Method for preparing layers of non-stoichiometric palladium oxide
The method of dissolving palladium (II) salts, aging, and low-temperature curing with stabilizing agents and initiators effectively synthesizes non-stoichiometric palladium oxide layers, overcoming the challenge of Pd(0) formation, resulting in ultra-thin, conductive, and stable PdOx films for photovoltaic applications.
Patent Information
- Application Number
- PCT/ES2024/070350
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-08
- Filing Date
- 2024-06-05
- Publication Date
- 2024-12-12
AI Technical Summary
Current methods for preparing non-stoichiometric palladium oxide layers face challenges in achieving low-temperature synthesis without forming metallic Pd(0), which is necessary for producing ultra-thin, homogeneous, and continuous films suitable for photovoltaic applications, as high temperatures often result in the formation of Pd(0) and compromise semiconductor properties.
A method involving the dissolution of a palladium (II) salt in a solvent, followed by aging and deposition on a substrate, with thermal or ultraviolet curing at low temperatures to form non-stoichiometric palladium oxide layers, using stabilizing agents and initiators to prevent Pd(0) formation, allowing for the synthesis of ultra-thin, electrically conductive, and transparent PdOx layers.
This method enables the production of ultra-thin, transparent, and conductive PdOx layers with excellent electrical properties, suitable for photovoltaic and optoelectronic applications, while avoiding the formation of Pd(0) and ensuring the layers are homogeneous and continuous, thus preventing short circuits and enhancing device stability.
Smart Images

Figure ES2024070350_12122024_PF_FP_ABST
Abstract
Description
NON-STOICHIOMETRIC PALLADIUM OXIDE LAYER PREPARATION METHOD FIELD OF TECHNIQUE The present invention relates to a method for preparing non-stoichiometric palladium oxide layers. The present invention also relates to non-stoichiometric palladium oxide layers and uses of said layers, particularly in photovoltaic, optoelectronic, catalytic, and sensor applications. BACKGROUND OF THE INVENTION Metal halide perovskites possess unique properties as light-harvesting active materials, such as the fact that they can be synthesized in situ as thin films very easily and inexpensively. As a result, their use in photovoltaic cell manufacturing has generated significant interest due to the rapid increase in solar conversion efficiency since 2012. Currently, the record conversion efficiency exceeds 25%, surpassing not only other emerging photovoltaic technologies but also more dominant thin-film photovoltaic technologies, such as Si, CIGS, and CdTe thin-film solar cells. Typically, a solar cell has a sandwich configuration consisting of multiple layers of thin films including an electron transport layer (ETL), a light harvesting layer (perovskite semiconductor) and a hole transport layer (HTL) as well as electrodes such as anodes and cathodes for extracting the charges generated in the light harvesting layer. The first metal halide perovskite solar cells (PSCs) had a structure very similar to a dye-sensitized solar cell (DSSC). Thus, mesoporous T¡Ü2 is deposited on a transparent fluorine-doped tin oxide electrode (Fluorine Tin Oxide), acting as an electron-selective transport layer (ETL). The perovskite is then deposited, on which 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (spiro-OMeTAD) is deposited, acting as a hole-transport layer (HTL). The presence of selective electron and hole transport layers is essential to prevent electron-hole pair recombination once the photovoltaic material interacts with light. Depending on the arrangement of the ETL, HTL, and perovskite, there are different types of PSCs, such as conventional (NIP-type) versus inverted (PIN-type) cells, and mesoscopic (with a mesoporous TiCh layer) versus planar ones. Most mesoscopic devices use the conventional NIP-type architecture. Mesoscopic architectures generally have an advantage in terms of efficiency and stability. However, the formation of mesoporous TiO2 layers requires very high processing temperatures above 400°C to eliminate organic compounds and improve the crystallinity of the TiCh. These high temperatures also limit the type of solar cell architecture to conventional NIP-type cells, where the perovskite is deposited on the mesoporous material once heated.Inverted cells, this approach could not be used, as the mesoporous oxide would be deposited on the perovskite and heated, which cannot withstand high temperatures. Furthermore, there is solvent incompatibility, as the mesoporous oxide precursor is dissolved in polar solvents, typically alcohols, which are incompatible with perovskites. However, planar devices lack a mesoscopic layer and are significantly simpler to fabricate since they do not require heating to high temperatures. While studies on mesoscopic layers synthesized with low deposition temperatures have been published, most mesoscopic devices require a high processing temperature. In contrast, many more studies have been published on the low-temperature deposition of planar metal oxides. Moreover, the published efficiencies of planar devices have been increasing, reaching efficiencies exceeding 23% for conventional and inverted planar PSCs. Therefore, although mesoscopic cells still retain a performance advantage, the performance gap between mesoscopic and planar devices has narrowed in recent years, leading to a growing interest in planar devices. As a result, the issue of planar versus mesoscopic architecture is not considered as important.Furthermore, planar architectures using metal oxides with low processing temperatures are of great interest for flexible PSC applications, where flexible PET and PEN plastic substrates are used that do not withstand temperatures higher than 150 and 190°C respectively. While the maximum theoretical efficiency of perovskite solar cells has not yet been achieved, in recent years the focus of research has shifted from improving efficiency to improving device stability. PSCs typically exhibit accelerated performance decline under harsh environmental conditions, when exposed to lighting (especially high UV light), high temperature, and relative humidity (RH). There is, therefore, growing interest in improving the stability of PSCs. Among the charge-selective layers (CTLs), organic HTLs and ETLs are strongly affected by both low-voltage light and high temperatures and humidity. Therefore, the main motivation for using metal oxides is to improve stability, since fully inorganic materials generally show greater resistance to environmental conditions (low-voltage, high temperature, and high humidity). There are studies that demonstrate the stability advantage of CTL of metal oxides when compared to moisture-sensitive organic materials, such as poly(3,4-ethylenedioxythiophene):polyester(styrenesulfonic acid) (PEDOT:PSS), phenyl-C61-butyric acid methyl ester (PCBM)
[0015] and Spiro-OMeTAD. Furthermore, organic materials that require dopants, such as Spiro-OMeTAD, can result in lower stability at elevated temperatures or under illumination, i.e., conditions conducive to dopant diffusion. A good charge-selective transport layer (CTL) should exhibit favorable valence (V) and conduction (C) band energy level alignment with the perovskite for efficient electron and hole extraction, have good electron and hole mobility allowing efficient electron and hole extraction, have low optical absorption (visible transparent to maximize solar radiation reaching the perovskite), and should also result in low interfacial defects, and consequently low electron-hole recombination losses, at the interfaces. Many different metal oxides can satisfy the first three conditions. A major advantage of metal oxides (MOs) is that they are highly dispersed in the perovskite.X ) is that they are semiconductors that present different bandwidths, with valence bands (BV) and conduction bands (BC) at different energies depending on the metal that forms the metal oxide. This is extremely important for applications in photovoltaics and optoelectronics in general because it allows the energy levels of the BV and BC to be adjusted with respect to the active material (i.e. photovoltaic material) so that the MOs X can selectively conduct electrons or holes as efficiently as possible. This has a huge impact on device performance, for example, increasing solar energy conversion efficiency. In addition, the MOs X They can be prepared using a variety of methods from low-cost precursors, and many of these methods are compatible with low-cost processing. temperature (although this depends on the material, with some oxides being more likely to produce high-quality films processed at low temperatures compared to others). Typically, the most problematic part of preparing a good CTC is achieving low interfacial defects and low recombination losses at the interfaces. Furthermore, the crystal quality of the perovskite is significantly affected by the underlying CTC. For example, the contact angle of the CTC for the perovskite solution affects surface wetting and, consequently, perovskite nucleation and film growth. A useful parameter for characterizing the interface between the different charge transport layers and the perovskite is the surface recombination rate, with a lower surface recombination rate generally resulting in better performance.Some common charge transport layers, such as T¡O2 and NiOx, were found to have small surface recombination rates, consistent with efficient solar cells. However, it should be noted that, depending on the deposition conditions, the surface recombination rate for the same material can vary significantly. Overall, the interfaces within the device are key to understanding the correlations between PSC performance and CTL options. Currently, there are n-type metal oxide semiconductors that can selectively conduct electrons or p-type semiconductors that conduct holes. For example, the most commonly used n-type semiconductors are TiCh, ZnO, SnO2, and CeO. x . On the other hand, the most commonly used p-type semiconductors are non-stoichiometric metal oxides such as NiOx, V2O5, CuOx, CoOx, Cr3C>4, MoO x , MnO x . The search for new inorganic materials for use as HTL and ETL is ongoing, aiming to improve both PSC efficiency and stability. PdO x It is a p-type semiconductor mainly used as a catalyst for the dehydrogenation of organic liquids (important for H2 storage and its release), for the electrochemical reduction of CO2 to other molecules, decomposition of harmful gases in automobiles and as a resistive sensor. However, there are no studies on its use as HTL. PdOx is a non-stoichiometric metal oxide since Pd can have oxidation states Pd(0, II and IV). The presence of Pd(0), a metal, means that its semiconductor properties can be compromised, hence there is some reluctance to use PdO. xas HTL. In fact, if one searches the literature for information about its physical properties, one can see a great disparity in values for its bandwidth, which can range from 0 to 2.67 eV. (Phys. Chem. Chem. Phys., 2011 , 13, 15947- 15954. DOI 10.1039 / c1cp20923j). This is mainly due to the presence of Pd(O, II and IV). Its narrow bandwidth makes PdO x absorbs in the visible spectrum, so to obtain transparent films (>80% between 400-900 nm) ultra-thin layers (<50 nm) must be used. These ultra-thin layers must be homogeneous and continuous to avoid the generation of pinholes (small craters that form in the film during its drying process) that would cause short circuits in the device. Therefore, it is important to develop a method for the synthesis of ultra-thin layers of PdO. xwhere mainly Pd(ll) and Pd(IV) oxide are formed but Pd(0) is not formed (or is formed in a very small way). Most metal oxides can be synthesized by wet chemistry in the form of nanoparticles, which are then deposited as a thin layer. There are also other methods for direct synthesis of MO layers. X such as chemical vapor deposition, which involves several steps and is often laborious and tedious. However, one of the most promising methods is the in-situ synthesis of MO thin films. X by deposition of precursor solutions using standard deposition techniques such as spin coating, dip coating, Dr. Blade, ink jet printing, and subsequent thermal curing. However, the formation of metal oxides typically requires high temperatures, typically above 300–400°C. There are several methods for the synthesis of PdO. x. For example, the document “Microstructure and electrical properties of palladium oxide thin films for oxidizing gases detection” (Thin Solid Films, vol. 636 (2017)) describes the deposition of Pd(0) film by evaporation of a Pd(0) sheet and subsequent oxidation to PdO in the presence of O2 at temperatures between 500 and 800 °C, which makes it incompatible with flexible and thermolabile substrates. US 2014 / 0079954A1 describes a non-catalytic palladium precursor composition including a palladium salt and an organic amine, the composition being water-free. This composition enables the use of solution processing methods to form a palladium layer on a wide variety of substrates. In particular, this patent application describes an electronic device comprising a substrate and a palladium layer. This palladium layer has been formed by solution deposition of a non-catalytic palladium precursor composition and heating it to form the layer. Furthermore, the precursor composition comprises a palladium salt and an organic amine forming a complex, and wherein the total number of carbon atoms in the palladium salt and the organic amine combined are at least 12 (see claim 1). In a In another embodiment, this document refers to a solution of 0.2 M palladium acetate and 2 M octanoamine in toluene, which is deposited by spin coating on a glass slide to form a film and heated at 200-250 °C for a few minutes. The film first changed to black, then to a bright metallic color of very conductive metallic Pd(0) with a typically metallic conductivity of 104 S / cm. In this document, amines are used to dissolve high concentrations of Pd(AcO)2 and to produce thick films of Pd(AcO)2 for the subsequent formation of metallic Pd(0) films. The amines act as a reducing agent of Pd(II) to Pd(O). Large thicknesses are necessary because during the reduction of Pd(AcO)2 to Pd(O) for the formation of Pd films, significant shrinkage of the film occurs due to the change in density of Pd(AcO)2 (2.19 g / cm 3 ) to Pd(0) (12.02 g / cm 3). If continuous films of Pd are to be deposited, thick films of Pd(AcO)2 must be used as starting materials. EP2532768A1 describes a subject matter similar to the aforementioned patent application: a non-catalytic palladium precursor composition including a palladium salt and an organic amine, the composition being water-free. This composition enables the use of solution processing methods to form a palladium layer on a wide variety of substrates. In particular, this patent application describes a process for forming a conductive palladium layer on a substrate comprising a palladium precursor composition including a palladium salt and an organic amine, depositing the precursor composition on the substrate, and heating the precursor composition to form the conductive palladium layer (see claim 1, for example). Furthermore, the palladium salt and the organic amine can form an organometallic complex (see paragraph
[0016] , for example), although the organic amine can also function as a solvent (see paragraph
[0059] , for example). The deposition of the palladium precursor composition can be done by various techniques, such as dip coating, spin coating, spray coating, and other types of printing (see paragraph
[0076] , for example). The deposition of these compositions can result in layers from 10 nm to 50 pm (see paragraph
[0080] , for example), while the temperature to which the precursor composition is heated may be between 80 and 350 °C (see paragraph
[0022] , For example). It is therefore important to develop a method for the synthesis of ultra-thin layers of PdOx where mainly Pd(ll) and Pd(IV) oxide are formed but Pd(0) is not formed (or is formed in a very small way). Exposition of the invention Embodiments of the present invention provide, according to a first aspect, a method for preparing layers of non-stoichiometric palladium palladium oxide comprising the following steps: a) dissolving a palladium (II) salt in a polar or non-polar solvent; b) aging the solution in a thermostated bath or dry block, at a temperature of 30 to 70°C, for at least 10 minutes, subjecting the solution to stirring; c) depositing the aged solution on a substrate to form a wet layer; d) curing the wet layer by thermal curing or ultraviolet light curing. In an exemplary embodiment, the dissolution step a) comprises a stabilizing agent preferably selected from monoethanolamine, diethanolamine, theethanolamine monoethanolamine, diethanolamine, theethanolamine or combinations thereof. In an exemplary embodiment, in the aging step b) a solution of photoinitiators or thermal initiators that promote the formation of non-stoichiometric palladium oxide is added. In one embodiment, the photoinitiators are cationic, anionic and / or radical and the thermoinitiators are cationic and / or radical. In an exemplary embodiment, the cationic photoinitiators are selected from the group consisting of diphenyliodonium trifluoromethane sulfonate, 2-(4-methoxyphenyl)-4,6-bis(thichloromethyl)-1,3,5-thazin, and tri-p-tolysulfonium hexafluorophosphate, the anionic photoinitiators are selected from the group consisting of nifedipine and O-benzoyloxime acetophenone, the radical photoinitiators are benzophenone; and wherein the cationic thermoinitiators are selected from the group consisting of diphenyl(methyl)sulfonium tetrafluoroborate and diphenyliodonium trifluoromethane sulfonate, and the radical thermoinitiators are selected from the group consisting of 2,2'-azobisisobutyronitrile and 1,T-azobis(cyclohexanecarbonitrile). In an exemplary embodiment, in the aging step b) a solution of metal salts that act as precursors of metal nanoparticles, and / or a solution of metal oxides for the formation of mixed oxides is added. In one embodiment, the metal salts are salts of the metals selected from the group consisting of gold, silver, platinum and palladium, and wherein the metal oxides are oxides of the metals selected from the group consisting of nickel, zinc, vanadium, tin (IV), titanium (IV), iron, cobalt and indium. The deposition of the mixture onto the substrate can be carried out using different techniques, preferably selected from among spin coating, dip coating, spray coating, Dr. Blade or inkjet printing. In one embodiment, the substrate is flexible, rigid, or semi-rigid. In particular, the flexible substrate is preferably selected from the group consisting of indium tin oxide-coated polyethylene terephthalate, fluorine-doped tin oxide-coated polyethylene terephthalate, polyethylene naphthalate, polypropylene, polycarbonate, and polyimide; the rigid substrate is preferably glass or steel; and the semi-rigid substrate is preferably selected from the group consisting of foil, foam, nickel foil, and aluminum. In one embodiment, thermal curing is carried out at a temperature between 30 and 500°C, preferably at a temperature below 200°C, more preferably at a temperature between 100 and 175°C. In a particular embodiment, ultraviolet curing is combined with thermal curing at temperatures below 200°C. In an exemplary embodiment, the photoinitiator is the anionic photoinitiator nifedipine and the curing is a thermal curing below 200°C combined with ultraviolet curing in a time between 1 and 5 minutes. Furthermore, when a solution of metal salts acting as precursors of metal nanoparticles and / or a solution of metal oxides for the formation of mixed oxides is added in the aging step b), the method of the present invention may comprise a second thermal curing at temperatures above 200°C. Embodiments of the present invention also provide, according to a second aspect, layers of non-stoichiometric palladium oxide nanocrystals obtained according to the method of the first aspect. Furthermore, embodiments of the present invention also provide, according to a third aspect, a photovoltaic cell comprising at least one layer of palladium oxide according to the second aspect. In yet a fourth aspect, the present invention provides different uses of the non-stoichiometric palladium oxide layers of the second aspect in photovoltaic, optoelectronic, catalytic applications or as sensors. In the present invention, the terms "layer" or "layers" and "film" or "film" are used interchangeably and equivalently, so that the person skilled in the art will understand that the reference to a layer of non-stoichiometric palladium oxide (PdO x ) is equivalent to a non-stoichiometric palladium oxide film (PdO x ). The present invention relates to a method for obtaining ultra-thin layers (<50 nm) of non-stoichiometric palladium (II and IV) oxide (PdO x ) electrically conductive and transparent in the visible. The method consists of the in-situ synthesis of PdO xby depositing a solution of a metal-organic salt of Pd(II) (palladium(II) acetate Pd(AcO)2) conveniently formulated in organic solvents, both polar alkoxyalcohols (e.g. methoxyethanol or butoxyethanol) and apolar (e.g. chloroform, toluene, xylene, chlorobenzene). The precursor solution is deposited by conventional deposition techniques such as spin-coating, spray-coating, dip-coating, screen-printing or digital printing (ink-jet or microplotter) on a flexible substrate (ITO or FTO on PET or PEN), semi-rigid (Ni or Al sheets or foam) or rigid (ITO or FTO on glass). Once the film is deposited, it is heated at low temperature (30-350°C) to remove the solvent and form PdO. xAlternatively, a thermal initiator or a photoinitiator can be used to accelerate the reaction. Alternatively, thermal curing combined with UV curing or simply UV curing can also be applied. PdO films x The resulting PdO2s exhibit thicknesses below 50 nm with excellent electrically conductive properties and are highly transparent in the visible light spectrum. The synthesis of PdO2 x It is carried out with low temperature thermal curing (<175°C) such as UV curing due to the presence of a photo initiator or a thermo initiator that accelerates the reaction of semiconductor oxide formation and prevents the formation of metallic Pd (0). As the conditions for the in-situ synthesis of PdO x are soft, the present invention is compatible with the use of thermolabile flexible substrates (plastics). The PdO xIt is a p-type semiconductor that has optical (transparency), electrical (conductivity and carrier mobility) and electronic (work function, valence and conduction band energy level) properties necessary for its application as transparent layers for selective hole transport for the manufacture of new flexible optoelectronic devices such as photovoltaic cells, light-emitting diodes, photodetectors, liquid crystal displays, touch screens as well as anti-aesthetic materials, capacitors. The synthesis method also allows the incorporation of metallic nanoparticles of Au, Ag, and Pt and other metallic oxides of Ni, Ru, and Ir during the preparation of the precursor solution by adding the corresponding metallic salts (AgNCh, AgCICL, HAuCU) after the aging process. Once the solution is deposited, the nanoparticles are generated inside the PdO layer. xduring the curing process for the formation of nanocomposite of metallic nanoparticles and PdO x The presence of metallic nanoparticles inside the PdO matrix x makes the electrical, optical and catalytic properties of the PdO nanocomposite x can be modified appropriately. Thus, the method for manufacturing PdO films x and its nanocomposites comprises the following steps: I. Dissolution of an organometallic palladium salt (eg palladium(ll) acetate (Pd(AcO)2), Palladium(ll) acetate trimer (Pd3(AcO)e), Palladium(ll) trifluoroacetate, Palladium(II) bis(triethylphosphine)chloride(l I), palladium(II) bis(dimethylglyoximate), (Pd(dmg)2, allylpalladium(ll) chloride Bis(triphenylphosphine)palladium(l I) diacetate), palladium(II) acetylacetonate (Pd(acac)2) Dichloro(ethylenediamine)palladium(ll), in a polar solvent (eg Alkoxyalcohols (Methoxyethanol, Ethoxyethanol), dimethylformamide (DMF),) or nonpolar (toluene, xylene, chloroform, Ethyl acetate) in the presence or absence of agents stabilizers (eg MEA, DEA or TEA). II. Aging of the solution in a thermally stabilized bath or dry block at 30-70°C for several minutes (10-60 min) with stirring for the synthesis of Pd (II) complex mixtures. III. Alternatively, a solution of photo and thermal initiators that promote the formation of PdO can be added to the solution from step II. x 1. Photo initiators: a. Cationic (photoacids): Diphenyliodonium Trifluoromethane sulfonate, 2-(4-Methoxyphenyl)-4,6-bis(t-chloromethyl)-1,3,5-tzazin, T-p-tolylsulfonium Hexafluorophosphate b. Anionic (photobases): Nifedipine, Acetophenone O-Benzoyloxime c. Radicals (photoradicals): Benzophenone 2. Thermo initiators: a. Cationic: Diphenyl(methyl)sulfonium Tetrafluoroborate, Diphenyliodonium Trifluoromethanesulfonate b. Radicalahos (photoradicals) 2,2'-Azobisisobutyronitrile (AlBN), 1,1'- Azobis(cyclohexanecarbonitrile) IV. Alternatively, a solution of metal salts can be added to the solution from step II, which act as precursors for metal nanoparticles (Au, Ag, Pt, Pd...) and metal oxides (N¡O X , ZnO, VO X , SnÜ2, TiCh, FeOx , CoO x , lnO x ) as well as a combination of these salts for the formation of mixed oxides and their nanocomposites. V. Deposition of liquid solution from step II, III or IV by different deposition techniques (e.g. spin-coating, dip-coating, spray coating, Dr. Blade, ink-jet printing) on flexible substrates (e.g. PET-ITO, PET-FTO, PEN, PP, PC, polyimide), rigid (glass, steel) and semi-rigid (sheets, foam, Ni, Al paper) for the formation of a wet film. VI. Curing by heating, at a temperature between 30 and 500°C, preferably <200°C, and more preferably between 100-175°C for the elimination of solvent residues and the in-situ synthesis of PdO x . Alternatively, ultraviolet curing (UVC) or thermal curing preferably <200°C combined simultaneously with UVC curing is applied for the removal of organic compounds (solvents and counterions) and the in-situ synthesis of PdO. x . VIII. Alternatively, in the case of the use of solution from step III when Nifedipine is used as an anionic photoinitiator, a thermal curing preferably at 200°C combined simultaneously with a LIV curing at short times (2 to 4 min) is applied for the in-situ synthesis of the metallic Pd(0) layers. IX. Alternatively, in the case of using the solution from step IV, a second curing is carried out at T> 200°C for the generation of metallic nanoparticles and metallic oxides inside the PdOx. The invention presented, therefore, consists of the direct in-situ synthesis of an ultra-thin layer (<50nm) of transparent conductive PdOx from the spicoating deposition of a solution of an organometallic palladium (II) salt with the possibility of being formulated together with a thermal initiator and / or a photoinitiator. The precursor solution is formulated in both polar (methoxyethanol, DMF) and apolar (toluene, chloroform, chlorobenzene, xylene) organic solvents with good Theological properties (viscosity and surface tension) which provides high wettability for the formation of transparent conductive layers with high homogeneity and excellent adhesion to the substrate. Once the film is formed, a low-temperature thermal curing process is applied, combined (or not) with UV curing. During low-temperature heat treatment (<180°C) and / or UV light, the initiators decompose to form a radical or a strong acid that accelerates the PdO formation reaction. x . In this way, films with high electrical conductivity (100 Scm-1) of PdO are obtained. xwith a composition of Pd(ll) and Pd(IV) (no presence of Pd(0) is observed) when deposited from apolar solvents (chloroform, toluene) with high transparency (transparency> 85% between 400nm < X > 1000nm) due to the formation of a homogeneous and continuous layer with ultra-thin thicknesses (thickness <50nm) and with excellent mechanical properties. The resulting film is homogeneous and continuous (no islands are formed) when temperatures <200°C are used. For the generation of homogeneous and continuous ultrathin layers it is necessary not to produce Pd(0) but PdO (d = 8.3 g / mL) and PdÜ2 (d = 6.8 g / mL) which have a density lower than that of Pd(0) (d = 12.0 g / mL) and closer to that of Pd(AcO)2 (d = 2.3 g / mL). This has a positive effect on the generation of a continuous PdO film. x(II, IV) since the film does not contract abruptly during drying. Otherwise, discontinuous films with island formation would be generated. The layers must be homogeneous and continuous, as otherwise, this would be detrimental to solar cell manufacturing, as it could generate pinholes (small craters that form in the film during its drying process), leading to short circuits in the device. By changing the reaction conditions, Pd(0) layers with metallic conductive properties can also be obtained. This requires simultaneously combining thermal curing at 200°C with UV curing using a photobase (nifedipine) to significantly accelerate the reaction. Thus, highly conductive Pd films of up to 3000 Scrrr are obtained in just 3 minutes at 200°C. 1 This may be of interest as transparent electrodes, as well as catalysts for applications in electrochemistry. The present invention results in a set of advantages. In particular, the MOs X P-type MOs have demonstrated great potential as HTMs. Furthermore, they have significant advantages over organic HTMs, due to the fact that MOs X They exhibit improved long-term inherent material stability, greater resistance to environmental conditions, and low cost, making them ideal materials for improving PSC performance and enhancing their stability. Since perovskite materials are sensitive to moisture and oxygen, device degradation occurs primarily in the area where the perovskite film is directly exposed to air. Therefore, HTMs not only perform well The role of perovskite hole extraction and hole transport not only protects the perovskite film from direct contact with the metal electrode and air, thereby delaying its degradation. It is well known that metal oxides exhibit better barrier properties against O2 and moisture than organic materials. BRIEF DESCRIPTION OF THE DRAWINGS The above and other features and advantages will be more fully understood from the following detailed description of some embodiment examples, merely illustrative and not limiting, with reference to the accompanying drawings, in which: FIG. 1: Schematic of the in-situ synthesis process of PdO x . FIG 2: Electrical conductivity and transparency (400-1000 nm) of PdO layers x prepared from 0.05 M Pd(AcO)2 in methoxyethanol and heated at different temperatures for 10 min. FIG 3: A) Thermogravimetric analysis (TGA) of Pd(AcO)2 in methoxyethanol from 50 to 300°C. B) TGA at 150, 200 and 300°C. FIG. 4: A) Conductivity and B) Transparency of PdO x heated to 150 and 200°C. FIG. 5: Stability study of 0.05 M Pd(AcO)2 solutions in methoxyethanol and DMF for the synthesis of PdO films x prepared at 200°C. FIG. 6: A) Pd(AcO)2 in toluene at 175°C. B) Pd(AcO)2 in chloroform at 175°C. FIG. 7: Comparison between two PdO precursors x : A) 0.05 M Pd(AcO)2 and B) 0.017 M Pd3(AcO)e in chloroform at 175°C. FIG. 8: Comparison between PdO x from a solution of 0.05 M Pd(AcO)2 in chloroform with thermal curing and thermal curing + UV: A) Conductivity vs curing time and B) conductivity vs thermal curing temperature with and without UV exposure for 40 min of curing. FIG. 9: PdO layers xsynthesized by thermal curing with and without UV curing for 40 min. a) Pd(AcO)20.05 M in chloroform with b) Pd(AcO)20.05 M in chloroform with a thermoinitiator (Diphenyl(methyl)sulfonium Tetrafluoroborate 0.005 M), c) Pd(AcO)2 0.05 M in chloroform with a photoacid (Diphenyliodonium Trifluoromethane sulfonate 0.0025 M) and d) Pd(AcO)2 in chloroform with a photobase (nifedipine 0.01 M). FIG.10: X-ray diffractogram of PdO x deposited from Pd(AcO)2 in methoxyethanol and heated at various temperatures for 30 min. FIG. 11: XPS spectrum of PdO x deposited from Pd(AcO)2 in methoxyethanol and toluene heated at 175°C for 30 min. FIG. 12: PdO x films synthesized from 0.05 M Pd(AcO)2 in chloroform with a photobase (0.01 M nifedipine) with thermal curing at 200°C with and without IIV curing. FIG. 13: X-ray diffractogram of PdO xdeposited from 0.1 M Pd(AcO)2 and 0.01 M nifedipine (PBG) in chloroform and heated at 200°C for 5 min with and without curing IIV. DETAILED DESCRIPTION OF SOME EXAMPLES OF IMPLEMENTATION An example of the operation of the invention based on obtaining non-stoichiometric palladium oxide layers is described below. In this example, the PdO precursor solution is formulated. A standard procedure consists of dissolving 0.05 M palladium (II) acetate (2.2 g) in methoxyethanol (10 mL). The mixture is initially stirred and a portion of the Pd(AcO) dissolves. The mixture is then heated in a dry block at 30-70°C for 10-60 min. It was found that after 5 min all the Pd(AcO) dissolves. Based on the data extracted from the absorbance spectra, it was decided to use this solution as the PdO precursor solution. xa 0.05 M Pd(AcO)2 solution aged for 60 min. Initially, a thin film of Pd(AcO)2 was deposited on a glass substrate by spin coating at a speed of 2000 rpm for 20 s and subjected to a treatment between 150 and 500 °C for 30 min. FIG. 1 shows the in-situ synthesis procedure. After heating, a uniform and homogeneous layer of PdO is obtained. x which unexpectedly shows good conductivities (10 S / cm) and high transparency at low temperatures (<200 °C). Unlike other metal acetates, the best conductivity (10 S / cm) is reached between 175 and 200 °C (FIG. 2). The optical transparency between 400 and 1000 nm remains constant at around 85% with the heating temperature. This evolution is very well correlated with the thermogravimetric analysis (TGA) of PdO. xwith temperatures (FIG. 3), where most of the Pd(OAc)2 weight is lost between 125 and 200 °C, by decomposition (or evaporation) to the loss of mainly the acetate. This behavior is certainly unusual for metal acetates that typically need higher temperatures (>300°C) for the decomposition of metal acetates and formation of the corresponding metal oxides. From TGA, the final composition of the film at 250 °C can be obtained, which in this case corresponds to Pd0O,8, which means that there is a defect of O atoms with respect to Pd. This indicates that under this heat treatment, not only PdO is formed, but also Pd(0). Palladium oxide is therefore non-stoichiometric. It should be noted that TGA is performed at a temperature gradient of 10°C / min, which does not accurately represent the conditions encountered in the in-situ synthesis process. In the process of the invention, once the film is deposited, it is heated on a ceramic plate directly to the working temperature, reaching thermal equilibrium after a few seconds. Therefore, if the thermogravimetric analysis is performed at a fixed temperature (isothermal thermogravimetric analysis), the real working conditions are better reproduced. Figure 3B shows the isothermal TGA at 200 and 300°C. It is observed that at 200°C, PdO (Pd(ll)) is formed, while at 300°C, mainly metallic Pd(O) is formed. FIG. 4 shows the kinetics of in-situ synthesis of PdO x at different temperatures. To follow the reaction, the conductivity and transparency of the PdO films are plotted. xheated to 150 and 200°C and its evolution over time. It can be seen that for 200°C the maximum conductivity is reached practically after one minute of heating, while for 150°C at least 5 minutes are needed for the film to show conductivity and it is after 15-20 min when it reaches maximum conductivity. The reaction kinetics, as expected, depend on the heating temperature: at 200°C the reaction is faster than at 150°C, but better conductivities are obtained at 150°C, which is an advantage since one of the objectives is to create electrically conductive layers at the lowest possible temperature. It is worth noting that at 200°C, after 45 minutes, the conductivity begins to decrease. This may be due to the formation of Pd (0), which can lead to contraction of the PdO layer due to its high density, generating discontinuity in the film.As for transparency, it can be seen that both temperatures give very similar results with transparencies between 400 and 1000 nm of approximately 80%. One of the drawbacks of using methoxyethanol as a solvent is that the precursor solution exhibits some instability over time. FIG. 5 shows the conductivity and transparency of a PdO film. x formed from a solution with different days of preparation. From the third day of preparation of the Pd(AcO)2 solution in In methoxyethanol, the conductivity drops abruptly by about 5 orders of magnitude. However, in DMF, the Pd(AcO)2 solution is stable for at least 21 days, generating PdO films. xwith stable conductivity and transparency over this time interval. It's worth noting that the maximum conductivity with DMF is an order of magnitude lower than with methoxyethanol. This is another advantage of the method; the solvent can be changed depending on the need to improve certain properties. Similarly, another advantage of this invention is that Pd(AcO) is soluble in nonpolar solvents, something very unusual in ionic compounds. Thus, the precursor solution of Pd(AcO) can be formulated in toluene, xylene, chlorobenzene, and chloroform at the concentrations of interest. The resulting films are also homogeneous and show good conductive properties and transparency. FIG. 6 shows conductivity and transparency data for PdO films. xprepared from 0.05 M solutions of Pd(AcO)2 in toluene (FIG. 6A) and chloroform (FIG. 6B). In chloroform, better conductivities are obtained, but worse transparencies. This is because thicker films of about 80 nm thickness are generated. However, for solutions of Pd(AcO)2 in toluene, 40 nm films are generated. It is known that at a lower boiling point of the solvent, thicker films are formed when deposited by spin coating. In situ synthesis of PdO x from solutions in apolar solvents is very important because these are fully compatible with lead halide perovskites and allow their use in both PIN and NIP solar cells. Polar solvents, such as alcohols or DMF, strongly degrade lead halide perovskites (dissolve them), so no solutions formulated in polar solvents can be deposited on them. It is worth noting that Pd3(AcO)e can also be used as a precursor to PdO x with satisfactory results as shown in FIG. 7. Pd3(AcO)e is soluble in both polar and nonpolar solvents. One process improvement is to combine thermal curing with UV curing simultaneously. FIG. 8 shows how UV curing substantially improves the obtained conductivities. It can be observed that, in general, exposure to UV light results in PdO. x with an improvement in conductivity of more than 3 orders of magnitude. It can be seen that the reaction kinetics are greatly improved with the presence of UV curing. If the solutions are also formulated with photoinitiators (photoacids and photobases) and thermoinitiators, the PdO formation reaction is accelerated. x especially at low temperatures temperatures. PdO layers are shown in FIG. 9 xsynthesized from solutions of Pd(AcO)2 in chloroform with a thermoinitiator (Diphenyl(methyl)sulfonium Tetrafluoroborate), a photoacid (Diphenyliodonium Trifluoromethane sulfonate) and a photobase (Nifedipine). It can be observed that, in general, the use of thermo- and photoinitiators improves the conductivities achieved. It is worth noting that both photoinitiators can be activated with heat treatments, and thermoinitiators can be activated under exposure to UV light, although not optimally. Structural characterization As previously mentioned, PdO x It is a p-type semiconductor. It is a non-stoichiometric metal oxide since Pd can have oxidation states Pd(O, II and IV). However, the presence of Pd(O), a metal, can compromise its semiconductor properties, hence there is some reluctance to use PdO. xas HTL. In fact, if one searches the literature for information about its physical properties, one can see a great disparity of values for its bandwidth that can fluctuate in the range of 0-2.67 eV. (Phys. Chem. Chem. Phys., 2011 , 13, 15947-15954. DOI 10.1039 / c1cp20923j). This is mainly due to the presence of Pd(O, II and IV). Its narrow bandwidth makes PdO x absorbs in the visible spectrum, so to obtain transparent films (>80% between 400-900 nm) ultra-thin layers (<50 nm) must be used. These ultra-thin layers must be homogeneous and continuous to avoid the generation of pinholes (small craters that form in the film during its drying process) that would cause short circuits in the device. Therefore, it is important to develop a method for the synthesis of ultra-thin layers of PdOx where mainly Pd(ll) and Pd(IV) oxide are formed but Pd(0) is not formed (or is formed in a very small way). One way to determine the presence of Pd(0), PdO, and PdÜ2 is through X-ray diffraction (XRD) structure analysis. X-ray diffraction patterns of PdO are shown in FIG. 10. x deposited from Pd(AcO)2 in methoxyethanol and heated at various temperatures for 30 min. The resulting PdO films x They are amorphous up to 250°C, with no characteristic peaks of crystal planes that can be attributed to Pd, PdO, and PdÜ2. From 300°C onwards, peaks of metallic Pd crystal planes are observed. This does not mean that Pd, PdO, or PdÜ2 do not form at lower temperatures, but rather that the resulting films are amorphous or formed by very small nanochstals. It should be noted that PdO films are synthesized. x ultrathin with thicknesses <40 nm. The PdO layers have also been characterized. xby X-ray photoelectron spectroscopy (XPS), a surface analytical technique that provides information on the surface composition, both qualitative and quantitative, and is commonly used to estimate the stoichiometry (with an error of approximately 10%), oxidation state and electronic structure of the elements that exist on the surface of a material. This technique is used for surface characterization since only information is obtained from the first 10 nm of a material, making it ideal for ultrathin layers of PdO x synthesized by the method of the invention. FIG. 11 shows the XPS spectra of two PdO samples. xdeposited from a solution of 0.05 M Pd(AcO)2 in toluene and methoxyethanol at 175°C for 30 min. After heating, mainly non-stoichiometric PdO is obtained, with the presence of different Pd species with different oxidation states (Pd(0), Pd(II) and Pd(IV)) under identical conditions depending on the solvent used. For PdO films x deposited from solutions of Pd(AcO)2 in methoxyethanol, 70% PdO, 20% Pd(O) and 10% PdO2 are obtained. For PdO films x deposited from solutions of Pd(AcO)2 in toluene, we obtain only 50% PdO and 50% PdÜ2. In this case, the presence of Pd(O) is less than 1%, as intended to maintain the semiconductor properties of PdO. x . This may be due to the influence of the solvent: alcohols are reducing agents that can facilitate the REDOX reaction of reduction of Pd(ll) to Pd(0). Synthesis of Pd(0) films As previously mentioned, another advantage of the invention is that by changing the reaction conditions, Pd(0) layers with metallic conductive properties can also be selectively synthesized. This requires simultaneously combining thermal curing at 200°C with LIV curing using a photobase (Nifedipine) to significantly accelerate the reaction. Thus, highly conductive Pd films of up to 3000 Scrrr are obtained in just 1.5 minutes. 1 . FIG. 12 shows how the conductivity varies for different thermal curing + LIV curing times. For times longer than 3 min, it can be seen how the conductivity decreases, probably due to the total or partial oxidation of Pd(0) to Pd(II, IV) to form PdO. x . If the results in the absence of exposure to LIV are compared, much lower conductivity values are observed, probably due to the formation of mainly PdO layers. xinstead of metallic Pd. With LIV, the reaction is much faster, which confirms that the formation of the photobase upon irradiation with LIV plays an important role in the reaction of metallic Pd layer formation. FIG. 13 shows that the metallic Pd layers are also amorphous at 200 °C with and without LIV curing. The scope of the present invention is defined in the appended claims.
Claims
CLAIMS 1. Method for preparing non-stoichiometric palladium oxide layers comprising the following steps: a) dissolving a palladium (II) salt in a polar or non-polar solvent; b) aging the solution in a thermostated bath or dry block at a temperature of 30 to 70°C for at least 10 minutes, with the solution being stirred; c) depositing the aged solution on a substrate to form a wet layer; d) curing the wet layer by thermal curing or ultraviolet light curing.
2. The method according to claim 1, wherein the dissolving step a) comprises a stabilizing agent preferably selected from monoethanolamine, diethanolamine, triethanolamine monoethanolamine, diethanolamine, triethanolamine or combinations thereof.
3. The method according to claim 1 or 2, wherein in the aging step b) a solution of photoinitiators or thermoinitiators that favor the formation of non-stoichiometric palladium oxide is added.
4. The method according to claim 3, wherein the photoinitiators are cationic, anionic and / or radical and the thermoinitiators are cationic and / or radical.
5. The method according to claim 4, wherein the cationic photoinitiators are selected from the group consisting of trifluoromethane diphenyliodonium sulfonate, 2-(4-methoxyphenyl)-4,6- bis(th-chloromethyl)-1,3,5-thazin and tri-p-tolylsulfonium hexafluorophosphate, the anionic photoinitiators are selected from the group consisting of nifedipine and O-benzoyloxime acetophenone, the radical photoinitiators are benzophenone; and wherein the cationic thermoinitiators are selected from the group consisting of diphenyl(methyl)sulfonium tetrafluoroborate and diphenyliodonium trifluoromethane sulfonate, and the radical thermoinitiators are selected from the group consisting of 2,2'-azobisisobutyronithiol and 1,T-azobis(cyclohexanecarbonithiol).
6. The method according to any one of the preceding claims, wherein in the aging step b) the following is added: - a solution of metal salts that act as precursors to metal nanoparticles, and / or - a solution of metal oxides for the formation of mixed oxides.
7. The method according to claim 6, wherein the metal salts are salts of the metals selected from the group consisting of gold, silver, platinum and palladium, and wherein the metal oxides are oxides of the metals selected from the group consisting of nickel, zinc, vanadium, tin (IV), titanium (IV), iron, cobalt and indium.
8. The method according to any one of the preceding claims, wherein the deposition is carried out by one of the techniques selected from spin coating, dip coating, spray coating, Dr. Blade or inkjet printing.
9. The method according to any one of the preceding claims, wherein the substrate is flexible, rigid or semi-rigid.
10. The method according to claim 9, wherein the flexible substrate is selected from the group consisting of indium tin oxide coated polyethylene terephthalate, fluorine doped tin oxide coated polyethylene terephthalate, polyethylene naphthalate, polypropylene, polycarbonate and polyimide, the rigid substrate is glass or steel and the semi-rigid substrate is selected from the group consisting of foil, foam, nickel foil and aluminum.
11. The method according to any one of the preceding claims, wherein the thermal curing is carried out at a temperature between 30 and 500°C, preferably at a temperature below 200°C, more preferably at a temperature between 100 and 175°C.
12. The method according to any one of the preceding claims, wherein the ultraviolet curing is combined with thermal curing at temperatures below 200°C.
13. The method according to any one of claims 3 to 12, wherein the photoinitiator is the anionic photoinitiator nifedipine and the curing is a thermal curing of less than 200°C combined with ultraviolet curing in a time of between 1 and 5 minutes.
14. The method according to any of claims 6 to 12, further comprising a second thermal curing at temperatures greater than 200°C.
15. Non-stoichiometric palladium oxide layers obtained according to the method defined in claims 1 to 14.
16. Photovoltaic cell comprising at least one layer of palladium oxide according to claim 15.
17. Use of the non-stoichiometric palladium oxide layers according to claim 15 in photovoltaic, optoelectronic, catalytic applications or as sensors.
Citation Information
Patent Citations
Low-temperature solution preparation method for indium oxide transparent semiconductor film
CN106783564A
Palladium precursor composition and process for forming a conductive palladium layer
EP2532768A1
Catalytic nickel oxide sheet, method for obtaining it and use thereof
EP3988208A1
Photocatalyst material and nanometric coating obtained from the same
ES2929948A1