Fluorescent tracing polyester Anti-scaling agent, and preparation method and use thereof

The fluorescent tracer polyester scale inhibitor prepared by microwave-assisted two-step method solves the problems of harsh reaction conditions and complicated detection in the existing technology, realizes low-cost and efficient online monitoring and real-time control, and has excellent scale inhibition performance and biodegradability.

WO2024235350A1PCT designated stage expired Publication Date: 2024-11-21LINGNAN NORMAL UNIV

Patent Information

Application Number
PCT/CN2024/101125
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-10
Filing Date
2024-06-25
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing methods for synthesizing fluorescently labeled water treatment agents involve harsh reaction conditions and complex preparation processes, making them unsuitable for industrial production. Furthermore, the concentration detection of traditional water treatment agents is cumbersome, making online monitoring and real-time control difficult.

Method used

A fluorescent tracer polyester scale inhibitor with a six-membered ring structure was prepared by microwave-assisted two-step condensation reaction using citric acid, polyethylene glycol, and amino acids as raw materials. This inhibitor is used to chelate scale-forming ions such as calcium ions in water to form stable complexes, enabling online monitoring and real-time control.

Benefits of technology

The prepared polyester scale inhibitor is low in cost, has good biodegradability, excellent fluorescence properties, can monitor the agent concentration online, reduces water waste, improves production efficiency, and has excellent scale inhibition properties for calcium phosphate and calcium carbonate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024101125_21112024_PF_FP_ABST
    Figure CN2024101125_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a fluorescent tracing polyester anti-scaling agent, and a preparation method and use thereof, belonging to the technical field of water treatment chemicals. Using citric acid, polyethylene glycol and amino acid as raw materials, by means of a two-step condensation reaction, a polyester anti-scaling agent containing a six-membered ring structure is formed, and the average molecular weight of the polyester anti-scaling agent is 1000-5000. The prepared polyester anti-scaling agent is biodegradable, green and environment-friendly, and has a chelating solubilizing effect with scale-forming cations in water and a scale lattice distortion effect, which can be used for preventing sediment formation in circulating cooling water, and thereby achieving the purpose of anti-scaling. The polyester anti-scaling agent has excellent calcium phosphate and / or calcium carbonate anti-scaling properties. The polyester anti-scaling agent has a six-membered conjugated structure, which allows for excellent fluorescence performance, and the fluorescence intensity and concentration of the aqueous solution are directly proportional, such that the anti-scaling agent fluorescence on-line monitoring can be achieved, and the usage amount of the anti-scaling agent can be controlled in real time, so that the operation level of the water treatment device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

A fluorescent tracer polyester scale inhibitor and its preparation method and application Technical Field

[0001] The invention relates to the technical field of treatment agents for circulating cooling water, and in particular to a fluorescent tracer polyester scale inhibitor, a preparation method and application thereof. Background Art

[0002] During the operation of circulating cooling water systems, scaling can reduce heat exchange efficiency and even cause production downtime, resulting in significant economic losses for industrial production. Adding water treatment antiscaling agents to the cooling water is a relatively economical and commonly used method to mitigate scaling. Furthermore, water treatment chemical concentration is a crucial parameter. Traditionally, chemical concentration testing requires sampling and testing, a complex process with numerous interfering factors, making it inadequate for online measurement and real-time control. This can result in concentrations that are too low, rendering them ineffective, or too high, resulting in waste and increased water pollution. Research using fluorescent tracer technology for online detection and automated dosing control of water treatment chemicals is a hot topic in the water treatment chemical industry and has already been implemented. This system can promptly detect insufficient chemical concentration in circulating cooling water systems and quickly implement appropriate measures, achieving the "prevention-first" principle of circulating cooling water treatment. This system maximizes chemical effectiveness and ensures smooth and reliable operation of the circulating water system. It also saves chemical resources, significantly reduces the workload of analytical operators, and improves economic efficiency.

[0003] Currently, two methods are commonly used to synthesize fluorescently labeled water treatment agents. One is to modify a polymer and obtain it by transamidation reaction between an organic fluorescent derivative and the polymer under high temperature and high pressure. This method has harsh reaction conditions and requires the labeled polymer to be resistant to high-temperature decomposition, which limits its further development and application. For example, European Patent EP-A475602 describes a method for preparing fluorescently labeled polyacrylates or polyacrylamides by transamination reaction of tryptophan, a fluorescent substance containing an amino group. The lower limit of the agent concentration can be detected by measuring the fluorescence intensity to 1 ppm. Another method is to copolymerize a monomer containing both a fluorescent group and a polymerizable double bond with other monomers under relatively mild conditions. This method often requires the preparation of a fluorescent monomer containing a double bond, which is complicated to prepare. For example, Chinese Patent CN200910028143.2 describes a fluorescent tracer scale inhibitor and its preparation method. Aqueous solution with a solid content of 20 to 50 wt% is obtained by free radical polymerization of aconitic acid or its salt, a monomer containing an ethylenically unsaturated double bond, and a benzyloxy monomer containing a pyrene fluorescent group. U.S. Patent No. 20040135125A1 discloses a method for preparing a fluorescent group-labeled scale inhibitor. The method first involves reacting naphthalene anhydride with an amine compound containing a polymerizable group, and then copolymerizing the product with other monomers. Environmentally friendly water treatment scale inhibitors are increasingly used, and there is an urgent need to develop online detection technologies for their concentrations. For example, Chinese Patent No. CN102910746 discloses a method for preparing fluorescent polyaspartic acid. Hydroxylated polysuccinimide (which needs to be prepared by reacting polysuccinimide synthesized from aspartic acid polycondensation with monoethanolamine) and N-epoxypropylcarbazole are stirred at 75°C in a nitrogen atmosphere with boron trifluoride etherate catalyst for 4 to 10 hours. The remaining polysuccinimide structural units are then subjected to alkaline hydrolysis, and the polymer is precipitated in ethanol. After vacuum drying, the fluorescent polyaspartic acid is obtained. The prepared fluorescent polyaspartic acid is not easily degraded, is not environmentally friendly, has multiple preparation steps, is complex, and requires an anhydrous environment, making it unsuitable for industrial production.

[0004] Summary of the Invention

[0005] The purpose of the present invention is to address the deficiencies in the prior art and provide a fluorescent tracer polyester scale inhibitor, a preparation method thereof, and an application thereof. The synthesized polyester scale inhibitor has a unique six-membered ring structure, which enables it to produce excellent fluorescent properties. When the polyester scale inhibitor is added to circulating water, the polyester scale inhibitor has a chelating and solubilizing effect, and undergoes a chelating reaction with other scale-forming ions such as calcium ions and magnesium ions in the water, generating a well-water-soluble and relatively stable complex under certain conditions, thereby reducing the concentration of scale-forming ions and preventing acid radical ions from forming deposits with them, thereby achieving the purpose of scale inhibition. Online monitoring and real-time control of the amount of scale inhibitor added can be achieved, thereby reducing the waste of water resources and improving production efficiency.

[0006] The first object of the present invention is to provide a method for preparing a fluorescent tracer polyester scale inhibitor, wherein citric acid, polyethylene glycol and amino acid raw materials are used to form a polyester scale inhibitor containing a six-membered ring structure through a two-step condensation reaction, and the average molecular weight of the polyester scale inhibitor is 1000 to 5000.

[0007] Preferably, the method comprises the following steps:

[0008] After citric acid and polyethylene glycol are evenly mixed, the mixture is placed in a microwave reactor for a first microwave reaction. After the reaction is completed, amino acids are added and stirred evenly, followed by a second microwave reaction. The mixture is dried to obtain a degradable polyester scale inhibitor.

[0009] Preferably, the molar ratio of the citric acid to the polyethylene glycol is 1:1, and the polyethylene glycol is polyethylene glycol 400 and polyethylene glycol 200.

[0010] Preferably, the temperature of the first microwave reaction is 120-160° C., the power is 100-400 W, and the time is 1-5 min.

[0011] Preferably, the amino acid is at least one of L-cysteine, glycine, alanine, valine, leucine, isoleucine, methionine, proline, tryptophan, serine, tyrosine, phenylalanine, asparagine, glutamine, threonine, aspartic acid, glutamic acid, lysine, arginine and histidine.

[0012] Preferably, the molar ratio of the amino acid to citric acid is 0.1 to 1:1.

[0013] Preferably, the temperature of the second microwave reaction is 100-140° C., the power is 100-300 W, and the time is 5-30 min.

[0014] The second object of the present invention is to provide a fluorescent tracer polyester scale inhibitor prepared by the above preparation method.

[0015] The third object of the present invention is to provide the use of the above polyester scale inhibitor in preventing calcium phosphate and calcium carbonate scale in circulating cooling water.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] (1) The present invention uses polyethylene glycol, anhydrous citric acid and amino acids as raw materials to prepare a degradable fluorescent polyester scale inhibitor with intrinsic fluorescent properties through a simple, economical and safe two-step one-pot condensation reaction. The raw materials are cheap and easy to obtain, which greatly reduces the cost of the scale inhibitor and is suitable for industrial production. Nitrogen atoms are inserted into the structure of the polyester scale inhibitor, which is prepared at normal pressure, has a small molecular weight and good water solubility, and therefore has excellent biodegradability and less pollution to the environment. In addition, it contains a unique six-membered ring structure, which enables it to produce excellent fluorescent properties. The concentration of its aqueous solution is directly proportional to the fluorescence intensity, which can realize fluorescent online monitoring and real-time control of the amount of scale inhibitor added, so as to reduce the waste of water resources and scale inhibitors and improve production efficiency.

[0018] (2) The polyester scale inhibitor prepared by the present invention has chelating solubilization and scale lattice distortion effects, and undergoes a chelating reaction with scale-forming cations in water to generate a well-water-soluble and relatively stable complex, and is adsorbed on scale-forming microcrystals to prevent the continuous growth of crystals, thereby achieving the purpose of scale inhibition. It has excellent calcium phosphate and calcium carbonate scale inhibition performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] FIG1 is a nuclear magnetic hydrogen spectrum of the fluorescent tracer polyester scale inhibitor of Example 1 of the present invention;

[0020] FIG2 is an infrared spectrum of the fluorescent tracer polyester scale inhibitor of Example 1 of the present invention;

[0021] FIG3 is a fluorescence spectrum of an aqueous solution of a fluorescent polyester scale inhibitor of different concentrations according to Example 1 of the present invention;

[0022] FIG4 is a linear relationship diagram of the fluorescence intensity and concentration of the fluorescent polyester scale inhibitor aqueous solution in Example 1 of the present invention;

[0023] FIG5 is a scale inhibition rate curve of the fluorescent polyester scale inhibitor to calcium phosphate in Example 1 of the present invention;

[0024] FIG6 is a scale inhibition rate curve of the fluorescent polyester scale inhibitor to calcium carbonate in Example 6 of the present invention;

[0025] FIG7 is a biodegradation rate curve of the fluorescent polyester scale inhibitor of Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0027] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0028] Example 1

[0029] A method for preparing a fluorescent tracer polyester scale inhibitor comprises the following steps:

[0030] 1.5g (7.8mmol) of citric acid and 3.12g of polyethylene glycol 400 (PEG400) were weighed and placed in a 10mL dry beaker. The mixture was placed in a microwave reactor for the first microwave reaction. The microwave power was 200W and the temperature was 160℃ for 1min. After the reaction, 0.66g (5.46mmol) of cysteine ​​was added. After magnetic stirring, the mixture was subjected to a second microwave reaction. The microwave power was 200W and the temperature was 140℃ for 30min. The product was vacuum dried to obtain a fluorescent polyester scale inhibitor. The scale inhibitor had a calcium phosphate scale inhibition rate of 96% at 25mg / L and a 20-day biodegradation rate of 86.1%. The relationship between the fluorescence intensity (F) and concentration (C) of the aqueous solution was: F = 40.84C–4.43, and the square correlation coefficient R 2 =0.9994.

[0031] Example 2

[0032] A method for preparing a fluorescent tracer polyester scale inhibitor comprises the following steps:

[0033] Weigh 1.5g (7.8mmol) of citric acid and 3.12g of PEG400 in a 10mL dry beaker and place them in a microwave reactor for the first microwave reaction. The microwave power is 200W and the temperature is 160℃ for 1min. After the reaction, 0.57g (4.68mmol) of cysteine ​​is added. After magnetic stirring, the second microwave reaction is carried out. The microwave power is 200W and the temperature is 140℃ for 30min. The product is vacuum dried to obtain a fluorescent polyester scale inhibitor. The scale inhibitor has a calcium phosphate scale inhibition rate of 96.4% at 30mg / L and a 20-day biodegradation rate of 88.3%. The relationship between the fluorescence intensity (F) and concentration (C) of the aqueous solution is: F = 34.53C-4.25, and the correlation coefficient square R 2 =0.9987.

[0034] Example 3

[0035] A method for preparing a fluorescent tracer polyester scale inhibitor comprises the following steps:

[0036] Weigh 1.5g (7.8mmol) of citric acid and 3.12g of PEG400 in a 10mL dry beaker and place it in a microwave reactor for the first microwave reaction. The microwave power is 200W and the temperature is 140℃ for 2min. After the reaction, 0.38g (3.12mmol) of cysteine ​​is added. After magnetic stirring, the second microwave reaction is carried out. The microwave power is 200W and the temperature is 140℃ for 30min. The product is vacuum dried to obtain a fluorescent polyester scale inhibitor. The scale inhibitor has a calcium phosphate scale inhibition rate of 95% at 35mg / L and a 20-day biodegradation rate of 92.3%. The relationship between the fluorescence intensity (F) and concentration (C) of the aqueous solution is: F = 30.25C-2.13, and the correlation coefficient square R 2 =0.9984.

[0037] Example 4

[0038] A method for preparing a fluorescent tracer polyester scale inhibitor comprises the following steps:

[0039] 1.5g (7.8mmol) of citric acid and 1.56g of polyethylene glycol 200 (PEG200) were weighed and placed in a 10mL dry beaker. The mixture was placed in a microwave reactor for the first microwave reaction. The microwave power was 200W and the temperature was 140°C for 4 minutes. After the reaction, 0.41g (2.34mmol) of arginine was added. After magnetic stirring, the mixture was subjected to a second microwave reaction. The microwave power was 200W and the temperature was 150°C for 10 minutes. The product was vacuum dried to obtain a fluorescent polyester scale inhibitor. The scale inhibitor had a calcium carbonate scale inhibition rate of 90.6% at 40mg / L and a 20-day biodegradation rate of 83.1%. The relationship between the fluorescence intensity (F) and concentration (C) of the aqueous solution was: F = 37.54C + 3.13, and the square of the correlation coefficient R 2 =0.9988.

[0040] Example 5

[0041] A method for preparing a fluorescent tracer polyester scale inhibitor comprises the following steps:

[0042] Weigh 1.5g (7.8mmol) of citric acid and 3.12g of PEG400 in a 10mL dry beaker and place it in a microwave reactor for the first microwave reaction. The microwave power is 400W and the temperature is 160℃ for 1min. After the reaction, 0.57g (5.46mmol) of serine is added. After magnetic stirring, a second microwave reaction is carried out. The microwave power is 100W and the temperature is 140℃ for 25min. The product is vacuum dried to obtain a fluorescent polyester scale inhibitor. The scale inhibitor has a calcium phosphate scale inhibition rate of 99.6% at 40mg / L and a 20-day biodegradation rate of 87.3%. The relationship between the fluorescence intensity (F) and concentration (C) of the aqueous solution is: F=8.96C, and the square of the correlation coefficient R 2 =0.9972.

[0043] Example 6

[0044] A method for preparing a fluorescent tracer polyester scale inhibitor comprises the following steps:

[0045] Weigh 1.5g (7.8mmol) of citric acid and 3.12g of polyPEG400 in a 10mL dry beaker and place them in a microwave reactor for the first microwave reaction. The microwave power is 100W and the temperature is 140℃ for 5min. After the reaction, 0.62g (4.68mmol) of aspartic acid is added. After magnetic stirring, the second microwave reaction is carried out. The microwave power is 200W and the temperature is 140℃ for 25min. The product is vacuum dried to obtain a fluorescent polyester scale inhibitor. The scale inhibitor has a calcium carbonate scale inhibition rate of 92.3% at 25mg / L and a 20-day biodegradation rate of 82.6%. The relationship between the fluorescence intensity (F) and concentration (C) of the aqueous solution is: F = 32.46C + 4.53, and the square of the correlation coefficient R 2 =0.9983.

[0046] Example 7

[0047] A method for preparing a fluorescent tracer polyester scale inhibitor comprises the following steps:

[0048] Weigh 1.5g (7.8mmol) of citric acid and 3.12g of PEG200 in a 10mL dry beaker and place them in a microwave reactor for the first microwave reaction. The microwave power is 200W and the temperature is 150℃ for 3min. After the reaction is completed, 0.59g (7.8mmol) of glycine is added. After magnetic stirring, a second microwave reaction is carried out. The microwave power is 300W and the temperature is 160℃ for 5min. The product is vacuum dried to obtain a fluorescent polyester scale inhibitor. The scale inhibitor has a phosphate-calcium scale inhibition rate of 95.3% at 30mg / L and a 20-day biodegradation rate of 86.5%. The relationship between the fluorescence intensity (F) and concentration (C) of the aqueous solution is: F = 38.55C + 3.86, and the square of the correlation coefficient R 2 =0.9987.

[0049] Example 8

[0050] A method for preparing a fluorescent tracer polyester scale inhibitor comprises the following steps:

[0051] 1.5g (7.8mmol) of citric acid and 1.56g of PEG200 were weighed and placed in a 10mL dry beaker. The mixture was placed in a microwave reactor for the first microwave reaction. The microwave power was 300W and the temperature was 160°C for 1 minute. After the reaction, 0.74g (6.24mmol) of threonine was added. After magnetic stirring, the mixture was subjected to a second microwave reaction. The microwave power was 200W and the temperature was 150°C for 10 minutes. The product was vacuum dried to obtain a fluorescent polyester scale inhibitor. The scale inhibitor had a calcium phosphate scale inhibition rate of 96.4% at 40mg / L and a 20-day biodegradation rate of 81.4%. The relationship between the fluorescence intensity (F) and concentration (C) of the aqueous solution was: F = 30.57C + 4.25, and the square of the correlation coefficient R was 0. 2 =0.9992.

[0052] Example 9

[0053] A method for preparing a fluorescent tracer polyester scale inhibitor comprises the following steps:

[0054] Weigh 1.5g (7.8mmol) of citric acid and 1.56g of PEG200 in a 10mL dry beaker and place it in a microwave reactor for the first microwave reaction. The microwave power is 200W and the temperature is 130℃ for 5min. After the reaction, 0.46g (3.12mmol) of lysine is added. After magnetic stirring, the second microwave reaction is carried out. The microwave power is 200W and the temperature is 140℃ for 30min. The product is vacuum dried to obtain a fluorescent polyester scale inhibitor. The scale inhibitor has a calcium carbonate scale inhibition rate of 91.3% at 40mg / L and a 20-day biodegradation rate of 75.3%. The relationship between the fluorescence intensity (F) and concentration (C) of the aqueous solution is: F = 36.58C + 3.47, and the square of the correlation coefficient R 2 =0.9989.

[0055] Example 10

[0056] A method for preparing a fluorescent tracer polyester scale inhibitor comprises the following steps:

[0057] 1.5g (7.8mmol) of citric acid and 1.56g of PEG200 were weighed and placed in a 10mL dry beaker. The mixture was placed in a microwave reactor for the first microwave reaction. The microwave power was 200W and the temperature was 150℃ for 3min. After the reaction, 0.57g (3.9mmol) of glutamine was added. After magnetic stirring, the mixture was subjected to a second microwave reaction. The microwave power was 100W and the temperature was 120℃ for 30min. The product was vacuum dried to obtain a fluorescent polyester scale inhibitor. The scale inhibitor had a calcium phosphate scale inhibition rate of 53% at 25mg / L and a 20-day biodegradation rate of 73.2%. The relationship between the fluorescence intensity (F) and concentration (C) of the aqueous solution was: F = 80.66C + 2.37, and the correlation coefficient squared R 2 =0.9986.

[0058] Example 11

[0059] A method for preparing a fluorescent tracer polyester scale inhibitor comprises the following steps:

[0060] Weigh 1.5g (7.8mmol) of citric acid and 3.12g of PEG400 in a 10mL dry beaker and place it in a microwave reactor for the first microwave reaction. The microwave power is 100W and the temperature is 120℃ for 5min. After the reaction, 1.15g (7.8mmol) of glutamic acid is added. After magnetic stirring, a second microwave reaction is carried out. The microwave power is 100W and the temperature is 110℃ for 30min. The product is vacuum dried to obtain a fluorescent polyester scale inhibitor. The scale inhibitor has a calcium carbonate scale inhibition rate of 40.6% at 25mg / L and a 20-day biodegradation rate of 73.7%. The relationship between the fluorescence intensity (F) and concentration (C) of the aqueous solution is: F = 25.51C + 5.03, and the square of the correlation coefficient R 2 =0.9981.

[0061] Figure 1 is the nuclear magnetic resonance hydrogen spectrum of the fluorescent tracer polyester scale inhibitor of Example 1 of the present invention. As can be seen from Figure 1, the two (-CH2) peaks from citric acid are at 2.86ppm and 2.35ppm, the (-CH2) peak from polyethylene glycol is at 3.70ppm, the (-CH2) peak from the six-membered ring is at 4.28ppm, and the (-CH2-SH) peak from L-Cys is at 3.13ppm. The a and b marked in Figure 1 are the peaks of hydrogen on carbon No. 4 when the six-membered ring is not ring-formed, a is the signal peak of hydrogen on carbon No. 4 when the carboxyl group of L-Cys on the right side of the six-membered ring is not dehydrated to form an ester bond with the hydroxyl group on citric acid, and b is the signal peak of hydrogen on carbon No. 4 when the amino group of L-Cys on the left side of the six-membered ring is not dehydrated to form an amide bond with the carboxyl group of citric acid.

[0062] Figure 2 is the infrared spectrum of the fluorescent tracer polyester scale inhibitor of Example 1 of the present invention. As can be seen from Figure 2, at 3448 cm -1 There is an absorption peak at 2879cm -1 There is an absorption peak near 2589cm, indicating the presence of -CH2- groups. -1 The absorption peak at 1719 cm -1 There is an absorption peak, indicating the presence of -C(=O)O- group, 1654cm -1 、1525cm -1 The absorption peak at 1105 cm -1 The presence of an absorption peak indicates the presence of a -C-O-C- group.

[0063] The fluorescence properties of aqueous solutions of fluorescent polyester scale inhibitors with different concentrations were measured under the conditions of excitation wavelength of 350 nm, slit width of 20 nm and voltage of 440 V. The concentrations of the fluorescent polyester scale inhibitors were 1 mg / L, 2 mg / L, 3 mg / L, 6 mg / L, 9 mg / L, 12 mg / L, 15 mg / L, 18 mg / L, 21 mg / L and 24 mg / L, respectively.

[0064] Figure 3 is a fluorescence spectrum of different concentrations of fluorescent polyester scale inhibitor aqueous solution in Example 1 of the present invention. As shown in Figure 3, different concentrations of fluorescent polyester scale inhibitors all emit strong emission peaks at 428nm, and have excellent fluorescence properties. The peak height of different concentrations of fluorescent polyester scale inhibitors at 428nm is plotted against the concentration. Figure 4 is a linear relationship diagram of the fluorescence intensity and concentration of the fluorescent polyester scale inhibitor aqueous solution in Example 1 of the present invention. As shown in Figure 4, the fluorescence intensity and concentration of the fluorescent polyester scale inhibitor aqueous solution are in a good positive linear relationship, where the square of the correlation coefficient R 2 Reached 0.9994.

[0065] 1. Scale inhibition performance of calcium phosphate

[0066] The scale inhibition performance of calcium phosphate is tested by static scale inhibition test method. The scale inhibition test solution composition is: CaCl2 content 250mg / L (calculated as CaCO3), KH2PO4 content 5mg / L (calculated as PO4 3- The scale inhibition test solution was kept in a water bath at 80°C for 10 hours and filtered. The mother liquor was then prepared into ammonium phosphomolybdate solution. The absorbance of the ammonium phosphomolybdate solution prepared from the mother liquor was tested using a visible light spectrophotometer according to the ammonium phosphomolybdate method. The formula Calculate the scale inhibition rate (η) of the scale inhibitor to calcium phosphate. a 、A b They are the absorbance values ​​of blank heated control solution, scale inhibitor added solution, and blank unheated solution. The absorbance values ​​are related to the PO4 3- The content is directly proportional.

[0067] Calcium phosphate scale inhibition performance was tested by preparing scale inhibition test solutions containing the fluorescent scale inhibitor prepared in Example 1 at concentrations of 0, 1, 2, 5, 8, 12, 16, 20, and 24 mg / L. The mother solution was prepared into ammonium phosphomolybdate solution, and the absorbance was measured. The data are listed in Table 1.

[0068] Table 1 Absorbance values ​​of calcium phosphate scale inhibition test

[0069] Note: a Blank heating test solution; bThe blank test solution is not heated.

[0070] Figure 5 shows the scale inhibition rate curve of the fluorescent polyester scale inhibitor against calcium phosphate in Example 1 of the present invention. Within the experimental concentration range, as the concentration of the fluorescent polyester scale inhibitor solvent increases, the scale inhibition rate against Ca₃(PO₄)₂ also gradually increases. At a concentration of 24 mg / L, the scale inhibition rate against calcium phosphate reaches 96.6%.

[0071] 2. Scale inhibition performance of calcium carbonate

[0072] The calcium carbonate scale inhibition test is conducted using a static scale inhibition test method. The scale inhibition test solution consists of: 250 mg / L CaCl2 (calculated as CaCO3), 500 mg / L NaHCO3 (calculated as CaCO3), 152 mg / L Na2B4O7·10H2O, and a certain amount of scale inhibitor. The scale inhibition test solution is placed in a water bath at 80°C for 10 hours, filtered, and then titrated with a standard solution of disodium ethylenediaminetetraacetic acid (EDTA-2Na) to remove the calcium carbonate in the mother solution. 2+ Concentration, according to the formula Calculate the scale inhibition rate (η) of the scale inhibitor to calcium carbonate. a 、V b The volume consumed when EDTA-2Na standard solution is used to titrate blank heated control solution, scale inhibitor, and blank unheated solution respectively (mL). This volume is consistent with the Ca content in the mother liquor after scale inhibition solution filtration. 2+ The concentration is directly proportional.

[0073] Calcium carbonate scale inhibition performance was tested by preparing the fluorescent scale inhibitor prepared in Example 6 at concentrations of 0, 0.5, 1, 2, 4, 8, 12, 16, 20, and 24 mg / L. The mother liquor was titrated with EDTA-2Na standard solution. The volume of EDTA-2Na standard solution consumed is listed in Table 2.

[0074] Table 2 Consumption of EDTA-2Na standard solution volume

[0075] Note: a Heat the test solution for the blank; b The test solution is not heated as blank.

[0076] Figure 6 shows the scale inhibition rate curve of the fluorescent polyester scale inhibitor against calcium carbonate in Example 6 of the present invention. Within the experimental concentration range, the scale inhibition rate against calcium carbonate gradually increases with increasing concentration of the fluorescent polyester scale inhibitor solution. At a concentration of 25 mg / L, the scale inhibition rate against calcium carbonate is 92.3%.

[0077] 3. Biodegradability

[0078] Biodegradability testing was conducted using the shaking table method. ① Phosphate buffer solution: 8.50g KH2PO4, 21.75g ​​K2HPO4, 33.40g Na2HPO4·2H2O, and 1.70g NH4Cl dissolved in distilled water, diluted to 1000mL. ② Inoculum preparation: Activated sludge from a water purification plant was aerated for 48 hours, then allowed to settle for 2 hours. The supernatant was discarded and set aside. ③ The test solution components were: 50mg / L fluorescent tracer polyester scale inhibitor, 55mg / L CaCl2, 22mg / L MgSO4, 80mg / L (NH4)2SO4, 0.6mg / L FeCl3, 2mL / L phosphate buffer, and 20mg / L inoculum. ④ Using the above test solution composition, place 50mL of the test solution in a 100mL Erlenmeyer flask, seal with plastic wrap, and place in a 30°C water bath in a constant-temperature shaker at 120rpm. At the same time, a blank experiment was performed. The chemical oxygen demand (COD) concentration of the samples was measured using the potassium permanganate method on the 1st, 7th, 14th, 21st, and 28th day after the start of the experiment. According to the formula: D (%) = (1-(C t -C bt ) / (C0-C b0 ))×100 to calculate the biodegradation rate (D) of fluorescent tracer polyester scale inhibitor. Where: C t is the COD concentration of the inoculated reaction solution with scale inhibitor added at time t, mg / L; C bt is the COD concentration value of the blank experiment at time t, mg / L; C0 is the initial COD concentration value of the inoculated reaction solution with scale inhibitor added, mg / L; C b0 is the initial COD concentration value of the blank experiment, mg / L.

[0079] Figure 7 shows the biodegradation curve of the fluorescent polyester scale inhibitor of Example 6 of the present invention. The biodegradation rate gradually increases with time. The degradation rate is fast at the beginning and then gradually slows down. At 28 days, the biodegradation rate reaches 92.3%, which is easily degradable.

[0080] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0081] Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if such changes and modifications fall within the scope of the claims and their equivalents, the present invention is intended to include such changes and modifications.

Claims

1. A method for preparing a fluorescent tracer polyester scale inhibitor, characterized in that: The polyester scale inhibitor containing a six-membered ring structure is formed by a two-step condensation reaction using citric acid, polyethylene glycol and amino acid as raw materials. The average molecular weight of the polyester scale inhibitor is 1000-5000.

2. The method for preparing the fluorescent tracer polyester scale inhibitor according to claim 1, characterized in that: The following steps are involved: After citric acid and polyethylene glycol are evenly mixed, the mixture is placed in a microwave reactor for a first microwave reaction. After the reaction is completed, amino acids are added and stirred evenly, and then a second microwave reaction is performed. The mixture is dried to obtain a degradable polyester scale inhibitor.

3. The method for preparing the fluorescent tracer polyester scale inhibitor according to claim 2, characterized in that: The molar ratio of the citric acid to the polyethylene glycol is 1:1, and the polyethylene glycol is polyethylene glycol 400 or polyethylene glycol 200.

4. The method for preparing the fluorescent tracer polyester scale inhibitor according to claim 2, characterized in that: The temperature of the first microwave reaction is 120-160° C., the power is 100-400 W, and the time is 1-5 min.

5. The method for preparing the fluorescent tracer polyester scale inhibitor according to claim 2, characterized in that: The amino acid is at least one of cysteine, glycine, alanine, valine, leucine, isoleucine, methionine, proline, tryptophan, serine, tyrosine, phenylalanine, asparagine, glutamine, threonine, aspartic acid, glutamic acid, lysine, arginine and histidine.

6. The method for preparing the fluorescent tracer polyester scale inhibitor according to claim 2, characterized in that: The molar ratio of the amino acid to citric acid is 0.1 to 1:

1.

7. The method for preparing the fluorescent tracer polyester scale inhibitor according to claim 2, characterized in that: The temperature of the second microwave reaction is 100-140° C., the power is 100-300 W, and the time is 5-30 min.

8. A fluorescent tracer polyester scale inhibitor prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the fluorescent tracer polyester scale inhibitor according to claim 8 in preventing calcium phosphate scale and calcium carbonate scale in circulating cooling water.

Citation Information

Patent Citations

  • Use of branched polyesters based on citric acid as an additive in dish soaps, cleaning agents, detergents, or a formulation for water treatment

    CN104704104A

  • Amino acid fluorescent tracing scale inhibitor and preparation method and application thereof

    CN110117086A

  • Synthesis method and application of glycolic acid polymer and derivative thereof

    CN114456364A

  • Fluorescent tracing polyester scale inhibitor as well as preparation method and application thereof

    CN117126380A

Cited By

  • Novel macromolecular scale inhibitor and preparation method thereof

    CN121517703A