Flame-retardant sheet composition for lithium secondary battery, characterized by delaying spread of fire, and flame-retardant sheet using same

The flame retardant sheet composition with a thermoplastic binder and inorganic flame retardant effectively delays fire spread and prevents thermal runaway in lithium secondary batteries by absorbing heat and maintaining structural integrity, addressing the inefficiencies of existing solutions.

WO2024262683A1PCT designated stage expired Publication Date: 2024-12-26KOREA MARITIME UNIV IND ACADEMIC COOPERATION FOUND
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/008977
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-19
Filing Date
2023-06-27
Publication Date
2024-12-26

AI Technical Summary

Technical Problem

Lithium secondary batteries face issues with thermal runaway and fire spread due to internal short circuits, which existing fire extinguishing systems struggle to prevent effectively, especially in sealed packs, and current flame-retardant solutions are either inefficient or impractical for use between battery cells.

Method used

A flame retardant sheet composition using a thermoplastic binder with a glass transition temperature up to 130°C, combined with an inorganic flame retardant and glass network former, to absorb heat and delay fire spread, which can be easily applied between lithium secondary battery cells without increasing module size or structural stress.

Benefits of technology

The solution effectively absorbs heat to prevent thermal runaway, reduces the risk of fire spread, and maintains structural integrity by not expanding at high temperatures, thus preventing secondary damage and toxic gas generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023008977_26122024_PF_FP_ABST
    Figure KR2023008977_26122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a flame-retardant sheet composition for a lithium secondary battery, characterized by delaying the spread of fire, and a flame-retardant sheet using same and, more specifically, to a sheet composition for delaying the spread of fire by controlling the temperature during thermal runaway, wherein the sheet composition includes: 20-40 parts by weight of at least one thermoplastic binder selected from polyvinyl acetate, polyvinyl alcohol, polyethylene, polyvinyl acetate-versatate, polyethylene-vinyl acetate, polyurethane, polystyrene, polyacrylate, polymethacrylate resin, polyacrylamide, and polyethylene terephthalate; 1-10 parts by weight of an organic binder; 1-5 parts by weight of a crosslinking agent; 30-50 parts by weight of an inorganic flame retardant; 10-20 parts by weight of a glass network former; 1-5 parts by weight of a plasticizer; 1-5 parts by weight of an additive; and 50-150 parts by weight of a solvent.
Need to check novelty before this filing date? Find Prior Art

Description

Flame-retardant sheet composition for lithium secondary batteries having fire spread delay properties and flame-retardant sheet using the same

[0001] The present invention relates to a flame-retardant sheet composition for a lithium secondary battery and a flame-retardant sheet using the same, and more specifically, to a flame-retardant sheet composition inserted between lithium secondary battery cells to prevent or delay the spread of fire due to thermal runaway of the lithium secondary battery and a flame-retardant sheet using the same.

[0002]

[0003] As modern society develops and industries develop, the importance of solar power and wind power is increasing as we seek to reduce the use of fossil fuels that cause global warming, such as coal.

[0004] However, solar and wind power generation are significantly affected by weather, requiring storage of the electricity generated for use when needed. Therefore, lithium secondary batteries are used to store electricity to efficiently utilize the generated energy.

[0005] In particular, the electric vehicle business is experiencing an increasing trend of expansion, and accordingly, domestic and foreign companies are actively pursuing lithium secondary battery production as a new business area.

[0006] Lithium secondary batteries have the advantages of high energy density and relatively long-term use, and are therefore being used in electric vehicles and energy storage systems (ESS). However, fire and explosion phenomena caused by thermal runaway in lithium-ion batteries remain unresolved issues.

[0007] The above thermal runaway phenomenon is caused by an internal short circuit in one or more cells due to damage to the separator caused by various factors such as mechanical, electrical, and thermal factors, and the starting temperature occurs at about 130℃ or higher in relation to the separator collapse temperature.

[0008] Some fire extinguishing systems have been developed both domestically and internationally to prevent the aforementioned thermal runaway phenomenon. However, not only are they difficult to prevent the literally runaway heat within the confined pack space and the resulting fire or explosion, but even if an effective fire extinguishing agent is developed, the high-pressure gas emitted from the thermally expanding cells and packs makes it difficult for the agent to effectively reach the source of the fire. Furthermore, most fire extinguishing agents cannot effectively cool the pack. Consequently, inefficient fire extinguishing methods are limited to waiting for a fire to break out in all cells or submerging the entire battery pack in water for cooling.

[0009] To solve this problem, a method has been proposed to prevent thermal runaway by manufacturing sheets made of flame-retardant ceramic fibers or porous foam and then inserting them between each cell to block the increase in heat. However, it is not easy to lower the temperature of adjacent cells, which is close to 900℃, to below 130℃ with a simple heat-resistant or flame-retardant ceramic sheet, and the use of thick flame-retardant ceramic insulation material causes the module to become too large and the room temperature heat transfer coefficient is too low due to the characteristics of the porous flame-retardant material, which causes heat to accumulate inside the cell or module, which also causes problems such as deterioration of the battery cell or cause a fire.

[0010] Furthermore, according to Korean Patent Publication No. 10-2022-0150347, a multi-layer structure with five layers is used to manage the heat of a battery. However, in the case of the above structure, the thickness of the sheet layers increases, which not only has a significant effect on the price increase, but also acts as a stress increase factor due to the use of intumescent insulation in the structure in the event of a fire, which reduces structural integrity. Furthermore, in the case of the above thick sheet layers, a sheet layer as thin as 2 to 4 mm is required between individual pouch cells, but this cannot be applied, and there is a disadvantage in that it has to be added to a module or assembly that contains multiple cells.

[0011] Accordingly, domestic companies that have improved the above problems have developed and proposed flame-retardant plastic materials that are relatively fire-resistant, such as polyphenylene oxide (PPO), a thermosetting engineering plastic, and polyamide (PA), a nylon resin, and polybutylene terephthalate (PBT). However, these were developed for the purpose of slowing down the spread of fire by being applied to the outside of cells, and were not used as compositions or components that prevent thermal runaway between cells.

[0012] In addition, a composition with a large amount of water-glass (20% or more) added is being used as a fire-prevention coating agent, but in this case, it is weak to humidity and moisture and easily changes shape when exposed to water, which limits its use. In addition, even if water-glass is added in an amount of less than 20%, there is a problem with the composition dissolving in water, so the development of a composition that does not dissolve in water and an additional process is essential.

[0013]

[0014] Accordingly, the present invention is intended to solve the above problems, and the technical task of the present invention is to provide a flame-retardant sheet composition for lithium secondary batteries having fire spread delay characteristics and a flame-retardant sheet using the same so as to prevent problems such as fires caused by thermal runaway that can occur in electric vehicles, ESS facilities, and portable power stations where fires frequently occur.

[0015]

[0016] In order to solve the above-described technical problem, the present invention provides a thermoplastic binder comprising: 20 to 40 parts by weight of at least one thermoplastic binder selected from polyvinyl acetate, polyvinyl alcohol, polyethylene, polyvinylacetate-versatate, poly(ethylene-vinylacetate), polyurethane, polystyrene, polyacrylate, polymethacrylate, polyacrylamide, and polyethylene terephthalate; 1 to 20 parts by weight of an organic binder; 1 to 5 parts by weight of a crosslinking agent; 30 to 50 parts by weight of an inorganic flame retardant; 10 to 20 parts by weight of a glass network former; 1 to 5 parts by weight of a plasticizer; A flame-retardant sheet composition for a lithium secondary battery is provided, comprising 1 to 5 parts by weight of an additive; and 50 to 150 parts by weight of a solvent, wherein the thermoplastic binder has a glass transition temperature of at most 130°C and absorbs heat by the thermoplastic binder to delay thermal runaway or fire spread.

[0017] Preferably, the organic binder is characterized by including at least one of methyl cellulose, ethyl cellulose, polyvinyl chloride, polyvinyl alcohol, butadiene rubber, polyvinyl butyral (PVB), acrylonitrile butadiene styrene (ABS), and polyamide (alcohol-soluble polyamide resin).

[0018] Preferably, the glass mesh former is characterized by including at least one of sodium silicate, potassium silicate, glass powder, glass fiber, organic phosphate, inorganic phosphate, and boron oxide that melts at at least 300°C to form a glass mesh structure.

[0019] Preferably, the sheet composition further comprises a diluting solvent comprising at least one of water, alcohol, and a mixture thereof, wherein the sheet composition and the diluting solvent are diluted in a weight ratio of 100:1 to 50.

[0020] Another object of the present invention is to provide a flame-retardant sheet for a lithium secondary battery formed using the above composition.

[0021]

[0022] The flame-retardant sheet composition for lithium secondary batteries of the present invention, which is a means for solving the above problem, absorbs heat using a thermoplastic binder having a glass transition temperature of up to 130°C, thereby having the effect of preventing or delaying the spread of fire in electric vehicles, ESS facilities, and portable power stations without a suitable fire extinguishing agent in the event of a fire.

[0023] In addition, the composition has the effect of being able to freely change its shape by diluting it with water or alcohol and a mixture thereof so that it can be manufactured in the form of a sheet that is easy to attach and insert onto the surface of a secondary battery pack where fire spread delay is desired.

[0024] In particular, when the composition is applied between adjacent lithium battery packs, it has the effect of cooling the heat generated from the cells that are problematic in the event of a fire in the lithium battery pack, and also has the effect of reducing thermal runaway due to an abnormally high temperature reaction.

[0025] In addition, the composition can reduce the generation of toxic gases at high temperatures by using an inorganic flame retardant instead of a toxic halogen element, and has the effect of preventing secondary damage by not applying pressure to adjacent battery packs or structures as the sheet does not expand at high temperatures.

[0026]

[0027] Figure 1 shows the results of a rapid drying test of a flame retardant sheet according to one embodiment of the present invention.

[0028] Figure 2 is an example of a room temperature bending test of a flame retardant sheet according to one embodiment of the present invention.

[0029] Figure 3 shows the results of a transition temperature test of a flame retardant sheet according to one embodiment of the present invention.

[0030] Figure 4 is a specimen after a transition temperature confirmation test according to one embodiment of the present invention.

[0031] Figures 5 and 6 are specimens after a transition temperature confirmation test according to another embodiment of the present invention.

[0032] Figure 7 shows the location of a thermocouple for checking thermal runaway in a flame retardant sheet according to one embodiment of the present invention.

[0033] Figure 8 is a thermal runaway test process according to one embodiment of the present invention.

[0034] Figure 9 is a graph showing the temperature per minute at each thermocouple section of a thermal runaway specimen according to one embodiment of the present invention.

[0035]

[0036] The present invention is susceptible to various modifications and embodiments. Specific embodiments are illustrated and described in detail in the drawings. However, this is not intended to limit the present invention to specific embodiments, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention. Throughout the description of each drawing, similar reference numerals have been used to designate similar components.

[0037] The terminology used in this application is only used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this application, it should be understood that the terms "comprise" or "have" indicate the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0038] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Terms defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and shall not be interpreted in an idealized or overly formal sense unless explicitly defined herein.

[0039] In one aspect, the present invention is a flame-retardant sheet composition for a lithium secondary battery that absorbs heat by a thermoplastic binder to delay thermal runaway or fire spread, characterized in that it comprises 20 to 40 parts by weight of a thermoplastic binder, 1 to 20 parts by weight of an organic binder, 1 to 5 parts by weight of a crosslinking agent, 30 to 50 parts by weight of an inorganic flame retardant, 10 to 20 parts by weight of a glass network former, 1 to 5 parts by weight of a plasticizer, and 1 to 5 parts by weight of an additive.

[0040] Below, we will explain the specific features of each of the above components.

[0041] First, the thermoplastic binder, like the inorganic flame retardant described below, acts to prevent or delay the spread of fire in the event of a fire or thermal runaway. Specifically, the thermoplastic binder has a glass transition temperature or melting point of 130°C or lower, so that when a fire occurs due to thermal runaway, it absorbs heat and transforms into a high-viscosity liquid form. This liquid interacts with other flame retardants and glass mesh formers described below to maintain a high-viscosity slurry form, thereby absorbing a large amount of heat and delaying the further spread of the fire.

[0042] If a thermoplastic binder with a glass transition temperature or melting point of 130℃ or higher is used, it is functionally meaningless as it cannot delay the spread of fire as it cannot absorb heat initially.

[0043] Meanwhile, as the thermoplastic binder, it is preferable to use a water-based binder or a water-dispersible powder binder to reduce toxic substances in the event of a fire, or to use a binder using a non-halogen volatile solvent that produces relatively little toxic gases.

[0044] More preferably, the thermoplastic binder includes at least one of polyvinyl acetate, polyvinyl alcohol, polyethylene, polyvinylacetate-versatate, poly(ethylene-vinylacetate), polyurethane, polystyrene, polyacrylate, polymethacrylate, polyacrylamide, and polyethylene terephthalate.

[0045] Meanwhile, it is preferable that the thermoplastic binder is included in an amount of 20 to 40 parts by weight. If the content of the thermoplastic binder is less than 20 parts by weight, the heat absorption is small due to the small binder content, so the thickness of the sheet layer cannot but increase accordingly. In addition, if it is included in an amount exceeding 40 parts by weight, the sheet cannot maintain its initial shape and flows downward due to heat because it cannot maintain a high viscosity slurry form, and there is a problem that the sheet flows downward due to heat and the fire spreads after catching fire with organic matter.

[0046] Next, the organic binder is a composition that acts as a binding agent that binds the thermoplastic binder, the inorganic flame retardant, and the glass mesh former, and it is preferable to use a binder that can be dissolved in water or an organic solvent, has a relatively high melting point, and maintains a sheet layer by moisture.

[0047] This is because the thermoplastic binder has low solubility in water and organic solvents. Moreover, since the thermoplastic binder alone can only produce a mixed form with the inorganic flame retardant described below, it is impossible to form a sheet layer in which the inorganic flame retardant is evenly dispersed. Therefore, the organic binder serves as an auxiliary binder that complements the problems of the thermoplastic binder.

[0048] Specifically, it is preferable to use a non-halogen organic binder as the organic binder. For example, other organic binders may include one or more of polyvinyl chloride, polyvinyl alcohol, butadiene rubber, polyvinyl butyral (PVB), acrylonitrile butadiene styrene (ABS), and alcohol-soluble polyamide resin, or methyl cellulose or ethyl cellulose as a cellulose-based binder.

[0049] However, the cellulose-based binders, such as methyl cellulose or ethyl cellulose, have relatively low binding strength compared to other organic binders, such as polyvinyl chloride and polyvinyl alcohol. Therefore, it is preferable to use them in a mixed form with other organic binders rather than using them alone.

[0050] Therefore, it is preferable that the methyl cellulose or ethyl cellulose and the other organic binder are included in a weight ratio of 0.1 to 1.5: 1. If the methyl cellulose or ethyl cellulose is used alone or included in an amount greater than the above ratio, there is a problem of deterioration in mechanical properties due to low binding force. In addition, if the cellulose-based binder is not included, cracks may occur in the process of forming the sheet as the crack resistance property is reduced. In this regard, in the case of the sheet composition to which the cellulose is not added, if a solvent with rapid volatility is used or the sheet is dried at a temperature higher than room temperature in order to control the drying time of the sheet, some cracks may occur in the coating film as shown in FIG. 1. Therefore, in order to control the crack resistance of the sheet as described above, it is preferable to include cellulose in the sheet composition or to adjust the volatilization conditions of the solvent.

[0051] Meanwhile, it is preferable that the organic binder is included in an amount of 1 to 20 parts by weight. If the content of the organic binder is less than 1 part by weight, the role of the binder is weakened, making it difficult to efficiently disperse the inorganic flame retardant and the thermoplastic binder. On the other hand, if the content of the organic binder exceeds 20 parts by weight, the specific gravity of the thermoplastic binder decreases, which makes it difficult to control the temperature in the event of a fire due to thermal runaway. Next, the crosslinking agent plays a role in enhancing the bonding strength between the aforementioned thermoplastic binder and the organic binder.

[0052] In this regard, the crosslinking agent may be a peroxide such as benzoyl peroxide or dicumyl peroxide, or an amide or amine such as bisacrylamide, methylene bisacrylamide, tetramethylethylenediamine (TMEDA), or triethyl amine (TEA). In addition, a urea such as dimethyloldihydroxyethylene urea (DMEU) may also be used, if necessary.

[0053] In addition to the above crosslinking agent, a crosslinking initiator may be further included, and preferably, a persulfate-based crosslinking initiator such as ammonium persulfate or potassium persulfate is used to impart excellent strength and flexibility to the sheet.

[0054] Meanwhile, it is preferable that the cross-linking agent is included in an amount of 1 to 5 parts by weight. If the content of the cross-linking agent is less than 1 part by weight, the mechanical properties are not improved, and if it exceeds 5 parts by weight, the residual cross-linking agent remaining after reaction actually reduces the properties of the sheet.

[0055] Next, the inorganic flame retardant imparts flame retardant properties to the sheet. It helps the heat-sensitive thermoplastic binder absorb heat without burning, thereby stably maintaining a high-viscosity slurry form. Therefore, it is preferable to use a hydroxide or carbohydrate, a composition used to impart flame retardancy to plastics, as the inorganic flame retardant.

[0056] In relation to this, most hydroxides such as aluminum hydroxide (Al(OH)3), calcium hydroxide (Ca(OH)2), magnesium hydroxide (Mg(OH)2), and titanium hydroxide (Ti(OH)4) can be used as the inorganic flame retardant, and carbonates, which are relatively inexpensive carbonate-based inorganic flame retardants such as calcium carbonate (CaCO3) and magnesium carbonate (MgCO3), can also improve the fire resistance of the sheet.

[0057] However, the inorganic flame retardants usable in the present invention are not limited to the above examples, and any inorganic flame retardant that undergoes an endothermic reaction while undergoing thermal decomposition at a relatively low temperature can be used without limitation.

[0058] Meanwhile, it is preferable that the inorganic flame retardant is included in an amount of 30 to 50 parts by weight. If the flame retardant is included in an amount of less than 30 parts by weight, it is difficult to maintain a high viscosity slurry form, and if it is included in an amount exceeding 50 parts by weight, the flame retardant properties may be improved, but the effect of absorbing heat by the thermoplastic binder is reduced due to a decrease in the content of the thermoplastic binder. In addition, in the case of an inorganic flame retardant with a high oil absorption, such as calcium carbonate, if it is included in an excessive amount, there is also a problem with formability.

[0059] Next, the glass mesh former melts at high temperatures and transforms into a highly viscous amorphous liquid form, which assists in the heat absorption of the thermoplastic binder to lower the temperature in the event of a fire caused by thermal runaway in a lithium secondary battery.

[0060] Examples of the above glass network forming agent may include at least one of a glass-like powder containing silicon (Si), boron (B), and phosphorus (P), a powder or aqueous solution in the form of sodium silicate or potassium silicate, glass powder, glass fiber, water glass, organic or inorganic phosphate, aluminum phosphate, ammonium polyphosphate, and a low-melting-point oxide such as boron trioxide (B2O3).

[0061]

[0062] In this regard, it is preferable that the glass mesh former be included in an amount of 10 to 20 parts by weight. If the glass mesh former is included in an amount of less than 10 parts by weight, the effect as an auxiliary thermoplastic binder is minimal, and if it is included in an amount of more than 20 parts by weight, when using a glass-type powder, the oil absorption is high, which causes problems in formability.

[0063] Next, a plasticizer is included to impart flexibility to the sheet and further enhance water resistance. Therefore, the plasticizer preferably includes at least one of phthalates, natural oils, esterified oils, and mixtures thereof.

[0064] Preferably, the phthalate may be at least one of dibutyl phthalate, dodecyl phosphate, and tricrecyl phosphate, and the natural oil may be at least one of organic phosphates, fish oil, corn oil, and soybean oil.

[0065] In this regard, it is preferable that the plasticizer be included in an amount of 1 to 5 parts by weight. If the content of the plasticizer is less than 1 part by weight, there is a problem of insufficient flexibility of the sheet. On the other hand, if the content of the plasticizer is included in an amount exceeding 5 parts by weight, although the flexibility of the sheet is improved, the mechanical strength of the sheet is lowered, and the drying time of the sheet is delayed.

[0066] Meanwhile, the additive serves to improve the chemical properties of the sheet composition. In addition, a dispersant, viscosity modifier, anti-coagulant, etc. may be included as needed.

[0067] Therefore, preferred examples of the additives include polyethylene glycol, sodium polyacrylate, pentaerythritol, glycerol trioleate, and polysaccharides, which may be selected as needed.

[0068] However, it is preferred that the additive be added in an amount of 1 to 5 parts by weight. If the additive is included in an amount of less than 1 part by weight, the additive content may be less than the total sheet composition ratio, resulting in a minimal effect. On the other hand, if the additive is included in an amount exceeding 5 parts by weight, the mechanical properties may be affected due to the remaining excess additive after reaction, and this may lead to an increase in unit price.

[0069] Finally, the solvent serves to uniformly disperse the sheet composition and improve the formability and workability of the composition in sheet form. Therefore, the worker can adjust the type and amount of solvent as needed.

[0070] Specifically, the solvent may include one or more of water or alcohol as needed. That is, the selection of the solvent is preferably made in consideration of the drying time of the sheet composition, which may vary depending on the types of the thermoplastic binder and the organic binder.

[0071] Therefore, it is preferable to use a solvent that can be completely volatile when mixed with the sheet composition and dried at room temperature for one week.

[0072] In relation to the above alcohols, it is preferable to use ethanol and isopropyl alcohol, which are relatively harmless to workers and the surrounding environment and have excellent workability. In addition, acetone, toluene, tetrahydrofuran, methyl ethyl ketone, etc. can be used, but are not limited thereto.

[0073] Meanwhile, the solvent affects the dispersibility and mixing of the composition. Therefore, it is preferable to include 50 to 150 parts by weight of the solvent. This can control the dispersibility depending on the absorption amount of the inorganic flame retardant and the glass mesh forming body.

[0074] Meanwhile, in addition to the above solvent, it is preferable to additionally dilute 1 to 50 parts by weight of the same solvent as the above solvent for the dilution purpose based on 100 parts by weight of the sheet composition.

[0075] If the solvent ratio for the above dilution purpose is less than 1 part by weight, there is a problem that the degree of improvement in workability is small compared to the diluted amount, and if it is included in excess of 50 parts by weight, the flowability and drying properties may be affected due to excessive dilution.

[0076] In relation to this, the solvent used for the above solvent and dilution volatilizes by at least 90 wt% during the process of drying the composition to form a sheet layer.

[0077]

[0078] Meanwhile, in another aspect, the present invention relates to a sheet manufactured from the flame-retardant sheet composition. The sheet comprises a thermoplastic binder having a glass transition temperature or melting point of 130°C or lower, thereby absorbing heat and transforming into a high-viscosity liquid when a fire occurs due to thermal runaway. That is, the transformed high-viscosity liquid is mixed with the inorganic flame retardant and the glass network forming body to maintain a high-viscosity slurry form, thereby absorbing a large amount of heat and delaying the spread of additional fire.

[0079] In relation to this, when manufacturing a sheet using the above sheet composition, it is preferable that the organic binder in the composition includes cellulose, such as methyl cellulose or ethyl cellulose, and the other organic binder in a weight ratio of 0.1 to 1.5:1, or is formed solely by the other organic binder. This is because, in the case of a sheet composition to which the cellulose is not added, cracks may occur in some parts of the sheet, as shown in Fig. 1, when drying is performed using a rapidly volatile solvent or at a temperature higher than room temperature in order to control the drying time of the sheet.

[0080] In relation to this, it is preferable that the formed sheet form a sheet layer having a thickness of at least 1 mm. If the thickness of the sheet layer is less than 1 mm, the flame retardant properties, heat diffusion prevention or delay properties are insufficient, and if the thickness of the sheet layer exceeds 5 mm, it takes a long time to dry the sheet to form it. Therefore, if a sheet having a thickness of at least 5 mm is required, it is preferable to manufacture and use multiple thin sheet layers of 5 mm or less.

[0081] Meanwhile, the above sheet can be formed into a sheet by applying a coating composition as needed. However, it is preferable that the thickness of the sheet does not exceed 5 mm.

[0082] Meanwhile, the above sheet can be manufactured by dispersing it using a ball mill, high-speed mixing device, ring mill device, etc.

[0083] Hereinafter, the present invention will be described in detail with examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention should not be construed as being limited to the examples described below. The examples of the present invention are provided to more fully explain the present invention to those of average skill in the art.

[0084]

[0085] <Test Example 1> Test to confirm bendability, resilience, and water resistance

[0086] (1) Preparation of specimens 1 to 6

[0087] To verify the mechanical properties of the sheet composition, sheets with a thickness of 1 to 3 mm were manufactured using the mixing ratios in Table 1 below to produce specimens of Examples 1 to 6.

[0088] Type Raw material name (unit: parts by weight) Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Thermoplastic binder Vinyl acetate copolymer 30 32 32 30 32 32 Organic binder Polyvinyl alcohol 3--6-- Polyamide binder -2--4- Polyvinyl butyral--2--4 Methyl cellulose 32 2--- Crosslinking agent Benzoyl peroxide 22 22 2 Dimethylol dihydroxyethylene urea 11-11-methylene-bisacrylamide 0.3 ... Magnesium 18.218.218.218.218.218.2 Calcium Carbonate 444444 Glass Mesh Forming agent Glass powder 2.62.62.62.62.62.62.6 Glass fiber 1.31.31.31.31.31.3 Water glass 1.31.3-1.31.3- Aluminum phosphate 2.62.62.62.62.62.6 Ammonium polyphosphate 5.25.25.25.25.25.25.2 Plasticizer Dibutyl phthalate 1.31.321.31.32 Tricresyl phosphate 2.52.52.52.52.52.5 Fish oil------ Corn oil 0.30.3-0.30.3- Additive Sodium polyacrylate 0.90.80.010.90.80.01 Pentaerythritol 2.92.62.62.92.62.6span #800.30.3-0.30.3-polyethylene glycol--2--2glycerol trioleate--1.3--1.3solventwater100--100--ethanol-12080-12080toluene--40--40

[0089] (2) Preparation of specimens for comparative examples 1 and 2

[0090] In order to compare the fire spread delay characteristics of the specimens of Examples 1 to 6, ceramic fibers and glass powder were mixed with organic / inorganic binders, respectively, to produce plate-shaped sheets as comparative examples.

[0091] Specifically, for Comparative Example 1, a 6 mm thick sheet was manufactured in the form of a plate by adding an organic / inorganic binder to ceramic fibers with excellent insulation and fire resistance.

[0092] For Comparative Example 2, a 1 mm thick sheet was manufactured by mixing powder of porous foam glass (manufacturer: Poraver, Grade: 1 to 2 mm) with excellent insulation and fire resistance with a binder. Next, the manufactured sheet was bonded to one side of a separate 6 mm thick mica plate to manufacture a sheet with a total thickness of 7 mm.

[0093]

[0094] (3) Bending and water resistance tests of the specimen

[0095] In this test example, the bendability and water resistance of the manufactured specimen at room temperature were confirmed.

[0096] First, for bendability, the degree of bending of the manufactured specimen was confirmed by manually bending it, and the degree to which the shape of the specimen was restored to its original shape was confirmed. The evaluation results are as shown in Table 2 below. In relation to this, the test results were marked as '○' for no abnormality, '△' for cracking, and 'X' for destruction.

[0097] Additionally, water resistance was confirmed by immersing the sheet in distilled water at room temperature for 24 hours, and the sheet's durability was assessed by bending and hand contact. The test evaluation method was the same as for bendability, and the test results are shown in Table 2 below.

[0098] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Bendability before immersion ○○○○○○△X Restorability ○○○○○○XX Bending after immersion ○○○○○○△X Sticks to hands ○○○○○○○○

[0099] According to the above results, as shown in Fig. 2, it was confirmed that the specimens of Examples 1 to 6 had excellent bendability and restorability before being immersed in distilled water. In addition, the bendability was also excellent without any cracks after being immersed in distilled water for 24 hours. On the other hand, in the case of Comparative Example 1 containing glass fiber, it was confirmed that some micro-uniformities occurred in the bending before being immersed, and it was confirmed that these did not return to their initial shape when bent. In addition, the bendability after being immersed in distilled water for 24 hours was also the same as the uniformity before being immersed.

[0100] Additionally, in the case of Comparative Example 2 containing glass powder, the specimen was destroyed upon bending. After immersion in distilled water for 24 hours, the bendability was also the same as before immersion.

[0101] Meanwhile, it was confirmed that the water resistance of all examples 1 to 6 and comparative examples 1 and 2 was excellent as there was no staining on the hands after immersion in distilled water for 24 hours.

[0102]

[0103] <Test Example 2> Heat transfer temperature confirmation test

[0104] (1) Preparation of heat transfer temperature specimens using the compositions of Examples 1 to 3 and Comparative Examples 1 and 2

[0105] In order to confirm the heat transfer temperature of the specimen, a 3 mm layer of the compositions of Examples 1 to 3 was formed on the upper surface of a mica plate having a thickness of 0.5 mm, and a 0.5 mm mica plate was covered on the upper surface of the applied composition to prepare a sandwich-shaped specimen.

[0106] Comparative Examples 1 and 2 formed a layer by applying a 6 mm composition to the same mica plate, and covered the upper surface of the applied composition with a 0.5 mm mica plate to manufacture a specimen having the same structure as the above example. At this time, the manufactured specimen was naturally dried for one week.

[0107]

[0108] (2) Heat transfer test

[0109] In order to confirm the heat transfer of the specimen, one side of the manufactured specimen was heated with a butane gas torch at 1,000°C for 10 minutes, and the temperature of the opposite side of the heated specimen was observed with a thermal imaging camera.

[0110] Figure 3 shows the test process and results of Example 1, and the surface temperature of the opposite mica layer was confirmed to be 115.3°C. In addition, as shown in Figure 4, it was confirmed that the inner sheet was partially melted, thereby controlling a stable temperature.

[0111] Additionally, in the case of Examples 2 and 3, it was confirmed that the surface temperature of the mica layer on the opposite side of the heating was maintained at a level of approximately 120°C.

[0112] On the other hand, in the case of the comparative example 1 specimen using glass fiber as shown in Fig. 5, the temperature of the surface of the mica layer on the opposite side was confirmed to be 237.5℃ after 7 minutes, and it was confirmed that part of the specimen was damaged.

[0113] Additionally, in the case of the comparative example 2 specimen using porous glass powder as shown in Fig. 6, the specimen surface was not damaged, but the temperature of the opposite mica layer surface was confirmed to be 252°C.

[0114] From the above results, it was confirmed that when a flame retardant sheet is applied between lithium secondary battery packs, thermal runaway is bound to occur when the specimens of Comparative Example 1 or Comparative Example 2, excluding Examples 1 to 3, are applied.

[0115]

[0116] (3) Lithium secondary battery thermal runaway test

[0117] A simulated thermal runaway environment for a lithium secondary battery was created using the manufactured Example 1 specimen to determine whether fire spread. At this time, the thickness of the Example 1 specimen was manufactured to be 2 mm.

[0118] In order to check whether a fire occurred in battery pack 1 or 2 by time zone, thermocouple 1 was installed on one side of cell 1 as a fire occurrence area, as shown in Fig. 7, thermocouple 2 was installed on the specimen of Example 1 to check the internal temperature of cell 1, and thermocouple 3 was installed on one side of cell 2. Next, as shown in Fig. 8, the specimen prepared in Fig. 7 was placed in a specific closed space, and a fire was caused by heating one side of cell 1 to check the thermocouple by time zone in the narrow space.

[0119] As a comparative example, two lithium battery packs were bonded together without a separate sheet layer and tested using the same method as above.

[0120] The results of the thermal runaway test are shown in Fig. 9. Referring to this, in the case of the specimen of Example 1, the temperature of thermocouple 1 in cell 1 where the fire occurred rose to over 500°C within 5 minutes. On the other hand, thermocouple 2 close to cell 2 maintained a temperature of 200°C for 10 minutes, and it was confirmed that thermocouple 3 attached to the sheet maintained a temperature of less than 100°C.

[0121] On the other hand, in the case of the comparative example, it was confirmed that the temperatures of thermocouples 1 to 3 increased rapidly after about 2 minutes, and after 4 minutes, thermal runaway occurred in thermocouple 2, causing the temperature to rise to 800℃.

[0122] Therefore, from the results of the above examples, it was confirmed that the flame-retardant sheet composition of the present invention includes a thermoplastic binder having a glass transition temperature of up to 130°C, an organic binder, an inorganic flame retardant, and a glass network former, and that the thermoplastic binder absorbs heat to delay thermal runaway or fire spread. In addition, when a sheet is manufactured using the composition, it has excellent bendability and resilience, and a sheet with a thin thickness of 1 to 5 mm can be manufactured, and thus it is expected that it can be sufficiently applied to electric vehicles, ESS facilities, portable power stations, etc., and delay thermal runaway or fire spread of secondary batteries.

[0123]

[0124] The above description is merely an illustrative illustration of the technical idea of ​​the present invention, and those skilled in the art will appreciate that various modifications and variations can be made without departing from the essential characteristics of the present invention. Therefore, the embodiments disclosed in the present invention are intended to illustrate rather than limit the technical idea of ​​the present invention, and the scope of the technical idea of ​​the present invention is not limited by these embodiments. The scope of protection of the present invention should be interpreted according to the claims, and all technical ideas within a scope equivalent thereto should be interpreted as being included in the scope of the rights of the present invention.

Claims

1. 20 to 40 parts by weight of at least one thermoplastic binder selected from polyvinyl acetate, polyvinyl alcohol, polyethylene, polyvinylacetate-versatate, poly(ethylene-vinylacetate), polyurethane, polystyrene, polyacrylate, polymethacrylate, polyacrylamide, and polyethylene terephthalate; 1 to 20 parts by weight of organic binder; 1 to 5 parts by weight of crosslinking agent; 30 to 50 parts by weight of inorganic flame retardant; 10 to 20 parts by weight of glass mesh forming agent; 1 to 5 parts by weight of plasticizer; 1 to 5 parts by weight of additive; and A sheet composition comprising 50 to 150 parts by weight of a solvent, A flame-retardant sheet composition for a lithium secondary battery, characterized in that the thermoplastic binder has a glass transition temperature of up to 130°C and absorbs heat by the thermoplastic binder to delay thermal runaway or fire spread.

2. In paragraph 1, A flame-retardant sheet composition for a lithium secondary battery, characterized in that the organic binder comprises at least one of methyl cellulose, ethyl cellulose, polyvinyl chloride, polyvinyl alcohol, butadiene rubber, polyvinyl butyral (PVB), acrylonitrile butadiene styrene (ABS), and polyamide (alcohol-soluble polyamide resin).

3. In paragraph 1, A flame-retardant sheet composition for a lithium secondary battery, characterized in that the glass mesh former comprises at least one of sodium silicate, potassium silicate, glass powder, glass fiber, organic phosphate, inorganic phosphate, and boron oxide that melts at at least 300°C to form a glass mesh structure.

4. In paragraph 1, The above sheet composition further comprises a diluting solvent comprising at least one of water, alcohol and mixtures thereof, A flame-retardant sheet composition for a lithium secondary battery, characterized in that the above sheet composition and the diluting solvent are diluted at a weight ratio of 100:1 to 50.

5. A flame-retardant sheet for a lithium secondary battery formed using a composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Olefinic resin composition and heat-resistant olefinic resin molding using the same

    JP2011213858A

  • Thermal runaway prevention sheet

    JP2018206605A

  • Fireproof sheet and battery

    JP2020136100A

  • FPCB Position sensor

    KR1020240061896A

  • KR20230063553A