving sidewall passivation 332 to minimize or prevent sidewall wetting.
[0036] Unfortunately, passivation cleaning is not always effective. In other words, even after cleaning, some passivation layer may still remain on the solder cap 350, which is undesirable. Solder sidewall wetting may still occur.
[0037] Based on the various embodiments disclosed herein, in order to address problems associated with conventional IC packages and structures, a wetting barrier is proposed to prevent solder sidewall wetting. The proposed wetting barrier can prevent sidewall wetting at least in the following ways: First, the wetting barrier can be shaped to prevent sidewall wetting in a physical form. Second, the wetting barrier can be formed from a material that chemically prevents sidewall wetting.
[0038] Figure 4 illustrates an example IC structure 400 for mitigating sidewall wetting problems according to one or more embodiments of the present invention. As shown, the IC structure 400 may include a die 410. For example, the die 410 may be a flip chip (FC) die. The IC structure 400 may also include one or more die interconnects 430 on one side of the die 410. The die interconnects 430 may be conductive to enable the die 410 to couple with other components. Thus, the die interconnects 430 may be connected to the active side of the die 410. In one embodiment, it may be assumed that each die interconnect 430 is similar to the other die interconnects 430. Therefore, a description of the die interconnects 430 will be provided.
[0039] The die interconnect 430 may include a bond post 440 formed on the die 410. The bond post 440 may be formed of a conductive material, such as copper (Cu). A first surface (e.g., a bottom surface) of the bond post 440 may face the die 410. For example, the first surface of the bond post 440 may contact one side (e.g., the active side) of the die 410.
[0040] The grain interconnect 430 may also include a wetting barrier 460 on the second surface of the bond post 440. For example, the wetting barrier 460 may contact the second surface of the bond post 440. The wetting barrier 460 may be formed of a conductive material. In one embodiment, the wetting barrier 460 may be formed of the same material as the bond post 440 (e.g., Cu). In another embodiment, the wetting barrier 460 may be formed of a different material (e.g., nickel (Ni), aluminum (Al), chromium (Cr), etc.).
[0041] The die interconnect 430 may further include a solder cap 450 on the wetting barrier 460. As shown, the solder cap 450 may contact the wetting barrier 460. However, this is not absolutely necessary. There may be other intermediary elements or components between the solder cap 450 and the wetting barrier 460. In fact, the solder post 440 does not need to contact the die 410, and the wetting barrier 460 does not need to contact the solder post 440. Regardless of the presence of intermediary elements, it is sufficient to form an electrical path such that the die 410 is electrically coupled to the solder cap 450 at least via the solder post 440 and the wetting barrier 460.
[0042] In Figure 4, the wetting barrier 460 is illustrated as a collar-shaped structure (e.g., 3-5 μm overhang) below the solder cap 450. That is, the wetting barrier 460 may be wider than the solder post 440. The wetting barrier 460 may also be wider than the solder cap 450. The shape of the wetting barrier 460 serves as a solid barrier to prevent wetting of the solder sidewalls of the solder post 440, for example, during solder reflow. Thus, a passivation layer is not required during manufacturing. It will be appreciated that, in at least some embodiments, the disclosed technical advantages include the elimination of the need for passivation cleaning, and the ability of the solder cap 450 to remain free of a passivation layer.
[0043] Another technical advantage of the proposed IC structure is its complete compatibility with existing bump processes. In other words, almost no further processing is required. Using two-step optical patterning to independently control the size of the solder cap and solder pillars allows for smaller solder caps with larger under-bump metallization (UBM) for fine-pitch applications.
[0044] As mentioned above, the wetting barrier 460 can be formed of the same or different material as the solder post 440. When the wetting barrier 460 is formed of a different material, that material can be selected to also provide a chemical barrier for wetting the solder sidewalls. Generally, the wetting barrier 460 should preferably have "worse" solderability than the solder post 440. That is, forming a solder joint with the wetting barrier 460 should be more difficult than forming a solder joint with the solder post 440.
[0045] More formally, the weldability of a material can be defined as a measure of how easily a material can be bonded together. Under this definition, a material with "high" weldability can be bonded more easily than a material with "low" weldability. Therefore, when the wetting barrier 460 and the weld post 440 are formed of different materials, it is preferable that the weldability of the wetting barrier 460 is lower than that of the weld post 440. For example, if the weld post 440 is formed of Cu, then the wetting barrier 460 can be formed of metals such as Ni, Al, or Cr.
[0046] The grain interconnect 430 may additionally include an optional low-wetting layer 470, which may be formed on at least a portion of the surface of the wetting barrier 460 not covered by the solder post 440. In Figure 4, the low-wetting layer 470 (e.g., 1-3 μm thick) is shown formed on the overhang of the wetting barrier 460. The low-wetting layer 470 can also provide physical barrier protection. More importantly, when the low-wetting layer 470 (e.g., Ni, Al, Cr, etc.) is formed of a material (e.g., Cu) having lower solderability than the solder post 440, it can provide chemical barrier protection.
[0047] The IC structure 400 in Figure 4 is just one of many embodiments of the proposed IC structure. Figures 5A-5G, 6A-6G, 7A-7G, and 8A-8G illustrate examples of various stages in fabricating embodiments of other IC structures. Again, multiple die interconnects are illustrated in these figures. However, for the sake of simplicity, only one die interconnect is described because it is recognized that other die interconnects can be fabricated similarly.
[0048] Figures 5A-5G illustrate the various stages of manufacturing the IC structure 500. Figure 5A illustrates the stages in which solder pillars 540 and wetting barriers 560 can be formed on a die 510 (e.g., an FC die). The solder pillars 540 can be formed from a conductive material (e.g., Cu) on the die 510. The first surface (e.g., the bottom surface) of the solder pillar 540 can face the die 510. For example, the first surface of the solder pillar 540 can contact one side of the die 510 (e.g., the active side). Furthermore, a wetting barrier 560 can be formed on the solder pillar 540.
[0049] The procedure to reach stage 5A can be as follows. Initially, a first photoresist 585 can be deposited on the die 510. The first photoresist 585 can be patterned to have a first opening corresponding to the contacts (not shown) of the die 510. This can then be followed by forming a solder post 540 within the first opening and up to the height of the first photoresist 585 such that the second surface of the solder post 540 is exposed to the top surface of the first photoresist 585. For example, the solder post 540 can be formed by electroplating metal (e.g., Cu) up to the top surface of the first photoresist 585.
[0050] Subsequently, a wetting barrier 560 can be formed on the exposed second surface of the weld post 540. If the weld post 540 and the wetting barrier 560 are formed of the same material (e.g., Cu), the wetting barrier 560 can be formed by continuing electroplating the same conductive material on the weld post 540 to a height above the first photoresist 585. Note that the wetting barrier 560 can be formed while the first photoresist 585 is still in place. Since there is no masking constraint above the first photoresist 585, continued electroplating can produce a slight overgrowth on the top side above the first photoresist 585 to form a dangle. As a result, the wetting barrier 560 can be wider than the weld post 540.
[0051] Figure 5B illustrates the stages in which a low-wetting layer 570 can be formed on the exposed surface of the wetting barrier 560. Preferably, the low-wetting layer 570 has lower solderability than the solder post 540, that is, solder is more difficult to adhere to the low-wetting layer 570 compared to the solder post 540. For example, if the solder post 540 is formed of Cu, the low-wetting layer 570 can be formed by electroplating Ni, Al, Cr, etc. Note that if Ni is used, this is quite standard in Cu bump processes. The low-wetting layer 570 can also be formed while the first photoresist 585 is still in place.
[0052] Figure 5C illustrates the stage in which a second photoresist 595 can be deposited on the first photoresist 585 to cover the low wetting layer 570.
[0053] Figure 5D illustrates a stage in which the second photoresist 595 can be patterned to form a second opening to expose a portion of the surface of the low-wetting layer 570. The width of the second opening formed in the second photoresist 595 can be smaller than the width of the first opening formed in the first photoresist 585. The smaller width of the second opening allows for accommodative alignment misalignment.
[0054] Figure 5E illustrates the stages in which solder material 555 can be deposited on the exposed portion of the low-wetting layer 570 within the second opening. For example, solder material 555 can be electroplated onto the low-wetting layer 570. Subsequently, the first and second photoresists 585 and 595 can be removed.
[0055] Figure 5F illustrates the stage after the removal of the first and second photoresists 585, 595. In this stage, the exposed low-wetting layer 570 may undergo plasma treatment. For example, if the low-wetting layer 570 is formed of nickel, an N2+O2 plasma treatment may be performed to further reduce the solderability of the low-wetting layer 570 via oxidation.
[0056] Figure 5G illustrates the stages in which seed layer etching and solder reflow can be performed to form solder cap 550 while removing the first and second photoresists 585, 595.
[0057] In one scenario, stage 5B of Figure 5 is optional. That is, the formation of the low-wetting layer 570 is not required. In this case, the procedure can skip stage 5B, that is, it can proceed from stage 5A to stage 5C. Stage 5F of Figure 5 is also optional. That is, plasma treatment to oxidize the low-wetting layer 570 is not required. In this case, the procedure can skip stage 5F, that is, it can proceed from stage 5E to stage 5G. Of course, if the low-wetting layer 570 is not formed (that is, stage 5B is skipped), then stage 5F can also be skipped.
[0058] Figures 6A-6G illustrate the stages of manufacturing the IC structure 600. Figure 6A illustrates the stage in which bond pillars 640 can be formed on a die 610 (e.g., an FC die). Bond pillars 640 can be formed from a conductive material (e.g., Cu) on the die 610. The first surface of the bond pillar 640 can face the die 610. For example, the first surface of the bond pillar 640 can contact one side of the die 610 (e.g., the active side).
[0059] The procedure to reach stage 6A can be as follows. Initially, a first photoresist 685 can be deposited on the die 610. The first photoresist 685 can be patterned to have first openings corresponding to the contacts (not shown) of the die 610. This can then be followed by forming a solder post 640 within the first opening and up to the height of the first photoresist 685 such that the second surface of the solder post 640 is exposed to the top surface of the first photoresist 685. For example, the solder post 640 can be formed by electroplating metal (e.g., Cu) up to the top surface of the first photoresist 685.
[0060] Figure 6B illustrates the stages in which a wetting barrier 660 can be formed on the solder post 640. If the solder post 640 (e.g., Cu) and the wetting barrier 660 (e.g., Ni) are formed of different materials, the wetting barrier 660 can be formed by electroplating a different material onto the solder post 640 to a height above the first photoresist 685. Note that the wetting barrier 660 can be formed while the first photoresist 685 is still in place. Since there is no masking constraint above the first photoresist 685, electroplating can create a mushroom-shaped or collar-shaped wetting barrier 660 above the solder post 640. As a result, the wetting barrier 660 can be wider than the solder post 640.
[0061] Figure 6C illustrates the stage in which a second photoresist 695 can be deposited on the first photoresist 685 to cover the wetting barrier 660.
[0062] Figure 6D illustrates a stage in which the second photoresist 695 can be patterned to form a second opening to expose a portion of the surface of the wetting barrier 660. The width of the second opening formed in the second photoresist 695 can be smaller than the width of the first opening formed in the first photoresist 685, for example, to accommodate alignment offset.
[0063] Figure 6E illustrates a stage in which solder material 655 can be deposited on the exposed portion of the wetting barrier 660 within the second opening. For example, solder material 655 can be electroplated onto the wetting barrier 660. Subsequently, the first and second photoresists 685 and 695 can be removed.
[0064] Figure 6F illustrates the stage after the removal of the first and second photoresists 685, 695. In this stage, the exposed wetting barrier 660 may undergo plasma treatment. For example, if the exposed wetting barrier 660 is formed of nickel, an N2+O2 plasma treatment may be performed to further reduce the solderability of the exposed wetting barrier 660 via oxidation.
[0065] Figure 6G illustrates the stages in which seed layer etching and solder reflow can be performed to form solder cap 650 while removing the first and second photoresists 685, 695.
[0066] In another scenario, the stage in Figure 6F can be optional. That is, plasma treatment may not be required. In this case, the procedure can skip the stage in Figure 6F, that is, it can proceed from the stage in Figure 6E to the stage in Figure 6G.
[0067] Figures 7A-7G illustrate the various stages of manufacturing the IC structure 700. Figure 7A illustrates the stages in which solder pillars 740 and wetting barriers 760 can be formed on a die 710 (e.g., an FC die). The solder pillars 740 can be formed from a conductive material (e.g., Cu) on the die 710. The first surface (e.g., the bottom surface) of the solder pillar 740 can face the die 710. For example, the first surface of the solder pillar 740 can contact one side of the die 710 (e.g., the active side). Furthermore, a wetting barrier 760 can be formed on the solder pillar 740.
[0068] The procedure to reach stage 7A can be as follows. Initially, a first photoresist 785 can be deposited on the die 710. The first photoresist 785 can be patterned to have first openings corresponding to the contacts (not shown) of the die 710. This can then be followed by forming a solder post 740 within the first opening and up to the height of the first photoresist 785 such that the second surface of the solder post 740 is exposed to the top surface of the first photoresist 785. For example, the solder post 740 can be formed by electroplating metal (e.g., Cu) up to the top surface of the first photoresist 785.
[0069] Subsequently, a wetting barrier 760 can be formed on the exposed second surface of the weld post 740. Electroplating with the same or different conductive material can continue on the weld post 740 to a height above the first photoresist 785 to form the wetting barrier 760. The wetting barrier 760 can be formed while the first photoresist 785 is still in place. Since there is no masking constraint above the first photoresist 785, continued plating can produce a slight overgrowth on the top side above the first photoresist 785 to form a drap. As a result, the wetting barrier 760 can be wider than the weld post 740.
[0070] Figure 7B illustrates the stages in which a low-wetting layer 770 can be formed on the exposed surface of the wetting barrier 760. Preferably, the low-wetting layer 770 has lower solderability than the solder post 740. For example, if the solder post 740 is formed of Cu, the low-wetting layer 770 can be formed by electroplating Al, Cr, etc. The low-wetting layer 770 can also be formed while the first photoresist 785 is still in place.
[0071] Figure 7C illustrates the stage in which a second photoresist 795 can be deposited on the first photoresist 785 to cover the low wetting layer 770.
[0072] Figure 7D illustrates a stage in which the second photoresist 795 can be patterned to form a second opening to expose a portion of the surface of the low-wetting layer 770. The width of the second opening formed in the second photoresist 795 can be smaller than the width of the first opening formed in the first photoresist 785.
[0073] Figure 7E illustrates a stage where the exposed portion of the low wetting layer 770 can be etched to expose a portion of the wetting barrier 760. This can then be followed by forming a contact layer 780 on the exposed portion of the wetting barrier 760. For example, the contact layer 780 can be formed by plating a conductive material (such as Ni) on the exposed portion of the wetting barrier 760.
[0074] Figure 7F illustrates the stage in which solder material 755 can be deposited on the contact layer 780 within the second opening. For example, solder material 755 can be electroplated onto the contact layer 780. Subsequently, the first and second photoresists 785 and 795 can be removed.
[0075] Figure 7G illustrates the stages in which seed layer etching and solder reflow can be performed to form solder cap 750 while removing the first and second photoresists 785, 795.
[0076] In one scenario, stage 7B can be optional. That is, the formation of the low-wetting layer 770 is not required. In this case, the procedure can skip stage 7B, i.e., proceed from stage 7A to stage 7C. Furthermore, if the low-wetting layer 770 is not formed (i.e., stage 7B is skipped), the wetting barrier 760 will be exposed after stage 7D, in which the second opening is formed in the second photoresist 785. Thus, the procedure can proceed directly to the formation of the contact layer 780.
[0077] Figures 8A-8G illustrate the various stages of manufacturing the IC structure 800. Figure 8A illustrates the stages in which a first bond post 840 and a wetting barrier 860 can be formed on a die 810 (e.g., an FC die). The first bond post 840 can be formed from a conductive material (e.g., Cu) on the die 810. A first surface (e.g., a bottom surface) of the first bond post 840 can face the die 810. For example, the first surface of the first bond post 840 can contact one side of the die 810 (e.g., the active side). Furthermore, a wetting barrier 860 can be formed on the first bond post 840.
[0078] The procedure to reach stage 8A can be as follows. Initially, a first photoresist 885 can be deposited on the die 810. The first photoresist 885 can be patterned to have first openings corresponding to the contacts (not shown) of the die 810. This can then be followed by forming first post 840s within the first openings up to the height of the first photoresist 885 such that the second surface of the first post 840 is exposed to the top surface of the first photoresist 885. For example, the first post 840 can be formed by electroplating metal (e.g., Cu) up to the top surface of the first photoresist 885.
[0079] Subsequently, a wetting barrier 860 can be formed on the exposed second surface of the first weld post 840. Electroplating with the same or different conductive material can continue on the first weld post 840 to a height above the first photoresist 885 to form the wetting barrier 860. The wetting barrier 860 can be formed while the first photoresist 885 is still in place. Since there is no masking constraint above the first photoresist 885, continued electroplating can produce a slight overgrowth on the top side above the first photoresist 885 to form a dangle. As a result, the wetting barrier 860 can be wider than the first weld post 840.
[0080] Figure 8B illustrates the stages in which a low-wetting layer 870 can be formed on the exposed surface of the wetting barrier 860. Preferably, the low-wetting layer 870 has lower solderability than the first solder post 840. For example, if the first solder post 840 is formed of Cu, the low-wetting layer 870 can be formed by plating Al, Cr, etc. The low-wetting layer 870 can also be formed while the first photoresist 885 is still in place.
[0081] Figure 8C illustrates the stage in which a second photoresist 895 can be deposited on the first photoresist 885 to cover the low wetting layer 870.
[0082] Figure 8D illustrates a stage in which the second photoresist 895 can be patterned to form a second opening to expose a portion of the surface of the low-wetting layer 870. The width of the second opening formed in the second photoresist 895 can be smaller than the width of the first opening formed in the first photoresist 885.
[0083] Figure 8E illustrates a stage in which a second weld post 890 can be formed on the exposed portion of the low-wetting layer 870 within the second opening. For example, a conductive material (e.g., Cu) can be plated onto the low-wetting layer 870 within the second opening.
[0084] Figure 8F illustrates the stage in which a contact layer 880 can be formed on the second weld post 890 within the second opening. For example, the contact layer 880 can be formed by plating a conductive material (such as Ni) onto the second weld post 890.
[0085] In Figure 8F, after the contact layer 880 is formed, solder material 855 can be deposited on the contact layer 880 within the second opening. For example, solder material 855 can be electroplated onto the contact layer 880. Subsequently, the first and second photoresists 885 and 895 can be removed.
[0086] Figure 8G illustrates the stages in which seed layer etching and solder reflow can be performed to form solder cap 850 while the first and second photoresists 885 and 895 are being removed.
[0087] Figures 9A-9E illustrate different example embodiments of IC packages. Figure 9A illustrates IC package 900A including substrate 920 (which includes conductive pads 925) and IC structure 400 of Figure 4. Figure 9B illustrates IC package 900B including substrate 920 (which includes conductive pads 925) and IC structure 500 of Figure 5G. Figure 9C illustrates IC package 900C including substrate 920 (which includes conductive pads 925) and IC structure 600 of Figure 6G. Figure 9D illustrates IC package 900D including substrate 920 (which includes conductive pads 925) and IC structure 700 of Figure 7G. Figure 9E illustrates IC package 900E including substrate 920 (which includes conductive pads 925) and IC structure 800 of Figure 8G. Note that in each of the IC packages 900A-900E, the dies 410, 510, 610, 710, and 810 can be electrically coupled to the conductive pads 925 of the substrate 920 at least via solder caps 450, 550, 650, 750, and 850, solder posts 440, 540, 640, 740, and 840, and wetting barriers 460, 560, 660, 760, and 860.
[0088] Figure 10 illustrates a flowchart of an example method 1000 for manufacturing an IC package (such as any of IC structures 400, 500, 600, 700, and 800). In block 1010, a bonding pillar can be formed on the die such that the first face of the bonding pillar faces the die.
[0089] In block 1020, a wetting barrier can be formed on the second surface of the weld post. The wetting can be formed such that the width of the wetting barrier is greater than the width of the weld post.
[0090] Figure 11 illustrates a flowchart of an example program for implementing blocks 1010 and 1020. In block 1110, a first photoresist can be deposited on the grain. In block 1120, the first photoresist can be patterned to have a first opening, which can correspond to a contact point of the grain. In block 1130, a solder post can be formed within the first opening such that a second surface of the solder post is exposed to the top surface of the first photoresist. For example, the solder post can be formed by electroplating a conductive material (e.g., Cu) up to the top surface of the first photoresist. In one embodiment, blocks 1110, 1120, and 1130 can correspond to Figures 5A, 6A, 7A, and 8A.
[0091] In block 1140, a wetting barrier can be formed on the exposed second surface of the weld post. For example, the wetting barrier can be formed by depositing a conductive material on the weld post while a first photoresist remains in place. The wetting barrier can be formed from the same or a different material as the weld post. In one embodiment, block 1140 can correspond to Figures 5A, 6B, 7A, and 8A.
[0092] Referring back to Figure 10, in one state, method 1000 can proceed from block 1020 to block 1050. In block 1050, a solder cap can be formed on the wetting barrier such that the grains are electrically coupled to the solder cap at least via the pillars and the wetting barrier.
[0093] Figure 12 illustrates a flowchart of an example procedure for implementing block 1050 when proceeding from block 1020. In block 1210, a second photoresist can be deposited on the first photoresist to cover the wetting barrier. In one embodiment, block 1210 can correspond to Figure 6C.
[0094] In block 1220, the second photoresist can be patterned to have a second opening to expose a portion of the wetting barrier. The width of the second opening can be smaller than the width of the first opening. In one embodiment, block 1220 can correspond to Figure 6D.
[0095] In block 1230, solder material can be deposited on the exposed portion within the second opening of the wetting barrier. In one embodiment, block 1230 can correspond to FIG6E.
[0096] After depositing solder material, the first and second photoresists can be removed in block 1240. Subsequently, plasma treatment can be performed in block 1250 (which may be optional). In one embodiment, blocks 1240 and 1250 may correspond to FIG. 6F.
[0097] Following block 1240 or 1250, in block 1260, seed layer etching and solder reflow can be performed. In one case, block 1260 can correspond to Figure 6G.
[0098] Referring back to Figure 10, in another embodiment, method 1000 can proceed from block 1020 to block 1030 before proceeding to block 1050. In block 1030, a low-wetting layer can be formed on at least a portion of the surface of the wetting barrier not covered by the weld post. Preferably, the low-wetting layer has lower solderability than the weld post.
[0099] Figure 13 illustrates a flowchart of an example program for implementing block 1030. In block 1310, a low-wetting layer can be formed on the wetting barrier while the first photoresist is still in place. In one case, block 1310 can correspond to Figures 5B, 7B, and 8B.
[0100] Referring back to Figure 10, in a further embodiment, method 1000 can proceed from block 1030 to block 1050. As previously indicated, in block 1050, a solder cap can be formed on the wetting barrier such that the grains are electrically coupled to the solder cap at least via the solder pillar and the wetting barrier.
[0101] Figure 14 illustrates a flowchart of an example procedure for implementing block 1050 when proceeding from block 1030. In block 1410, a second photoresist can be deposited on the first photoresist to cover a low-wetting layer. In one embodiment, block 1410 can correspond to Figure 5C.
[0102] In block 1420, the second photoresist can be patterned to have a second opening to expose a portion of the low-wetting layer. The width of the second opening can be smaller than the width of the first opening. In one embodiment, block 1420 can correspond to Figure 5D.
[0103] In block 1430, solder material can be deposited on the exposed portion within the second opening of the low-wetting layer. In one embodiment, block 1430 can correspond to FIG5E.
[0104] After depositing solder material, the first and second photoresists can be removed at block 1440. Subsequently, plasma treatment can be performed at block 1450 (which may be optional). In one embodiment, blocks 1440 and 1450 may correspond to Figure 5F.
[0105] Following block 1440 or 1450, in block 1460, seed layer etching and solder reflow can be performed. In one case, block 1460 can correspond to Figure 5G.
[0106] Referring back to Figure 10, in another state, method 1000 can proceed from block 1030 to block 1040. In block 1040, a contact layer can be formed on the wetting barrier such that the contact layer is between the wetting barrier and the solder cap.
[0107] Figure 15 illustrates a flowchart of an example program for implementing block 1040. In block 1510, a second photoresist can be deposited on the first photoresist to cover a low-wetting layer. In one embodiment, block 1510 can correspond to Figure 7C.
[0108] In block 1520, the second photoresist can be patterned to have a second opening to expose a portion of the surface of the low-wetting layer. The width of the second opening can be smaller than the width of the first opening. In one embodiment, block 1520 can correspond to FIG7D.
[0109] In block 1530, the exposed portion of the low wetting layer can be etched to expose a portion of the wetting barrier. In block 1540, a contact layer can be formed on the exposed portion of the wetting barrier. For example, a conductive material (e.g., Ni) can be plated on the exposed portion of the wetting barrier. In one embodiment, blocks 1530 and 1540 can correspond to FIG7E.
[0110] Referring back to Figure 10, the method can proceed from block 1040 to block 1050. As previously indicated, in block 1050, a solder cap can be formed on the wetting barrier such that the grains are electrically coupled to the solder cap at least via the solder pillar and the wetting barrier.
[0111] Figure 16 illustrates a flowchart of an example procedure for implementing block 1050 when proceeding from block 1040. In block 1610, solder material can be deposited on the contact layer within the second opening. In one embodiment, block 1610 can correspond to Figure 7F.
[0112] After depositing solder material, in block 1620, the first and second photoresists can be removed. Subsequently, in block 1630, seed layer etching and solder reflow can be performed. In one case, blocks 1620 and 1630 can correspond to Figure 7G.
[0113] Figure 17 illustrates a flowchart of another example program for implementing block 1040 of Figure 10. In this example program, another weld pillar is formed. Therefore, for ease of distinction, the weld pillar formed in block 1010 will be referred to as the first weld pillar. A low-wetting layer can then be formed on the first weld pillar.
[0114] In block 1710, a second photoresist can be deposited on the first photoresist to cover a low-wetting layer. In one state, block 1710 can correspond to Figure 8C.
[0115] In block 1720, the second photoresist can be patterned to have a second opening to expose a portion of the surface of the low-wetting layer. The width of the second opening can be smaller than the width of the first opening. In one embodiment, block 1720 can correspond to FIG8D.
[0116] In block 1730, a second weld post can be formed on the low-wetting layer within the second opening. For example, a conductive material (e.g., Cu) can be plated on the exposed portion of the low-wetting layer. In one embodiment, block 1730 can correspond to FIG8E.
[0117] In block 1740, a contact layer can be formed on the second weld post. For example, a conductive material (e.g., Ni) can be plated on the contact layer. In one case, block 1740 can correspond to FIG8F.
[0118] Figure 18 illustrates a flowchart of an example procedure for implementing block 1050 when proceeding from block 1040, as implemented via the blocks of Figure 17. In block 1810, solder material can be deposited on the contact layer within the second opening. Alternatively, block 1810 can correspond to Figure 8F.
[0119] After depositing solder material, in block 1820, the first and second photoresists can be removed. Subsequently, in block 1830, seed layer etching and solder reflow can be performed. In one case, blocks 1820 and 1830 can correspond to Figure 8G.
[0120] Figure 19 illustrates various electronic devices according to different embodiments of this invention that can be integrated with any of the aforementioned IC packages and structures 400, 500, 600, 700, 800, 900A, 900B, 900C, 900D, 900E. For example, mobile phone device 1902, laptop computer device 1904, and fixed-location terminal device 1906 can each be generally considered as user equipment (UE) and may include devices 1900 incorporated into IC packages and structures 400, 500, 600, 700, 800, 900A, 900B, 900C, 900D, 900E as described herein. Devices 1902, 1904, and 1906 illustrated in Figure 19 are merely exemplary. Other electronic devices may also include IC packages and structures 400, 500, 600, 700, 800, 900A, 900B, 900C, 900D, and 900E. These electronic devices include, but are not limited to, a group of devices (e.g., electronic devices) that include the following: mobile devices, handheld personal communication system (PCS) units, portable data units (such as personal digital assistants), GPS-enabled devices, navigation devices, set-top boxes, music players, video players, entertainment units, fixed-location data units (such as instrument reading devices), communication devices, smartphones, tablets, computers, wearable devices, servers, routers, electronic devices implemented in motor vehicles, Internet of Things (IoT) devices, or any other device that stores or retrieves data or computer instructions, or any combination thereof.
[0121] The devices and functionalities disclosed above can be designed and configured in computer files (e.g., RTL, GDSII, GERBER, etc.) stored on computer-readable media. Some or all of these files can be provided to a manufacturing processor that manufactures devices based on such files. The resulting products may include semiconductor wafers, which are subsequently diced into semiconductor dies and packaged as described herein.
[0122] Each implementation instance is described in the following numbered clauses.
[0123] Clause 1: An integrated circuit (IC) structure comprising: a die; a solder post on the die, a first surface of the solder post facing the die; a wetting barrier on a second surface of the solder post, the width of the wetting barrier being greater than the width of the solder post; and a solder cap on the wetting barrier such that the die is electrically coupled to the solder cap at least via the solder post and the wetting barrier.
[0124] Clause 2: The IC structure as described in Clause 1 further includes: a low wetting layer on at least a portion of the surface of the wetting barrier not covered by the solder pillar.
[0125] Clause 3: IC structure as described in Clause 2, wherein the low wetting layer has lower solderability than the solder post.
[0126] Clause 4: An IC structure as described in any of Clauses 2-3, wherein the low wetting layer is formed of any combination of nickel (Ni), aluminum (Al), and chromium (Cr).
[0127] Clause 5: IC structure as in any of Clauses 2-4, wherein the low wetting layer is formed between the wetting barrier and the solder cap.
[0128] Clause 6: An IC structure as described in any of Clauses 2-5, wherein the solder post is a first post, and wherein the IC structure further includes: a second solder post on the low wetting layer; and a contact layer between the second solder post and the solder cap.
[0129] Clause 7: The IC structure as described in Clause 6, wherein the contact layer is formed of nickel (Ni).
[0130] Clause 8: The IC structure of any of Clauses 2-5 further includes: a contact layer between the wetting barrier and the solder cap.
[0131] Clause 9: The IC structure as described in Clause 8, wherein the contact layer is formed of nickel (Ni).
[0132] Clause 10: IC structure as in any of Clauses 2-9, wherein the width of the wetting barrier is greater than the width of the solder cap.
[0133] Clause 11: An IC structure as described in any of Clauses 2-10, wherein the solder post and the wetting barrier are formed of the same conductive material.
[0134] Clause 12: The IC structure as described in Clause 11, wherein the solder pillar and the wetting barrier are formed of copper (Cu).
[0135] Clause 13: An IC structure as described in any of Clauses 2-10, wherein the solder pillar and the wetting barrier are formed of different conductive materials.
[0136] Clause 14: The IC structure as described in Clause 13, wherein the solder pillar is formed of copper (Cu) and wherein the wetting barrier is formed of nickel (Ni).
[0137] Clause 15: An IC structure as described in any of Clauses 2-14, wherein the IC structure is incorporated into a device selected from the group consisting of: music players, video players, entertainment units, navigation devices, communication devices, mobile devices, mobile phones, smartphones, personal digital assistants, fixed-location terminals, tablet computers, computers, wearable devices, Internet of Things (IoT) devices, laptops, servers, and devices in motor vehicles.
[0138] Clause 16: A method of manufacturing an integrated circuit (IC) structure, the method comprising: forming a solder post on a die, a first surface of the solder post facing the die; forming a wetting barrier on a second surface of the solder post, the width of the wetting barrier being greater than the width of the solder post; and forming a solder cap on the wetting barrier such that the die is electrically coupled to the solder cap at least via the solder post and the wetting barrier.
[0139] Clause 17: The method of Clause 16, wherein forming the weld pillar and forming the wetting barrier comprises: depositing a first photoresist on the grain; patterning the first photoresist to have a first opening; forming the weld pillar in the first opening such that a second surface of the weld pillar is exposed to the top surface of the first photoresist; and forming a wetting barrier on the exposed second surface of the weld pillar with the first photoresist in place.
[0140] Clause 18: The method of Clause 17, wherein the weld pillar is formed by plating copper (Cu) in the first opening, or wherein the wetting barrier is formed by plating Cu or nickel (Ni) on the weld pillar, or both.
[0141] Clause 19: The method of any of Clauses 17-18, wherein forming the solder cap comprises: depositing a second photoresist on the first photoresist to cover the wetting barrier; patterning the second photoresist to have a second opening to expose a portion of the wetting barrier, the width of the second opening being smaller than the width of the first opening; depositing solder material on the exposed portion of the wetting barrier within the second opening; removing the first and second photoresists after depositing the solder material; and performing seed layer etching and solder reflow after removing the first and second photoresists.
[0142] Clause 20: The method of Clause 19, wherein forming the solder cap further comprises: performing a plasma treatment of the wetting barrier after removing the first and second photoresists and before performing seed layer etching and solder reflow.
[0143] Clause 21: The method of any of Clauses 17-18 further includes: forming a low wetting layer on at least a portion of the surface of the wetting barrier not covered by the weld post, wherein the low wetting layer has lower weldability than the weld post.
[0144] Clause 22: The method of Clause 21, wherein the low wetting layer is formed of any combination of nickel (Ni), aluminum (Al) and chromium (Cr).
[0145] Clause 23: The method of any of Clauses 21-22, wherein forming the low wetting layer comprises: forming the low wetting layer on the wetting barrier while the first photoresist is still in place, and wherein forming the solder cap comprises: depositing a second photoresist on the first photoresist to cover the low wetting layer; patterning the second photoresist to have a second opening to expose a portion of the surface of the low wetting layer, the width of the second opening being smaller than the width of the first opening; depositing solder material on the exposed portion of the low wetting layer within the second opening; removing the first and second photoresists after depositing the solder material; and performing seed layer etching and solder reflow after removing the first and second photoresists.
[0146] Clause 24: The method of Clause 23, wherein forming the solder cap further comprises: performing a plasma treatment of the wetting barrier after removing the first and second photoresists and before performing seed layer etching and solder reflow.
[0147] Clause 25: The method of any of Clauses 17-18 further includes: forming a contact layer on the wetting barrier such that the contact layer is between the wetting barrier and the solder cap.
[0148] Clause 26: The method of Clause 25, wherein forming the contact layer further comprises: depositing a second photoresist on the first photoresist to cover the low wetting layer; patterning the second photoresist to have a second opening to expose a portion of the surface of the low wetting layer, the width of the second opening being smaller than the width of the first opening; etching the exposed portion of the low wetting layer to expose a portion of the wetting barrier; and forming the contact layer on the exposed portion of the wetting barrier, wherein forming the solder cap comprises: depositing solder material on the contact layer within the second opening; removing the first and second photoresists after depositing the solder material; and performing seed layer etching and solder reflow after removing the first and second photoresists.
[0149] Clause 27: The method of Clause 26, wherein the contact layer is formed by plating nickel (Ni) onto the exposed portion of the wetting barrier.
[0150] Clause 28: The method of Clause 25, wherein the weld post is a first weld post, wherein forming the contact layer comprises: depositing a second photoresist on the first photoresist to cover the low wetting layer; patterning the second photoresist to have a second opening to expose a portion of the surface of the low wetting layer, the width of the second opening being smaller than the width of the first opening; forming a second weld post on the low wetting layer within the second opening; and forming the contact layer on the second weld post, wherein forming the weld cap comprises: depositing solder material on the contact layer within the second opening; removing the first and second photoresists after depositing the solder material; and performing seed layer etching and solder reflow after removing the first and second photoresists.
[0151] Clause 29: The method of Clause 28, wherein the second weld post is formed by plating copper (Cu) on the low wetting layer, or wherein the contact layer is formed by plating nickel (Ni) on the second weld post, or both.
[0152] Clause 30: An integrated circuit (IC) package comprising: a substrate including conductive pads; and an IC structure disposed on the substrate, the IC structure comprising: a die; a bonding post on the die, a first surface of the bonding post facing the die; a wetting barrier on a second surface of the bonding post, the width of the wetting barrier being greater than the width of the bonding post; and a solder cap on the wetting barrier such that the die is electrically coupled to the conductive pads of the substrate at least via the solder cap, the bonding post, and the wetting barrier.
[0153] Clause 31: An IC package as described in Clause 30, wherein the IC structure further includes: a low-wetting layer on at least a portion of the surface of the wetting barrier not covered by the solder pillar, the low-wetting layer having greater solder wetting resistance than the solder pillar.
[0154] Clause 32: An integrated circuit (IC) package comprising: a substrate including conductive pads; and an IC structure disposed on the substrate, the IC structure being any of the IC structures described in Clauses 1-14.
[0155] As used herein, the terms “user equipment” (or “UE”), “user device”, “user terminal”, “client device”, “communication device”, “wireless device”, “wireless communication device”, “handheld device”, “mobile device”, “mobile terminal”, “mobile station”, “handheld device”, “access terminal”, “user equipment”, “user terminal”, “user station”, “terminal”, and variations thereof can be used interchangeably to represent any suitable mobile or stationary device capable of receiving wireless communication and / or navigation signals. These terms include, but are not limited to, music players, video players, entertainment units, navigation devices, communication devices, smartphones, personal digital assistants, fixed-location terminals, tablet computers, computers, wearable devices, laptops, servers, in-vehicle equipment in motor vehicles, and / or other types of portable electronic devices that are typically carried by an individual and / or have communication capabilities (e.g., wireless, cellular, infrared, short-range radio, etc.). These terms are also intended to include devices that communicate with another device capable of receiving wireless communication and / or navigation signals (such as via short-range wireless, infrared, wired connections, or other connections), regardless of whether satellite signal reception, auxiliary data reception, and / or positioning-related processing occur on that device or on that other device. Furthermore, these terms are intended to include all devices, including wireless and wired communication devices capable of communicating with the core network via a radio access network (RAN), and via the core network, the UE can connect to external networks (such as the Internet) and other UEs. Of course, other mechanisms for connecting to the core network and / or the Internet are also possible for the UE, such as on wired access networks, wireless local area networks (WLANs) (e.g., based on IEEE 802.11), etc. The UE can implement this via any of several types of devices, including but not limited to printed circuit (PC) cards, CF memory devices, external or internal modems, wireless or wired telephones, smartphones, tablets, tracking devices, asset tags, etc. The communication link through which the UE can send signals to the RAN is called an uplink channel (e.g., reverse traffic channel, reverse control channel, access channel, etc.). The communication link through which the RAN can send signals to the UE is called a downlink or forward link channel (e.g., paging channel, control channel, broadcast channel, forward traffic channel, etc.). As used herein, the term traffic channel (TCH) can refer to an uplink / reverse traffic channel or a downlink / forward traffic channel.
[0156] Wireless communication between electronic devices can be based on various technologies, such as Code Division Multiple Access (CDMA), W-CDMA, Time Division Multiple Access (TDMA), Frequency Division Multiple Access (FDMA), Orthogonal Frequency Division Multiplexing (OFDM), Global System for Mobile Communications (GSM), 3GPP Long Term Evolution (LTE), 5G New Radio, Bluetooth (BT), Bluetooth Low Energy (BLE), IEEE 802.11 (WiFi) and IEEE 802.15.4 (Zigbee / Thread), or other protocols that can be used in wireless communication networks or data communication networks. Bluetooth Low Energy (also known as Bluetooth LE, BLE, and Bluetooth Smart) is a wireless personal area network technology designed and marketed by the Bluetooth Special Interest Group (SOTUS) to provide significantly reduced power consumption and cost while maintaining similar communication range. BLE was incorporated into the major Bluetooth standard in 2010, using Bluetooth Core Specification version 4.0 and updated in Bluetooth 5.
[0157] The term "exemplary" is used herein to mean "serving as an example, illustration, or representation." Any detail described herein as "exemplary" is not to be construed as superior to other instances. Similarly, the term "example" does not imply that all instances include the features, advantages, or modes of operation discussed. Furthermore, specific features and / or structures may be combined with one or more other features and / or structures. Additionally, at least a portion of the apparatus described herein may be configured to perform at least a portion of the methods described herein.
[0158] It should be noted that the terms “connection,” “coupling,” or any variation thereof mean any direct or indirect connection or coupling between elements, and may cover the presence of an intermediate element between two elements through which the two elements are “connected” or “coupled” together, unless the connection is explicitly disclosed as a direct connection.
[0159] The use of designations such as "first," "second," etc., to refer to elements in this document does not limit the number and / or order of those elements. Rather, these designations are used as a convenient way to distinguish between two or more elements and / or instances of elements. Similarly, unless otherwise stated, a collection of elements may include one or more elements.
[0160] As will be appreciated by those skilled in the art to which this invention pertains, information and signals can be represented using any of a variety of different techniques and skills. For example, data, instructions, commands, information, signals, bits, symbols, and chips that may be referred to throughout the foregoing description can be represented by voltage, current, electromagnetic waves, magnetic fields or magnetic particles, light fields or light particles, or any combination thereof.
[0161] Nothing described or illustrated in this case is intended to designate any part, action, feature, benefit, advantage, or equivalent to be offered to the public, whether or not such part, action, feature, benefit, advantage, or equivalent is described in the claim.
[0162] In the detailed description above, it can be seen that different features are grouped together in the examples. This manner of disclosure should not be construed as reflecting an intention that the claimed example has more features than those explicitly mentioned in the corresponding claim. Rather, the case may include all features less than those of the individual examples disclosed. Therefore, the appended claims should thus be considered as being incorporated into the description, where each claim may be a separate instance. Although each claim may be a separate instance, it should be noted that while dependent claims in the claims may refer to a specific combination having one or more claims, other instances may also cover or include combinations of that dependent claim with the subject matter having any other dependent claims, or combinations of any feature with other dependent and independent claims. Such combinations are presented herein unless it is explicitly stated that no particular combination is intended. Furthermore, it is also intended that features of a claim may be included in any other independent claim, even if the claim is not directly subordinate to that independent claim.
[0163] It should also be noted that the methods, systems, and apparatuses disclosed in this description or claim may be implemented by devices including means for performing corresponding actions and / or functions of the disclosed methods.
[0164] Furthermore, in some instances, an individual action may be subdivided into one or more sub-actions, or may contain one or more sub-actions. Such sub-actions may be included in the disclosure of the individual action or may be part of the disclosure of the individual action.
[0165] Although the foregoing illustrations provide illustrative examples of this case, it should be noted that various changes and modifications may be made without departing from the scope of this case as defined in the appended claims. The functions and / or actions in the method claims of the various examples of this case described herein need not necessarily be performed in any particular order. Furthermore, well-known elements will not be described in detail or may be omitted to avoid obscuring the relevant details of the various forms and examples disclosed herein. Moreover, although elements of this case may be described or claimed in the singular, the plural is also contemplated unless explicitly stated to be limited to the singular.
[0166] 100: IC package 110: Grain 120:Substrate 125: solder pad 130: Die-to-die interconnect 140: Welding column 150: Welding cap 200: IC package 210: Grain 220:Substrate 225: solder pad 230: Die-to-die interconnect 240: Weld column 250: Welding cap 300: IC Structure 310: Grain 330: Die Interconnect 332: Sidewall passivation 340: Copper Pillar 350: Welding cap 400: IC Structure 410: Grain 430: Die-to-die interconnect 440: Weld column 450: Welding cap 460: Wetting Barrier 470: Low wetting layer 500: IC Structure 510: Grain 540: Welding column 550: Welding cap 555: Solder material 560: Wetting Barrier 570: Wetting layer 585: First photoresist 595: Second photoresist 600: IC Structure 610: Grain 640: Welding column 650: Welding cap 655: Solder material 660: Wetting Barrier 685: Second photoresist 695: First photoresist 700: IC Structure 710: Grain 740: Welding column 750: Welding cap 755: Solder material 760: Wetting Barrier 770: Low wetting layer 780: Contact layer 785: First photoresist 795: Second photoresist 800: IC Structure 810: Grain 840: First weld column 850: Welding cap 855: Solder material 860: Wetting Barrier 870: Low wetting layer 880: Contact layer 885: First photoresist 890: Second weld column 895: Second photoresist 900A: IC package 900B: IC package 900C: IC package 900D: IC package 900E: IC package 920:Substrate 925: Conductive pad 1000: Method 1010: Square 1020: Square 1030: Square 1040: Square 1050: Square 1110: Square 1120: Square 1130: Square 1140: Square 1210: Square 1220: Square 1230: Square 1240: Square 1250: Square 1260: Square 1310: Square 1410: Square 1420: Square 1430: Square 1440: Square 1450: Square 1460: Square 1510: Square 1520: Square 1530: Square 1540: Square 1610: Square 1620: Square 1630: Square 1710: Square 1720: Square 1730: Square 1740: Square 1810: Square 1820: Square 1830: Square 1900: Device 1902: Mobile phone equipment 1904: Laptop computer 1906: Fixed-location terminal equipment
[0167] Domestic storage information (please note in order of storage institution, date, and number) none Overseas storage information (please note in the order of storage country, institution, date, and number) none
Claims
1. An integrated circuit (IC) structure, comprising: One grain; The weld post on the grain, a first surface of the weld post facing the grain; A wetting barrier on a second surface of the solder post, the width of the wetting barrier being greater than the width of the solder post; a low wetting layer on at least a portion of a surface of the wetting barrier not covered by the solder post; and a solder cap on the wetting barrier, electrically coupled to a conductive pad of a substrate, such that the die is electrically coupled to the conductive pad of the substrate at least via the solder cap, the solder post, and the wetting barrier, wherein the solder post and the wetting barrier are formed of the same conductive material.
2. The IC structure of claim 1, wherein the low wetting layer has a lower solderability than the solder post.
3. The IC structure as claimed in claim 1, wherein the low wetting layer is formed of any combination of nickel (Ni), aluminum (Al) and chromium (Cr).
4. The IC structure of claim 1, wherein the low wetting layer is formed between the wetting barrier and the solder cap.
5. The IC structure as claimed in claim 4, wherein the solder post is a first solder post, and wherein the IC structure further includes: A second weld post on the low wetting layer; and a contact layer between the second weld post and the weld cap.
6. The IC structure as described in claim 5, wherein the contact layer is formed of nickel (Ni).
7. The IC structure as described in Request 1 further includes: A contact layer between the wetting barrier and the weld cap.
8. The IC structure as claimed in claim 7, wherein the contact layer is formed of nickel (Ni).
9. The IC structure of claim 1, wherein the width of the wetting barrier is greater than the width of the solder cap.
10. The IC structure as claimed in claim 1, wherein the solder pillar and the wetting barrier are formed of copper (Cu).
11. The IC structure of claim 1, wherein the IC structure is incorporated into a device selected from the group consisting of: a music player, a video player, an entertainment unit, a navigation device, a communication device, a mobile device, a mobile phone, a smartphone, a digital assistant, a fixed-location terminal, a tablet computer, a computer, a wearable device, an Internet of Things (IoT) device, a laptop computer, a server, and a motor vehicle.
12. A method of manufacturing an integrated circuit (IC) structure, the method comprising the steps of: forming a solder post on a die, a first surface of the solder post facing the die; forming a wetting barrier on a second surface of the solder post, the width of the wetting barrier being greater than the width of the solder post; forming a low-wetting layer on at least a portion of a surface of the wetting barrier not covered by the solder post; and forming a solder cap on the wetting barrier and electrically coupling it to a conductive pad of a substrate such that the die is electrically coupled to the conductive pad of the substrate at least via the solder cap, the solder post, and the wetting barrier, wherein the solder post and the wetting barrier are formed of the same conductive material.
13. The method of claim 12, wherein forming the weld pillar and forming the wetting barrier comprises the steps of: depositing a first photoresist on the grain; patterning the first photoresist to have a first opening; forming the weld pillar in the first opening such that the second surface of the weld pillar is exposed to a top surface of the first photoresist; and forming the wetting barrier on the exposed second surface of the weld pillar when the first photoresist is in place.
14. The method of claim 13, wherein the weld pillar is formed by plating copper (Cu) in the first opening, or wherein the wetting barrier is formed by plating Cu on the weld pillar, or both.
15. The method of claim 13, wherein forming the solder cap comprises the following steps: depositing a second photoresist on the first photoresist to cover the wetting barrier; patterning the second photoresist to have a second opening to expose a portion of the wetting barrier, the width of the second opening being smaller than the width of the first opening; depositing a solder material on the exposed portion of the wetting barrier within the second opening; removing the first photoresist and the second photoresist after depositing the solder material; and performing a seed layer etching and a solder reflow after removing the first photoresist and the second photoresist.
16. The method of claim 15, wherein forming the solder cap further comprises the steps of: performing a plasma treatment on the wetting barrier after removing the first photoresist and the second photoresist and before performing the seed layer etching and the solder reflow.
17. The method of claim 12, wherein the low wetting layer has a lower weldability than the weld post.
18. The method of claim 12, wherein the low wetting layer is formed of any combination of nickel (Ni), aluminum (Al) and chromium (Cr).
19. The method of claim 12, wherein forming the low-wetting layer comprises the steps of: forming the low-wetting layer on the wetting barrier while the first photoresist is still in place, and wherein forming the solder cap comprises the steps of: depositing a second photoresist on the first photoresist to cover the low-wetting layer; patterning the second photoresist to have a second opening to expose a portion of a surface of the low-wetting layer, the width of the second opening being smaller than the width of the first opening; depositing a solder material on the exposed portion of the low-wetting layer within the second opening; removing the first photoresist and the second photoresist after depositing the solder material; and performing a seed layer etching and a solder reflow after removing the first photoresist and the second photoresist.
20. The method of claim 19, wherein forming the solder cap further comprises the steps of: performing a plasma treatment on the wetting barrier after removing the first photoresist and the second photoresist and before performing the seed layer etching and the solder reflow.
21. The method of claim 12 further includes the step of: forming a contact layer on the wetting barrier such that the contact layer is between the wetting barrier and the solder cap.
22. The method of claim 21, wherein forming the contact layer comprises the steps of: depositing a second photoresist on the first photoresist to cover the low wetting layer; patterning the second photoresist to have a second opening to expose a portion of the surface of the low wetting layer, the width of the second opening being smaller than the width of the first opening; etching the exposed portion of the low wetting layer to expose a portion of the wetting barrier; and forming the contact layer on the exposed portion of the wetting barrier, wherein forming the solder cap comprises the steps of: depositing a solder material on the contact layer within the second opening; removing the first photoresist and the second photoresist after depositing the solder material; and performing a seed layer etching and a solder reflow after removing the first photoresist and the second photoresist.
23. The method of claim 22, wherein the contact layer is formed by plating nickel (Ni) onto the exposed portion of the wetting barrier.
24. The method of claim 21, wherein the weld post is a first weld post, wherein forming the contact layer comprises the steps of: depositing a second photoresist on the first photoresist to cover the low-wetting layer; patterning the second photoresist to have a second opening to expose a portion of a surface of the low-wetting layer, the width of the second opening being smaller than the width of the first opening; forming a second weld post on the low-wetting layer within the second opening; and forming the contact layer on the second weld post, wherein forming the weld cap comprises: A solder material is deposited on the contact layer within the second opening; after depositing the solder material, the first photoresist and the second photoresist are removed; After removing the first photoresist and the second photoresist, a seed layer etching and a solder reflow are performed.
25. The method of claim 24, wherein the second solder post is formed by plating copper (Cu) on the low wetting layer, or wherein the contact layer is formed by plating nickel (Ni) on the second solder post, or both.
26. An integrated circuit (IC) package, comprising: A substrate including a conductive pad; The IC structure disposed on the substrate includes: a die; a bonding post on the die, a first surface of the bonding post facing the die; a wetting barrier on a second surface of the bonding post, the width of the wetting barrier being greater than the width of the bonding post; a low wetting layer on at least a portion of a surface of the wetting barrier not covered by the bonding post; and a solder cap on the wetting barrier, electrically coupled to a conductive pad of a substrate, such that the die is electrically coupled to the conductive pad of the substrate at least via the solder cap, the bonding post, and the wetting barrier, wherein the bonding post and the wetting barrier are formed of the same conductive material.
27. The IC package of claim 26, wherein the low wetting layer has a lower solderability than the solder post.
28. The IC package of claim 26, wherein the solder post is a first solder post, and wherein the IC structure further includes: A second weld post on the low wetting layer; and a contact layer between the second weld post and the weld cap.
29. The IC package as described in claim 26 further includes: A contact layer between the wetting barrier and the weld cap.
30. The IC package of claim 26, wherein the solder pillar and the wetting barrier are formed of copper (Cu).
Citation Information
Patent Citations
Bump structure and forming the same
TW201413896A