Heat-resistant vinyl ester resin and preparation method therefor

By using phenolic epoxy resin, a combination of polyfunctional epoxy resin and a variety of crosslinking monomers in vinyl ester resin, the crosslinking density and glass transition temperature of the resin are improved, and the thermal deformation temperature in the prior art is solved The problem of insufficient use is achieved in high temperature scenarios above 200°C, and good mechanical and corrosion resistance are maintained.

WO2024250803A1PCT designated stage expired Publication Date: 2024-12-12HUACHANG POLYMER EAST CHINA UNIV OFSCI & TECH

Patent Information

Application Number
PCT/CN2024/083984
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-09
Filing Date
2024-03-27
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

The thermal deformation temperature of existing vinyl ester resins is insufficient and cannot meet the needs of high-temperature scenarios, especially when the long-term working temperature of vinyl ester glass flake cement reaches 100-180℃ and the accident temperature reaches above 200℃.

Method used

Using a combination of vinyl ester resin prepolymer, crosslinking monomer, coupling agent and polymerization inhibitor, the reaction of phenolic epoxy resin and multifunctional epoxy resin is combined to increase the crosslink density and glass transition temperature, and combine it with The combination of a variety of crosslinked monomers such as styrene and trimethylolpropane triacrylate and triallyl cyanate enhances the high temperature resistance of the resin.

Benefits of technology

The glass transition temperature of vinyl ester resin is achieved to reach above 200℃, maintain good mechanical properties and corrosion resistance, and is suitable for high temperature scenarios above 200℃, and the preparation process is low, the process is simple, and suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024083984_12122024_PF_FP_ABST
    Figure CN2024083984_12122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the field of organic polymer compounds, and in particular, to heat-resistant vinyl ester resin and a preparation method therefor. In the present invention, phenolic epoxy resin and low-viscosity multifunctional epoxy resin are specifically selected to be compounded, react with an unsaturated acid, and then be cross-linked with a specific crosslinking monomer. High-temperature resistance of the obtained vinyl ester resin is improved and is far higher than that in the prior art, and the vinyl ester resin can resist a temperature of 200°C and even a temperature of 230°C or above, still has good mechanical properties and corrosion resistance, has moderate viscosity, can adapt to various molding processes and use scenarios, and can meet the use requirements in various fields, thereby further expanding the use range of the heat-resistant vinyl ester resin.
Need to check novelty before this filing date? Find Prior Art

Description

Heat-resistant vinyl ester resin and preparation method thereof Technical Field

[0001] The present invention belongs to the field of organic polymer compounds, in particular to the field under IPC classification number C08L51 / 00, and more specifically to a heat-resistant vinyl ester resin and a preparation method thereof. Background Art

[0002] Vinyl ester resin is obtained by the addition reaction of epoxy resin and unsaturated monocarboxylic acid containing double bonds. It retains the basic chain segments of epoxy resin, which has excellent corrosion resistance and mechanical properties, and also has unsaturated double bonds, which also has good processing properties. Therefore, vinyl ester resin is widely used in the fields of chemical industry, metallurgy, construction, etc., and is often used as anti-corrosion coatings or for the preparation of anti-corrosion products. Among them, high cross-link density phenolic epoxy vinyl ester resin is popular in the market due to its excellent resistance to high temperature, solution, acid and alkali, and oxidation. It is particularly suitable for application scenarios such as desulfurization equipment and high-temperature chimneys.

[0003] However, the thermal deformation temperature of bisphenol A epoxy vinyl ester resin currently on the market can only reach about 110°C, which can no longer meet the use requirements in certain fields. For example, the long-term working temperature of vinyl ester glass flake mortar reaches 100-180°C, and the accident temperature reaches above 200°C. When the use temperature exceeds 180°C, the strength of the mortar decreases, causing peeling and falling accidents. In order to meet the use requirements of high-temperature scenes, it is necessary to develop a vinyl ester resin that can withstand higher temperatures. Prior art CN 109867912B discloses a thermosetting resin composition, which is mainly composed of epoxy resin, unsaturated polyester active ester resin and vinyl benzyl modified phenolic resin. It has the advantages of good dielectric properties, high peel strength and good high temperature resistance, but its glass transition temperature can only reach 170°C at most, which still cannot meet the needs of some current specific use scenarios.

[0004] Summary of the Invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a heat-resistant vinyl ester resin with high cross-linking density, good mechanical properties and corrosion resistance, moderate viscosity, good processing performance, and the ability to withstand high temperatures above 200°C.

[0006] The present invention also aims to provide a method for preparing the above-mentioned heat-resistant vinyl ester resin with low cost, simple process and the ability to be industrially expanded.

[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0008] A heat-resistant vinyl ester resin, the raw materials of which include vinyl ester resin prepolymer, crosslinking monomer, coupling agent and polymerization inhibitor A;

[0009] Preferably, the raw materials of the vinyl ester resin prepolymer include: novolac epoxy resin, multifunctional epoxy resin, unsaturated monocarboxylic acid, catalyst and inhibitor B.

[0010] Preferably, the raw materials include, by weight, 45 to 55 parts of vinyl ester resin prepolymer, 45 to 60 parts of crosslinking monomer, 0.3 to 1 part of coupling agent and 0.02 to 0.05 part of polymerization inhibitor A;

[0011] Preferably, the mass ratio of the vinyl ester resin prepolymer to the cross-linking monomer is 0.8 to 1.2:1.

[0012] Further preferably, the raw materials include 49 to 51 parts of vinyl ester resin prepolymer, 48 to 60 parts of cross-linking monomer, 0.5 to 0.7 parts of coupling agent and 0.03 to 0.04 parts of polymerization inhibitor A in parts by weight.

[0013] Preferably, the vinyl ester resin prepolymer comprises, by weight, 25 to 40 parts of novolac epoxy resin, 4 to 8 parts of multifunctional epoxy resin, 0.015 to 0.03 parts of polymerization inhibitor B, 15 to 20 parts of unsaturated monocarboxylic acid and 0.01 to 0.02 parts of catalyst.

[0014] Preferably, the mass ratio of the novolac epoxy resin to the multifunctional epoxy resin is 5 to 7:1.

[0015] Further preferably, the vinyl ester resin prepolymer comprises, by weight, 27 to 30 parts of novolac epoxy resin, 4 to 6 parts of multifunctional epoxy resin, 0.02 to 0.03 parts of inhibitor B, 16 to 17 parts of unsaturated monocarboxylic acid and 0.5 to 0.6 parts of catalyst.

[0016] Preferably, the epoxy value of the novolac epoxy resin is 0.45 to 0.6 eq / 100 g.

[0017] Preferably, the novolac epoxy resin is selected from one or more of multifunctional o-cresol epoxy resin, bisphenol A novolac epoxy resin, and phenol novolac epoxy resin.

[0018] Preferably, the multifunctional epoxy resin is selected from one or more of AG-70, AG-80, and AFG-90.

[0019] The present invention selects a novolac epoxy resin with an epoxy value of 0.45 to 0.6 eq / 100 g as a raw material. After curing, the crosslinking density is high, and the resin exhibits excellent heat resistance and chemical resistance. However, the resin has a high viscosity and poor processing properties. After crosslinking with a vinyl monomer, the mechanical properties deteriorate significantly, and the toughness decreases, limiting its use. Furthermore, when novolac epoxy resin is used alone to react with an unsaturated carboxylic acid and then crosslink with a vinyl monomer, the glass transition temperature of the cured product can only reach about 170°C, which still cannot meet the use requirements of a higher heat-resistant temperature. The inventors have found in their research that by adding an appropriate amount of multifunctional epoxy resin and novolac epoxy resin to jointly react, the high-temperature resistance of the resulting product has been improved beyond expectations, with the glass transition temperature being able to reach 200°C or even above 230°C, and substantially maintaining good mechanical properties and corrosion resistance. It is speculated that this may be because the viscosity of multifunctional epoxy resin is lower than that of phenolic epoxy resin and it contains more epoxy groups. The multifunctional epoxy resin is doped into the phenolic epoxy resin, which reduces the rigid structure content to a certain extent and increases the cross-linking reaction point, thereby improving the mechanical properties of the cross-linked product. The specific addition amount can control the viscosity of the product within a moderate range, and has good wettability for a variety of materials, improves the synthetic operation performance, and is convenient to use; on the other hand, the multifunctional epoxy resin increases the density of active functional groups in the composite resin, further increases the cross-linking density, and greatly improves the heat resistance temperature of the cross-linked product. At the same time, the dense cross-linking structure also achieves improved corrosion resistance.

[0020] Preferably, the polymerization inhibitor A and the polymerization inhibitor B are independently selected from one or more of tert-butylhydroquinone, p-hydroxyanisole, tert-butylcatechol, p-benzoquinone, hydroquinone and methylhydroquinone.

[0021] Preferably, the polymerization inhibitor B is p-hydroxyanisole.

[0022] Preferably, the polymerization inhibitor A is a combination of two or more of tert-butylhydroquinone, p-hydroxyanisole, tert-butylcatechol, p-benzoquinone, hydroquinone and methylhydroquinone;

[0023] Preferably, the polymerization inhibitor A is a combination of tert-butylcatechol and hydroquinone;

[0024] More preferably, the mass ratio of tert-butylcatechol to hydroquinone is 5.5-6:1.

[0025] Preferably, the unsaturated monocarboxylic acid is selected from acrylic acid, α-butenoic acid, methacrylic acid, crotonic acid, and cinnamic acid.

[0026] Preferably, the catalyst includes one or more of trimethylamine, pyridine, dimethyl sulfide, diethylene glycol dimethyl ether, triphenylphosphine, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyldimethylamine, imidazole, 1-methylimidazole, 2-ethyl-4-methylimidazole, and 2-heptadecylimidazole.

[0027] Preferably, the catalyst is a combination of two or more of trimethylamine, pyridine, dimethyl sulfide, diethylene glycol dimethyl ether, triphenylphosphine, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyldimethylamine, imidazole, 1-methylimidazole, 2-ethyl-4-methylimidazole, and 2-heptadecylimidazole.

[0028] More preferably, the catalyst is a combination of triphenylphosphine and benzyltrimethylammonium chloride.

[0029] More preferably, the mass ratio of triphenylphosphine to benzyltrimethylammonium chloride is 1:3.6-3.7.

[0030] Preferably, the crosslinking monomer is selected from one or more of styrene, vinyltoluene, methyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, lauryl methacrylate, trimethylolpropane triacrylate, triallyl cyanurate, trimethylolpropane tri(methacrylate), pentaerythritol triacrylate and dipentaerythritol hexaacrylate.

[0031] Further preferably, the cross-linking monomer is a combination of styrene and pentaerythritol triacrylate; the mass ratio of styrene to pentaerythritol triacrylate is 1.4 to 2:1;

[0032] More preferably, the cross-linking monomer is a combination of styrene, trimethylolpropane triacrylate and triallyl cyanurate; and the mass ratio of styrene, trimethylolpropane triacrylate and triallyl cyanurate is 6-6.5:3-3.5:1.

[0033] The present invention specifically selects a combination of two or more cross-linking monomers. When styrene and pentaerythritol triacrylate are used as cross-linking monomers, a higher cross-linking density can be achieved compared to using a single cross-linking monomer, raising the glass transition temperature of the vinyl ester resin to above 200°C. The inventors creatively discovered in their research that when a ternary cross-linking monomer of styrene, trimethylolpropane triacrylate, and triallyl cyanurate is selected, the glass transition temperature of the vinyl ester resin is further increased to above 230°C, far exceeding the level of the prior art. The inventors speculate that this may be because the molecular structures of styrene and pentaerythritol triacrylate are quite different, resulting in greater intermolecular forces and slightly lower compatibility; while triallyl cyanurate has similar polarity to styrene and a similar density to trimethylolpropane triacrylate, thereby improving the compatibility of the system, further increasing the cross-linking density, and significantly improving the high-temperature resistance of the vinyl ester resin. At the same time, triallyl cyanurate introduces a triazine group into the system, which can increase heat resistance and thermal oxygen resistance.

[0034] Preferably, the coupling agent is selected from one or more of methyltrimethoxysilane, vinyltrichlorosilane, γ-(methacryloyloxy)propyltrimethoxysilane, maleic acid amidopropyltriethoxysilane, and aminoethylaminopropyltrimethoxysilane.

[0035] Another aspect of the present invention provides a method for preparing the heat-resistant vinyl ester resin, comprising the following steps:

[0036] S1: Novolac epoxy resin, multifunctional epoxy resin, and polymerization inhibitor B are mixed according to weight parts, unsaturated monocarboxylic acid is added, and after stirring evenly, a catalyst is added and the temperature is raised to react to obtain a vinyl ester resin prepolymer;

[0037] S2: adding polymerization inhibitor A, crosslinking monomer and coupling agent to the vinyl ester resin prepolymer, and continuing to stir and react to obtain a heat-resistant vinyl ester resin.

[0038] Preferably, in step S1, the novolac epoxy resin and the multifunctional epoxy resin are first heated to 75-85° C. and melted, and then the polymerization inhibitor B is added and mixed evenly.

[0039] Preferably, the temperature of the temperature-raising reaction in step S1 is 105-120°C;

[0040] Preferably, the heating rate of the temperature-raising reaction is 8-10°C / h, and the final temperature is controlled at 110-120°C.

[0041] Preferably, the specific steps of the temperature reaction are: turning on the cooling water, controlling the heating rate to 8-10°C / h, and controlling the final temperature to 110-120°C; starting from the temperature reaching 110°C, sampling and testing the epoxy value and acid value every 0.5h, and the reaction is terminated when the epoxy value is less than or equal to 0.02eq / 100g and the acid value is less than or equal to 15mgKOH / g, thereby obtaining a vinyl ester resin prepolymer.

[0042] Preferably, in step S2, the vinyl ester resin prepolymer is first cooled to 75-85° C., and then the polymerization inhibitor A, the cross-linking monomer and the coupling agent are added, and the mixture is stirred and reacted for 0.5-1 hour to obtain the heat-resistant vinyl ester resin.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] 1. The heat-resistant vinyl ester resin of the present invention can withstand high temperatures above 200°C, with a maximum temperature of 232.5°C, meeting the needs of various fields and further expanding the scope of application of the heat-resistant vinyl ester resin;

[0045] 2. The heat-resistant vinyl ester resin of the present invention still retains good mechanical properties and has the corrosion resistance of the vinyl ester resin itself, and has higher application value;

[0046] 3. The heat-resistant vinyl ester resin of the present invention has a moderate viscosity of 500 to 700 mPa·s at 25°C, and is adaptable to various composite material molding processes such as hand lay-up, vacuum infusion, RTM, and pultrusion, thereby increasing convenience and universality of use.

[0047] 4. The heat-resistant vinyl ester resin of the present invention has good wetting and adhesion to carbon fiber and glass fiber, which can effectively improve their stability in use and extend the service life of the material;

[0048] 5. The preparation process of the heat-resistant vinyl ester resin used in the present invention is low-cost and simple, can be adapted to large-scale production, and has extremely high industrial value. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] FIG1 is a DSC curve of the heat-resistant vinyl ester resin of Example 1;

[0050] FIG2 is a DSC curve of the heat-resistant vinyl ester resin of Example 2;

[0051] FIG3 is a DSC curve of the heat-resistant vinyl ester resin of Example 3;

[0052] FIG4 is a DSC curve of the heat-resistant vinyl ester resin of Example 4;

[0053] FIG5 is a DSC curve of the heat-resistant vinyl ester resin of Comparative Example 1;

[0054] FIG6 is a DSC curve of the heat-resistant vinyl ester resin of Comparative Example 2;

[0055] FIG7 is an HDT curve of the heat-resistant vinyl ester resin of Example 1;

[0056] FIG8 is an HDT curve of the heat-resistant vinyl ester resin of Example 2;

[0057] FIG9 is an HDT curve of the heat-resistant vinyl ester resin of Example 3;

[0058] FIG10 is an HDT curve of the heat-resistant vinyl ester resin of Example 4;

[0059] FIG11 is a HDT curve of the heat-resistant vinyl ester resin of Comparative Example 1;

[0060] FIG12 is an HDT curve of the heat-resistant vinyl ester resin of Comparative Example 2. DETAILED DESCRIPTION

[0061] Unless otherwise specified, all reagents in the examples of the present invention are from conventional commercial sources.

[0062] Example 1

[0063] This embodiment provides a heat-resistant vinyl ester resin, the raw materials of which are vinyl ester resin prepolymer, crosslinking monomers styrene and pentaerythritol triacrylate, coupling agent γ-(methacryloyloxy)propyltrimethoxysilane, and polymerization inhibitors tert-butylcatechol and hydroquinone;

[0064] The raw materials of the vinyl ester resin prepolymer are: phenol novolac epoxy resin, multifunctional epoxy resin AG-70, methacrylic acid, catalysts triphenylphosphine and benzyltrimethylammonium chloride, and inhibitor p-hydroxyanisole.

[0065] The raw material dosage and preparation method are as follows:

[0066] S1: 275.2 kg of phenol novolac epoxy resin SQPN-048 (purchased from Shandong Shengquan New Materials Co., Ltd.) and 51.9 kg of multifunctional epoxy resin AG-70 (purchased from Shanghai Huayi Resin Co., Ltd.) were put into a reactor, heated to 80 ° C and melted, and then 0.2 kg of p-hydroxyanisole (CAS No.: 150-76-5) was added, kept warm at 80 ± 2 ° C, stirred for 0.5 h, and 162.9 kg of methacrylic acid (CAS No.: 7 9-41-4), stirred evenly, added 1.14 kg of triphenylphosphine (CAS No.: 603-35-0) and 4.17 kg of benzyltrimethylammonium chloride (CAS No.: 56-93-9), turned on the cooling water, controlled the reactor heating rate to 9±1°C / h, and finally the reactor temperature reached 115±2°C. Starting from the temperature reaching 110°C, the epoxy value and acid value were tested every 0.5h. The reaction was terminated when the epoxy value decreased to less than 0.02eq / 100g and the acid value decreased to less than 15mgKOH / g, to obtain a vinyl ester resin prepolymer;

[0067] S2: Cool the vinyl ester resin prepolymer to 80°C, add 0.265 kg of tert-butylcatechol (CAS No.: 27213-78-1), 0.045 kg of hydroquinone (CAS No.: 123-31-9), 293.0 kg of styrene (CAS No.: 100-42-5), 201.3 kg of pentaerythritol triacrylate (CAS No.: 3524-68-3), and 5.1 kg of γ-(methacryloyloxy)propyltrimethoxysilane KH570 (purchased from Jiangxi Chenguang New Materials Co., Ltd.), and continue stirring for 1.0 h to obtain a heat-resistant vinyl ester resin.

[0068] Example 2

[0069] This embodiment provides a heat-resistant vinyl ester resin, the raw materials of which are vinyl ester resin prepolymer, crosslinking monomers styrene and pentaerythritol triacrylate, coupling agent γ-(methacryloyloxy)propyltrimethoxysilane, and polymerization inhibitors tert-butylcatechol and hydroquinone;

[0070] The raw materials of the vinyl ester resin prepolymer are: phenol novolac epoxy resin, multifunctional epoxy resin AG-80, methacrylic acid, catalysts triphenylphosphine and benzyltrimethylammonium chloride, and inhibitor p-hydroxyanisole.

[0071] The raw material dosage and preparation method are as follows:

[0072] S1: 279.7 kg of phenol novolac epoxy resin SQPN-048 (purchased from Shandong Shengquan New Materials Co., Ltd.) and 45.8 kg of multifunctional epoxy resin AG-80 (purchased from Shanghai Huayi Resin Co., Ltd.) were put into a reactor, heated to 80° C. and melted, and then 0.23 kg of p-hydroxyanisole was added, kept warm at 80±2° C., stirred for 0.5 h, 165.4 kg of methacrylic acid was added, stirred evenly, 1.15 kg of triphenylphosphine and 4.23 kg of benzyltrimethylammonium chloride were added, the cooling water was turned on, and the heating rate of the reactor was controlled to 9±1° C. / h, and the final reactor temperature reached 115±2° C. Starting from the temperature reaching 110° C., the epoxy value and acid value were tested every 0.5 h. The reaction endpoint was when the epoxy value decreased to below 0.02 eq / 100 g and the acid value decreased to below 15 mg KOH / g, to obtain a vinyl ester resin prepolymer;

[0073] S2: Cool the vinyl ester resin prepolymer to 80°C, add 0.27 kg of tert-butylcatechol, 0.046 kg of hydroquinone, 386.7 kg of styrene, 204.4 kg of pentaerythritol triacrylate, and 6.7 kg of γ-(methacryloyloxy)propyltrimethoxysilane KH570 (purchased from Jiangxi Chenguang New Materials Co., Ltd.), and continue stirring for 1.0 h to obtain a heat-resistant vinyl ester resin.

[0074] Example 3

[0075] This embodiment provides a heat-resistant vinyl ester resin, the raw materials of which are vinyl ester resin prepolymer, crosslinking monomers styrene, trimethylolpropane triacrylate and triallyl cyanurate, coupling agent γ-(methacryloyloxy)propyltrimethoxysilane, and polymerization inhibitors tert-butylcatechol and hydroquinone;

[0076] The raw materials of the vinyl ester resin prepolymer are: bisphenol A novolac epoxy resin SQAN-203, multifunctional epoxy resin AG-70, methacrylic acid, catalysts triphenylphosphine and benzyltrimethylammonium chloride, and inhibitor p-hydroxyanisole.

[0077] The raw material dosage and preparation method are as follows:

[0078] S1: 297 kg of bisphenol A novolac epoxy resin SQAN-203 (purchased from Shandong Shengquan New Materials Co., Ltd.) and 45.8 kg of multifunctional epoxy resin AG-70 (purchased from Shanghai Huayi Resin Co., Ltd.) were put into a reactor, heated to 80° C. and melted, and then 0.22 kg of p-hydroxyanisole was added. The mixture was kept warm at 80±2° C. and stirred for 0.5 h. 160.4 kg of methacrylic acid was added and stirred evenly. 1.12 kg of triphenylphosphine and 4.10 kg of benzyltrimethylammonium chloride were added. The cooling water was turned on and the heating rate of the reactor was controlled to 9±1° C. / h. The final reactor temperature reached 115±2° C. From the time the temperature reached 110° C., the epoxy value and acid value were tested every 0.5 h. The reaction was terminated when the epoxy value decreased to below 0.02 eq / 100 g and the acid value decreased to below 15 mg KOH / g, thereby obtaining a vinyl ester resin prepolymer.

[0079] S2: Cool the vinyl ester resin prepolymer to 80°C, add 0.26 kg of tert-butylcatechol, 0.045 kg of hydroquinone, 288.6 kg of styrene, 150.9 kg of trimethylolpropane triacrylate, 47.4 kg of triallyl cyanurate, and 5.0 kg of γ-(methacryloyloxy)propyltrimethoxysilane KH570 (purchased from Jiangxi Chenguang New Materials Co., Ltd.) and continue stirring for 1.0 h to obtain a heat-resistant vinyl ester resin.

[0080] Example 4

[0081] This embodiment provides a heat-resistant vinyl ester resin, the raw materials of which are vinyl ester resin prepolymer, crosslinking monomers styrene, trimethylolpropane triacrylate and triallyl cyanurate, coupling agent γ-(methacryloyloxy)propyltrimethoxysilane, and polymerization inhibitors tert-butylcatechol and hydroquinone;

[0082] The raw materials of the vinyl ester resin prepolymer are: bisphenol A novolac epoxy resin SQAN-203, multifunctional epoxy resin AG-80, methacrylic acid, catalysts triphenylphosphine and benzyltrimethylammonium chloride, and inhibitor p-hydroxyanisole.

[0083] The raw material dosage and preparation method are as follows:

[0084] S1: 299.2 kg of bisphenol A novolac epoxy resin SQAN-203 (purchased from Shandong Shengquan New Materials Co., Ltd.) and 44.7 kg of multifunctional epoxy resin AG-80 (purchased from Shanghai Huayi Resin Co., Ltd.) were put into a reactor, heated to 80° C. and melted, and then 0.22 kg of p-hydroxyanisole was added. The mixture was kept warm at 80±2° C. and stirred for 0.5 h. 161.7 kg of methacrylic acid was added and stirred evenly. 1.13 kg of triphenylphosphine and 4.14 kg of benzyltrimethylammonium chloride were added. The cooling water was turned on and the heating rate of the reactor was controlled to 9±1° C. / h. The final reactor temperature reached 115±2° C. Starting from the temperature reaching 110° C., the epoxy value and acid value were tested every 0.5 h. The reaction was terminated when the epoxy value decreased to below 0.02 eq / 100 g and the acid value decreased to below 15 mg KOH / g, thereby obtaining a vinyl ester resin prepolymer.

[0085] S2: Cool the vinyl ester resin prepolymer to 80°C, add 0.26 kg of tert-butylcatechol, 0.045 kg of hydroquinone, 288.6 kg of styrene, 150.9 kg of trimethylolpropane triacrylate, 47.4 kg of triallyl cyanurate, and 5.0 kg of γ-(methacryloyloxy)propyltrimethoxysilane KH570 (purchased from Jiangxi Chenguang New Materials Co., Ltd.) and continue stirring for 1.0 h to obtain a heat-resistant vinyl ester resin.

[0086] Comparative Example 1

[0087] This embodiment provides a heat-resistant vinyl ester resin, the raw materials of which are vinyl ester resin prepolymer, crosslinking monomers styrene, trimethylolpropane triacrylate and triallyl cyanurate, coupling agent γ-(methacryloyloxy)propyltrimethoxysilane, and polymerization inhibitors tert-butylcatechol and hydroquinone;

[0088] The raw materials of the vinyl ester resin prepolymer are: epoxy resin NPEL-128, methacrylic acid, and catalyst benzyltrimethylammonium chloride.

[0089] The raw material dosage and preparation method are as follows:

[0090] S1: 361.5 kg of epoxy resin NPEL-128 was added to a reactor, heated to 80°C and melted, and then 158.5 kg of methacrylic acid was added, kept warm at 80±2°C, stirred for 0.5 h, and 0.92 kg of benzyltrimethylammonium chloride was added. The cooling water was turned on, and the heating rate of the reactor was controlled to 9±1°C / h. The final reactor temperature reached 115±2°C. After the temperature reached 100°C, the epoxy value and acid value were tested every 0.5 h. The reaction was terminated when the epoxy value dropped below 0.02 eq / 100 g and the acid value dropped below 15 mg KOH / g, thereby obtaining a vinyl ester resin prepolymer.

[0091] S2: Cool the vinyl ester resin prepolymer to 80°C, add 0.32 kg of tert-butylcatechol, 0.06 kg of hydroquinone, 281.1 kg of styrene, 145.6 kg of trimethylolpropane triacrylate, 46.1 kg of triallyl cyanurate, and 5.8 kg of γ-(methacryloyloxy)propyltrimethoxysilane KH570, and continue stirring for 1.0 h to obtain a heat-resistant vinyl ester resin.

[0092] Comparative Example 2

[0093] This embodiment provides a heat-resistant vinyl ester resin, the raw materials of which are vinyl ester resin prepolymer, crosslinking monomers styrene, trimethylolpropane triacrylate and triallyl cyanurate, coupling agent γ-(methacryloyloxy)propyltrimethoxysilane, and polymerization inhibitors tert-butylcatechol and hydroquinone;

[0094] The raw materials of the vinyl ester resin prepolymer are: phenolic epoxy resin NPPN-638S, methacrylic acid, and catalyst benzyltrimethylammonium chloride.

[0095] The raw material dosage and preparation method are as follows:

[0096] S1: 344.3 kg of phenolic epoxy resin NPPN-638S was added to a reactor, heated to 80°C and melted, and then 162.9 kg of methacrylic acid was added. The temperature was kept at 80±2°C and stirred for 0.5 h. 3.95 kg of benzyltrimethylammonium chloride was added. The cooling water was turned on and the heating rate of the reactor was controlled to 9±1°C / h. The final reactor temperature reached 115±2°C. After the temperature reached 100°C, the epoxy value and acid value were tested every 0.5 h. The reaction was terminated when the epoxy value dropped below 0.02 eq / 100 g and the acid value dropped below 15 mg KOH / g, thereby obtaining a vinyl ester resin prepolymer.

[0097] S2: Cool the vinyl ester resin prepolymer to 80°C, add 0.33 kg of tert-butylcatechol, 0.06 kg of hydroquinone, 288.8 kg of styrene, 149.6 kg of trimethylolpropane triacrylate, 47.3 kg of triallyl cyanurate, and 6.0 kg of γ-(methacryloyloxy)propyltrimethoxysilane KH570, and continue stirring for 1.0 h to obtain a heat-resistant vinyl ester resin.

[0098] Performance Testing

[0099] 1. The mechanical properties and heat resistance of the heat-resistant vinyl ester resins of Examples 1-4 and Comparative Examples 1-2 were tested. The test methods and results are shown in Table 1. Six parallel samples of the heat-resistant vinyl ester resins of each Example and Comparative Example were prepared, and the average value was calculated. The DSC curves and HDT curves of the heat-resistant vinyl ester resins of Examples 1-4 and Comparative Examples 1-2 are shown in Figures 1-12, respectively.

[0100] Table 1

[0101] 2. Corrosion resistance test

[0102] Corrosion resistance testing was conducted in accordance with industry standard HG / T 5876-2021: The heat-resistant vinyl ester resins of Examples 1 to 4 and Comparative Examples 1 to 2 were cured into pure resin castings. Bend bars and 50*50mm specimens were then prepared in accordance with GB / T 2567-2008. These specimens were immersed in corrosive media (distilled water, toluene, 30% hydrochloric acid, and 50% sulfuric acid) to evaluate their corrosion resistance. The evaluation method consisted of removing the specimens at regular intervals to observe their appearance and testing their weight change rate, flexural strength and modulus, and Barcol hardness. The results of the toluene immersion test at 25°C are reported in Table 2, the results of the distilled water immersion test at 100°C are reported in Table 3, the results of the 30% hydrochloric acid immersion test at 40°C are reported in Table 4, and the results of the 50% sulfuric acid immersion test at 60°C are reported in Table 5.

[0103] Table 2

[0104] According to the evaluation criteria of the industry standard HG / T 5876-2021, the heat-resistant vinyl ester resins of Examples 1 to 4 and Comparative Examples 1 to 2 are resistant to toluene solvent at room temperature (25°C) within 30 days, that is, the heat-resistant vinyl ester resins of Examples 1 to 4 still maintain good toluene resistance.

[0105] Table 3

[0106] According to the evaluation criteria of the industry standard HG / T 5876-2021, the heat-resistant vinyl ester resins of Examples 1 to 4 can withstand immersion in distilled water at 100°C within 30 days, while the heat-resistant vinyl ester resins of Comparative Examples 1 to 2 are moderately resistant.

[0107] Table 4

[0108] According to the evaluation criteria of the industry standard HG / T 5876-2021, the heat-resistant vinyl ester resins of Examples 1 to 4 and Comparative Examples 1 to 2 can withstand immersion in 30% hydrochloric acid at 40°C within 30 days.

[0109] Table 5

[0110] According to the evaluation criteria of the industry standard HG / T 5876-2021, the heat-resistant vinyl ester resins of Examples 1 to 4 can withstand 50% sulfuric acid immersion at 60°C within 30 days, while Comparative Examples 1 to 2 are relatively resistant.

Claims

1. A heat-resistant vinyl ester resin, characterized in that: Its raw materials include vinyl ester resin prepolymer, cross-linking monomer, coupling agent and inhibitor A; The raw materials of the vinyl ester resin prepolymer include: phenolic epoxy resin, multifunctional epoxy resin, unsaturated monocarboxylic acid, catalyst and inhibitor B.

2. The heat-resistant vinyl ester resin according to claim 1, characterized in that The raw materials include, by weight, 45 to 55 parts of vinyl ester resin prepolymer, 45 to 60 parts of crosslinking monomer, 0.3 to 1 part of coupling agent and 0.02 to 0.05 part of inhibitor A; The vinyl ester resin prepolymer comprises, by weight, 25 to 40 parts of phenolic epoxy resin, 4 to 8 parts of multifunctional epoxy resin, 0.015 to 0.03 parts of inhibitor B, 15 to 20 parts of unsaturated monocarboxylic acid and 0.5 to 1 part of catalyst.

3. The heat-resistant vinyl ester resin according to claim 1 or 2, characterized in that: The epoxy value of the phenolic epoxy resin is 0.45 to 0.6 eq / 100 g.

4. The heat-resistant vinyl ester resin according to claim 3, characterized in that The novolac epoxy resin is selected from one or more of multifunctional o-cresol epoxy resin, bisphenol A novolac epoxy resin and phenol novolac epoxy resin.

5. The heat-resistant vinyl ester resin according to claim 1 or 2, characterized in that: The multifunctional epoxy resin is selected from one or more of AG-70, AG-80 and AFG-90.

6. The heat-resistant vinyl ester resin according to claim 1 or 2, characterized in that: The crosslinking monomer is selected from one or more of styrene, vinyl toluene, methyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, lauryl methacrylate, trimethylolpropane triacrylate, triallyl cyanurate, trimethylolpropane tri(methacrylate), pentaerythritol triacrylate and dipentaerythritol hexaacrylate.

7. The heat-resistant vinyl ester resin according to claim 1 or 2, characterized in that: The polymerization inhibitor A and the polymerization inhibitor B are independently selected from one or more of tert-butylhydroquinone, p-hydroxyanisole, tert-butylcatechol, p-benzoquinone, hydroquinone and methylhydroquinone.

8. The heat-resistant vinyl ester resin according to claim 1 or 2, characterized in that: The catalyst includes one or more of trimethylamine, pyridine, dimethyl sulfide, diethylene glycol dimethyl ether, triphenylphosphine, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyldimethylamine, imidazole, 1-methylimidazole, 2-ethyl-4-methylimidazole, and 2-heptadecylimidazole.

9. A method for preparing a heat-resistant vinyl ester resin according to any one of claims 1 to 8, characterized in that: The steps include: S1: mixing phenolic epoxy resin, multifunctional epoxy resin and polymerization inhibitor B according to weight parts, adding unsaturated monocarboxylic acid, stirring evenly, adding catalyst, heating and reacting to obtain vinyl ester resin prepolymer; S2: adding inhibitor A, crosslinking monomer and coupling agent to the vinyl ester resin prepolymer, and continuing to stir and react to obtain a heat-resistant vinyl ester resin.

10. The method for preparing a heat-resistant vinyl ester resin according to claim 9, characterized in that: The temperature of the heating reaction in step S1 is 105-120°C.

Citation Information

Patent Citations

  • A thermosetting resin composition and prepregs and laminates prepared therefrom

    CN109867912B

  • Modified high-temperature-resistant epoxy vinyl ester resin and glass flake daub thereof

    CN116554696A

  • Heat-resistant vinyl ester resin and preparation method thereof

    CN116804074A

  • Halogen-free flame-retardant vinyl ester resin, preparation method thereof and composite resin

    CN116948145A

  • Vinyl ester resin, vinyl ester resin composition, and its cured product

    JP2004067815A

Cited By

  • Cured substance of phosphonium styryl modified unsaturated resin and preparation method of cured substance

    CN119505177A