LÂMINA DE BARBEAR OU DEPILAR COMPREENDENDO UM PARILENO E TITÂNIO

A titanium-parylene coating on razor blades addresses the issues of non-uniformity and environmental concerns of PTFE coatings, providing improved lubrication and durability with reduced cutting force.

BR112025025066A2Pending Publication Date: 2026-11-10BIC VIOLEX SINGLE MEMBER SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
BR112025025066
Authority / Receiving Office
BR · BR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-02
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing razor blade lubrication coatings made of perfluoroalkyl or polyfluoroalkyl substances like PTFE lack uniformity, reduce hardness and corrosion resistance due to high sintering temperatures, and pose environmental concerns.

Method used

A razor blade with a first layer of titanium and a second layer of parylene, applied through thin-film deposition, which improves adhesion and reduces cutting force.

Benefits of technology

The titanium-parylene coating results in a more uniform, durable, and environmentally friendly lubrication layer with reduced cutting force, enhancing shaving performance and durability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present disclosure relates to a razor blade provided with a first layer comprising titanium and a second layer comprising a parylene The present disclosure also relates to a razor cartridge comprising at least one razor blade provided with a first layer comprising titanium and a second layer comprising a parylene. The present disclosure further relates to method for coating a razor blade with a first layer comprising titanium and a second layer comprising a parylene.
Need to check novelty before this filing date? Find Prior Art

Description

1 / 29 “RAZING OR DEPILATING BLADE COMPRISING A PARYLENE AND TITANIUM” CROSS-REFERENCE TO RELATED REQUESTS

[0001] This request claims priority over the Request for European Patent EP 23174334.5, filed on May 19, 2023, the full content of which is incorporated herein by reference. TECHNICAL FIELD

[0002] The present invention relates to the field of razor blades. More specifically, the present invention relates to razor blades comprising lubrication layers. BACKGROUND

[0003] Shaving heads (also known as safety razor heads, shaving cartridges, or safety razor cartridges) are generally part of a shaving assembly that includes a shaving handle. A shaving head typically comprises one or more cutting members, each including a razor blade, and being disposed between a main longitudinal side and a rear longitudinal side of the shaving head. In use, a user holds the shaving handle in the shaving direction and places the shaving head in contact with a portion of skin. By moving the shaving head in the shaving direction, unwanted hairs are removed.

[0004] Razor blades for razor cartridges typically comprise a lubrication layer. Because lubrication layers are typically applied by coating, they may also be called lubrication coatings. The purpose of the lubrication layer is to reduce the cutting force required during the shaving process. By reducing the required cutting force, the Petition 870250104623, dated 11 / 14 / 2025, pp. 91 / 133 2 / 29 A razor or epilator can exhibit better glide during the shaving or epilation action, which in turn would facilitate the use of the razor or epilator. Additionally, the reduction in cutting force required can result in less pulling force exerted on the hairs and consequently on the hair follicles, which can reduce discomfort for the user. Furthermore, the lubrication coating can also reduce friction between the razor or epilator blade and the user's skin, which can also improve the glide of the razor or epilator. In addition, the reduced cutting force required and the better glide can result in a better shaving or epilation result, for example, fewer short and prickly hairs, light cuts and deep cuts.

[0005] Typically, lubricating coatings for razor blades are made of a perfluoroalkyl or polyfluoroalkyl (PFAS) substance, such as polytetrafluoroethylene (PTFE). Razor blades coated with PTFE are effective at cutting hair, exhibit little friction on the skin, and a low degree of traction on the hair.

[0006] However, PTFE coatings can also have disadvantages. First, PTFE coatings are typically applied by spraying PTFE particles onto a razor blade and subsequently sintering these particles at temperatures above the melting point of PTFE. The resulting coating may lack uniformity, which in turn can result in reduced shaving performance of the razor blades. Furthermore, the increased temperatures during the sintering step can reduce the hardness and corrosion resistance of the razor blade. Finally, PTFE is a highly persistent material and is therefore a subject of environmental concerns.

[0007] The present disclosure aims to address one or more of the above-mentioned issues in the optimization of lubrication layers. SUMMARY

[0008] In a first aspect, the present revelation is Petition 870250104623, dated 11 / 14 / 2025, pp. 92 / 133 3 / 29 refers to a razor or depilatory blade having a first layer comprising titanium and a second layer comprising parylene.

[0009] In some embodiments, the first layer may comprise titanium as metallic titanium.

[0010] In some embodiments, parylene may be selected from the group of Parylene-N, Parylene-C, Parylene-F and combinations thereof and, in particular, parylene may be selected from Parylene-N and / or Parylene-C.

[0011] In some embodiments, the razor blade may comprise a cutting edge portion and the first layer and second layer may be provided in the cutting edge portion.

[0012] In some embodiments, the razor blade or shaving device may be configured to be disposed within a cartridge of the razor or shaving device.

[0013] In some embodiments, the first layer may have a thickness between about 5 nm and about 70 nm, more specifically between about 10 nm and about 60 nm and, in particular, between about 20 nm and about 50 nm.

[0014] In some embodiments, the second layer may have a thickness between about 0.005 pm and about 5 pm, more specifically between about 0.02 pm and about 2 pm and, in particular, between about 0.1 pm and about 1 pm.

[0015] In some embodiments, the second layer may not comprise holes, in particular holes with a diameter between about 5 nm and about 200 nm.

[0016] In some embodiments, the second layer may comprise less than 1% by weight, more specifically less than 0.1% by weight and, in particular, none or substantially no polytetrafluoroethylene.

[0017] In some forms, the razor or shaving blade may be additionally fitted with a hard coating. Petition 870250104623, dated 11 / 14 / 2025, pp. 93-133 4 / 29

[0018] In some embodiments, the rigid coating may comprise a ceramic, metallic and / or non-metallic coating.

[0019] In some embodiments, the ceramic may comprise a boride and / or a carbide and, in particular, titanium diboride.

[0020] In some applications, the ceramic may comprise titanium, boron, and carbon.

[0021] In some embodiments, the non-metallic coating may comprise diamond-like carbon.

[0022] In some embodiments, the metal of the hard coating may comprise chromium.

[0023] In some embodiments, the first layer may be placed between the rigid coating and the second layer.

[0024] In some embodiments, the first layer may be provided directly on the razor or shaving blade. Alternatively, in some embodiments, the hard coating may be provided directly on the razor or shaving blade. Alternatively, in some embodiments, an intermediate layer may be provided on the razor or shaving blade and the hard coating may be provided on the intermediate layer. In some embodiments, the intermediate layer may comprise a metal, more specifically niobium and / or titanium, even more specifically titanium and, in particular, metallic titanium.

[0025] In some embodiments, the razor or shaving blade may essentially comprise or consist of a metal, in particular a stainless steel.

[0026] In some embodiments, the cross-section of the cutting edge portion may have a substantially symmetrical tapered geometry terminating in a blade tip, the cross-section may have a central longitudinal axis originating from the blade tip, and the cutting edge portion may have a thickness between 1.5 pm and 2.4 pm measured at a distance of 5 pm along the central longitudinal axis of the blade tip.

[0027] In a second aspect, the present revelation is Petition 870250104623, dated 11 / 14 / 2025, pp. 94 / 133 5 / 29 refers to a razor or shaving device cartridge comprising at least one razor or shaving blade according to any of the preceding claims.

[0028] In a third aspect, the present disclosure relates to a method for coating a razor blade. The method comprises coating a razor blade with a first layer comprising titanium, more specifically by physical vapor deposition, and coating the razor blade with a second layer comprising parylene, more specifically by chemical vapor deposition (CVD).

[0029] In some embodiments, coating the razor or shaving blade with titanium may be done before coating the razor or shaving blade with parylene.

[0030] In some embodiments, the coating of the razor or shaving blade with the first layer comprising titanium can be done by ion bombardment.

[0031] In some embodiments, coating the razor blade with parylene by chemical vapor-phase deposition may comprise sublimating a dimer of a parylene precursor, pyrolyzing the sublimated dimer of a parylene precursor to achieve parylene precursor monomers, and depositing the parylene precursor monomers onto the razor blade or shaving blade.

[0032] In some embodiments, the sublimation of the dimer of a parylene precursor can be carried out at a temperature between about 130 °C and about 190 °C, more specifically between about 150 °C and about 180 °C and / or at a pressure between about 0.5 Torr and about 2 Torr, more specifically between about 0.8 Torr and about 1.2 Torr.

[0033] In some embodiments, the pyrolysis of the sublimated dimer of a parylene precursor can be carried out at a temperature of between about 400 °C and about 800 °C, more specifically between about 500 °C and about 700 °C and / or at a pressure between about 0.2 Torr and about 1 Torr, more Petition 870250104623, dated 11 / 14 / 2025, pp. 95-133 6 / 29 specifically between approximately 0.4 Torr and approximately 0.6 Torr.

[0034] In some embodiments, the deposition of the parylene precursor monomers can be carried out at a temperature between about 10 °C and about 50 °C, more specifically between about 17 °C and about 28 °C and / or at a pressure between about 0.01 Torr and about 0.5 Torr, more specifically between about 0.05 Torr and about 0.2 Torr.

[0035] In some embodiments, the method for coating a razor or shaving blade may further comprise an annealing step, in particular, the razor or shaving blade may be annealed at a temperature between about 300 °C and about 400 °C, more specifically at a temperature between about 330 °C and about 370 °C in an inert gas atmosphere, in particular after the deposition of parylene.

[0036] In some forms, the razor or shaving blade may be annealed for a duration of between about 10 and about 20 minutes, more specifically between about 1 minute and about 5 minutes. BRIEF DESCRIPTION OF THE FIGURES

[0037] Figure 1 is a schematic drawing of the edge portion of a razor blade in cross-sectional view, with a first layer and a second layer provided on the edge portion of the blade.

[0038] Figure 2 is a schematic drawing of the edge portion of a razor blade in cross-sectional view, wherein a first layer and a second layer are provided on the edge portion of the blade on top of a rigid coating and an intermediate layer.

[0039] Figure 3 is a schematic drawing of the edge portion of a razor blade in cross-sectional view, wherein a first sublayer and a second sublayer are provided in the edge portion of the blade on top of the first coating and a hard coating.

[0040] Figure 4 shows a comparison of the shear force of the third sample batch and the first comparative sample batch. Petition 870250104623, dated 11 / 14 / 2025, pp. 96 / 133 7 / 29

[0041] Figure 5 shows a comparison of the shear force of the first, second, third and fourth sample batch.

[0042] Figure 6 shows a comparison of the shear force of the third sample batch and the fifth sample batch.

[0043] Figure 7 shows a comparison of the frictional force of the second sample batch compared to a second comparative sample batch.

[0044] Figure 8 shows a comparison of the shear force of the sixth sample batch and the first comparative sample batch. DETAILED DESCRIPTION

[0045] Hereafter, a detailed description will be given of the present disclosure. The terms or words used in the description and aspects of the present disclosure should not be interpreted restrictively, as having only their common or dictionary meanings, and should, unless expressly defined otherwise in the description below, be interpreted according to their usual technical meaning, as established in the relevant technical field. The detailed description will refer to specific modalities to better illustrate the present disclosure; however, it should be understood that the disclosure presented is not limited to these specific modalities.

[0046] As mentioned above, the lubricating coatings typically used for razor blades are made of a perfluoroalkyl or polyfluoroalkyl (PFAS) substance, such as polytetrafluoroethylene (PTFE), since razor blades coated with PTFE are effective at cutting hair, exhibit little friction on the skin, and low traction on the hair.

[0047] However, PTFE coatings may lack uniformity as a result of particle spray deposition, which in turn may result in reduced shaving or hair removal performance of razors or shaving blades. Furthermore, increased temperatures (for extended periods) during the sintering step may reduce hardness and... Petition 870250104623, dated 11 / 14 / 2025, pp. 97 / 133 8 / 29 resistance to corrosion from razor blades or shaving. Additionally, PTFE is a highly persistent material and is therefore a subject of environmental concerns.

[0048] An emerging alternative to PTFE coatings (or any other PFAS coating) are coatings comprising selected polymers from the parylene group, which also exhibit a low coefficient of friction. However, parylene coatings may not adhere to razor blades or shaving blades.

[0049] It has been surprisingly discovered that by first depositing titanium on the razor blade or shaving blade and subsequently depositing parylene on the razor blade or shaving blade, the adhesion of the parylene can be improved.

[0050] Consequently, in a first aspect, the present disclosure relates to a razor or shaving blade having a first layer comprising titanium and a second layer comprising parylene. The razor or shaving blade according to the first aspect exhibits a low cutting force. Cutting force is a measure of the amount of force required to cut hair.

[0051] In this way, it was surprisingly found that, in addition to resulting in improved adhesion, the use of the first layer comprising titanium can result in a reduction in the required shear force.

[0052] The adhesion of PTFE coatings to a razor blade is typically made possible by the use of a chromium coating. However, it has been found that the adhesion of parylene to chromium can be weak, which can result in an increase in the required cutting forces. The increased cutting forces required can result from the parylene coating being removed from the razor blade during shaving or hair removal. Removal can occur as early as the first shave or hair removal when the parylene is supplied in chromium, but may only occur gradually when the parylene is supplied in titanium. Surprisingly, it has been found that by supplying a titanium layer, as opposed to chromium, for the parylene to adhere to, the required cutting force of the razor blade is reduced. Petition 870250104623, dated 11 / 14 / 2025, pp. 98 / 133 9 / 29 can be substantially reduced.

[0053] In some embodiments, the first layer may comprise titanium as metallic titanium. Metallic titanium may be particularly suitable for parylene to bond to. The term “metallic titanium” is widely known and, among others, receives its common meaning in the art. Additionally or alternatively, the term “metallic titanium” may refer to a reduced state of titanium wherein its oxidation number is 0. Additionally or alternatively, the term “metallic titanium” may refer to the titanium atoms comprised in the first layer forming metallic bonds with each other. In some embodiments, the first layer may consist of, or essentially consist of, titanium (as detailed above).

[0054] In some embodiments, parylene may be selected from the group of Parylene-N, Parylene-C, Parylene-F and combinations thereof. In particular, in some embodiments, parylene may be selected from Parylene-N and / or Parylene-C. It has been surprisingly found that a second layer comprising Parylene-N may result in reduced shear force compared with other parylenes. However, a second layer comprising Parylene-C may result in lower shear force after multiple uses of the razor or shaving blade, compared with Parylene-N.

[0055] In some forms, the second layer may consist of, or essentially consist of, parylene (as detailed above).

[0056] The term “parylene” refers to a polymer whose backbone consists of para-benzenediyl rings -C6H4 connected by 1,2-ethanediyl bridges -CH2-CH2-. Substitution of the para-benzenediyl rings results in different types of parylenes.

[0057] N-parylene (or parylene-N) is an unsubstituted parylene. N-parylene can be obtained by polymerization of para-xylylene. N-parylene consists of the following repeating unit: Petition 870250104623, dated 11 / 14 / 2025, pp. 99 / 133 10 / 29

[0058] Parylene-C (or parylene-C) is a gold-colored parylene. Parylene-C can be obtained by polymerization of 2,8-dichlorotrichloro[8.2.2.24,7]hexadeca-1(12),4,6,10,13,15-hexaene. Parylene-C consists of the following repeating unit:

[0059] Parylene-F (or parylene-F) is a fluorinated parylene, in particular where the four hydrogens in the aryl ring are replaced by fluorine. Parylene-F can be obtained by polymerization of 4,5,7,8,12,13,15,16Octafluoro[2.2]paracyclophane. Parylene-F consists of the following repeating unit: FF

[0060] Additionally, it was surprisingly found that the combination of Parylene-C and Parylene-N results in a reduced shear strength compared to a second layer comprising Parylene-C or Parylene-N. In particular, the second layer may comprise a first sublayer comprising Parylene-C and a second sublayer comprising Parylene-N. In some embodiments, the first sublayer comprising Parylene-C may be provided in the first layer and the second sublayer comprising Parylene-N may be provided in the first sublayer. In some alternative embodiments, the first sublayer may comprise Parylene-N and the second sublayer may comprise Parylene-C.

[0061] In some embodiments, the razor or shaving blade may essentially comprise or consist of a metal, in particular a stainless steel. Stainless steel razor or shaving blades may exhibit high strength, hardness and corrosion resistance. In addition, the blades Petition 870250104623, dated 11 / 14 / 2025, pp. 100 / 133 11 / 29 stainless steel razors or shaving blades may be easier to process compared to, for example, ceramic razors or shaving blades. The razor or shaving blade may have been ground to form an edge. More specifically, the razor or shaving blade may be shaped so that it terminates in a cutting edge portion having substrate sides that converge to a substrate edge. Consequently, in some embodiments, the razor blade may comprise a cutting edge portion, and the first layer and second layer may be provided in the cutting edge portion. As mentioned above, the second layer comprising parylene may be configured to act as a lubricating coating. The lubricating coating may improve the cutting of hairs by the razor or shaving blade. Therefore, it may be beneficial to provide the first layer and second layer at least in the cutting edge portion.

[0062] When referring to a cutting edge portion that is provided with a first layer and a second layer, it should be understood that such reference does not merely refer to the strict geometric edge of the razor or shaving blade, but rather to the edge in view of the cutting action it performs. Therefore, the term cutting edge portion is also intended to encompass the parts of the sides of the razor or shaving blade that are immediately adjacent to the strict geometric edge of the cutting edge portion.In exemplary embodiments, the region forming the cutting edge portion extends away from the strict geometric edge of the cutting edge portion along a central longitudinal axis of the cutting edge portion by a distance of: approximately 5 pm or less, approximately 10 pm or less, approximately 15 pm or less, approximately 25 pm or less, approximately 50 pm or less, approximately 75 pm or less, approximately 100 pm or less, approximately 125 pm or less, approximately 150 pm or less, approximately 175 pm or less, or approximately 200 pm or less. The first layer and / or second layer may generally follow the surface and contour of the underlying cutting edge portion. In particular, the second layer may form the outermost layer arranged in the razor blade or shaving blade. Therefore, the second layer may... Petition 870250104623, dated 11 / 14 / 2025, pp. 101 / 133 12 / 29 form the edge of the blade.

[0063] In some embodiments, the first layer may have a thickness between about 5 nm and about 70 nm, more specifically between about 10 nm and about 60 nm and, in particular, between about 20 nm and about 50 nm. In some embodiments, the second layer may have a thickness between about 0.005 pm and about 5 pm, more specifically between about 0.02 pm and about 2 pm and, in particular, between about 0.1 pm and about 1 pm.

[0064] In some embodiments, the razor blade may be configured to be disposed within a razor cartridge. The use of lubricating coatings, such as the second layer, may be particularly beneficial for razor blades used in razor cartridges.

[0065] In some embodiments, the razor or shaving blade may additionally be provided with a hard coating. The hard coating may improve the hardness of the razor or shaving blades, thereby increasing the blade's durability, in particular its service life. In some embodiments, the hard coating may comprise a ceramic, metallic and / or non-metallic coating. In some embodiments, the ceramic may comprise a boride and / or a carbide and, in particular, titanium diboride. In some embodiments, the ceramic may comprise titanium, boron and carbon. In some embodiments, the metal of the hard coating may comprise chromium. In some embodiments, the non-metallic coating may comprise diamond-like carbon.

[0066] When referring to a hard coating, it should be understood that the coating itself may be more rigid than the coated cutting edge portion and / or that the coated cutting edge portion may be hardened in its entirety, compared to an uncoated substrate portion. The hardness of the hard coating or coated cutting edge portion can be determined using a nanoindenter. During the nanoindentation process, a rigid tip whose properties (mechanical properties, geometry, tip radius, etc.) are known penetrates the hard coating sample to be analyzed. For example, Petition 870250104623, dated 11 / 14 / 2025, pp. 102 / 133 13 / 29 A Berkovich tip can be used for indentation tests. The load applied to the indenter tip was increased as the tip penetrated further into the sample until a penetration depth of 50 to 100 nm was reached. At this point, the load was kept constant for a period of time and then the indenter was removed. The area of ​​residual indentation in the sample was measured. The hardness H is defined as the maximum load Pmax divided by the residual indentation area A: Pm max A

[0067] In some embodiments, the hard coating or cutting edge portion may exhibit hardness between about 5 GPa and about 30 GPa, more specifically between about 10 GPa and about 20 GPa.

[0068] In some embodiments, the first layer may be disposed between the hard coating and the second layer. As mentioned above, the second layer may form the outermost layer provided in the razor or shaving blade. Consequently, the first layer may be provided closer to the razor or shaving blade than the second layer, and the hard coating may be disposed closer to the razor or shaving blade than the first layer.

[0069] In some embodiments, the first layer may be provided directly on the razor or shaving blade. In this case, the razor or shaving blade may not comprise a hard coating.

[0070] Alternatively, in some embodiments, the hard coating may be provided directly on the razor or shaving blade. In particular, a hard coating comprising, essentially consisting of or consisting of, a metal, in particular chromium, may be disposed directly on the razor or shaving blade.

[0071] Some rigid coatings, in particular rigid coatings comprising a ceramic, may exhibit improved adhesion to a razor blade or shaving blade when an intermediate layer bonds the Petition 870250104623, dated 11 / 14 / 2025, pp. 103 / 133 14 / 29 rigid coating to razor or shaving blade. Consequently, in some embodiments, an intermediate layer may be provided on the razor or shaving blade and the rigid coating may be provided on the intermediate layer. In some embodiments, the intermediate layer comprises titanium and / or niobium, more specifically titanium and, in particular, metallic titanium.

[0072] Figure 1 shows the cutting edge portion 100 of a first exemplary razor blade 10 according to the first aspect. In the cutting edge portion 100, a first layer 102 comprising titanium is provided. A second layer 104 comprising parylene is provided in the first layer 102, in particular as the outermost layer provided in the razor or shaving blade 10.

[0073] Figure 2 shows the cutting edge portion 200 of a second exemplary razor blade 20 according to the first aspect. In the cutting edge portion 200, an intermediate layer 206 is provided, in which a rigid coating 208 is provided. The rigid coating 208 of the exemplary razor blade 20 may, in particular, be a ceramic. In the rigid coating 208, a first layer 202 comprising titanium is provided. A second layer 204 comprising parylene is then provided in the first layer 202, in particular as the outermost layer.

[0074] Figure 3 shows the cutting edge portion 300 of a third exemplary razor blade 30 according to the first aspect. In the cutting edge portion 300, a hard coating 308 is provided directly. Some hard coatings, for example, chrome, may not require an intermediate layer. In the hard coating 300, a first layer 302 comprising titanium is provided. In the first layer 302, a first sublayer 304a comprising Parylene-C is provided and in the same a second sublayer 304b comprising Parylene-N.

[0075] As will be explained in more detail below, the first layer and the second layer can be applied using thin-film deposition technologies. In particular, the first layer can be deposited by Petition 870250104623, dated 11 / 14 / 2025, pp. 104 / 133 15 / 29 physical vapor deposition. In addition, the second layer can be deposited by chemical vapor deposition. As a result, the first and second layers can be applied to relatively small blade edge portions. In particular, the first and second layers can be applied to smaller blade edge portions compared to conventional PTFE coatings prepared by spraying. Smaller blade edge portions can reduce the cutting force required during shaving or hair removal. Consequently, in some embodiments, the cross-section of the cutting edge portion may have a substantially symmetrical tapered geometry terminating in a blade tip, the cross-section may have a central longitudinal axis originating from the blade tip, and the cutting edge portion may have a thickness between 1.5 µm and 2.4 µm measured at a distance of 5 µm along the central longitudinal axis of the blade tip.In some embodiments, the edge portion of the blade has a thickness between about 4.6 pm and about 6.8 pm, in particular between about 4.62 and about 6.74 pm, measured at a distance of about 20 pm along the central longitudinal axis of the blade tip. In some embodiments, the edge portion of the blade has a thickness between about 10.3 pm and 14.4 pm, in particular between about 10.32 and about 14.35 pm, measured at a distance of about 50 pm along the central longitudinal axis of the blade tip. In some embodiments, the edge portion of the blade has a thickness between about 19.8 pm and 27.6 pm, in particular between about 19.82 and about 27.52 pm, measured at a distance of about 100 pm along the central longitudinal axis of the blade tip.

[0076] The razor or depilatory blades described above may be manufactured by any suitable means. More specifically, the preparation and grinding of the blade substrate may be carried out by any suitable means, for example, as disclosed in US 2017 / 136641 A1, which is incorporated by reference in its entirety.

[0077] In some forms, the second layer may comprise less than 1% by weight, more specifically less than 0.1% by weight. Petition 870250104623, dated 11 / 14 / 2025, pp. 105 / 133 16 / 29 and, in particular, none or substantially none of polytetrafluoroethylene (PTFE) or any other perfluoroalkyl or polyfluoroalkyl substance (PFAS). As mentioned above, the second layer comprising parylene can be used to replace lubrication coatings comprising PTFE (or any other PFAS). Furthermore, as mentioned above, the first and second layers can be applied by thin-film deposition technologies, as opposed to PTFE coatings which require a spraying step. Thin-film deposition technologies can allow for the deposition of more uniform layers compared to spraying. Additionally, thin-film deposition technologies can allow for the deposition of the layer with fewer defects compared to spraying. Consequently, in some embodiments, the second layer may not comprise holes, in particular without holes with a diameter between about 5 nm and about 200 nm.

[0078] In a second aspect, the present disclosure relates to a razor or shaving device cartridge comprising at least one razor or shaving blade as described above. As mentioned above, the lubrication coating provided by the second layer may be particularly beneficial for razor or shaving blades for razor or shaving device cartridges.

[0079] In a third aspect, the present disclosure relates to a method for coating a razor blade. The method comprises coating a razor blade with a first layer comprising titanium, more specifically by physical vapor phase deposition, and coating the razor blade with a second layer comprising parylene, more specifically by chemical vapor phase deposition.

[0080] In some embodiments, the titanium coating of the razor blade can be applied before the parylene coating of the razor blade. Consequently, the parylene can be deposited onto the titanium, thus improving the adhesion of the parylene to the razor blade.

[0081] In some forms, the blade coating Petition 870250104623, dated 11 / 14 / 2025, pp. 106 / 133 17 / 29 of shaving or depilatory blades with a first layer comprising titanium can be made by ion bombardment. In some embodiments, the coating of the shaving or depilatory blade with a first layer comprising titanium can be carried out, in particular, by DC ion bombardment, RF ion bombardment, closed-field unbalanced magnetron sputtering (CFUMS), ion beam ion bombardment, cathodic arc deposition and high-power impulse magnetron sputtering (HiPIMS) using titanium targets sintered in an Ar atmosphere.

[0082] Examples of chemical vapor deposition (CVD) technologies include Low Pressure CVD (LPCVD), Atmospheric Pressure CVD (APCVD), Atomic Layer Deposition (ALD), and Metalorganic CVD (MOCVD) using precursors. In some embodiments, coating the razor blade with parylene by chemical vapor deposition may comprise the steps of sublimating a dimer of a parylene precursor, pyrolyzing the sublimated dimer of a parylene precursor to achieve parylene precursor monomers, and depositing the parylene precursor monomers onto the razor blade, in particular in such a way that the parylene precursor monomers polymerize. Parylene precursor monomers can polymerize on the razor blade or depilate during or after deposition. Polymerization of parylene precursor monomers can lead to the formation of a parylene layer.If the second layer comprises a first sublayer containing a first parylene, such as Parylene-C, and a second sublayer containing a second parylene, such as Parylene-N, the above steps of chemical vapor deposition (sublimation, pyrolysis, and deposition) can be performed individually for each sublayer.

[0083] In some embodiments, the sublimation of the dimer of a parylene precursor can be carried out at a temperature between about 130 °C and about 190 °C, more specifically between about 150 °C and about 180 °C. Petition 870250104623, dated 11 / 14 / 2025, pp. 107 / 133 18 / 29 and / or at a pressure between about 0.5 Torr and about 2 Torr, more specifically between about 0.8 Torr and about 1.2 Torr.

[0084] In some embodiments, the pyrolysis of the sublimated dimer of a parylene precursor can be carried out at a temperature between about 400 °C and about 800 °C, more specifically between about 500 °C and about 700 °C and / or at a pressure between about 0.2 Torr and about 1 Torr, more specifically between about 0.4 Torr and about 0.6 Torr.

[0085] In some embodiments, the deposition of the parylene precursor monomers can be carried out at a temperature between about 10 °C and about 50 °C, more specifically between about 17 °C and about 28 °C and / or at a pressure between about 0.01 Torr and about 0.5 Torr, more specifically between about 0.05 Torr and about 0.2 Torr.

[0086] In some embodiments, the method may comprise a film growth step after the deposition of the parylene precursor monomers, wherein the film growth step is carried out at a temperature between about 50 °C and about 100 °C, more specifically between about 60 °C and about 80 °C, and / or at a pressure between about 0.0001 Torr and about 0.05 Torr, more specifically between about 0.0005 Torr and about 0.002 Torr. The film growth step may improve the polymerization of the parylene precursor monomers deposited on the razor blade or shaving blade.

[0087] In some embodiments, the method for coating a razor blade may additionally comprise an annealing step. In this case, the razor blade may be annealed at a temperature between about 300 °C and about 400 °C, more specifically at a temperature between about 330 °C and about 370 °C in an inert gas atmosphere, particularly after the deposition of parylene, or if performed after the film growth step. In some embodiments, the razor blade may be annealed for a duration between about 10 and about 20 minutes, more specifically between about 1 minute and about 5 minutes. If the annealing exceeds 20 minutes, the hardness and / or corrosion resistance of the razor blades may be compromised. Petition 870250104623, dated 11 / 14 / 2025, pp. 108 / 133 19 / 29 Degrade. In some embodiments, the razor or shaving blade may be annealed in an inert atmosphere, more specifically a nitrogen or argon atmosphere. The annealing step may reduce the cutting force required during shaving or shaving. Without wishing to be limited by theory, it is believed that the annealing step may increase the crystallinity of parylene, which may result in an increase in the strength of parylene, which in turn may reduce the cutting force required. Furthermore, the softening of parylene during the annealing step may also further increase the uniformity of the second layer. The annealing step may reduce surface defects in the second layer, for example, reducing its porosity.

[0088] As mentioned above, a hard coating can be provided on the razor or shaving blade. Therefore, the razor or shaving blade can be coated with a hard coating, in particular before being coated with the first layer. The razor or shaving blade can be coated with a hard coating, for example, using chemical vapor deposition or physical vapor deposition processes. Exemplary hard coating deposition processes are described in US documents 2018 / 215056 A1 and US 10,442,098 B2, both of which are incorporated by reference in their entirety.

[0089] As mentioned above, an intermediate layer can be provided on the razor blade. Consequently, the razor blade can be coated with an intermediate layer, in particular before being coated with the hard coating. The razor blade can be coated with the intermediate layer similarly to the method of coating the razor blade with the first layer. Consequently, in some embodiments, the coating of the razor blade with the intermediate layer, in particular an intermediate layer comprising titanium, can be carried out by ion bombardment. In some embodiments, the coating of the razor blade with an intermediate layer can be carried out, in particular, by DC ion bombardment. Petition 870250104623, dated 11 / 14 / 2025, pp. 109 / 133 20 / 29 RF ion bombardment, closed-field unbalanced magnetron ion bombardment (CFUMS), ion beam ion bombardment, cathodic arc deposition and high-power pulse magnetron ion bombardment (HiPIMS) using sintered metal targets, in particular titanium targets sintered in an Ar atmosphere. EXPERIMENTAL SECTION SAMPLE PREPARATION

[0090] Five different sample lots (first, second, third, fourth, and fifth sample lots) were prepared according to the first aspect. In addition, a comparative first sample lot and a comparative second sample lot not according to the first aspect were also prepared. 1. FIRST SAMPLE BATCH (TITANIUM+PARYLENE-C)

[0091] The first sample batch according to the first aspect comprises a first layer comprising titanium and a second layer comprising Parylene-C. The first sample batch was prepared according to the following protocol:

[0092] Ten stainless steel razor or shaving blades were stacked in blade holders in a rotating attachment of a deposition chamber. The deposition chamber comprised a titanium target and a TiB2 target. In the event that a chromium layer was also deposited, for example, as a capping layer, the deposition chamber also comprised a chromium target.

[0093] A preparatory sequence of steps was performed prior to the deposition of the intermediate layer, to perform chemical thinning by ion bombardment. The deposition chamber was evacuated to a base pressure of 10 to 5 Torr using vacuum means. Then, Ar gas was introduced from an Ar gas source into the chamber to a pressure of 8 mTorr (8.10 to 3 Torr). The loaded bayonets were rotated in the rotating attachment at a constant speed of 6 rpm using a motor, all targets and, notably, the Ti and TiB2 targets were operated Petition 870250104623, dated 11 / 14 / 2025, pp. 110 / 133 21 / 29 under DC current control at 0.2 A. A DC voltage of 200 to 600 V was applied to the stainless steel blades for 4 minutes. The chemical grinding step by ion bombardment assists in removing impurities from the blade substrates and targets through argon ion bombardment.

[0094] Subsequently, the coating process itself was carried out.

[0095] In a first sequence of steps for the formation of an intermediate layer, the chamber pressure was adjusted to 3 mTorr. The Ti and TiB2 target(s) were operated under DC current control at 3 and 0.2 A, respectively, while a DC voltage of 0 to 50 V was applied to the rotating blades. By adjusting the deposition time, a Ti layer of 20 to 40 nm was deposited on the edge of the blade samples.

[0096] In a second sequence of steps, a rigid TiB2 coating was deposited after the deposition of the Ti interlayer. The rigid coating deposition also occurred at a pressure of 3 mTorr. The Ti, Cr (if present), and TiB2 targets were operated simultaneously, with the current in the Cr and Ti targets set to 0.2 A and the current in the TiB2 target set to 3 A. The current in the Ti and Cr targets was used to prevent elements from depositing on that target. A DC bias voltage of 150 to 350 V was applied to the rotating blades. By adjusting the deposition time, a TiB2 layer of 150 to 300 nm was deposited on the Ti layer.

[0097] In a third sequence, a first layer was deposited onto the hard coating. The first layer was also deposited at a pressure of 3 mTorr. The titanium target was operated under DC current control between 3 and 10 A while a DC voltage of 0 to 50 V was applied to the rotating blades. By adjusting the deposition time, a titanium layer with a thickness of 20 to 40 nm was deposited onto the razor blades.

[0098] In a fourth sequence of steps for the formation of the second layer, the rotating attachment was transferred to a second deposition chamber comprising a vaporizer, a pyrolysis chamber, a Petition 870250104623, dated 11 / 14 / 2025, pp. 111 / 133 22 / 29 deposition chamber, a cold trap, and a mechanical vacuum pump. Subsequently, the second chamber was evacuated to a base pressure of 1 Torr. The Parylene-C precursor dimers were vaporized at a temperature of 175 °C. Subsequently, the pressure in the chamber was reduced to 0.5 Torr and the Parylene-C precursor dimers were pyrolyzed to form Parylene-C precursor monomers at a temperature of 680 °C. Subsequently, the formed Parylene-C precursor monomers were deposited at a temperature of 25 °C at a pressure of 0.1 Torr. The temperature was then increased to 70 °C at a pressure of 0.001 Torr.

[0099] In a fifth sequence of steps for annealing razor blades, the second chamber was filled with argon at atmospheric pressure and heated to a temperature of 350 °C for 10 minutes to anneale the razor blades. After cooling to room temperature, the razor blades that met the first aspect were removed from the second chamber. 2. SECOND SAMPLE LOT (TITANIUM+PARYLENE-N)

[0100] The second sample lot according to the first aspect was prepared analogously to the first sample lot, except that the Parylene-N precursor dimers were used as opposed to the Parylene-C precursor dimers in the fourth sequence of steps. 3. THIRD SAMPLE LOT (TITANIUM+PARYLENE-C+PARYLENE-N)

[0101] The third sample batch according to the first aspect was prepared analogously to the first sample batch, except that after the deposition of Parylene-C, the fourth sequence of steps was repeated using Parylene-N precursor dimers to deposit a first sublayer comprising Parylene-C and a second sublayer comprising Parylene-N. 4. FOURTH SAMPLE LOT (TITANIUM+PARYLENE-F)

[0102] The fourth sample lot was prepared analogously to the first sample lot, except for the precursor dimers of Petition 870250104623, dated 11 / 14 / 2025, pp. 112 / 133 23 / 29 Parylene-F may have been used in opposition to the precursor dimers of Parylene-C in the fourth sequence of steps. 5. FIFTH SAMPLE LOT (TITANIUM+PARYLENE-C+PARYLENE-N - WITHOUT ANNEALING)

[0103] A fifth sample batch was prepared by coating the razor blades or shaving blades in the same way as for the third sample batch; however, the fifth sequence of steps was not performed. Thus, the fifth sample batch was not annealed. 6. SIXTH SAMPLE LOT (TITANIUM+PARYLENE-N - UNANNEALED)

[0104] A sixth sample batch was prepared by coating the razor blades or shaving blades in the same way as for the second sample batch; however, the fifth sequence of steps was not performed. Therefore, the sixth sample batch was not annealed. 7. FIRST COMPARATIVE SAMPLE LOT (CHROMIUM + PARYLENE-C + PARYLENE-N)

[0105] A first comparative sample batch was prepared analogously to the first sample batch, but coating the razor or shaving blades with chrome instead of titanium in the third sequence of steps. 8. SECOND COMPARATIVE SAMPLE LOT (CHROME)

[0106] A second comparative sample lot was prepared. The second comparative sample lot was subjected to the first step sequence and the second step sequence. In addition, the second comparative sample lot was subjected to the third step sequence; however, it was coated with chrome instead of titanium. The second comparative sample lot did not go through the fourth step sequence or the fifth step sequence. 9. THIRD COMPARATIVE SAMPLE LOT (CHROMIUM + PARYLENE-N - WITHOUT ANNEALING)

[0107] A third comparative sample batch was prepared analogously to the sixth sample batch, but coating the slides with Petition 870250104623, dated 11 / 14 / 2025, pp. 113 / 133 24 / 29 Shaving or waxing with chrome instead of titanium in the third step sequence. CUTTING FORCE EXPERIMENT

[0108] The shear strength of the first, second, third, fourth and fifth sample batch, as well as the first comparative sample batch, was determined.

[0109] Ten blades per sample batch were subjected to 10 consecutive cuts in a moving woolen felt. The blades were placed individually in a holder connected to a load cell. The load cell was used to measure the load on the blade during the cutting action.

[0110] The test results are presented in Figures 4 to 6, which are labeled as follows. The “Y” axis shows the required cutting force in “kg”, the “X” axis indicates the number of cuts. The first sample batch is denoted by the letter “A”, the second sample batch is denoted by the letter “B”, the third sample batch is denoted by the letter “D”, the fourth sample batch is denoted by the letter “C”, and the fifth sample batch is denoted by the letter “E”. The first comparative sample batch is denoted by the letter “F”. The sixth sample batch is denoted by the letter “H”. The third comparative sample batch is denoted by the letter “I”.

[0111] Figure 4 shows a comparison of the shear force of the third sample batch and the first comparative sample batch. As shown in Figure 4, razor blades comprising the first layer comprising titanium exhibit a significantly reduced shear force compared to razor blades comprising the first layer comprising chromium.

[0112] Figure 5 shows a comparison of the shear force of the first, second, third, and fourth sample batches. As shown in Figure 5, the razor blades comprising a second layer comprising Parylene-N (second sample batch) exhibit a lower shear force during the first cuts; however, the shear force required increases with the number of cuts until it is greater than that of the coated blades. Petition 870250104623, dated 11 / 14 / 2025, pp. 114 / 133 25 / 29 with Parylene-C (first sample batch). On the other hand, blades coated with Parylene-C (first sample batch) exhibit a higher required cutting force during the first use. Razor blades coated with a first sublayer comprising Parylene-C and a second sublayer comprising Parylene-N (third sample batch) outperform the first and second sample batches during all 10 cuts. Razor blades comprising a second layer comprising Parylene-F (fourth sample batch) exhibit a consistently higher cutting force compared to the other parylenes.

[0113] Figure 6 shows a comparison of the shear force of the third sample batch and the fifth sample batch. As shown in Figure 6, annealed razor blades exhibit significantly reduced shear force compared to non-annealed razor blades.

[0114] Figure 7 shows a comparison of the frictional force in the unit “grams” (Y-axis) of the second sample batch “B” compared to the second comparative sample batch “G”. The X-axis shows the distance traveled on the paper in millimeters. For this test, the felt was replaced with a cellulose paper. A razor blade from the second sample batch was placed parallel to the paper, and the paper was allowed to move, and the frictional force was measured along the distance traveled. The test was then repeated for the second comparative sample batch. As shown in Figure 7, the frictional force of the second sample batch is significantly lower compared to the second comparative sample batch.

[0115] Figure 8 shows a comparison of the shear force of the sixth sample batch and the first comparative sample batch. As shown in Figure 8, razor blades comprising the first layer comprising titanium exhibit a significantly reduced shear force compared to razor blades comprising the first layer comprising chromium. ASPECTS Petition 870250104623, dated 11 / 14 / 2025, pages 115 / 133 26 / 29

[0116] 1. A razor or depilatory blade having a first layer comprising titanium and a second layer comprising parylene.

[0117] 2. The razor or shaving blade, according to aspect 1, wherein the first layer comprises titanium as metallic titanium.

[0118] 3. The razor blade or shaving blade in accordance with any of the above aspects, wherein the parylene is selected from the group of Parylene-N, Parylene-C, Parylene-F and combinations thereof, and in particular wherein the parylene is selected from Parylene-N and / or Parylene-C.

[0119] 4. A razor or shaving blade, according to any of the preceding aspects, wherein the razor or shaving blade comprises a cutting edge portion and wherein the first layer and the second layer are provided in the cutting edge portion.

[0120] 5. The razor blade or shaving device, according to any of the preceding aspects, wherein the razor blade is configured to be disposed within a cartridge of the razor blade or shaving device.

[0121] 6. The razor blade or shaving blade, according to any previous aspect, the first layer having a thickness between about 5 nm and about 70 nm, more specifically between about 10 nm and about 60 nm and in particular between about 20 nm and about 50 nm.

[0122] 7. The razor blade or shaving blade in accordance with any of the above aspects, wherein the second layer has a thickness between about 0.005 pm and about 5 pm, more specifically between about 0.02 pm and about 2 pm and in particular between about 0.1 pm and about 1 pm.

[0123] 8. A razor blade or shaving blade, according to any of the preceding aspects, wherein the second layer does not comprise holes, in particular without holes with a diameter between about 5 nm and about 200 nm.

[0124] 9. The razor blade or shaving blade, according to any of the preceding aspects, wherein the second layer may comprise less than 1% by weight, more specifically less than 0.1% by weight and, in particular, Petition 870250104623, dated 11 / 14 / 2025, pp. 116 / 133 27 / 29 none or substantially none polytetrafluoroethylene.

[0125] 10. A razor or shaving blade, according to any of the preceding aspects, wherein the razor blade is additionally provided with a hard coating, more specifically wherein the hard coating comprises a ceramic, metallic and / or non-metallic coating.

[0126] 11. The razor or shaving blade, according to aspect 10, wherein the ceramic comprises a boride and / or a carbide and, in particular, titanium diboride or titanium, boron and carbon.

[0127] 12. A razor or shaving blade, according to aspect 10 or 11, wherein the metal of the hard coating comprises chrome.

[0128] 13. A razor or shaving blade, according to any of aspects 10 to 12, wherein the non-metallic coating comprises diamond-like carbon.

[0129] 14. The razor blade or shaving blade in accordance with any of the above aspects, wherein the first layer is disposed between the hard coating and the second layer.

[0130] 15. The razor or shaving blade in accordance with any of the above aspects, wherein the first layer is supplied directly on the razor or shaving blade;

[0131] or wherein the hard coating is supplied directly to the razor or shaving blade;

[0132] or wherein an intermediate layer is provided in the razor or shaving blade and the hard coating is provided in the intermediate layer, more specifically wherein the intermediate layer comprises niobium or titanium and, in particular, wherein the intermediate layer comprises metallic titanium.

[0133] 16. The razor or shaving blade according to any of the preceding aspects, wherein the razor or shaving blade essentially comprises or consists of a metal, in particular a stainless steel.

[0134] 17. The razor blade or shaving blade, according to Petition 870250104623, dated 11 / 14 / 2025, pp. 117 / 133 28 / 29 any of aspects 4 to 16, wherein the cross-section of the cutting edge portion has a substantially symmetrical tapered geometry terminating in a blade tip, wherein the cross-section has a central longitudinal axis originating from the blade tip and wherein the cutting edge portion has a thickness between 1.5 pm and 2.4 pm measured at a distance of 5 pm along the central longitudinal axis of the blade tip.

[0135] 18. A razor or shaving device cartridge comprising at least one razor or shaving blade according to any of the preceding aspects.

[0136] 19. A method for coating a razor blade or shaving blade, wherein the method comprises:

[0137] - coating a razor blade or shaving blade with a first layer comprising titanium, more specifically by physical vapor phase deposition, and

[0138] - coating the razor blade with a second layer comprising a parylene, more specifically by chemical vapor phase deposition.

[0139] 20. The method, according to aspect 19, whereby the coating of the razor blade or shaving blade with titanium is done before the coating of the razor blade or shaving blade with parylene.

[0140] 21. The method, according to aspect 19 or 20, wherein the coating of the razor blade or shaving blade with the first layer comprising titanium is made by ion bombardment.

[0141] 22. The method according to any of aspects 19 to 21, wherein the coating of the razor or depilatory blade with parylene by chemical vapor deposition comprises:

[0142] - sublime a dimer of a parylene precursor,

[0143] - pyrolyze the sublimated dimer of a parylene precursor to obtain parylene precursor monomers,

[0144] - deposit the parylene precursor monomers Petition 870250104623, dated 11 / 14 / 2025, pp. 118 / 133 29 / 29 on the razor blade or shaving blade.

[0145] 23. The method according to any aspect 22, wherein the sublimation of the dimer of a parylene precursor is carried out at a temperature between about 130 °C and about 190 °C, more specifically between about 150 °C and about 180 °C and / or at a pressure between about 0.5 Torr and about 2 Torr, more specifically between about 0.8 Torr and about 1.2 Torr.

[0146] 24. The method according to any aspect 22 or 23, wherein the pyrolysis of the sublimated dimer of a parylene precursor is carried out at a temperature of between about 400 °C and about 800 °C, more specifically between about 500 °C and about 700 °C and / or at a pressure between about 0.2 Torr and about 1 Torr, more specifically between about 0.4 Torr and about 0.6 Torr.

[0147] 25. The method according to any of aspects 22 to 24, wherein the deposition of the parylene precursor monomers is carried out at a temperature between about 10 °C and about 50 °C, more specifically between about 17 °C and about 28 °C and / or at a pressure between about 0.01 Torr and about 0.5 Torr, more specifically between about 0.05 Torr and about 0.2 Torr.

[0148] 26. The method according to any of aspects 19 to 25 further comprising an annealing step, in particular wherein the razor blade or shaving blade is annealed at a temperature between about 300 °C and about 400 °C, more specifically at a temperature between about 330 °C and about 370 °C in an inert gas atmosphere, in particular after the deposition of parylene.

[0149] 27. The method, according to aspect 26, whereby the razor blade is annealed for a duration of between about 10 and about 20 min, more specifically between about 1 min and about 5 min. Petition 870250104623, dated 11 / 14 / 2025, pp. 119 / 133

Claims

1 / 3 CLAIMS 1. Razor or depilatory blade characterized by having a first layer comprising titanium and a second layer comprising parylene.

2. A razor or shaving blade, according to claim 1, characterized in that the first layer comprises titanium, such as metallic titanium.

3. A razor or shaving blade, according to any of the preceding claims, characterized in that the parylene is selected from the group of Parylene-N, Parylene-C, Parylene-F and combinations thereof, and in particular in that the parylene is selected from Parylene-N and / or Parylene-C.

4. A razor or shaving blade, according to any of the preceding claims, wherein the razor or shaving blade is characterized by comprising a cutting edge portion, with the first layer and second layer being provided in the cutting edge portion.

5. A razor or shaving blade, according to any of the preceding claims, wherein the razor or shaving blade is characterized by being configured to be disposed within a cartridge of the razor or shaving apparatus.

6. A razor or shaving blade, according to any of the preceding claims, characterized in that the first layer has a thickness between about 5 nm and about 70 nm, more specifically between about 10 nm and about 60 nm, and in particular between about 20 nm and about 50 nm.

7. A razor or shaving blade, according to any of the preceding claims, characterized in that the second layer has a thickness between about 0.005 pm and about 5 pm, more specifically between about 0.02 pm and about 2 pm, and in particular between about 0.1 pm and about 1 pm.

8. A razor or shaving blade, according to any previous claim, characterized in that the second layer does not comprise holes, in particular holes with a diameter between about 5 nm and about 200 nm. Petition 870250104623, dated 14 / 11 / 2025, pp. 120 / 133 2 / 3 9. A razor or shaving blade, according to any of the preceding claims, characterized in that the second layer may comprise less than 1% by weight, more specifically less than 0.1% by weight, and in particular, no or substantially no polytetrafluoroethylene.

10. Razor or shaving blade, according to any of the preceding claims, the razor blade being characterized by being additionally provided with a hard coating, more specifically the hard coating comprising a ceramic, metallic and / or non-metallic coating.

11. A razor or shaving blade, according to claim 10, characterized in that the first layer is disposed between the rigid coating and the second layer.

12. A razor or shaving blade, according to any of the preceding claims, characterized in that the first layer is provided directly on the razor or shaving blade; or in that the hard coating is provided directly on the razor or shaving blade; or in that an intermediate layer is provided on the razor or shaving blade and the hard coating is provided on the intermediate layer, more specifically in that the intermediate layer comprises niobium or titanium and, in particular, in that the intermediate layer comprises metallic titanium.

13. Razor or shaving blade, according to any previous claim, the razor or shaving blade being characterized by essentially comprising or consisting of a metal, in particular a stainless steel.

14. Razor or depilatory cartridge, characterized by comprising at least one razor or depilatory blade as defined in any of the preceding claims.

15. Method for coating a razor or shaving blade, the method being characterized by comprising: Petition 870250104623, dated 11 / 14 / 2025, pp. 121 / 133 3 / 3 - coating a razor or shaving blade with a first layer comprising titanium, more specifically by physical vapor deposition, and - coating the razor blade with a second layer comprising parylene, more specifically by chemical vapor deposition. Petition 870250104623, dated 11 / 14 / 2025, pp. 122 / 133