Silicone, silicone composition and printing plate precursor using same

A silicone composition with specific structural units and additives addresses flexibility and handling issues, achieving flexible and image-reproducible cured products for printing plates.

WO2026234993A1PCT designated stage Publication Date: 2026-11-12TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016055
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-11-18
Filing Date
2026-04-22
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing photosensitive silicones used in applications like flexographic printing plates and stereolithography 3D printing face issues with flexibility and handling due to insufficient flexibility and challenges in film formation and image reproduction.

Method used

A silicone composition with a polydiorganosiloxane structure and organosiloxane structure, featuring repeating D units and T units, along with specific functional groups and molecular weight ranges, is developed to enhance flexibility and image reproducibility, incorporating a photoradical initiator and metal compounds for improved handling and curing.

Benefits of technology

The silicone composition allows for the production of flexible cured products with enhanced handling properties and improved image reproduction, enabling deeper relief patterns and reduced fluidity, suitable for printing plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026016055_12112026_PF_FP_ABST
    Figure JP2026016055_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a silicone excellent in handling properties and image reproducibility and capable of obtaining a cured product having excellent flexibility. The silicone has a polydiorganosiloxane structure represented by the following general formula (1) and an organosiloxane structure represented by the following general formula (2).
Need to check novelty before this filing date? Find Prior Art

Description

Silicone, silicone composition, and printing plate using the same

[0001] The present invention relates to silicone, silicone compositions and their cured products, printing plate masters and methods for manufacturing printing plates using silicone compositions, and methods for manufacturing printed materials.

[0002] Silicones, whose main chain consists of siloxane bonds in which silicon and oxygen are alternately bonded, are widely used in various applications due to their excellent heat resistance, electrical insulation, water repellency, and chemical resistance. Among these, photosensitive silicones, which harden when exposed to light such as ultraviolet rays, are used as components for semiconductors and electronic parts, as well as in photocurable paints, inks, adhesives, and printing plates for lithographic printing. Regarding photosensitive silicones, for example, radiation-curable silicone rubber compositions containing organopolysiloxanes of a specific structure having acrylic or methacrylic groups, phenyl ester derivatives having acrylic groups, radiation sensitizers, and photosensitive dyes have been proposed (see, for example, Patent Document 1); curable resin compositions containing silicone resins of a specific structure containing (meth)acryloxy groups including alkylene linking groups (see, for example, Patent Document 2); and photocurable resins containing copolymers having specific amounts of methacrylate-oxypropyl-methylsiloxane repeating units and dimethylsiloxane repeating units, methacrylate-oxypropyl-terminated dimethylsiloxane, and phosphine oxide photoinitiators (see, for example, Patent Document 3).

[0003] Japanese Patent Publication No. 2013-95805, Japanese Patent Publication No. 2013-151609, Japanese Patent Publication No. 2023-527381

[0004] While the technologies described in Patent Documents 1 and 2 can produce hardened products with high hardness, they suffer from insufficient flexibility in applications requiring flexibility, such as flexographic printing plates, as described later. Furthermore, although the photocurable resin described in Patent Document 3 is suitably used for stereolithography printing of 3D objects, its liquid state at room temperature presents challenges in handling, such as film formation, and image reproduction.

[0005] Accordingly, an object of the present invention is to provide a silicone that is excellent in handleability and image reproducibility, and that can yield a cured product with excellent flexibility.

[0006] In order to solve the above problems, the present invention mainly has the following configuration. <1> A silicone having a polydiorganosiloxane structure represented by the following general formula (1) and an organosiloxane structure represented by the following general formula (2).

[0007] In the above general formula (1), R 1 and R 2 each independently represent a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, an aryl group having 6 to 12 carbon atoms, a (meth)acryloxyalkyl group having 6 to 12 carbon atoms, a glycidoxyalkyl group having 6 to 12 carbon atoms, or a (3,4-epoxycyclohexyl)alkyl group having 8 to 15 carbon atoms. m represents a range of 6 to 10,000. The m number of R 1 and R 2 may each be the same or different. In the above general formula (2), R 3 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, an aryl group having 6 to 12 carbon atoms, a (meth)acryloxyalkyl group having 6 to 12 carbon atoms, a glycidoxyalkyl group having 6 to 12 carbon atoms, a (3,4-epoxycyclohexyl)alkyl group having 8 to 15 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms. R 4 represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a bond to Si of another diorganosiloxane structure or organosiloxane structure. Provided that, among R 1 to R 3 , at least one is a (meth)acryloxyalkyl group having 6 to 12 carbon atoms. <2> The silicone according to <1>, having a weight average molecular weight of 15,000 to 500,000. <3> The silicone according to <1> or <2>, having 0.01 to 2.0 mol / kg of (meth)acryloxyalkyl groups. <4> The silicone according to any one of <1> to <3>, containing 0.01 to 10 mol% of the organosiloxane structure represented by the general formula (2). <5> R in the general formula (1) 1 and R2 The silicone according to any one of <1> to <4>, wherein all of the groups are methyl groups. <6> In the above general formula (2), R 4 The silicone according to any one of <1> to <5>, wherein R is bonded to another diorganosiloxane structure or Si of an organosiloxane structure. <7> In the general formula (1) and the general formula (2) above, R 1 ~R 3 The silicone according to any one of <1> to <6>, wherein at least one of them is an alkenyl group having 2 to 8 carbon atoms. <8> In the above general formula (1) and the above general formula (2) R 1 ~R 3 A silicone according to any one of <1> to <7>, wherein at least one of the silicones is an aryl group having 6 to 12 carbon atoms. A silicone composition comprising a silicone according to any one of <1> to <8> and a metal compound containing a metal selected from titanium, zirconium, tin, and aluminum, wherein the metal compound is a metal compound selected from a metal alkoxide containing the metal, a metal acylate, a metal siloxide, a complex of the metal and a β-diketone compound, a complex of the metal and a β-ketoester compound, a complex of the metal and a β-diester compound, and a complex of the metal and a cyclic diene compound. A silicone composition comprising a silicone according to any one of <1> to <8> and a photoradical initiator. A cured product obtained by curing the silicone composition according to <9> or <10>. A printing plate master having a resin layer made of the silicone composition according to <9> or <10> on a substrate. A method for manufacturing a printing plate, comprising, in this order, an exposure step of irradiating the printing plate master described in <13> and <12> with light to partially photocrosslink the resin layer, and a development step of removing the unexposed portion of the resin layer. A method for manufacturing a printed material, comprising the steps of attaching ink to the relief of the printing plate obtained by the manufacturing method described in <14> and <13>, and transferring the ink to a substrate.

[0008] The silicone of the present invention offers excellent handling properties and image reproduction capabilities. The silicone of the present invention allows for the production of cured products with superior flexibility.

[0009] The silicone of the present invention has a polydiorganosiloxane structure represented by the following general formula (1) and an organosiloxane structure represented by the following general formula (2).

[0010]

[0011] In the above general formula (1), R 1 and R 2 each independently represent a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, an aryl group having 6 to 12 carbon atoms, a (meth)acryloxyalkyl group having 6 to 12 carbon atoms, a glycidoxyalkyl group having 6 to 12 carbon atoms, or a (3,4-epoxycyclohexyl)alkyl group having 8 to 15 carbon atoms. m represents a range of 6 to 10,000. The m R 1 and R 2 groups may each be the same or different.

[0012] In the above general formula (2), R 3 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, an aryl group having 6 to 12 carbon atoms, a (meth)acryloxyalkyl group having 6 to 12 carbon atoms, a glycidoxyalkyl group having 6 to 12 carbon atoms, a (3,4-epoxycyclohexyl)alkyl group having 8 to 15 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms. R 4 represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a bond to Si of another diorganosiloxane structure or organosiloxane structure.

[0013] Provided that, among R 1 to R 3 , at least one is a (meth)acryloxyalkyl group having 6 to 12 carbon atoms.

[0014] In general formulas (1) to (2), examples of the alkyl group having 1 to 8 carbon atoms include methyl group, ethyl group, propyl group, butyl group, heptyl group, octyl group and the like.

[0015] Examples of the alkenyl group having 2 to 8 carbon atoms include vinyl group, allyl group, butenyl group, pentenyl group, hexenyl group, heptenyl group, octenyl group and the like.

[0016] Examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a naphthyl group, and the like.

[0017] Examples of the (meth)acryloxyalkyl group having 6 to 12 carbon atoms include a 3-acryloxypropyl group, a 3-methacryloxypropyl group, an 8-methacryloxyoctyl group, and the like. Here, (meth)acryloxy is a general term for acryloxy and methacryloxy, and the number of carbon atoms refers to the total number of carbon atoms in the (meth)acryloxy group and the alkyl group.

[0018] Examples of the glycidoxyalkyl group having 6 to 12 carbon atoms include a 3-glycidoxypropyl group, an 8-glycidoxyoctyl group, and the like. Here, the number of carbon atoms refers to the total number of carbon atoms in the glycidoxy group and the alkyl group.

[0019] Examples of the (3,4-epoxycyclohexyl)alkyl group having 8 to 15 carbon atoms include a 2-(3,4-epoxycyclohexyl)ethyl group and the like. Here, the number of carbon atoms refers to the total number of carbon atoms in the epoxy group, the cyclohexyl group, and the alkyl group.

[0020] Examples of the aralkyl group having 7 to 12 carbon atoms include a benzyl group, a phenylethyl group, a phenylpropyl group, and the like. Here, the number of carbon atoms refers to the total number of carbon atoms in the aryl group and the alkyl group.

[0021] The polydiorganosiloxane structure represented by the general formula (1) is a linear polydiorganosiloxane structure that is a repetition of bifunctional siloxane units (D units). Hereinafter, the diorganosiloxane unit structure in the general formula (1) may be referred to as "D unit", and the polydiorganosiloxane structure represented by the general formula (1) may be referred to as "repeating D unit". The organosiloxane structure represented by the general formula (2) is a trifunctional siloxane unit (T unit). Hereinafter, the organosiloxane structure represented by the general formula (2) may be referred to as "T unit".

[0022] The organopolysiloxanes and silicone resins described in the aforementioned Patent Documents 1 and 2 may have D units, but because they are obtained by hydrolysis and polycondensation of alkoxysilanes used as raw materials, D units and T units tend to be randomly linked, and do not have repeating D units. Therefore, the cured products of these resins had insufficient flexibility. In contrast, the silicone of the present invention has repeating D units with m = 6 to 10,000, thereby enabling the production of a cured product with excellent flexibility. On the other hand, general polydiorganosiloxanes composed of D units are liquid at room temperature, which presents challenges in handling, such as film formation, and image reproducibility. In contrast, the silicone of the present invention, by having repeating D units and T units, introduces a branched structure into a flexible chain-like polymer, suppressing the fluidity of the polymer. This makes it possible to produce a polymer that is easy to form films and has good handling properties. Furthermore, the silicone of the present invention has a (meth)acryloxyalkyl group with 6 to 12 carbon atoms, which increases the contrast in curing degree between exposed and unexposed areas in photolithography pattern processing, thereby improving image reproducibility.

[0023] (Repeating D units) In general formula (1), m is in the range of 6 to 10,000. If m is less than 6, the flexibility derived from the chain-like polydiorganosiloxane structure is not easily expressed, and the flexibility of the cured product is insufficient. From the viewpoint of further improving the flexibility of the cured product, m is preferably 20 or more, and more preferably 40 or more. On the other hand, when used as a silicone composition, from the viewpoint of compatibility with other components, m is preferably 5,000 or less, and more preferably 2,000 or less.

[0024] In general formula (1), R 1 and R 2 It is preferable that all of these are methyl groups. In other words, it is preferable that the repeating D units have a polydimethylsiloxane structure, which can further improve the flexibility of the cured product.

[0025] (T unit) In general formula (2), R 3 A (meth)acryloxyalkyl group having 6 to 12 carbon atoms is preferred.

[0026] In general formula (2), R 4 It is preferable that this is a bond with another diorganosiloxane structure or Si of an organosiloxane structure. 4 This type of bonding allows for the formation of crosslinking points between silicone molecules via T units, thereby suppressing the fluidity of the flexible chain polymer and reducing surface tack in molded articles such as films made of silicone or films made of silicone compositions described later. Furthermore, in pattern processing using photolithography, it is possible to suppress the diffusion of radicals caused by the fluidity of silicone, thereby further improving image reproducibility.

[0027] (Silicone) The weight-average molecular weight (Mw) of the silicone of the present invention is preferably 15,000 or more, and more preferably 20,000 or more, from the viewpoint of improving the chemical resistance of the cured product. When the silicone of the present invention is used in the printing plate master described later, swelling due to various inks can be suppressed by improving chemical resistance. On the other hand, the Mw of the silicone is preferably 500,000 or less, and more preferably 300,000 or less, from the viewpoint of improving the solubility of the silicone in the developer and forming a deep relief pattern.

[0028] Here, the Mw of silicone can be measured by gel permeation chromatography (GPC) using polystyrene as the standard substance. When two or more types of silicone are present, the Mw of silicone refers to the Mw of the two or more silicones as a whole.

[0029] The silicone of the present invention preferably contains 0.01 to 2.0 mol / kg of (meth)acryloxyalkyl group. Having 0.01 mol / kg or more of (meth)acryloxyalkyl group allows for a higher contrast between exposed and unexposed areas and a deeper relief depth in photolithography pattern processing. Furthermore, when used as a printing plate, swelling of the relief in relation to the ink can be further suppressed. A (meth)acryloxyalkyl group content of 0.1 mol / kg or more is more preferable. On the other hand, having 2.0 mol / kg or less of (meth)acryloxyalkyl group suppresses excessive reaction in exposed areas during photolithography pattern processing, thereby improving image reproducibility. Furthermore, a deeper relief pattern can be formed. A (meth)acryloxyalkyl group content of 1.0 mol / kg or less is more preferable.

[0030] Here, the amount of (meth)acryloxyalkyl group in the silicone is 1 In 1H-NMR measurement, it can be determined from the integral value of H derived from (meth)acryloxyalkyl groups. The amount of (meth)acryloxyalkyl groups in silicone is 1 The mol / kg value obtained from the H-NMR measurement shall be rounded to two decimal places by rounding the third decimal place. However, if it is 1.0 mol / kg or more, 1 The mol / kg value obtained from the H-NMR measurement should be rounded to one decimal place by rounding the second decimal place. If two or more types of silicone are contained, this refers to the total content of (meth)acryloxyalkyl groups in the two or more silicones combined.

[0031] The silicone of the present invention has R in general formula (1) and general formula (2). 1 ~R 3Preferably, at least one of these is an alkenyl group having 2 to 8 carbon atoms. Having an alkenyl group having 2 to 8 carbon atoms improves the solubility of the unexposed areas in the developer during photolithography pattern processing, allowing for the formation of deeper relief patterns. Furthermore, it can further improve image reproducibility. 3 It is more preferable that it has an alkenyl group having 2 to 8 carbon atoms. As mentioned above, the R of each D unit in the repeating D unit 1 and R 2 These may be different, and if there are multiple T units, the R of each T unit 3 They may be different. In this case, multiple R 1 , R 2 , R 3 It is also preferable that any part of it has an alkenyl group having 2 to 8 carbon atoms.

[0032] The silicone of the present invention has R in general formula (1) and general formula (2). 1 ~R 3 Preferably, at least one of these is an aryl group having 6 to 12 carbon atoms. Having an aryl group with 6 to 12 carbon atoms increases the glass transition temperature of the silicone, further suppressing its fluidity and improving image reproducibility in pattern processing by photolithography. 3 It is more preferable that it has an aryl group having 6 to 12 carbon atoms. As mentioned above, the R of each D unit in the repeating D unit 1 and R 2 These may be different, and if there are multiple T units, the R of each T unit 3 They may be different. In this case, multiple R 1 , R 2 , R 3 It is also preferable that any part of it has an aryl group having 6 to 12 carbon atoms.

[0033] The silicone of the present invention preferably contains 0.01 to 10 mol% of organosiloxane structures (T units) represented by general formula (2), with the total amount of each siloxane unit constituting the silicone being 100 mol%. By containing 0.01 mol% or more of T units, the fluidity of the silicone can be further suppressed, and image reproducibility can be further improved in pattern processing by photolithography. Furthermore, surface tack of molded articles such as films made of silicone or silicone compositions described later can be suppressed. The T unit content is more preferably 0.10 mol% or more. On the other hand, by setting the T unit content to 10 mol% or less, the solubility of unexposed areas in the developer can be improved in pattern processing by photolithography, and a deep relief pattern can be formed. The T unit content is more preferably 7.0 mol% or less, and even more preferably 1.0 mol% or less.

[0034] Here, since each siloxane unit that makes up silicone has one Si atom, the total Si atoms that make up silicone are considered to be 100 mol%, and the mol% of Si atoms that make up each siloxane unit is the content (mol%) of that siloxane unit.

[0035] The content of the organosiloxane structure represented by general formula (2) is: 29 In Si-NMR measurement, this can be determined by calculating the ratio of the integral value of Si derived from the organosiloxane structure represented by general formula (2) to the total integral value of Si derived from the organosilane. The content of the organosiloxane structure represented by general formula (2) is 29 The mol% obtained from the Si-NMR measurement shall be rounded to two decimal places by rounding the third decimal place. However, if it is 1.0 mol% or more, 29 The mol% obtained from the Si-NMR measurement shall be rounded to one decimal place by rounding the second decimal place. Also, if it is 10 mol% or more, 29The mol% obtained from the Si-NMR measurement value shall be rounded to the nearest integer, with the first decimal place being rounded off. If two or more types of silicone are present, the total content in units of T refers to the total content of the two or more silicones.

[0036] The silicone of the present invention can be obtained, for example, by polycondensation of an α,ω-terminal silanol polydiorganosiloxane having a structure corresponding to repeating D units, a silane monomer corresponding to T units, and other silane monomers as needed.

[0037] α,ω-terminal silanol polydiorganosiloxanes having a structure corresponding to repeating D units can be obtained by hydrolysis and dehydration condensation of diorganosilane monomers. In this case, the degree of polymerization of the resulting polydiorganosiloxane, i.e., the value of m, can be controlled by adjusting the amount (molar ratio) of water added to the diorganosilane monomer.

[0038] Examples of diorganosilane monomers include dimethoxymethylsilane, dimethoxydimethylsilane, diethoxydimethylsilane, dimethoxymethylvinylsilane, dimethoxymethylphenylsilane, dimethoxydiphenylsilane, dimethoxy(3-acryloxypropyl)methylsilane, dimethoxy(3-methacryloxypropyl)methylsilane, dimethoxy(3-glycidoxypropyl)methylsilane, and dimethoxy(2-(3,4-epoxycyclohexyl)ethyl)methylsilane. Two or more of these may be used.

[0039] Alternatively, commercially available α,ω-terminal silanol polydiorganosiloxanes may be used, such as DMS-S12, DMS-S14, DMS-S21, DMS-S27, DMS-S32, DMS-S33, DMS-S35, DMS-S42, DMS-S45, DMS-S51, PDS-0338 (all manufactured by Gelest, INC.), X-21-5841, KF-9701 (all manufactured by Shin-Etsu Chemical Co., Ltd.). Two or more of these may be used.

[0040] Various functional groups may be introduced into the siloxane chain by reacting a diorganosilane with an α,ω-terminal silanol polydiorganosiloxane.

[0041] Examples of silane monomers corresponding to the T unit include trimethoxymethylsilane, triethoxymethylsilane, trimethoxyethylsilane, trimethoxypropylsilane, trimethoxyvinylsilane, trimethoxy(7-octenyl)silane, trimethoxyphenylsilane, trimethoxy(phenylethyl)silane, trimethoxynaphthylsilane, trimethoxy(3-acryloxypropyl)silane, trimethoxy(3-methacryloxypropyl)silane, trimethoxy(8-methacryloxyoctyl)silane, trimethoxy(3-glycidoxypropyl)silane, trimethoxy(8-glycidoxyoctyl)silane, trimethoxy(2-(3,4-epoxycyclohexyl)ethyl)silane, and hydrolyzed products thereof.

[0042] Other silane monomers include, for example, silane monomers having structures corresponding to tetrafunctional siloxane units (Q units) and monofunctional siloxane units (M units). Examples of silane monomers corresponding to Q units include tetramethoxysilane, tetraethoxysilane, and their hydrolysates. Examples of silane monomers corresponding to M units include methoxytrimethylsilane and its hydrolysates.

[0043] It is preferable to carry out a polycondensation reaction of the above α,ω-terminal silanol polydiorganosiloxane, the above silane monomer, and optionally other silane monomers in the presence of an organic solvent or without a solvent.

[0044] The organic solvent can be appropriately selected considering the stability of the resulting silicone and the volatility of the organic solvent. Examples of organic solvents include aliphatic or aromatic hydrocarbons, halogenated hydrocarbons, linear or cyclic ketone compounds, and linear or cyclic ether compounds. Two or more of these may be included. Among these, aliphatic hydrocarbons are preferred from the viewpoint of solubility of α,ω-terminal silanol polydiorganosiloxanes. The boiling point of the organic solvent is preferably 80°C or higher and 200°C or lower. Examples of such organic solvents include linear or branched aliphatic hydrocarbons having 6 to 9 carbon atoms, and alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, ethylcyclohexane, dimethylcyclohexane, and trimethylcyclohexane. Two or more of these may be included, and commercially available solvents in which these organic solvents are pre-mixed, such as those shown below, may be used.

[0045] Examples of branched aliphatic hydrocarbon mixtures include Marcazole 8 (manufactured by Maruzen Petrochemical Co., Ltd.), "Isopar®" C, "Isopar®" E (both manufactured by ExxonMobil Chemicals), IP Solvent 1016 (manufactured by Idemitsu Kosan Co., Ltd.), and "Isozol®" 200 (manufactured by JX Nippon Oil & Energy Corporation).

[0046] Examples of alicyclic hydrocarbon mixtures include "Exsol®" DSP80 / 100, "Exsol®" DSP100 / 140, and "Exsol®" D30 (all manufactured by ExxonMobil Chemicals), as well as CS gasoline (manufactured by JX Nippon Oil & Energy Corporation).

[0047] Various conditions in polycondensation reactions can be set to suit the desired properties, taking into account the reaction scale, size and shape of the reaction vessel, etc. Examples of such conditions include catalyst type, reaction temperature, and reaction time.

[0048] In polycondensation reactions, acid catalysts or metal catalysts can be used as condensation catalysts.

[0049] Examples of acid catalysts include hydrochloric acid, acetic acid, formic acid, nitric acid, oxalic acid, sulfuric acid, phosphoric acid, polyphosphate, polycarboxylic acids and their anhydrides, and ion exchange resins. Two or more of these may be used.

[0050] Examples of metal catalysts include metal alkoxides, metal acylates, metal siloxides, complexes of the metal with a β-diketone compound, complexes of the metal with a β-ketoester compound, complexes of the metal with a β-diester compound, and complexes of the metal with a cyclic diene compound. Among these, compounds selected from metal alkoxides containing a metal selected from titanium and zirconium, complexes of the metal with a β-diketone compound, and complexes of the metal with a β-ketoester compound are preferred, and compounds selected from complexes of titanium with a β-diketone compound and complexes of titanium with a β-ketoester compound are even more preferred.

[0051] Examples of complexes between titanium and β-diketone compounds include diisopropoxybis((4-oxopento-2-en-2-yl)oxy)titanium, di-n-butoxybis((4-oxopento-2-en-2-yl)oxy)titanium, and tetrakis((4-oxopento-2-en-2-yl)oxy)titanium. Examples of complexes between titanium and β-ketoester compounds include diisopropoxybis((4-ethoxy-4-oxobuta-2-en-2-yl)oxy)titanium, and di-2-butoxybis((4-ethoxy-4-oxobuta-2-en-2-yl)oxy)titanium.

[0052] When a catalyst is used in the polycondensation reaction, the amount of catalyst added is preferably 0.1 to 10 parts by mass per 100 parts by mass of the total of the α,ω-terminated silanol polydiorganosiloxane and silane monomer used in the polycondensation.

[0053] The reaction temperature for the polycondensation reaction is preferably 50°C or higher and below the boiling point of the organic solvent, and the reaction time is preferably 1 to 100 hours.

[0054] (Silicone Composition) The silicone of the present invention can be used in compositions containing the silicone plus other necessary components. One preferred embodiment of the silicone composition of the present invention is a composition containing the above-mentioned silicone and a photoradical initiator. Such a silicone composition can be patterned by photolithography because the photoradical initiator absorbs light to generate radical species, which promotes the crosslinking reaction of the silicone polymer.

[0055] As a photoradical initiator, one that has absorption at a wavelength of 365 nm is preferred. Such a photoradical initiator generates radicals when exposed to light emitted from a light source containing light at a wavelength of 365 nm, thereby promoting the radical polymerization reaction. Examples of light sources containing light at a wavelength of 365 nm (i-line) include high-pressure mercury lamps and ultra-high-pressure mercury lamps. In particular, ultra-high-pressure mercury lamps are preferred because they have high i-line intensity.

[0056] Examples of photoradical initiators having absorption at a wavelength of 365 nm include 2,2-diethoxyacetophenone, 2,2-dimethoxy-1,2-diphenylethane-1-one (manufactured by BASF Japan Ltd., “Irgacure®” 651), 1-hydroxycyclohexylphenyl-ketone (manufactured by BASF Japan Ltd., “Irgacure®” 184), 2-hydroxy-2-methyl-1-phenyl-propan-1-one (manufactured by BASF Japan Ltd., “Irgacure®” 1173), 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propan-1-one (manufactured by BASF Japan Ltd., “Irgacure®” 127), and phenylglyoxy Examples include ric acid methyl ester (manufactured by BASF Japan Ltd., “Irgacure®” MBF), 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (manufactured by BASF Japan Ltd., “Irgacure®” 907), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone (manufactured by BASF Japan Ltd., “Irgacure®” 369), bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (manufactured by BASF Japan Ltd., “Irgacure®” 819), and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (manufactured by BASF Japan Ltd., “Irgacure®” TPO). Two or more of these may be used. Among these, 2,2-diethoxyacetophenone, "Irgacure®" 1173, "Irgacure®" 907, "Irgacure®" 819, and "Irgacure®" TPO are preferred from the viewpoint of compatibility and solubility with silicone.

[0057] From the viewpoint of promoting the radical polymerization reaction and further improving the chemical resistance of the cured product, the content of the photoradical initiator in the silicone composition is preferably 0.05 parts by mass or more, and more preferably 0.1 parts by mass or more, per 100 parts by mass of silicone. On the other hand, from the viewpoint of improving the storage stability of the silicone composition, the content of the photoradical initiator is preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of silicone.

[0058] The silicone composition of the present invention preferably further contains a crosslinking agent. The inclusion of a crosslinking agent promotes the crosslinking reaction of the silicone upon light irradiation, thereby allowing for easier pattern formation by photolithography.

[0059] The crosslinking agent preferably has functional groups such as (meth)acryloyl groups and mercapto groups, and more preferably has two or more of these functional groups in the molecule. Because these functional groups are highly reactive, they promote crosslinking with the aforementioned silicone and other crosslinking agents, and when used as a printing plate, they can further suppress swelling of the relief in relation to the ink. It may also have two or more of these functional groups.

[0060] Examples of crosslinking agents having a (meth)acryloyl group include 1,10-bis(acryloyloxy)decane, tricyclodecanedimethanol diacrylate, trimethylolpropane triacrylate, and X-22-2445, X-22-164, X-22-164AS, X-22-164A, X-22-164B, X-22-164C, and X-22-164E (all manufactured by Shin-Etsu Chemical Co., Ltd.).

[0061] Examples of crosslinking agents having mercapto groups include mercapto-modified silicone oils having mercapto groups at both ends of the molecule or on the side chains of the molecule. Examples of mercapto-modified silicone oils having mercapto groups at both ends of the molecule include X-22-167B, X-22-167C (both manufactured by Shin-Etsu Chemical Co., Ltd.), and DMS-SM21 (manufactured by Gelest, Inc.). Examples of mercapto-modified silicone oils having mercapto groups on the side chains of the molecule include KF-2001, KF-2004 (both manufactured by Shin-Etsu Chemical Co., Ltd.), SMS-022, SMS-042, SMS-142, and SMS-992 (all manufactured by Gelest, Inc.).

[0062] From the viewpoint of improving the crosslinking properties of the silicone and the adhesion of the cured product to the substrate, the content of the crosslinking agent in the silicone composition is preferably 1.0 part by mass or more, and more preferably 2.0 parts by mass or more, per 100 parts by mass of silicone. On the other hand, from the viewpoint of further improving the flexibility of the cured product, the content of the crosslinking agent is preferably 35 parts by mass or less, and more preferably 20 parts by mass or less, per 100 parts by mass of silicone.

[0063] Another preferred embodiment of the silicone composition of the present invention is a composition containing the above-described silicone and a metal compound containing a metal selected from titanium, zirconium, tin, and aluminum. Examples of metal compounds include metal alkoxides, metal acylates, metal siloxides, complexes of the metal with a β-diketone compound, complexes of the metal with a β-ketoester compound, complexes of the metal with a β-diester compound, and complexes of the metal with a cyclic diene compound. Two or more of these may be included. By including the above-mentioned metal compound, it is possible to bond with silanol groups and hydrolyzable groups contained in the silicone, or to promote bonding between silanol groups and hydrolyzable groups, thereby further suppressing the fluidity of the silicone composition and further improving image reproducibility in pattern processing by photolithography. As the metal, a metal selected from titanium, zirconium, and aluminum is more preferred, and titanium is even more preferred. As the metal compound containing titanium, compounds selected from complexes of titanium with a β-diketone compound and complexes of titanium with a β-ketoester compound are even more preferred.

[0064] Examples of titanium-containing metal alkoxides include tetramethoxytitanium, tetraethoxytitanium, tetrapropoxytitanium, tetraisopropoxytitanium, tetrabutoxytitanium, tetra-s-butoxytitanium, tetraisobutoxytitanium, and tetra-t-butoxytitanium.

[0065] Examples of titanium-containing metal acylates include those in which titanium is bonded to the carboxyl group of a carboxyl group-containing compound. Examples of carboxyl group-containing compounds include acetic acid, acrylic acid, methacrylic acid, propionic acid, and 2-ethylhexanoic acid.

[0066] Examples of titanium-containing metal siloxides include those in which titanium is bonded to a silanol group in a silanol group-containing compound. Examples of silanol group-containing compounds include trimethylsilanol, diphenylsilanediol, and α,ω-terminal silanol polydiorganosiloxanes.

[0067] Examples of complexes between titanium and β-diketone compounds, and complexes between titanium and β-ketoester compounds, include the compounds listed above as metal catalysts.

[0068] From the viewpoint of further improving image reproducibility, the content of the metal compound in the silicone composition is preferably 0.01 parts by mass or more, and more preferably 0.1 parts by mass or more, per 100 parts by mass of silicone. On the other hand, from the viewpoint of improving the storage stability of the silicone composition, the content of the metal compound in the silicone composition is preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, per 100 parts by mass of silicone.

[0069] The silicone composition of the present invention preferably further contains an organic solvent. Examples of organic solvents include those used in the synthesis of silicone (polycondensation reaction).

[0070] The silicone composition of the present invention can be produced, for example, by mixing silicone, a photoradical initiator and / or a metal compound, a crosslinking agent as needed, an organic solvent, and other components. A mixer is an example of a mixing device. It is preferable to stir and mix the components until they are homogeneous.

[0071] (Cured product) The silicone composition of the present invention can be cured to produce a cured product.

[0072] Examples of the shape of the cured product of the present invention include film-like structures such as flat thin films, flexible films, and multilayer films, as well as lattice-like and dome-like structures. The shape of the cured product is preferably film-like. Since the silicone of the present invention is easily film-forming, the silicone composition of the present invention is also suitable for film formation. From the viewpoint of further improving flexibility, the film thickness of the cured product is preferably 10 μm or more.

[0073] The cured product of the present invention can be obtained, for example, by exposing the silicone composition of the present invention to light. When forming a desired pattern with the cured product, it is preferable to pattern expose the silicone composition of the present invention and develop and remove the unexposed areas. As an example of a method for obtaining a cured product by pattern processing a film-like silicone composition, a method comprising the steps of (I) applying the silicone composition of the present invention to a substrate to form a coating film, (II) exposing and developing the coating film, and, if necessary, (III) heating the coating film after development will be described below.

[0074] (I) A step of applying the silicone composition of the present invention onto a substrate to form a coating film. Step (I) is a step of forming the silicone composition of the present invention as a uniform film on a substrate.

[0075] As a substrate, one with excellent dimensional stability against heat and physical stress is preferred. Examples include plastic sheets such as polyester; metal plates such as steel, stainless steel, and aluminum; and glass substrates such as soda-lime glass and alkali-free glass.

[0076] Coating methods include, for example, casting a silicone composition, coating using various coaters such as spin coaters, slit coaters, bar coaters, and applicators, and printing methods such as screen printing and inkjet printing. It is preferable to perform the coating in a way that obtains a coating film having a film thickness and film quality suitable for subsequent exposure and development processes.

[0077] It is preferable to dry (pre-bake) the coating film obtained after application. Examples of drying methods include vacuum drying and heat drying. Examples of heating devices include hot plates and ovens. The heating temperature is preferably 60 to 150°C, and the heating time is preferably 30 seconds to 2 hours.

[0078] (II) Step of exposure and development of the coating film Step (II) is a step of exposing the coating film obtained in step (I), curing the exposed parts, and removing the unexposed parts by development, thereby forming a desired pattern consisting of a cured product of the silicone composition of the present invention.

[0079] Exposure may be performed via a desired mask or without a mask. Examples of exposure machines include steppers, mirror projection mask aligners (MPAs), and parallel light mask aligners (PLAs). The exposure intensity is 10 to 10,000 J / m². 2 The typical exposure level is calculated based on a wavelength of 365 nm. Examples of exposure light sources include ultraviolet light such as i-lines, g-lines, and h-lines, as well as KrF (wavelength 248 nm) lasers and ArF (wavelength 193 nm) lasers.

[0080] Development methods include, for example, immersing the exposed coating in a developer solution and removing the unexposed areas of the coating using a brush-type or spray-type developer. The developer solution preferably contains a solvent that can dissolve or swell silicone, and may contain additives such as surfactants as needed. Examples of developers include hydrocarbon-based solvents and hydrocarbon / glycol ether mixed solvents. The developer solution temperature is preferably 15 to 50°C. After development, it is preferable to dry the developed coating at 50 to 70°C for about 10 to 120 minutes. If necessary, post-exposure by irradiation with active light in air or vacuum may be performed.

[0081] (III) Step of heating the developed coating The step in (III) is a step in which the curing reaction is further advanced by heating the developed coating, thereby improving the mechanical strength, heat resistance and chemical resistance of the resulting cured product.

[0082] Examples of heating devices include hot plates and ovens. The heating temperature is preferably 120 to 250°C, and the heating time is preferably 15 minutes to 2 hours.

[0083] (Printing Plates and Printing Plates) The silicone composition of the present invention can be suitably used for printing plates. In particular, it can be suitably used for flexographic printing plates and flexographic printing plate masters used in flexographic printing.

[0084] Flexographic printing is a printing method in which ink is applied to the raised relief of a flexographic printing plate, and then the relief is pressed onto the substrate, transferring the ink from the relief to the substrate. Flexographic printing, taking advantage of the flexibility of the flexographic printing plate, is widely used in applications such as paper containers, labels, flexible packaging, and electronics. In addition to solvent-based inks that use organic solvents, in recent years, water-based inks that primarily use water as a solvent, and active energy ray-cured inks that harden with active energy rays such as ultraviolet (UV) or electron beams (EB), have come into use in flexographic printing, from the perspective of reducing environmental impact. Flexographic printing plates are required to be resistant to swelling with these various inks, in order to suppress image swelling during printing and maintain stable print quality.

[0085] The silicone composition of the present invention, having excellent flexibility and chemical resistance in its cured product, possesses image reproducibility and flexibility suitable for flexographic printing, and can suppress swelling caused by various inks.

[0086] The printing plate master of the present invention has a resin layer made of the silicone composition of the present invention on a substrate. The substrate has the function of supporting the resin layer and the relief in the printing plate master or printing plate. The resin layer of the printing plate master is a layer for forming the relief, and the relief of the printing plate is obtained by forming an uneven pattern on the resin layer by photolithography.

[0087] The thickness of the resin layer is preferably 0.3 mm or more. A resin layer thickness of 0.3 mm or more is preferable because it allows the printing plate described later to have sufficient relief depth and improve printability. A resin layer thickness of 0.5 mm or more is more preferable. On the other hand, a resin layer thickness of 5 mm or less is preferable. This allows the active light rays during exposure to reach the bottom sufficiently, further improving image reproduction. A resin layer thickness of 3 mm or less is more preferable.

[0088] The resin layer preferably has a light transmittance of 50% or more per 1 mm thickness at a wavelength of 400 nm. A light transmittance of 50% or more allows the active light to reach the bottom sufficiently during exposure, so that the curing reaction proceeds appropriately and a highly sensitive printing plate can be produced. Furthermore, a light transmittance of 80% or more is even more preferable, as such a highly transparent resin layer suppresses light scattering, further improving sensitivity and image reproducibility.

[0089] The light transmittance of the resin layer at a wavelength of 400 nm can be measured by the following method. First, the ultraviolet-visible absorption spectrum of a printing plate with a resin layer on a substrate is measured using a spectrophotometer. Next, the resin layer is removed from the printing plate, and the ultraviolet-visible absorption spectrum of the substrate alone is measured. Using the ultraviolet-visible absorption spectrum of the substrate alone as a reference, the ultraviolet-visible absorption spectrum of the resin layer is calculated from the difference between the spectrum of the printing plate and the reference spectrum. The obtained ultraviolet-visible absorption spectrum and the thickness of the resin layer are used to calculate the light transmittance per 1 mm thickness of the resin layer at a wavelength of 400 nm.

[0090] Examples of substrates include plastic sheets such as polyester, and metal plates such as steel, stainless steel, and aluminum.

[0091] From the viewpoint of handling and flexibility, the thickness of the substrate is preferably 100 μm to 350 μm.

[0092] It is preferable to provide a primer layer or adhesive layer on at least one side of the substrate, which can improve the adhesion strength with the resin layer.

[0093] The printing plate master of the present invention preferably further comprises a cover film on the resin layer. The presence of the cover film protects the surface of the resin layer and suppresses the adhesion of foreign matter. The resin layer may be in contact with the cover film, or there may be one or more layers between the resin layer and the cover film. Examples of layers between the resin layer and the cover film include an anti-adhesion layer that prevents adhesion to the surface of the resin layer.

[0094] As the cover film, plastic sheets such as polyester (e.g., polyethylene terephthalate) or polyolefins (e.g., polyethylene and polypropylene) are preferably used. These plastic sheets have low ultraviolet absorption and high transparency, which can suppress the scattering of exposure light in the exposure process described later. The thickness of the cover film is preferably 10 to 150 μm. The surface of the cover film may also be roughened. Roughening the surface can improve the adhesion to the original image film.

[0095] The printing plate master according to the present invention may further have a thermal mask layer on the resin layer. In so-called CTP plates, drawing is performed directly on the thermal mask layer using a laser drawing machine without using an original image film. Preferably, the thermal mask layer has the function of blocking ultraviolet light and, when exposed using an infrared laser, absorbs the laser light and is instantaneously partially or completely sublimated or melted by the heat. This creates a difference in optical density between the laser-irradiated and unirradiated areas, allowing it to perform the same function as an original image film in a conventional exposure process.

[0096] Furthermore, an adhesion adjustment layer may be provided between the thermal mask layer and the resin layer. The adhesion adjustment layer can improve the adhesion between the thermal mask layer and the resin layer. Additionally, a release assist layer may be provided between the thermal mask layer and the cover film. The release assist layer can suppress cohesive failure of the thermal mask layer when the cover film is peeled off.

[0097] Next, the method for manufacturing a printing plate according to the present invention will be explained using the case in which a resin layer is present on the substrate as an example.

[0098] A resin layer is formed on the substrate. Methods for forming the resin layer include, for example, casting a resin layer-forming composition onto the substrate and drying it, bonding a separately formed resin layer sheet to a substrate on which a primer layer and adhesive layer have been formed as needed, or sandwiching the resin layer-forming composition between the substrate and a cover film and applying pressure under heating or without heating. The resin layer-forming composition can be obtained, for example, by adding a crosslinking agent, organic solvent, and other additives as needed to silicone and a photoradical initiator, and stirring or kneading to thoroughly mix them.

[0099] Next, the method for manufacturing a printing plate according to the present invention will be described. As a method for manufacturing a printing plate, from the viewpoint of productivity and image reproducibility of the printing plate, it is preferable to have an exposure step in which light is irradiated onto the printing plate master to partially photocrosslink the resin layer, and a development step in which the unexposed parts of the resin layer are removed, in that order.

[0100] First, the exposure process will be explained. If the printing plate is a CTP plate, and it has a cover film, this is peeled off, and an image is drawn on the thermal mask layer using a laser drawing machine. Then, ultraviolet light is irradiated to selectively photocrosslink the resin layer corresponding to the laser-irradiated area. If the printing plate does not have a thermal mask layer, ultraviolet light is irradiated through the original image film to selectively photocrosslink the exposed area of ​​the resin layer. As ultraviolet light, light with a wavelength of 300 to 400 nm is preferred. Examples of lamps used for ultraviolet irradiation include high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, xenon lamps, carbon arc lamps, and chemical lamps. In particular, if the reproducibility of fine lines and independent points is required, it is also possible to form a floor layer by short-time exposure (back exposure) from the substrate side before peeling off the cover film.

[0101] Next, the development process will be described. The exposed printing plate is immersed in a developer solution, and the unexposed areas of the resin layer are removed with the developer solution using a brush-type or spray-type developer, thereby forming a relief on the substrate. The developer solution preferably contains a solvent that can dissolve or swell silicone, and may contain additives such as surfactants as needed. The developer solution temperature during development is preferably 15 to 50°C.

[0102] For flexographic printing plates, the hardness of the relief is preferably 90 or less on the durometer A hardness scale, and more preferably 80 or less, from the viewpoint of further improving flexibility. On the other hand, from the viewpoint of further improving image reproducibility, the durometer A hardness is preferably 30 or more, and more preferably 40 or more.

[0103] (Method for manufacturing printed materials) The method for manufacturing printed materials of the present invention preferably includes the steps of applying ink to the relief of the printing plate obtained by the method described above, and transferring the ink to a substrate.

[0104] Examples of printing presses used in the method for manufacturing printed materials of the present invention include flexographic printing presses such as inline type, center drum type, and stack type.

[0105] Preferably, solvent inks, water-based inks, UV-curing inks, and EB-curing inks are used. Preferably, solvent inks contain pigments or dyes, vehicles, organic solvents, etc. More specifically, examples include XA-55 (manufactured by Sakata Inx Co., Ltd.). Preferably, water-based inks contain pigments, water-soluble resins, water, alcohols, etc. More specifically, examples include XS-903 (manufactured by DIC Corporation). Preferably, UV-curing inks contain pigments, resins such as acrylic oligomers, acrylate monomers, polymerization initiators, etc. More specifically, examples include PHA (manufactured by T&K Toka Co., Ltd.), "FLASH DRY" (registered trademark) (manufactured by Toyo Ink Co., Ltd.), and "UVAFLEX" (registered trademark) Y77 (manufactured by Zeller + Gmelin). Preferably, the EB-curing ink contains, for example, a pigment, a resin such as an acrylic oligomer, or an acrylate monomer. More specifically, examples include "GelFlex EB" (registered trademark) (manufactured by Sakata Inx Corporation).

[0106] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these. The names of the compounds used, for which abbreviations are used, are shown below.

[0107] (α,ω-Terminal silanol polydiorganosiloxanes) DMS-S12: α,ω-Terminal silanol polydimethylsiloxane (manufactured by Gelest, INC., weight-average molecular weight: 400-700, number of silanol groups in polymer chain: 2) DMS-S14: α,ω-Terminal silanol polydimethylsiloxane (manufactured by Gelest, INC., weight-average molecular weight: 1,000, number of silanol groups in polymer chain: 2) DMS-S21: α,ω-Terminal silanol polydimethylsiloxane (manufactured by Gelest, INC., weight-average molecular weight: 4,200, number of silanol groups in polymer chain: 2) DMS-S27: α,ω-terminally silanol polydimethylsiloxane (manufactured by Gelest, INC., weight-average molecular weight: 18,000, number of silanol groups in polymer chain: 2) DMS-S35: α,ω-terminally silanol polydimethylsiloxane (manufactured by Gelest, INC., weight-average molecular weight: 49,000, number of silanol groups in polymer chain: 2) DPhSi(OH) 2 : Diphenylsilanediol PDS-1615: α,ω-terminally silanol diphenylsiloxane-dimethylsiloxane copolymer (manufactured by Gelest, INC., weight-average molecular weight: 900-1,000, number of silanol groups in polymer chain: 2, diphenylsiloxane: 14-18 mol%)

[0108] (Bifunctional Silane Monomers) KBM-502: Dimethoxy(3-methacryloxypropyl)methylsilane (manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-22: Dimethoxydimethylsilane (manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-202SS: Dimethoxydiphenylsilane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0109] (Trifunctional Silane Monomers) KBM-503: 3-Methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-5803: 3-Methacryloxyoctyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-5103: 3-Acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-1003: Vinyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-103: Phenyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) KBM-13: Methyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0110] (Titanium Compounds) TC-750: Diisopropoxybis((4-ethoxy-4-oxobuta-2-en-2-yl)oxy) titanium solution, concentration 97.5% by weight, containing solvent 2-propanol ("Orgatics®" TC-750, manufactured by Matsumoto Fine Chemical Co., Ltd.) TA-21: Titanium tetran-n-butoxide ("Orgatics®" TA-21, manufactured by Matsumoto Fine Chemical Co., Ltd.) (Photoradical Initiator) IC-907: "Irgacure®" 907 (manufactured by BASF Japan Ltd.)

[0111] The evaluation of each synthesis example, example, and comparative example was carried out by the following method: (1) Solid content concentration: 1.0 g of the silicone solution obtained in each example and comparative example was weighed into an aluminum cup and heated on a hot plate at 250°C for 30 minutes to evaporate the liquid. The solid content remaining in the aluminum cup after heating was weighed and the solid content concentration [mass %] was calculated by (weight after heating / weight before heating) × 100.

[0112] (2) Weight-average molecular weight The silicone solutions obtained in each example and comparative example were diluted with tetrahydrofuran to a concentration of 0.25% by mass. The diluted solution was stirred at 100 rpm for 5 minutes using a mix rotor (MIX-ROTAR VMR-5, manufactured by AS ONE Corporation) to dissolve the silicone, and the filtrate filtered using a 0.2 μm filter (Z227536-100EA, manufactured by SIGMA Corporation) was used as the measurement sample. The GPC used was HLC-8220 (manufactured by Tosoh Corporation), and the column was a combination of TSKgel SuperHM-H (manufactured by Tosoh Corporation), TSKgel SuperHM-H (manufactured by Tosoh Corporation), and TSKgel SuperH2000 (manufactured by Tosoh Corporation) linked in that order. RI detection was performed using the RI detector built into the GPC. The sample input volume was 10 μL, the analysis time was 30 minutes, the flow rate was 0.4 mL / min, and the column temperature was 40°C. A calibration curve was prepared using polystyrene standards.

[0113] (3) Handling The resin layer of the printing plate master obtained in each example and comparative example was evaluated for handling based on tactile feel and condition, along with surface tackiness and film-forming properties, according to the following criteria: 5: No surface tackiness felt 4: Slight surface tackiness felt 3: Surface tackiness felt 2: Non-flowing viscous substance 1: Liquid.

[0114] (4) Photosensitivity The resin layer of the printing plate master obtained in each example and comparative example was exposed to light using a parallel light mask aligner (product name PLA-501F, manufactured by Canon Inc.) with a super high-pressure mercury lamp as the light source, through a mask having line and space patterns of widths of 100 μm, 80 μm, 60 μm, 50 μm, 40 μm, 30 μm, 20 μm, 15 μm, 10 μm and 5 μm, at an exposure dose of 2,000 mJ / cm². 2 Exposure was performed using the (i-line) with a gap of 100 μm.

[0115] Subsequently, the film was developed using "Isopar®" E (isoparaffin-based solvent, manufactured by ExxonMobil Chemical) at a developer temperature of 25°C, dried at 60°C for 60 minutes, and then further processed using a parallel light mask aligner (product name PLA-501F, manufactured by Canon Inc.) without a mask, at a light intensity of 12,000 mJ / cm². 2 The entire surface was exposed to light to obtain a flexographic printing plate.

[0116] Using a microscope, the relief of the flexographic printing plate was observed under magnification, and the relief depth was measured. Furthermore, the image reproduction quality was evaluated by using the narrowest line width among the formed reliefs as the resolution.

[0117] (5) Hardness The resin layer of the printing plate master obtained in each example and comparative example was subjected to a hardness test using an ultra-high pressure mercury lamp as the light source, without a mask, at a rate of 12,000 mJ / cm². 2The entire surface was exposed to light to obtain a flexographic printing plate. A circular sample with a diameter of 50 mm was cut from the obtained flexographic printing plate and placed on a 5 mm thick glass plate with the substrate side facing down. Under conditions of 23°C and 50% humidity, the needle of a durometer A hardness tester GS-709N (manufactured by Teclock Co., Ltd.) was gently pressed against the resin layer of the flexographic printing plate, and the hardness indicated by the needle was read. The hardness was measured at three randomly selected locations, and the average value was taken as the hardness. A hardness of 30 to 90 is preferred, and 40 to 80 is more preferred.

[0118] (6) Swelling properties with various inks As an indicator of swelling properties with various inks in each example and comparative example, the swelling properties with ethanol, a representative solvent that is particularly prone to swelling of the relief among the components commonly used in water-based inks and solvent-based inks, were evaluated.

[0119] The resin layer of the printing plate master obtained in each example and comparative example was subjected to a high-pressure mercury lamp as the light source, without a mask, at a pressure of 12,000 mJ / cm². 2 The entire surface was exposed to light to obtain a flexographic printing plate. The weight of each sample, cut from the obtained flexographic printing plate to a size of 2 cm x 2 cm, was measured, and then the samples were immersed in ethanol at 40°C for 24 hours. The weight of the samples after immersion was measured. The ease with which the samples swelled with various inks was evaluated using the following scoring system based on the weight change rate of the samples before and after immersion ({(weight after immersion - weight before immersion) / weight before immersion} × 100): Excellent: Weight change rate before and after ethanol immersion is less than 5% Very good: Weight change rate before and after ethanol immersion is 5% or more and less than 10% Good: Weight change rate before and after ethanol immersion is 10% or more and less than 15% Bad: Weight change rate before and after ethanol immersion is 15% or more.

[0120] (7) Tensile properties A resin film was formed on a PTFE sheet from the silicone composition obtained in each example and comparative example in the same manner as the formation of the resin layer in the printing plate original.

[0121] The resulting resin film was then subjected to a parallel light mask aligner (product name PLA-501F, manufactured by Canon Inc.) with a high-pressure mercury lamp as the light source, without using a mask, at a pressure of 12,000 mJ / cm². 2The entire surface was exposed to light to obtain a cured film.

[0122] The resulting cured film was peeled from the PTFE sheet, cut into 15 mm wide strips, and subjected to tensile testing at a tensile speed of 300 mm / min using a "Tensilon®" universal testing machine (RTG-1210, manufactured by Orientec Co., Ltd.). The elongation at the breaking point (unit: %GL) and the load at the breaking point (unit: MPa) were measured. Each measurement was performed twice, and the average value was calculated.

[0123] (8) Light transmittance per 1 mm thickness of resin layer at a wavelength of 400 nm Using the silicone compositions obtained in each example and comparative example, a resin layer was formed on a Tempax glass plate in the same manner as the resin layer formation for printing plates.

[0124] The ultraviolet-visible absorption spectrum of the resin layer obtained on a Tempax glass plate was measured using a spectrophotometer (Shimadzu MultiSpec-1500). Next, the resin layer was removed, and the ultraviolet-visible absorption spectrum of the substrate alone was measured and used as a reference. The ultraviolet-visible absorption spectrum of the resin layer was calculated from the difference between the spectrum of the resin layer obtained on the Tempax glass plate and the reference spectrum. Using the obtained ultraviolet-visible absorption spectrum and the film thickness of the resin layer, the light transmittance per 1 mm thickness of the resin layer at a wavelength of 400 nm was calculated.

[0125] (Example 1) In a 500 ml three-necked flask, 100 g of "Isopar®" E was placed as the solvent, 3.03 g of KBM-503 as the silane monomer constituting the T unit, and 2 g of TC-750 as the catalyst. The flask was immersed in an oil bath at 40°C and stirred for 30 minutes. Then, DMS-S21 was repeatedly added to the flask by filling a dropping funnel with the component constituting the D unit, and 100 g was added over 1 hour. No precipitation occurred in the flask contents during the addition of DMS-S21, and the solution was a homogeneous, colorless, transparent solution. Then, in order to promote polycondensation, the oil bath was heated to 120°C over 30 minutes. One hour after the start of heating, the internal temperature of the flask contents reached 100°C, and the mixture was heated and stirred for 2 hours thereafter (internal temperature 100-115°C). During the reaction, methanol and 2-propanol, the solvent contained in TC-750, distilled off. During heating and stirring, no precipitate formed in the solution in the flask, and it remained a uniform, clear solution.

[0126] After heating was complete, the contents of the flask were cooled to room temperature to obtain a silicone solution. The obtained silicone solution was transparent in appearance.

[0127] The solid content concentration of the obtained silicone solution was determined, and then "Isopar®" E was added to achieve a solid content concentration of 30% by mass, resulting in the silicone (SP-01) solution. The results of the evaluation using the method described above are shown in Table 1.

[0128] 5 g of silicone (SP-01) solution and 0.03 g of IC-907 as a photoradical initiator were added to a container, and the mixture was stirred until the components were homogeneous to obtain silicone composition (NS-01).

[0129] A 188 μm thick polyester (PET) film (Panaclea® ACM188, manufactured by Panac Co., Ltd.) with an adhesive layer was subjected to a casting of the obtained silicone composition (NS-01) onto the adhesive layer such that the resin layer thickness after drying was 1.0 mm. The composition was then dried at 60°C for 2.5 hours to form a resin layer and obtain a printing plate master. The results of the evaluation using the above method are shown in Table 2.

[0130] (Example 2) A silicone (SP-02) solution was obtained in the same manner as in Example 1, except that the amount of KBM-503 was changed as shown in Table 1. All of the obtained silicone solutions were transparent in appearance. The results of evaluation using the method described above are shown in Table 1.

[0131] Silicone composition (NS-02) was obtained in the same manner as in Example 1, except that silicone (SP-02) solution was used instead of silicone (SP-01) solution. A printing plate master was obtained in the same manner as in Example 1, except that silicone composition (NS-02) was used instead of silicone composition (NS-01). The results of evaluation using the above method are shown in Table 2.

[0132] (Examples 3-11) Silicone solutions (SP-03) to (SP-11) were obtained in the same manner as in Example 1, except that the type and amount of silicone raw materials were changed as shown in Table 1. All of the obtained silicone solutions were transparent in appearance. The results of evaluation using the method described above are shown in Table 1.

[0133] Silicone compositions (NS-03) to (NS-11) were obtained in the same manner as in Example 1, except that silicone solutions (SP-03) to (SP-11) were used instead of silicone solution (SP-01). Printing plates were obtained in the same manner as in Example 1, except that silicone compositions (NS-03) to (NS-11) were used instead of silicone composition (NS-01). The results of evaluation using the above method are shown in Table 2.

[0134]

[0135] In the table, Me represents a methyl group, MACPr represents a 3-methacryloxypropyl group, and Si represents a bond with another diorganosiloxane structure or Si in an organosiloxane structure.

[0136]

[0137] (Comparative Examples 1-2) Silicone (SP-12) to (SP-13) solutions were obtained in the same manner as in Example 1, except that the type and amount of silicone raw materials were changed as shown in Table 3. All of the obtained silicone solutions were transparent in appearance. The results of evaluation using the method described above are shown in Table 3.

[0138] Silicone compositions (NS-12) to (NS-13) were obtained in the same manner as in Example 1, except that silicone solutions (SP-12) to (SP-13) were used instead of silicone solution (SP-01). Printing plates were obtained in the same manner as in Example 1, except that silicone compositions (NS-12) to (NS-13) were used instead of silicone composition (NS-01). The results of evaluation using the above method are shown in Table 4.

[0139] (Comparative Example 3) As starting materials, 318.5 parts by mass (1.00 mol) of KBM-5803 and 914.0 parts by mass of isopropyl alcohol were mixed in the reactor. Once homogenized, 15.3 parts by mass of a 20% by mass aqueous solution of tetramethylammonium hydroxide and 95.5 parts by mass of water (total water 6.0 mol) were added, and the mixture was stirred at 25°C for 12 hours. Toluene was added, the mixture was washed with water, neutralized, and then the alcohol, toluene, etc. were removed by distillation. The solid content concentration of the obtained silicone solution was determined, and then "Isopar®" E was added to make the solid content concentration 30% by mass to obtain a silicone (SP-14) solution. The appearance of the obtained silicone solution was transparent. The results of evaluation by the above method are shown in Table 3.

[0140] Silicone composition (NS-14) was obtained in the same manner as in Example 1, except that silicone (SP-14) solution was used instead of silicone (SP-01) solution. A printing plate master was obtained in the same manner as in Example 1, except that silicone composition (NS-14) was used instead of silicone composition (NS-01). The results of evaluation using the above method are shown in Table 4.

[0141] (Comparative Example 4) α,ω-dimethoxypolydimethylsiloxane (m=4 (average)) was synthesized by the following method, and then a silicone (SP-15) solution was synthesized using it by the following method.

[0142] (Synthesis of α,ω-dimethoxypolydimethylsiloxane (m=4 (average))) In a 500 ml three-necked flask, 100 g of "Isopar®" E as the solvent, 120.2 g (1 mol) of KBM-22 as the silane monomer constituting the D unit, and 2.0 g of TC-750 as the catalyst were charged, and the flask was immersed in an oil bath at 40°C and stirred for 30 minutes. Then, to induce hydrolysis, 13.5 g (0.75 mol) of water was added to the flask over 1 hour using a dropper funnel. Subsequently, to induce polycondensation, the oil bath was heated to 120°C over 30 minutes. One hour after the start of heating, the internal temperature of the flask contents reached 100°C, and the mixture was heated and stirred for 2 hours thereafter (internal temperature 100-115°C). During the reaction, methanol and 2-propanol, the solvent contained in TC-750, distilled off.

[0143] After heating was complete, the contents of the flask were cooled to room temperature to obtain a silicone solution. The obtained silicone solution was transparent in appearance.

[0144] The solid content concentration of the obtained silicone solution was determined, and then "Isopar®" E was added to achieve a solid content concentration of 30% by mass to obtain the silicone (SP-15a) solution. The weight-average molecular weight (Mw) of silicone (SP-15a) was 342, and it was confirmed to be α,ω-dimethoxypolydimethylsiloxane with an average m=4.

[0145] (Synthesis of Silicone (SP-15) Solution) In a 500 ml three-necked flask, 333.3 g of Silicone (SP-15a) solution was added as a component constituting the repeating D unit, 39.2 g of KBM-503 as a silane monomer constituting the T unit, and 2.0 g of TC-750 as a catalyst. The flask was immersed in a 40°C oil bath and stirred for 30 minutes. Then, to induce hydrolysis, 4.7 g of water was added to the flask over 1 hour using a dropper funnel. No precipitation occurred in the flask contents during the addition of water, and the solution was a homogeneous, colorless, transparent solution. Subsequently, to induce polycondensation, the oil bath was heated to 120°C over 30 minutes. One hour after the start of heating, the internal temperature of the flask contents reached 100°C, and the mixture was heated and stirred for 2 hours (internal temperature 100-115°C). During the reaction, methanol and 2-propanol, the solvent contained in TC-750, distilled off. During heating and stirring, no precipitate formed in the solution in the flask, and it remained a uniform, clear solution.

[0146] After heating was complete, the contents of the flask were cooled to room temperature to obtain a silicone solution. The obtained silicone solution was transparent in appearance.

[0147] The solid content concentration of the obtained silicone solution was determined, and then "Isopar®" E was added to achieve a solid content concentration of 30% by mass, resulting in a silicone (SP-15) solution. The results of the evaluation using the method described above are shown in Table 3.

[0148] Silicone composition (NS-15) was obtained in the same manner as in Example 1, except that silicone (SP-15) solution was used instead of silicone (SP-01) solution. A printing plate master was obtained in the same manner as in Example 1, except that silicone composition (NS-15) was used instead of silicone composition (NS-01). The results of evaluation using the above method are shown in Table 4.

[0149] (Example 12) An α,ω-terminally silanol diphenylsiloxane-dimethylsiloxane copolymer (diphenylsiloxane: 8.4 mol%, m=60 (average)) was synthesized by the following method, and then a silicone (SP-16) solution was synthesized using it by the following method.

[0150] (Synthesis of α,ω-terminal silanol diphenylsiloxane-dimethylsiloxane copolymer (m=60 (average))) In a 500 ml three-necked flask, 100 g of "Isopar®" E was added as the solvent, 29.5 g of KBM-202SS as the silane monomer constituting the D unit, and 2 g of TC-750 as the catalyst. The flask was immersed in an oil bath at 40°C and stirred for 30 minutes. Subsequently, 100 g of DMS-S12 was added to the flask over 1 hour by filling a dropper funnel with the components that repeatedly constitute the D unit. Then, in order to promote polycondensation, the oil bath was heated to 120°C over 30 minutes. One hour after the start of heating, the internal temperature of the flask contents reached 100°C, and it was heated and stirred for 2 hours thereafter (internal temperature 100-115°C). During the reaction, methanol and 2-propanol, the solvent containing TC-750, distilled off.

[0151] After heating was complete, the contents of the flask were cooled to room temperature to obtain a silicone solution. The obtained silicone solution was transparent in appearance.

[0152] The solid content concentration of the obtained silicone solution was determined, and then "Isopar®" E was added to achieve a solid content concentration of 30% by mass, resulting in a silicone (SP-16a) solution.

[0153] The weight-average molecular weight (Mw) of the silicone (SP-16a) was 5200, and it was confirmed to be an α,ω-terminal silanol diphenylsiloxane-dimethylsiloxane copolymer with an average m of 60.

[0154] (Synthesis of Silicone (SP-16) Solution) In a 500 ml three-necked flask, 2.11 g of KBM-503 as the silane monomer constituting the T unit and 2 g of TC-750 as the catalyst were placed, and the flask was immersed in a 40°C oil bath and stirred for 30 minutes. Then, as the component constituting the repeated D unit, 333.33 g of Silicone (SP-16a) solution was added to the flask over 1 hour using a dropping funnel. Subsequently, to induce polycondensation, the oil bath was heated to 120°C over 30 minutes. One hour after the start of heating, the internal temperature of the flask contents reached 100°C, and the mixture was heated and stirred for 2 hours thereafter (internal temperature 100-115°C). During the reaction, methanol and 2-propanol, the solvent contained in TC-750, distilled off.

[0155] After heating was complete, the contents of the flask were cooled to room temperature to obtain a silicone solution. The obtained silicone solution was transparent in appearance.

[0156] The solid content concentration of the obtained silicone solution was determined, and then "Isopar®" E was added to achieve a solid content concentration of 30% by mass, resulting in a silicone (SP-16) solution. The results of the evaluation using the method described above are shown in Table 3.

[0157] Silicone composition (NS-16) was obtained in the same manner as in Example 1, except that silicone (SP-16) solution was used instead of silicone (SP-01) solution. A printing plate master was obtained in the same manner as in Example 1, except that silicone composition (NS-16) was used instead of silicone composition (NS-01). The results of evaluation using the above method are shown in Table 4.

[0158] (Example 13) A silicone (SP-17) solution was obtained in the same manner as in Example 1, except that the type and amount of silicone raw materials were changed as shown in Table 3. The obtained silicone solution was transparent in appearance. The results of evaluation using the method described above are shown in Table 3.

[0159] Silicone composition (NS-17) was obtained in the same manner as in Example 1, except that silicone (SP-17) solution was used instead of silicone (SP-01) solution. A printing plate master was obtained in the same manner as in Example 1, except that silicone composition (NS-17) was used instead of silicone composition (NS-01). The results of evaluation using the above method are shown in Table 4.

[0160]

[0161]

[0162] (Example 14) In a 500 ml three-necked flask, 100 g of "Isopar®" E was added as the solvent, 96.18 g (0.80 mol) of KBM-22 and 46.47 g (0.20 mol) of KBM-502 were added as components constituting the repeating D unit, and 2 g of TC-750 was added as the catalyst. The flask was immersed in an oil bath at 40°C and stirred for 30 minutes. Then, 17.66 g (0.98 mol) of water and 158.4 g of 2-propanol were added to the flask over 1 hour using a dropping funnel. Subsequently, the oil bath was heated to 120°C over 30 minutes for the purpose of polycondensation. One hour after the start of heating, the internal temperature of the flask contents reached 100°C, and the mixture was heated and stirred for 2 hours thereafter (internal temperature 100-115°C). During the reaction, methanol and 2-propanol distilled off.

[0163] After heating, the mixture was cooled to room temperature to obtain a solution of α,ω-dimethoxydimethylsiloxane-3-methacryloxypropylmethylsiloxane copolymer. The resulting solution was transparent in appearance.

[0164] To the entire volume of the obtained α,ω-dimethoxydimethylsiloxane-3-methacryloxypropylmethylsiloxane copolymer solution, 2.48 g (0.01 mol) of KBM-503 was added as a component constituting the T unit, and the flask was immersed in an oil bath at 40°C and stirred for 30 minutes. Then, 3.15 g (0.175 mol) of water and 28.35 g of 2-propanol were packed into a dropping funnel and added to the flask over 1 hour. Subsequently, the oil bath was heated to 120°C over 30 minutes for the purpose of polycondensation. One hour after the start of heating, the internal temperature of the flask contents reached 100°C, and heating and stirring were continued for 2 hours thereafter (internal temperature 100-115°C). During the reaction, methanol and 2-propanol distilled off.

[0165] After heating was complete, the contents of the flask were cooled to room temperature to obtain a silicone solution. The obtained silicone solution was transparent in appearance.

[0166] The solid content concentration of the obtained silicone solution was determined, and then "Isopar®" E was added to achieve a solid content concentration of 30% by mass, resulting in a silicone (SP-18) solution. The results of the evaluation using the method described above are shown in Table 5.

[0167] Silicone composition (NS-18) was obtained in the same manner as in Example 1, except that silicone (SP-18) solution was used instead of silicone (SP-01) solution. A printing plate master was obtained in the same manner as in Example 1, except that silicone composition (NS-18) was used instead of silicone composition (NS-01). The results of evaluation using the above method are shown in Table 8.

[0168] (Examples 15-18) Silicone (SP-19-22) solutions were obtained in the same manner as in Example 14, except that the type and amount of silicone raw materials were changed as shown in Table 5. The obtained silicone solutions were transparent in appearance. The results of evaluation using the method described above are shown in Table 5.

[0169] Silicone compositions (NS-19 to NS-22) were obtained in the same manner as in Example 1, except that silicone (SP-01) solution was replaced with silicone (SP-19 to NS-22) solution. Printing plates were obtained in the same manner as in Example 1, except that silicone compositions (NS-19 to NS-22) were replaced with silicone composition (NS-01). The results of evaluation using the above method are shown in Table 8.

[0170]

[0171] (Example 19) A silicone (SP-23) solution was obtained in the same manner as in Example 1, except that the type and amount of silicone raw materials were changed as shown in Table 6. The obtained silicone solution was transparent in appearance. The results of evaluation using the method described above are shown in Table 6.

[0172] Silicone composition (NS-23) was obtained in the same manner as in Example 1, except that silicone (SP-23) solution was used instead of silicone (SP-01) solution. A printing plate master was obtained in the same manner as in Example 1, except that silicone composition (NS-23) was used instead of silicone composition (NS-01). The results of evaluation using the above method are shown in Table 8.

[0173] (Example 20) In a 1000 ml three-necked flask, 100 g of "Isopar®" E was added as the solvent, 12.42 g (0.05 mol) of KBM-503 and 6.81 g (0.05 mol) of KBM-13 were added as silane monomers constituting the T unit, and 2 g of TC-750 was added as the catalyst. The flask was immersed in an oil bath at 40°C and stirred for 30 minutes. Then, for the purpose of hydrolysis, 0.90 g (0.05 mol) of water and 8.1 g of 2-propanol were added to the flask over 1 hour using a dropping funnel. Then, for the purpose of polycondensation, the oil bath was heated to 120°C over 30 minutes. One hour after the start of heating, the internal temperature of the flask contents reached 100°C, and it was heated and stirred for 2 hours thereafter (internal temperature 100-115°C). During the reaction, methanol and 2-propanol distilled off. After heating, the solution was cooled to room temperature to obtain a siloxane oligomer solution. The obtained solution was transparent in appearance.

[0174] The flask containing the siloxane oligomer solution was again immersed in a 40°C oil bath and stirred for 30 minutes. Then, DMS-S21 was repeatedly added to the flask at a rate of 420 g (0.1 mol) over 1 hour using a dropper funnel as the component constituting the D unit. No precipitation occurred in the flask contents during the addition of DMS-S21, and the solution remained uniform and colorless. Subsequently, the oil bath was heated to 120°C over 30 minutes for the purpose of polycondensation. One hour after the start of heating, the internal temperature of the flask contents reached 100°C, and the mixture was heated and stirred for 2 hours (internal temperature 100-115°C). Methanol distilled off during the reaction.

[0175] After heating was complete, the contents of the flask were cooled to room temperature to obtain a silicone solution. The obtained silicone solution was transparent in appearance.

[0176] The solid content concentration of the obtained silicone solution was determined, and then "Isopar®" E was added to achieve a solid content concentration of 30% by mass, resulting in a silicone (SP-24) solution. The results of the evaluation using the method described above are shown in Table 6.

[0177] Silicone composition (NS-24) was obtained in the same manner as in Example 1, except that silicone (SP-24) solution was used instead of silicone (SP-01) solution. A printing plate master was obtained in the same manner as in Example 1, except that silicone composition (NS-24) was used instead of silicone composition (NS-01). The results of evaluation using the above method are shown in Table 8.

[0178] (Examples 21-23) Silicone (SP-25-27) solutions were obtained in the same manner as in Example 20, except that the type and amount of silicone raw materials were changed as shown in Table 6. All of the obtained silicone solutions were transparent in appearance. The results of evaluation using the method described above are shown in Table 6.

[0179] Silicone compositions (NS-25 to NS-27) were obtained in the same manner as in Example 1, except that silicone (SP-25 to NS-27) solutions were used instead of silicone (SP-01) solution. Printing plates were obtained in the same manner as in Example 1, except that silicone compositions (NS-25 to NS-27) were used instead of silicone composition (NS-01) solution. The results of evaluation using the above method are shown in Table 8.

[0180]

[0181] (Examples 24-28) Silicone (SP-28-32) solutions were obtained in the same manner as in Example 1, except that the type and amount of silicone raw materials were changed as shown in Table 7. All of the obtained silicone solutions were transparent in appearance. The results of evaluation using the method described above are shown in Table 7.

[0182] Silicone compositions (NS-28 to NS-32) were obtained in the same manner as in Example 1, except that silicone (SP-01) solution was replaced with silicone (SP-28 to NS-32) solution. Printing plates were obtained in the same manner as in Example 1, except that silicone compositions (NS-28 to NS-32) were replaced with silicone composition (NS-01). The results of evaluation using the above method are shown in Table 8.

[0183]

[0184] In the table, Me represents a methyl group, AcPr represents a 3-acryloxypropyl group, Vi represents a vinyl group, and Si represents a bond with another diorganosiloxane structure or Si in an organosiloxane structure.

[0185]

[0186] (Examples 29-32) 5 g of silicone (SP-01) solution and 0.03 g of IC-907 as a photoradical initiator were added to a container, and the metal compounds listed in Table 9 were added. The mixture was stirred until the components were homogeneous to obtain silicone compositions (NS-33-36).

[0187] A printing plate master was obtained in the same manner as in Example 1, except that silicone compositions (NS-33 to NS-36) were used instead of silicone composition (NS-01). The results of evaluation using the method described above are shown in Table 9.

[0188] (Example 33) For the silicone composition (NS-01) prepared in Example 1, (8) the light transmittance per 1 mm thickness of the resin layer at 400 nm was measured.

[0189] The light transmittance per 1 mm thickness of the resin layer made of the silicone composition (NS-01) at 400 nm was 90%.

[0190]

Claims

1. Silicones having a polydiorganosiloxane structure represented by the following general formula (1) and an organosiloxane structure represented by the following general formula (2): In the above general formula (1), R 1 and R 2 Each independently represents a hydrogen atom, a C1-C8 alkyl group, a C2-C8 alkenyl group, a C6-C12 aryl group, a C6-C12 (meth)acryloxyalkyl group, a C6-C12 glycidoxyalkyl group, or a C8-C15 (3,4-epoxycyclohexyl)alkyl group; m represents a range of 6 to 10,000; m R 1 and R 2 These may be the same or different; in the general formula (2) above, R 3 R represents a hydrogen atom, a C1-C8 alkyl group, a C2-C8 alkenyl group, a C6-C12 aryl group, a C6-C12 (meth)acryloxyalkyl group, a C6-C12 glycidoxyalkyl group, a C8-C15 (3,4-epoxycyclohexyl)alkyl group, or a C7-C12 aralkyl group; R 4 This indicates a bond with a hydrogen atom, a C1-C6 alkyl group, or other diorganosiloxane structure or organosiloxane structure with Si; however, R 1 ~R 3 Of these, at least one is a (meth)acryloxyalkyl group having 6 to 12 carbon atoms.

2. The silicone according to claim 1, wherein the weight-average molecular weight is 15,000 to 500,000.

3. The silicone according to claim 1 or 2, having 0.01 to 2.0 mol / kg of (meth)acryloxyalkyl group.

4. The silicone according to claim 1 or 2, containing 0.01 to 10 mol% of the organosiloxane structure represented by the general formula (2).

5. R in the aforementioned general formula (1) 1 and R 2 are both methyl groups, the silicone according to claim 1 or 2.

6. R in the general formula (2) 4 The silicone according to claim 1 or 2, wherein the bond is with another diorganosiloxane structure or Si of an organosiloxane structure.

7. R in the above general formulas (1) and (2) 1 ~R 3 The silicone according to claim 1 or 2, wherein at least one of them is an alkenyl group having 2 to 8 carbon atoms.

8. R in the above general formulas (1) and (2) 1 ~R 3 The silicone according to claim 1 or 2, wherein at least one of them is an aryl group having 6 to 12 carbon atoms.

9. A silicone composition comprising the silicone according to claim 1 or 2 and a metal compound comprising a metal selected from titanium, zirconium, tin, and aluminum, wherein the metal compound comprises a metal compound selected from a metal alkoxide, metal acylate, metal siloxide, a complex of the metal and a β-diketone compound, a complex of the metal and a β-ketoester compound, a complex of the metal and a β-diester compound, and a complex of the metal and a cyclic diene compound.

10. A silicone composition containing the silicone and photoradical initiator according to claim 1 or 2.

11. A cured product obtained by curing the silicone composition according to claim 10.

12. A printing plate master having a resin layer made of the silicone composition according to claim 10 on a substrate.

13. A method for manufacturing a printing plate, comprising, in this order, an exposure step of irradiating the printing plate master according to claim 12 with light to partially photocrosslink the resin layer, and a development step of removing the unexposed portion of the resin layer.

14. A method for manufacturing a printed material, comprising the steps of: applying ink to the relief of a printing plate obtained by the manufacturing method described in claim 13; and transferring the ink to a substrate.