Heat-resistant alloy with nitrogen resistance, and cracking tube for an ammonia gas thermal cracking apparatus.
A heat-resistant alloy with optimized C, Mn, P, S, Ni, Cr, and optional Nb, Ti, Zr, W, Mo composition addresses nitriding and creep crack resistance issues in ammonia gas thermal cracking, ensuring high-temperature integrity and efficiency.
Patent Information
- Application Number
- BR112025024227
- Authority / Receiving Office
- BR · BR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-08
- Filing Date
- 2024-05-09
- Publication Date
- 2026-11-10
AI Technical Summary
The challenge is to develop a heat-resistant alloy that exhibits excellent nitriding resistance and high-temperature creep crack resistance, particularly for use in high-pressure ammonia gas thermal cracking processes, where nitrogen atoms generated by thermal cracking can nitride the alloy, compromising its integrity.
A heat-resistant alloy composition comprising specific percentages of C, Mn, P, S, Ni, Cr, and optionally Nb, Ti, Zr, W, and Mo, optimized for high-temperature performance and nitriding resistance, with a centrifugally cast body, ensuring high creep crack resistance and nitriding resistance.
The alloy demonstrates excellent nitriding resistance and high-temperature creep crack resistance, suitable for high-pressure ammonia gas thermal cracking apparatus, reducing facility volume and enhancing downstream processes like power generation.
Abstract
Description
1 / 21 Heat-resistant alloy with nitrogen resistance, and cracking tube for an ammonia gas thermal cracking apparatus. TECHNICAL FIELD
[0001] The present invention relates to a heat-resistant alloy with excellent resistance to nitriding. FUNDAMENTALS OF THE TECHNIQUE
[0002] Decarbonization is necessary to achieve carbon neutrality. The use of hydrogen gas is attracting attention as a next-generation energy source that does not generate carbon dioxide. However, there are challenges in the safe and efficient storage and transport of hydrogen gas.
[0003] Therefore, expectations are placed on ammonia. Ammonia is a hydrogen carrier with a high hydrogen density, is easy to liquefy for transport and storage, and can be stably imported from abroad. Although this ammonia can be used as fuel by burning it without cracking, the hydrogen gas obtained by thermal cracking of ammonia is used in many technologies, such as hydrogen power generation turbines, fuel cells, and hydrogen reduction steelmaking. For this reason, hydrogen production by thermal cracking of ammonia is very useful.
[0004] Patent Literature 1 discloses a thermal ammonia cracking apparatus that uses a catalyst. In this thermal ammonia cracking apparatus, ammonia gas preheated to about 300°C to 700°C is introduced into a reactor containing a catalyst, thereby thermally cracking the ammonia gas into hydrogen gas and nitrogen gas. Petition 870250101819, dated 06 / 11 / 2025, page 12 / 83 2 / 21 PRIOR ART DOCUMENT(S) PATENT DOCUMENT
[0005] Patent Document 1: Publication of Patent Application Japanese 2022-109042 SUMMARY OF THE INVENTION PROBLEM TO BE SOLVED BY THE INVENTION
[0006] In ammonia gas, the nitrogen atoms generated by thermal cracking diffuse into the alloy of the cracking tube and nitride the alloy. For this reason, the heat-resistant alloy that constitutes the cracking tube must have resistance to nitriding. In general, Al, Cr, Mo, and Ti are elements that facilitate the ease of combination with nitrogen to form nitrides, while a higher Ni content makes nitriding more difficult.
[0007] For example, in nitriding equipment (gas nitriding furnaces) for gas nitriding of metals, high-Ni stainless steels or Ni-based alloys are used as furnace materials.
[0008] The hydrogen production process via ammonia cracking is desirably a high-pressure process. This is advantageous for reducing the volume of mass production plants and for supplying downstream processes such as power generation. High pressure as used in this document refers to a pressure greater than about 1.0 MPa, with higher pressures being more desirable. In this context, operating at high pressure requires the cracking tube to have high-temperature creep rupture resistance.
[0009] One objective of the present invention is to provide a heat-resistant alloy that is excellent in nitriding resistance and high-temperature creep crack resistance. Petition 870250101819, dated 06 / 11 / 2025, page 13 / 83 3 / 21 WAYS TO SOLVE THE PROBLEMS
[0010] The heat-resistant alloy of the present invention comprises, in % by mass: C: 0.2% to 0.6% Yes: greater than 0% to 2.5% or less, Mn: greater than 0% to 2.0% or less, P: 0.03% or less, S: 0.03% or less, Ni: 33.0% to 50.0%, Cr: 24.0% to 50.0%, the remainder being Fe and impurities, and optionally including: Nb: greater than 0% to 1.8% or less, Rare earth elements: greater than 0% to 0.5% or less, Ti: greater than 0% to 0.5% or less, and / or Zr: greater than 0% to 0.5% or less W: greater than 0% to 2.0% or less and / or Mo: greater than 0% to 0.5% or less.
[0011] The heat-resistant alloy preferably comprises: C: 0.45% to 0.55% Yes: greater than 0% to 1.5% or less, Ni: 33.0% to 50.0%, Cr: 24.0% to 27.0% Nb: greater than 0% to 1.0% or less.
[0012] The heat-resistant alloy preferably comprises: C: 0.4% to 0.6%, Si: greater than 0% to 2.0% or less, Ni: 40.0% to 50.0% Petition 870250101819, dated 06 / 11 / 2025, p. 14 / 83 4 / 21 Cr: 24.0% to 38.0% Nb: 0.5% to 1.8%.
[0013] The heat-resistant alloy preferably comprises: C: 0.2% to 0.5% Ni: 40.0% to 50.0%, Cr: 30.0% to 50.0%, and optionally, Ti: greater than 0% to 0.4% or less.
[0014] The creep resistance of the heat-resistant alloy is ideally 20 MPa or more at 900°C for 1,000 hours.
[0015] The activation energy for nitrogen diffusion in the heat-resistant alloy is desirably 35 kJ / mol or more.
[0016] The heat-resistant alloy is preferably a centrifugally cast body.
[0017] The heat-resistant alloy is preferably used in a high-temperature atmosphere of 500°C or higher.
[0018] The cracking tube for a thermal ammonia gas cracking apparatus of the present invention can be formed from the heat-resistant alloy described above. EFFECTS OF THE INVENTION
[0019] The heat-resistant alloy according to the present invention is excellent in nitriding resistance and creep cracking resistance at high temperatures. Therefore, it is suitable for cracking tubes in ammonia gas thermal cracking apparatus used at high temperatures of 500°C or more. The cracking tube is particularly suitable for application in ammonia gas thermal cracking apparatus used in Petition 870250101819, dated 06 / 11 / 2025, page 15 / 83 5 / 21 high-pressure processes, which is advantageous for reducing the volume of mass production facilities and for supplying downstream processes such as power generation. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1: Figure 1 is a cross-sectional photograph of the microstructure of the test piece from Comparative Example 1.
[0021] Figure 2: Figure 2 is a graph representing the creep fracture resistance and the nitrided layer thickness for the test pieces of the First Example.
[0022] Figure 3: Figure 3 is a graph representing the creep rupture resistance and activation energy for the test pieces of the second example.
[0023] Figure 4: Figure 4 shows EPMA images of the test pieces from Inventive Example 1 and Comparative Example 1. METHOD FOR CARRYING OUT THE INVENTION
[0024] Hereafter, embodiments of the present invention will be described in detail. Unless otherwise specified, % means % by mass.
[0025] The heat-resistant alloy with excellent nitriding resistance of the present invention is used, for example, as a cracking tube in a thermal cracking apparatus for ammonia gas. The cracking tube, through which ammonia gas flows as feedstock, is heated from the outside between 500°C and 1000°C in a catalyst-free environment, where thermal cracking, represented by 2NH3^N2+3H2, is carried out to produce nitrogen gas and hydrogen gas.
[0026] The heat-resistant alloy with excellent nitriding resistance of the present invention comprises, in % by mass: C: 0.2% to 0.6% Petition 870250101819, dated 06 / 11 / 2025, page 16 / 83 6 / 21 Yes: greater than 0% to 2.5% or less, Mn: greater than 0% to 2.0% or less, P: 0.03% or less, S: 0.03% or less, Ni: 33.0% to 50.0%, Cr: 24.0% to 50.0%, with the remainder being Fe and impurities.
[0027] From here on, the reasons for limiting the components will be explained. C: 0.2% to 0.6%
[0028] C has the effect of improving castability and increasing high-temperature creep fracture resistance. It also has the effect of increasing high-temperature strength by forming carbides with Cr or optional elements such as Ti and Nb. Therefore, at least 0.2% is included. However, if the C content is too high, primary Cr7C3 carbides tend to form extensively, and excessive precipitation of secondary carbides during heat treatment leads to a decrease in ductility and toughness. Therefore, the upper limit is set at 0.6%. The lower limit for C content is preferably 0.20%, 0.25%, and more preferably 0.30%. The upper limit for C content is preferably 0.60%, 0.55%, and more preferably 0.50%. Yes: greater than 0% to 2.5% or less
[0029] Silicon (Si) is included as a deoxidizer in the molten alloy to enhance the fluidity of the molten alloy and to improve oxidation resistance. However, excessive addition of Si leads to a decrease in ductility, a decrease in high-temperature creep fracture resistance, and deterioration of Petition 870250101819, dated 06 / 11 / 2025, page 17 / 83 7 / 21 surface quality after casting and a decrease in weldability. Therefore, the upper limit for Si content is defined as 2.5%, preferably 2.0% and more preferably 1.7%. Mn: greater than 0% to 2.0% or less
[0030] Mn acts as a deoxidizer for the molten alloy, to fix S in the molten metal, thus improving weldability and ductility. However, excessive addition of Mn leads to a decrease in high-temperature creep fracture resistance and reduces oxidation resistance, so the upper limit is set at 2.0%. The Mn content is more preferably 1.5% or less. P: 0.03% or less, S: 0.03% or less
[0031] P and S are impurities that are inevitably introduced during melting, and a content of 0.03% or less is permitted. The amount of these impurities should be as low as possible and can be zero. Ni: 33.0% to 50.0%
[0032] Ni is an essential element for ensuring excellent nitriding resistance, as well as for ensuring cyclic oxidation resistance and microstructural stability, high-temperature creep resistance, and for stabilizing the austenitization of the heat-resistant alloy. Ni also contributes to improved high-temperature resistance and oxidation resistance through combined addition with Cr, or optionally with W, Ti, and Zr. It is also known as an element that contributes to improved nitriding resistance. This is because nitrogen hardly dissolves in Ni, and it is expected to have the effect of inhibiting nitrogen diffusion. Petition 870250101819, dated 06 / 11 / 2025, p. 18 / 83 8 / 21 in the material. Therefore, at least 33.0% Ni is included. On the other hand, even if Ni is added excessively, its effect saturates and is also economically disadvantageous, so the upper limit is set at 50.0%. The lower limit for the Ni content is preferably 37.0% and more preferably 40.0%. Cr: 24.0% to 50.0%
[0033] Cr contributes to improved high-temperature resistance and cyclic oxidation resistance. Furthermore, Cr, along with Ni and Fe, exhibits excellent heat resistance in high-temperature ranges above 1,000°C. Additionally, Cr combines with C to form carbides, which has the effect of increasing high-temperature resistance. Regarding nitriding, it is expected to provide the effect of suppressing the growth of the nitrided layer due to nitrogen diffusion, fixing nitrogen atoms through the formation of fine nitrides. Therefore, at least 24.0% is included. However, Cr is an element that readily combines with N, and C in Cr carbides (Cr23C6) is replaced by N, causing nitriding of the alloy. Furthermore, excessive formation of Cr carbides and Cr nitrides leads to a decrease in ductility; therefore, a lower content is preferable, and the upper limit is set at 50.0%.The lower limit for Cr content is 24.0% and the upper limit for Cr content is preferably 50.0%, 46.0%, and most preferably 43.0%. remaining iron and impurities
[0034] The remainder is Fe and impurities. Impurities include those that are inevitably mixed in during melting. Fe is an element that facilitates the entry and diffusion of nitrogen into the material, and a lower content is desirable for nitriding resistance. Although Fe is the remainder, it is desirable that the content Petition 870250101819, dated 06 / 11 / 2025, p. 19 / 83 9 / 21 of Fe should be up to 40.0%.
[0035] The heat-resistant alloy with the above composition may optionally contain the following elements. Nb: greater than 0% to 1.8% or less
[0036] Nb is an element that readily forms carbides and contributes to improved creep fracture resistance and high-temperature tensile strength. Nb also contributes to improved aging ductility. Regarding nitriding resistance, similar to Cr, it is expected to have the effect of suppressing the growth of the nitrided layer due to nitrogen diffusion by the fixation of nitrogen atoms through nitride formation. Therefore, optionally containing Nb is preferable. A lower limit for Nb of 0.3% is preferred. On the other hand, excessive addition of Nb causes a decrease in ductility, so the upper limit is 1.8%, preferably 1.5%. Rare earth elements (REM): greater than 0% to 0.5% or less
[0037] REM refers to the 18 elements, including the 15 elements of the lanthanide series from La to Lu in the periodic table, plus Y, Hf and Sc. The REM to be contained in the heat-resistant alloy may be primarily Ce, La and Nd, and it is preferable that the total amount of these three elements represent about 80% or more of the total rare earth elements and, more preferably, about 90% or more. REM dissolves in the base material and contributes to improved oxidation resistance, so it is desirable to contain them optionally. To exert these effects, when adding REM, it is preferable to add an appropriate amount with an upper limit of 0.5%. Petition 870250101819, dated 06 / 11 / 2025, p. 20 / 83 10 / 21 Ti: greater than 0% to 0.5% or less, and / or Zr: greater than 0% to 0.5% or less
[0038] Ti and Zr are optionally added, one or both, to improve oxidation resistance and high-temperature compressive creep resistance. Ti is an element that readily forms carbides and also contributes to improved high-temperature tensile strength. Regarding nitriding resistance, similar to Cr, it is expected to have the effect of suppressing the growth of the nitrided layer due to nitrogen diffusion by the fixation of nitrogen atoms through nitride formation. Zr also has a denitrifying effect. To obtain these effects, Ti and Zr can optionally be added. On the other hand, Ti is also an element that readily combines with N, and can cause deterioration of castability due to a decrease in the fluidity of the molten alloy, and there is a risk that machining may become difficult. Therefore, when added together, its upper limit is 0.5%, preferably 0.3%.Since Zr reduces hot workability (e.g., bending), when added, its upper limit is 0.5%, preferably 0.4%. W: greater than 0% to 2.0% or less, and / or Mo: greater than 0% to 0.5% or less
[0039] W and Mo are elements with properties that dissolve in the base material, strengthen the austenite phase of the base material, and improve creep crack resistance, and one or both may optionally be included. However, excessive W and Mo content leads to a decrease in ductility and carburization resistance. Furthermore, excessive W and Mo content leads to a decrease in the oxidation resistance of the base material, and Mo exerts twice the effect of W in an equivalent base. Petition 870250101819, dated 06 / 11 / 2025, page 21 / 83 11 / 21 Therefore, the upper limit when adding W is 2.0% and the upper limit when adding Mo is 0.5%. The upper limit for W is more preferably 1.8% and the upper limit for Mo is more preferably 0.4%. Ta: 0% to 0.5%
[0040] Ta may optionally be included to form carbides with the unavoidable impurity C contained in the alloy based on Ni, thus refining the crystal grains within the alloy based on Ni is used to improve the high-temperature resistance and corrosion resistance of the Ni-based alloy. However, excessive content can hinder the workability of the Ni-based alloy and cause a decrease in strength. Therefore, when adding Ta, an upper limit for its content is 0.5% and more preferably 0.3%.
[0041] In one embodiment, the heat-resistant alloy of the present invention comprises: C: 0.45% to 0.55% Yes: greater than 0% to 1.5% or less, Mn: greater than 0% to 2.0% or less, P: 0.03% or less, S: 0.03% or less, Ni: 33.0% to 50.0%, Cr: 24.0% to 27.0% Nb: greater than 0% to 1.0% or less, with the remainder being Fe and impurities, and optionally including: Rare Earth Elements: greater than 0% to 0.5% or less, Ti: greater than 0% to 0.5% or less. W: greater than 0% to 1.0% or less, and / or Mo: greater than 0% to 0.5% or less. Petition 870250101819, dated 06 / 11 / 2025, p. 22 / 83 12 / 21
[0042] In one embodiment, the heat-resistant alloy of the present invention comprises: C: 0.4% to 0.6% Yes: greater than 0% to 2.0% or less, Mn: greater than 0% to 2.0% or less, P: 0.03% or less, S: 0.03% or less, Ni: 40.0% to 50.0%, Cr: 24.0% to 38.0% Nb: 0.5% to 1.8%, with the remainder being Fe and impurities, and optionally including: Rare Earth Elements: greater than 0% to 0.5% or less, Ti: greater than 0% to 0.5% or less. W: greater than 0% to 1.0% or less, and / or Mo: greater than 0% to 0.5% or less.
[0043] In one embodiment, the heat-resistant alloy of the present invention comprises: C: 0.2% to 0.5% Yes: greater than 0% to 2.5% or less, Mn: greater than 0% to 2.0% or less, P: 0.03% or less, S: 0.03% or less, Ni: 40.0% to 50.0%, Cr: 30.0% to 50.0%, with the remainder being Fe and impurities, and optionally including: Nb: greater than 0% to 1.8% or less, Rare Earth Elements: greater than 0% to 0.5% or less, Ti: greater than 0% to 0.5% or less. Petition 870250101819, dated 06 / 11 / 2025, p. 23 / 83 13 / 21 W: greater than 0% to 1.0% or less, and / or Mo: greater than 0% to 0.5% or less.
[0044] The heat-resistant alloy of the present invention has excellent nitriding resistance. This is because the alloy contains a large amount of Ni, which is nitriding-resistant, forming a stable austenite phase, and because it does not contain many elements that readily combine with nitrogen atoms to form nitrogen compounds. Nitriding resistance can be determined, for example, by the thickness of the nitrided layer formed on the molten body under the nitriding environment shown in the Examples below.
[0045] Furthermore, the heat-resistant alloy of the present invention contains the elements described above and has a high activation energy for nitrogen diffusion and excellent resistance to nitriding. This can reduce the amount of nitrogen that penetrates the molten body in a nitriding environment and prevent thickening of the nitrided layer. The activation energy for nitrogen diffusion is preferably 35 kJ / mol or more, more preferably 38 kJ / mol or more, and even more preferably 40 kJ / mol or more. A higher activation energy for nitrogen diffusion is preferable. However, referring to the Second Example, the upper limit is 100 kJ / mol, preferably 80 kJ / mol.
[0046] The method for deriving the nitrogen diffusion activation energy is as follows. The heat-resistant alloy is exposed to a nitriding atmosphere at different temperatures, and the diffusion coefficient D at each temperature is derived according to the parabolic diffusion rule. Then, an Arrhenius plot is created from the reciprocal of the temperature and the natural logarithm of the diffusion coefficient D. Then, the Petition 870250101819, dated 06 / 11 / 2025, page 24 / 83 The activation energy of the heat-resistant alloy (14 / 21) was derived from the slope of the Arrhenius plot. The diffusion coefficient D was derived by taking data at multiple points in the range of 600°C to 950°C.
[0047] The heat-resistant alloy of the present invention has excellent creep crack resistance, especially high-temperature creep crack resistance. This is because it contains C, Ni, and optionally Nb and Ti. When used as a cracking tube in an ammonia gas thermal cracking apparatus, the creep crack resistance is preferably such that the cracking time is 1,000 hours or more at a test temperature of 900°C and a stress of 20 MPa, desirably 1,000 hours or more at a test temperature of 900°C and a stress of 25 MPa, and more desirably 1,000 hours or more at a test temperature of 900°C and a stress of 30 MPa.
[0048] The heat-resistant alloy of the present invention also has excellent casting capability. This is due to the component design which optimizes the content of alloying elements such as Ni and Cr, and takes into account the fluidity of the melt. A cast body made of the heat-resistant alloy of the present invention can be produced by mixing the component elements to be within the above composition range and using a casting method such as centrifugal casting or static casting.
[0049] As described above, the heat-resistant alloy of the present invention is excellent in nitriding resistance, high-temperature creep cracking resistance, and also in castability. Therefore, it is suitable for application in cracking tubes of ammonia gas thermal cracking apparatus used in nitriding environments where ammonia gas is present. Petition 870250101819, dated 06 / 11 / 2025, page 25 / 83 15 / 21 high pressure is supplied in a high temperature atmosphere of 500 °C or higher. Among them, a cracking tube made of the heat-resistant alloy of the present invention is particularly suitable for application in ammonia gas thermal cracking apparatus used in high-pressure processes, which is advantageous for reducing the volume of mass production installations and for supplying downstream processes such as power generation. EXAMPLES <<Primeiro Exemplo> >
[0050] Cracking tubes with the alloy compositions (unit: % by mass, remaining Fe and impurities) of Inventive Examples 1 to 3 and Comparative Examples 1 to 3 shown in Table 1 were produced by centrifugal casting and their casting capability was verified. Comparative Example 1 is SUS310S, Comparative Example 2 is Inconel 625 (registered trademark) and Comparative Example 3 is Hastelloy C276 (registered trademark). Table 1 C Si Mn P Ξ Ni Cr Nb Ti w REM Hey. Inventive 1 0.5 0.8 0.8 0.01 0.01 35 25 i}5 0.15 0 0 Hey. Inventive 2 Q5 1.6 1 0.01 0.01 45 31 l}8 0.15 0 0 Hey. Inventive J Q3 2.2 ^8 0.005 0.01 48 41 0 0.2 1 0 Hey. Comparative 1 0.01 0.3 1 0.02 0.001 20 24 0 0 0 0 Hey. Comparative 2 0.015 i}2 0.1 Q005 0.001 61 21.5 3.6 0.2 0 0^2 Ei. Comparative 3 0.01 I}1 1 0.04 0.01 55 16 0 0 0 0
[0051] Test specimens were cut from each of the cracking tubes obtained and a creep rupture test and an ammonia exposure test were conducted. The details of the tests are described below and the results are shown in Table 2. Petition 870250101819, dated 06 / 11 / 2025, page 26 / 83 16 / 21 Table 2 Creep fracture resistance at 50°C for 1,000 h (MPa) Thickness of nitrided layer at 600°C for 100°C (µm) Inventive Example 1 53.9 80.5 Inventive Example 2 46.9 22.1 Inventive Example 3 35.9 0 Comparative Example 1 8.0 108°C Comparative Example 2 18.6 12°C Comparative Example 1 approximately 20 20.2
[0052] The heat-resistant alloy of the present invention contains slightly higher amounts of carbon and silicon to optimize castability and exhibits superior castability compared to the materials listed as comparative examples. For production by the centrifugal casting method, excellent castability, i.e., good melt fluidity, is desirable, and the heat-resistant alloy of the present invention is reasonable in this respect. The evaluation of castability is carried out in the Second Example.
[0053] Furthermore, the heat-resistant alloy of the present invention has excellent resistance to oxidation at high temperatures. The elements that contribute to the resistance to oxidation at high temperatures are Ni and Cr. Ni itself is an element with high resistance to oxidation at high temperatures. Cr forms a chromium oxide film on the surface to protect the surface and suppress oxidation of the material.
[0054] The heat-resistant alloy of the present invention contains Ni and Cr in nearly equal amounts. Therefore, it is possible to have excellent high-temperature oxidation resistance with other Petition 870250101819, dated 06 / 11 / 2025, p. 27 / 83 17 / 21 properties, such as high resistance to creep rupture. < Creep Rupture Resistance Test >
[0055] The creep rupture resistance of the test pieces at a temperature of 900 °C for 1,000 hours was measured according to JIS Z 2271. The results are shown in Table 2. Note that the value for Comparative Example 2 is at 927 °C.
[0056] Creep resistance is preferably MPa or more, desirably 25 MPa or more, and most desirably 30 MPa or more. With reference to Table 2, it can be seen that all Inventive Examples have a creep rupture strength of at least 30 MPa, indicating that they have sufficient creep rupture strength. On the other hand, Comparative Examples 1 and 2 showed low creep rupture strength. Comparative Example 3 was approximately 20 MPa. Ammonia Exposure Test
[0057] The test piece was placed in a furnace tube located inside an electric furnace, and the interior of the furnace tube was replaced with nitrogen gas. Then, after raising the temperature of the furnace tube to 600°C, it was replaced with ammonia gas. The test piece was exposed to the ammonia gas for 100 hours and then removed.
[0058] Each of the test pieces was then polished in the thickness direction, and the cross-section was observed with an optical microscope to measure the thickness of the nitrided layer. The results are shown in Table 2. For reference, a microstructural cross-sectional photograph of the test piece from Comparative Example 1 is shown in Figure 1. The part indicated by reference number 10 is the nitrided layer.
[0059] Regarding nitriding properties, if the thickness of the nitrided layer formed by the ammonia exposure test is Petition 870250101819, dated 06 / 11 / 2025, page 28 / 83 18 / 21 of 100 µm or less, it can be determined that the nitriding resistance is good. With reference to Table 2, it can be seen that Inventive Examples 1 to 3, Comparative Example 2, and Comparative Example 3 have a nitrided layer thickness of 100 µm or less, indicating excellent nitriding resistance. On the other hand, Comparative Example 1, as shown in Figure 1, has a nitrided layer 10 with a thickness greater than 100 µm, indicating low nitriding resistance. As for Inventive Example 3, no nitrided layer was observed, indicating extremely excellent nitriding resistance. In Inventive Examples 1 and 2, a nitrided layer was formed, but in Inventive Example 2 it was as thin as 22.1 µm, and Inventive Example 1 was also 100 µm or less, showing good nitriding resistance. < Creep Crack Resistance and Nitriding Resistance >
[0060] The creep fracture resistance and the thickness of the nitrided layer formed by the ammonia exposure test for each of the test pieces described above were represented in a graph with creep fracture resistance on the vertical axis and nitrided layer thickness on the horizontal axis. The graph is shown in Figure 2.
[0061] In the graph in Figure 2, the further to the upper left, the better the creep resistance and the better the nitriding resistance. Inventive Examples 1 to 3 are located in the upper left corner of the graph, showing that they are excellent in creep resistance and nitriding resistance. In Figure 2, indicated by a dashed line is the range consisting of a nitrided layer thickness of 100 µm or less, which is considered to have nitriding resistance and a more desirable lower limit for creep resistance. Petition 870250101819, dated 06 / 11 / 2025, p. 29 / 83 19 / 21 for creep of 30 MPa or more. All Inventive Examples are within the dotted line, while all Comparative Examples are outside the dotted line. <<Segundo Exemplo> >
[0062] For the test pieces of Inventive Examples 1 to 3 and Comparative Examples 1 and 2 produced in the First Example, the nitrogen diffusion activation energy was derived and the casting capability was investigated. <Energia de Ativação>
[0063] The method for deriving the activation energy of nitrogen diffusion is as described above. The results are shown in Table 3. It was found that all Inventive Examples 1 to 3 have high activation energy for nitrogen diffusion. In particular, Inventive Example 3 showed a higher value compared to Inventive Examples 1 and 2. Comparative Example 2 also had a high activation energy for nitrogen diffusion. Table 3 includes the thickness of the nitrided layer of the First Example, and it can be seen that the higher the activation energy, the thinner the nitrided layer. Table 3 Activation energy (kJ / mol) Thickness of the nitrided layer at 600°C for 1000 h (pm) Creep rupture strength at 900°C for 1000 h (MPa) Casting capacity Inventive Ex. 1 38.2 80.5 53.9 Good Inventive Ex. 2 47.9 22.1 46.9 Good Inventive Ex. 5 63.7 0 35.9 Good Comparative Ex. 1 31.4 108.1 8.0 Fair Comparative Ex. 2 41.5 12.0 18.6 Poor Petition 870250101819, dated 06 / 11 / 2025, p. 30 / 83 20 / 21 < Creep Rupture Strength and Activation Energy >
[0064] Figure 3 shows a graph plotting creep rupture strength on the vertical axis and nitrogen diffusion activation energy on the horizontal axis. The creep rupture strength values are those measured in the First Example (see Table 3). In the graph in Figure 3, the further towards the upper right corner, the better the creep rupture strength and the higher the nitrogen diffusion activation energy, thus the better the nitriding resistance. Inventive Examples 1 to 3 are located in the upper right corner of the graph, indicating that they excel in creep rupture strength and nitriding resistance.Indicated by a dashed line in Figure 3 is the range defined by a desirable lower limit for the nitrogen diffusion activation energy of 35 kJ / mol or more, which is considered to have nitriding resistance, and a more desirable lower limit for creep rupture resistance of 30 MPa or more. All Inventive Examples are within the dashed line, while all Comparative Examples are outside the dashed line. <Capacidade de Fundição>
[0065] Castability was judged by observing the surface condition of the test pieces to assess the fluidity of the molten mass. Castability is rated in three grades: “Good”, “Fair”, and “Poor”. With reference to Table 3, all Inventive Examples 1 to 3 have good castability. This is due to the slightly higher addition of carbon and silicon. Comparative Example 2 has a relatively high activation energy but is poor in castability. <Análise EPMA>
[0066] For the test pieces of Inventive Example 1 and Example Petition 870250101819, dated 06 / 11 / 2025, p. 31 / 83 21 / 21 Comparative Example 1, the ammonia exposure test of the First Example was conducted by altering the temperature condition to 850 °C. The other conditions were the same as in the First Example. The nitrogen distribution in the obtained test pieces was analyzed by EPMA (Electron Probe Microanalyzer). Figure 4 shows (a) EPMA image of Inventive Example 1 and (b) EPMA image of Comparative Example 1. With reference to the figures (the reference signal 10 is a nitrided layer and the area below it is a test piece), the nitrided layer 10 is observed in both test pieces. But since Inventive Example 1 has a high activation energy for nitrogen diffusion, it can be seen that the nitrided layer formed 10 is significantly thinner compared to Comparative Example 1.
[0067] The above description is intended to explain the present invention and should not be interpreted as limiting the invention described in the claims or narrowing its scope. Furthermore, it is evident that the configuration of each part of the present invention is not limited to the examples described above, and various modifications are possible within the technical scope described in the claims. Petition 870250101819, dated 06 / 11 / 2025, page 32 / 83
Claims
1 / 2 - CLAIMS - 1. HEAT-RESISTANT ALLOY WITH NITROGEN RESISTANCE, the alloy, characterized in that it comprises, in mass %: C: 0.2% to 0.6%, Si: greater than 0% to 2.5% or less, Mn: greater than 0% to 2.0% or less, P: 0.03% or less, S: 0.03% or less, Ni: 33.0% to 50.0%, Cr: 24.0% to 50.0%, the remainder being Fe and impurities, and optionally including: Nb: greater than 0% to 1.8% or less, Rare earth elements: greater than 0% to 0.5% or less, Ti: greater than 0% to 0.5% or less, and / or Zr: greater than 0% to 0.5% or less, and W: greater than 0% to 2.0% or less and / or Mo: greater than 0% to 0.5% or less.
2. Heat-resistant alloy according to claim 1, characterized in that C: 0.45% to 0.55%, Si: greater than 0% to 1.5% or less, Ni: 33.0% to 50.0%, Cr: 24.0% to 27.0%, Nb: greater than 0% to 1.0% or less.
3. Heat-resistant alloy according to claim 1, characterized in that C: 0.4% to 0.6%, Si: greater than 0% to 2.0% or less, Ni: 40.0% to 50.0%, Cr: 24.0% to 38.0%, Nb: 0.5% to 1.8%.
4. Heat-resistant alloy according to claim 1, characterized in that C: 0.2% to 0.5%, Ni: 40.0% to 50.0%, Cr: 30.0% to 50.0%, and optionally, Ti: greater than 0% to 0.4% or less.
5. Heat-resistant alloy, according to any one of claims 1 to 4, characterized in that its creep rupture strength is 20 MPa or more at 900 °C for 1,000 hours.
6. Heat-resistant alloy according to any one of claims 1 to 4, characterized in that the activation energy for nitrogen diffusion is 35 kJ / mol or more.
7. Heat-resistant alloy according to any one of claims 1 to 4, characterized in that the heat-resistant alloy is a centrifugally cast body.
8. Heat-resistant alloy, according to any one of claims 1 to 4, characterized in that the heat-resistant alloy is used in a high-temperature atmosphere of 500°C or higher.
9. CRACKING TUBE FOR AN AMMONIA GAS THERMAL CRACKING APPARATUS, characterized in that it is formed from the heat-resistant alloy as defined in any one of claims 1 to 4. Petition 870250101819, dated 06 / 11 / 2025, page 36 / 83