Manufacturing method of circuit board protective film layer and circuit board

The Parylene film layer is formed on the circuit board through the vacuum deposition process, which solves the problem of toxic fluorine elements and waterproofing in the prior art, and achieves efficient protection and stable operation of the circuit board in harsh environments.

CN119095279APending Publication Date: 2024-12-06ZHONGLINGYUAN KUN AEROSPACE TECHNOLOGY (TIANJIN) CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411201426.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing circuit board waterproofing treatment technology uses toxic fluorine elements, and the waterproofing effect is not ideal, making it difficult to maintain normal operation in harsh environments.

Method used

采用真空沉积工艺在电路板上形成Parylene膜层,通过保护胶带覆盖非覆膜部件,形成偶联剂并在真空沉积设备中沉积Parylene膜层,确保膜层的牢固附着和均匀性。

Benefits of technology

It realizes the functions of the circuit board to be waterproof, moisture-proof, mildew-resistant, high and low temperature-resistant, and acid-resistant, and acid-resistant. It expands the application environment, such as harsh environments such as aerospace, aviation, and deep sea, and does not affect precision circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095279A_ABST
    Figure CN119095279A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a circuit board protective film layer and a circuit board. The manufacturing method comprises the following steps: covering a non-film-covered part on the circuit board with a protective adhesive tape; forming a coupling agent on the surface of the circuit board; the circuit board is put into vacuum deposition equipment to execute Parylene vacuum deposition, so that the surface of the circuit board is covered with a Parylene film layer; and removing the protective adhesive tape and the Parylene film layer on the protective adhesive tape. A Parylene film layer is formed on the circuit board by adopting a vacuum deposition process, so that a precise circuit on the circuit board is protected, and the circuit board is waterproof, moisture-proof, mould-proof, salt mist-resistant, high-low temperature-resistant and acid atmosphere-resistant, and cannot influence the precise circuit on the circuit board, the application environment of the circuit board is expanded, such as aerospace, aviation, deep sea and other severe environments, and the service life of the circuit board is prolonged. The coupling agent is formed on the surface of the circuit board, so that the Parylene film layer can be better formed on the surface of the circuit board and is not easy to fall off.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure generally relates to the technical field of manufacturing a protective film layer of a circuit board, and more specifically, to a method for manufacturing a protective film layer of a circuit board and a circuit board. Background Art

[0002] Circuit boards are also called circuit boards, PCB boards, printed (copper etching technology) circuit boards, etc. There are a lot of conductive circuits printed on the surface of the circuit board, or many electronic components are welded, and they are widely used in various electronic devices. Circuit boards rely on signal conduction in conductive circuits, so the circuit boards cannot touch water, otherwise it is very easy to cause short circuits or direct damage. In some fields, circuit boards need to have the functions of waterproof, moisture-proof, salt spray-proof, mildew-proof, high and low temperature resistant, and acidic atmosphere-resistant, so that the circuit boards can still work normally in harsh environments. Summary of the invention

[0003] Some embodiments of the present disclosure provide a method for manufacturing a protective film layer of a circuit board, comprising the following steps:

[0004] Use protective tape to cover the non-laminated parts on the circuit board;

[0005] forming a coupling agent on a surface of the circuit board;

[0006] Put the circuit board into a vacuum deposition device to perform Parylene vacuum deposition so that the surface of the circuit board is covered with a Parylene film layer; and

[0007] Remove the protective tape and the Parylene film layer on it.

[0008] In some embodiments, the method of covering the non-film-coated parts on the circuit board to be film-coated with a protective tape includes:

[0009] Polyimide amine tape is used to cover the non-film-coated parts on the circuit board to be filmed, and the non-film-coated parts include connectors, pin headers and threaded holes.

[0010] In some embodiments, forming a coupling agent on the surface of the circuit board comprises the following steps:

[0011] Prepare a coupling agent solution, wherein the solute is coupling agent a-174, accounting for 0.5% to 1.5% by weight, and the solute is isopropanol, accounting for 98.5% to 99.5% by weight;

[0012] Using an antistatic brush to evenly coat the coupling agent solution on the surface of the circuit board;

[0013] The circuit board coated with the coupling agent solution is dried at a temperature of 50° C. to 60° C. for 2 to 3 hours.

[0014] In some embodiments, placing the circuit board into a vacuum deposition device to perform Parylene vacuum deposition so that the surface of the circuit board is covered with a Parylene film layer comprises the following steps:

[0015] The circuit board is mounted in a deposition chamber of a vacuum deposition device, and the Parylene raw material is placed in an evaporation chamber of the vacuum deposition device;

[0016] The vacuum deposition equipment is evacuated to a vacuum degree of 0 to 3.5 Pa;

[0017] The vacuum deposition equipment performs vacuum deposition based on set deposition parameters, with an evaporation chamber temperature of 120°C to 135°C, a cracking chamber temperature of 690°C to 720°C, and a deposition chamber temperature of 20°C to 30°C.

[0018] In some embodiments, removing the protective tape and the Parylene film layer thereon comprises the following steps:

[0019] Use an antistatic knife to cut the Parylene film layer along the border of the protective tape;

[0020] The protective tape and the Parylene film layer thereon are peeled off.

[0021] In some embodiments, before placing the circuit board into a vacuum deposition device to perform Parylene vacuum deposition so that the surface of the circuit board is covered with a Parylene film layer, the manufacturing method further includes the following steps:

[0022] The test piece is used to perform Parylene film deposition in a vacuum deposition device to adjust the deposition parameters of the vacuum deposition device.

[0023] In some embodiments, using a test piece to perform Parylene film deposition in a vacuum deposition device to adjust the deposition parameters of the vacuum deposition device includes the following steps:

[0024] Place a test piece of known thickness into a vacuum deposition device and perform Parylene film deposition based on preset parameters;

[0025] Test the thickness, appearance and adhesion of the Parylene film on the test piece;

[0026] The deposition parameters of the vacuum deposition equipment are adjusted based on the test results of the test piece.

[0027] In some embodiments, before using the protective tape to cover the non-film-covered components on the circuit board, the manufacturing method further includes the following steps:

[0028] Clean the surface of the circuit board.

[0029] In some embodiments, cleaning the circuit board surface includes:

[0030] Plasma cleaning of the circuit board surface; and / or

[0031] Wipe the circuit board with anhydrous ethanol.

[0032] Some embodiments of the present disclosure provide a circuit board, comprising a Parylene film layer formed by the manufacturing method described in the aforementioned embodiment.

[0033] According to the technical solution of the embodiment of the present disclosure, a Parylene film layer is formed on a circuit board by a vacuum deposition process, so that the precision circuit on the circuit board is protected, and it can be waterproof, moisture-proof, mildew-proof, salt spray-proof, high and low temperature-resistant, and acidic atmosphere-resistant, and will not affect the precision circuit on the circuit board. The application environment of the circuit board is expanded, such as aerospace, aviation, deep sea and other harsh environments. A coupling agent is formed on the surface of the circuit board, so that the Parylene film layer can be better formed on the surface of the circuit board and is not easy to fall off. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The above and other features of the present disclosure will become more apparent from the following detailed description taken in conjunction with the accompanying drawings, in which:

[0035] Figure 1 A process flow chart of a method for manufacturing a protective film layer for a circuit board provided in some embodiments of the present disclosure.

[0036] Figure 2 for Figure 1 Specific flow chart of step S20;

[0037] Figure 3 for Figure 1 Specific flow chart of step S30;

[0038] Figure 4 for Figure 1 Specific flow chart of step S40;

[0039] Figure 5 for Figure 1 Specific flow chart of step S25 in FIG. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solutions and advantages of the present disclosure clearer, the present disclosure will be further described in detail below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.

[0041] The terms used in the embodiments of the present disclosure are only for the purpose of describing specific embodiments, and are not intended to limit the present disclosure. The singular forms "a", "said" and "the" used in the embodiments of the present disclosure and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings, and "multiple" generally includes at least two.

[0042] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0043] It should be understood that although the terms first, second, third, etc. may be used to describe structures in the disclosed embodiments, these structures should not be limited to these terms. These terms are only used to distinguish different structures. For example, without departing from the scope of the disclosed embodiments, a first component may also be referred to as a second component, and similarly, a second component may also be referred to as a first component.

[0044] As used herein, the words "if" and "if" may be interpreted as "at the time of" or "when" or "in response to determining" or "in response to detecting", depending on the context. Similarly, the phrases "if it is determined" or "if (stated condition or event) is detected" may be interpreted as "when it is determined" or "in response to determining" or "when detecting (stated condition or event)" or "in response to detecting (stated condition or event)", depending on the context.

[0045] It should also be noted that the term "includes", "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, so that a commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprising a ..." do not exclude the existence of other identical elements in the commodity or device including the elements.

[0046] In the related art, the waterproof treatment of the circuit board is usually carried out by coating the circuit board with a hydrophobic material, such as polytetrafluoroethylene (EPTFE), but the waterproof effect is not ideal, and the fluorine element is toxic and does not meet the environmental protection standards.

[0047] The present invention discloses a method for manufacturing a protective film layer of a circuit board, comprising the following steps: using a protective tape to cover non-film-coated parts on the circuit board; forming a coupling agent on the surface of the circuit board; placing the circuit board into a vacuum deposition device to perform Parylene vacuum deposition so that the surface of the circuit board is covered with a Parylene film layer; and removing the protective tape and the Parylene film layer thereon.

[0048] In the present disclosure, a vacuum deposition process is used to form a Parylene film layer on a circuit board, so that the precision circuit on the circuit board is protected, and it can be waterproof, moisture-proof, mildew-proof, salt spray-proof, high and low temperature-resistant, and acidic atmosphere-resistant, without affecting the precision circuit on the circuit board, and expanding the application environment of the circuit board, such as aerospace, aviation, deep sea and other harsh environments. A coupling agent is formed on the surface of the circuit board, so that the Parylene film layer can be better formed on the surface of the circuit board and is not easy to fall off.

[0049] The specific embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.

[0050] Dichlorodi-p-xylylene dimer, also known as c powder, CAS number: 28804-46-8, melting point 165-167℃, [1] is used to generate Parylene C raw material, which has a relatively broad industry prospect. Parylene is a polymer of p-xylene. It is widely used in the fields of aviation, aerospace, military, electronic optics, semiconductor materials, medical treatment, cultural heritage protection, etc. It has the characteristics of not easily damaging any electronic devices or substrates. It is a polymer raw material with good characteristics. Parylene film has good protection effect against water, o2, corrosion resistance, alkaline mist, etc. Parylene film not only has excellent dielectric properties, low dielectric loss and high dielectric strength, but also has excellent mechanical properties and radiation resistance. The high dielectric strength of Parylene is mainly due to the fact that Parylene can form a continuous, defect-free and other filler-free film. Parylene has excellent dimensional stability and low temperature performance, and provides 1.5KV, 2.0KV or even higher voltage breakdown performance without almost changing the device size. Therefore, Parylene can be used as a surface treatment and insulator for microelectronics and micromotors. Using high-purity Parylene as a passivation layer and dielectric layer can provide safe and stable protection.

[0051] Figure 1 A process flow chart of a method for manufacturing a circuit board protective film layer provided in some embodiments of the present disclosure, such as Figure 1 As shown, some embodiments of the present disclosure provide a method for manufacturing a protective film layer of a circuit board, the manufacturing method comprising the following steps:

[0052] S10: Use protective tape to cover non-laminated parts on the circuit board.

[0053] Specifically, some components or areas on the circuit board need to be electrically connected to external components and cannot be deposited with Parylene film layers with insulating properties. In order to avoid the formation of Parylene film layers on these components or areas, protective tape is used to cover them to form a mask. When the Parylene film layer is deposited as a whole, the Parylene film layer is formed on the mask, which is convenient for removal together with the mask later.

[0054] S20: forming a coupling agent on the surface of the circuit board.

[0055] Specifically, if the Parylene film layer is directly deposited on the surface of the circuit board, there may be a problem that the Parylene film layer is not firmly bonded to the circuit board surface. By forming a coupling agent, such as coupling agent A-174, on the surface of the circuit board, the adhesion of the Parylene film layer can be enhanced, so that the Parylene film layer is densely and firmly formed on the surface of the circuit board.

[0056] S30: placing the circuit board into a vacuum deposition device to perform Parylene vacuum deposition so that the surface of the circuit board is covered with a Parylene film layer.

[0057] Specifically, the solid particle raw material of Parylene is heated and sublimated into gas in the evaporation chamber of the vacuum deposition equipment. The gaseous Parylene enters the high-temperature cracking chamber of the vacuum deposition equipment along the vacuum pipeline and is decomposed into active monomers with free radicals. The active monomers with free radicals enter the deposition chamber of the vacuum deposition equipment along the vacuum pipeline and are adsorbed, deposited, and polymerized into long-chain polymers on the surface of the circuit board in the deposition chamber. During the entire vacuum coating process, the molecules are uniformly coated on the surface of the circuit board. The Parylene film layer deposited in the vacuum is uniform in thickness, dense, non-porous, transparent, and tension-free.

[0058] S40: Remove the protective tape and the Parylene film layer thereon.

[0059] Specifically, the protective tape and the Parylene film layer thereon are removed using an anti-static knife or other tool, so that the non-film-coated parts are exposed, which facilitates electrical connection with other external parts.

[0060] In these embodiments, a Parylene film layer is formed on the circuit board by a vacuum deposition process, so that the precision circuit on the circuit board is protected, and harmful substances such as water, moisture, and metal ions are prevented from affecting the precision circuit on the circuit board, thereby expanding the application environment of the circuit board, such as aerospace, aviation, deep sea and other harsh environments. A coupling agent is formed on the surface of the circuit board, so that the Parylene film layer can be better formed on the surface of the circuit board and is not easy to fall off.

[0061] In some embodiments, the step S10: covering the non-film-coated parts on the circuit board to be film-coated with a protective tape comprises:

[0062] Polyimide sub-sensitive tape is used to cover the non-film-coated parts on the circuit board to be filmed, and the non-film-coated parts include connectors, pin headers and threaded holes. These parts are used to electrically connect with external parts for signal interaction and cannot be covered by the insulating Parylene film layer. Therefore, a protective adhesive, such as polyimide sub-sensitive tape, is used to cover them to form a mask. When the Parylene film layer is formed by overall deposition, the Parylene film layer is formed on the mask, which is convenient for removal together with the mask later.

[0063] Polyimide sub-sensitive tape is used to form a mask for parts that do not need to be deposited, such as debugging points, pins, connectors and other locations. As a key link in the vacuum deposition process, the mask should adopt a reliable protection method to ensure that the mask is in place and there should be no leakage, poor protection and warping, especially at the edges and interfaces of the protection. If necessary, sealing treatment should be used. Necessary anti-static measures need to be taken when forming the mask. After the mask is formed, an appearance inspection is required to confirm the mask position to ensure that there is no leakage protection, excessive protection, or poor protection.

[0064] Figure 2 for Figure 1 The specific flow chart of step S20 is as follows: Figure 2 As shown, in some embodiments, the step S20: forming a coupling agent on the surface of the circuit board includes the following steps:

[0065] S21: prepare a coupling agent solution, wherein the solute is coupling agent a-174, accounting for 0.5% to 1.5% by weight, and the solute is isopropanol, accounting for 98.5% to 99.5% by weight.

[0066] Specifically, the coupling agent solution is prepared according to a set weight ratio, and the coupling agent a-174 and isopropanol are put into a measuring cup according to a set ratio, and stirred thoroughly.

[0067] S22: using an antistatic brush to evenly coat the coupling agent solution on the surface of the circuit board.

[0068] Specifically, an antistatic brush is used to evenly coat the coupling agent solution on the front and back surfaces of the circuit board. In some embodiments, the coupling agent solution may not be coated on the mask formed by the polyimide amine tape. The operator needs to complete the even coating of the coupling agent solution within two hours after the coupling agent solution is prepared and fully stirred to ensure even coating of the coupling agent.

[0069] S23: drying the circuit board coated with the coupling agent solution at a temperature of 50° C. to 60° C. for 2 to 3 hours.

[0070] Before deposition, drying and dehumidification should be performed to completely remove the water vapor and moisture adsorbed on the circuit board components to prevent moisture from affecting the deposition. At the same time, the applied coupling agent should be dried. The drying and dehumidification temperature is set to 55±3℃ for example, and the time is greater than 2.5 hours. The dried circuit board components should be subjected to Parylene film deposition within 24 hours. If it exceeds 24 hours, the circuit board should be dried again according to the above method before the next deposition.

[0071] Figure 3 for Figure 1 The specific flow chart of step S30 is as follows: Figure 3 As shown, the step S30: placing the circuit board into a vacuum deposition device to perform Parylene vacuum deposition so that the surface of the circuit board is covered with a Parylene film layer includes the following steps:

[0072] S31: Hanging the circuit board in a deposition chamber of a vacuum deposition device, and placing the Parylene raw material in an evaporation chamber of the vacuum deposition device.

[0073] Specifically, the circuit board is mounted in a deposition chamber in a vacuum deposition device, and multiple circuit boards can be mounted in the deposition chamber at the same time to simultaneously form Parylene films, and multiple circuit boards are arranged in a vertical interval in the deposition chamber of the vacuum deposition device. Parylene raw materials, such as Parylene C powder, are arranged in an evaporation chamber in the vacuum deposition device.

[0074] S32: Evacuate the vacuum deposition equipment to a vacuum degree of 0 to 3.5 Pa.

[0075] Specifically, the evaporation chamber, the cracking chamber and the deposition chamber of the vacuum deposition equipment are set to a vacuum state by using the vacuum pumping device of the vacuum deposition equipment, and the vacuum degree is, for example, 1 to 3 Pa, and specifically, 2 Pa.

[0076] S33: The vacuum deposition equipment performs vacuum deposition based on the set deposition parameters, the evaporation chamber temperature is 120°C to 135°C, the cracking chamber temperature is 690°C to 720°C, and the deposition chamber temperature is 20°C to 30°C.

[0077] Specifically, in the early stage of vacuum deposition, the equipment parameters are set, for example, the temperature of the evaporation chamber is set to 125°C, the temperature of the cracking chamber is set to 710°C, and the temperature of the deposition chamber is set to room temperature, for example, 25°C, to prepare for coating. During the vacuum deposition process, the temperature and vacuum degree of the evaporation chamber, cracking chamber and deposition chamber in the vacuum deposition equipment can be monitored in real time by the detector in the vacuum deposition equipment to ensure that they are within the specified error range.

[0078] In some embodiments, the Parylene film forming rate can also be detected during the vacuum deposition process to ensure that the film forming rate is within a specified range, that is, to ensure that the film forming rate monitored by the crystal oscillator film thickness meter in the vacuum deposition equipment meets the predetermined range.

[0079] Figure 4 for Figure 1 In the specific flow chart of step S40, in some embodiments, as Figure 4 As shown, the step S40: removing the protective tape and the Parylene film layer thereon comprises the following steps:

[0080] S41: Use an antistatic knife to cut the Parylene film layer along the boundary of the protective tape.

[0081] Specifically, since the Parylene film layer is evenly covered on the surface of the circuit board in the vacuum deposition equipment, including the surface of the mask, an anti-static knife is used to cut the Parylene film layer along the mask boundary to avoid the Parylene film layer on the peripheral area of ​​the mask from falling off when the mask is removed.

[0082] S42: Peeling off the protective tape and the Parylene film layer thereon.

[0083] The operator peels off the protective tape and the Parylene film layer thereon from the circuit board under anti-static measures, exposing the non-film-coated parts of the circuit board to facilitate electrical connection with other external parts.

[0084] In some embodiments, Figure 1 As shown, before step S30: placing the circuit board into a vacuum deposition device to perform Parylene vacuum deposition so that the surface of the circuit board is covered with a Parylene film layer, the manufacturing method further includes the following steps:

[0085] S25: using the test piece to perform Parylene film deposition in a vacuum deposition device to adjust deposition parameters of the vacuum deposition device.

[0086] Before the Parylene film is deposited on each batch of circuit boards, a test piece with a known thickness needs to be used for Parylene film deposition. The deposition parameters of the vacuum deposition equipment can be adjusted by testing the film thickness and adhesion after the Parylene film is deposited on the test piece.

[0087] Figure 5 for Figure 1 In the specific flow chart of step S25, in some embodiments, as Figure 5 As shown, the step S25: using the test piece to perform Parylene film deposition in a vacuum deposition device to adjust the deposition parameters of the vacuum deposition device includes the following steps:

[0088] S251: Place a test piece with known thickness into a vacuum deposition device and perform Parylene film deposition based on preset parameters.

[0089] Specifically, a test piece of known thickness is mounted in a deposition chamber of a vacuum deposition device, and a Parylene raw material is placed in an evaporation chamber of the vacuum deposition device. Parylene film deposition is performed based on preset parameters, and the predicted parameters include: evaporation chamber temperature and vacuum degree, cracking chamber temperature and vacuum degree, deposition chamber temperature and vacuum degree; deposition rate; deposition time, etc. The thickness of the test piece in some embodiments is measured, for example, using a micrometer.

[0090] S252: Check the thickness, appearance and adhesion of the Parylene film on the test piece.

[0091] Specifically, after the Parylene film layer is formed on the test piece, the test piece is taken out from the vacuum deposition device to inspect the thickness, appearance and adhesion of the Parylene film layer on the test piece.

[0092] Use a micrometer to check the thickness of the test piece with the Parylene film layer deposited on it. Subtract the known thickness of the test piece from the thickness and divide it by 2 to get the film thickness of the Parylene film layer under the current parameter environment. Confirm whether it meets the requirements for the deposition thickness of the Parylene film layer of the circuit board, and the standard is, for example, 20±2μm.

[0093] The operator uses the naked eye or optical inspection equipment to check the appearance of the test piece, inspect the appearance of the test piece and the deposition quality, and visually inspect under natural heat dissipation light or non-reflective white projection light (not less than 600LX) to confirm whether the appearance of the Parylene film is smooth, uniform, and transparent, and whether there are defects such as bubbles, white spots, peeling, wrinkles, and cracks.

[0094] The operator uses a grid knife to test the adhesion of the Parylene film layer. Specifically, the Parylene film layer on the test piece is scratched with a grid knife, and the scratched area is compacted with tape and then violently torn off. If the grid detachment ratio is less than or equal to 5%, the adhesion requirement is met.

[0095] S253: adjusting deposition parameters of the vacuum deposition equipment based on the detection result of the test piece.

[0096] Based on the above detection of the Parylene film layer on the test piece, it is confirmed whether the Parylene film layer meets the requirements. If not, the parameters of the vacuum deposition equipment are adjusted to repeat steps S251 and 252 until the Parylene film layer meets the requirements. At this time, the deposition parameters of the vacuum deposition equipment are determined as the parameters for the Parylene film deposition process of the circuit board to be deposited.

[0097] In some embodiments, Figure 1 As shown, before step S10: using protective tape to cover the non-film-coated parts on the circuit board, the manufacturing method further includes the following steps:

[0098] S00: Clean the surface of the circuit board.

[0099] Specifically, the circuit board surface should be clean, free of dust, debris, flux residue, oil and other excess materials to avoid affecting the film quality of the subsequent Parylene film layer. Therefore, it is necessary to clean the circuit board surface to remove the adsorbent dust, oil, fingerprints, handprints, etc. on the circuit board surface.

[0100] In some embodiments, plasma cleaning can be used to clean the surface of the circuit board. Plasma cleaning removes dirt and impurities by generating plasma and utilizing the interaction between high-energy particles of the plasma and the surface of the circuit board. Plasma cleaning can penetrate into the surface and interior of the circuit board for cleaning, and the cleaning effect is more thorough, and can remove organic substances and metal oxides that are difficult to clean. Compared with ultrasonic cleaning in conventional technology, it has a better cleaning effect on deep dirt, and will not affect the delicate electronic devices on the circuit board due to vibration like ultrasonic cleaning.

[0101] In some embodiments, the surface of the circuit board can be cleaned by wiping with anhydrous ethanol. Specifically, the operator uses a non-woven cloth to wipe the surface of the circuit board with anhydrous ethanol to remove adsorbed dust, oil, fingerprints, handprints, etc. on the surface of the circuit board.

[0102] In some embodiments, before step S40: removing the protective tape and the Parylene film layer thereon, the manufacturing method further comprises the following steps:

[0103] The circuit board with the Parylene film layer deposited thereon is subjected to a curing operation. For example, after the Parylene film layer is vacuum deposited on the circuit board, the circuit board is kept in a vacuum state in a deposition chamber of a vacuum deposition device for more than 2 hours to stabilize the properties of the Parylene film layer on the circuit board surface.

[0104] Some embodiments of the present disclosure provide a circuit board, comprising a Parylene film layer formed by the manufacturing method described in the aforementioned embodiment.

[0105] Finally, it should be noted that the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other. For the system or device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part description.

[0106] The above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them. Although the present disclosure has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present disclosure.

Claims

1. A method for manufacturing a protective film layer of a circuit board, It is characterized in that The following steps are involved: Use protective tape to cover the non-laminated parts on the circuit board; forming a coupling agent on a surface of the circuit board; Put the circuit board into the vacuum deposition equipment to perform Parylene vacuum deposition so that the surface of the circuit board is covered with the Parylene film layer; as well as Remove the protective tape and the Parylene film layer on it.

2. The method for manufacturing a circuit board protective film layer according to claim 1, It is characterized in that The method of using protective tape to cover the non-film-coated parts on the circuit board to be film-coated includes: Polyimide amine tape is used to cover the non-film-coated parts on the circuit board to be filmed, and the non-film-coated parts include connectors, pin headers and threaded holes.

3. The method for manufacturing a circuit board protective film layer according to claim 1, It is characterized in that The step of forming a coupling agent on the surface of the circuit board comprises the following steps: Prepare a coupling agent solution, wherein the solute is coupling agent a-174, accounting for 0.5% to 1.5% by weight, and the solute is isopropanol, accounting for 98.5% to 99.5% by weight; Using an antistatic brush to evenly coat the coupling agent solution on the surface of the circuit board; The circuit board coated with the coupling agent solution is dried at a temperature of 50° C. to 60° C. for 2 to 3 hours.

4. The method for manufacturing a circuit board protective film layer according to claim 1, It is characterized in that The step of placing the circuit board into a vacuum deposition device to perform Parylene vacuum deposition so that the surface of the circuit board is covered with a Parylene film layer comprises the following steps: The circuit board is mounted in a deposition chamber of a vacuum deposition device, and the Parylene raw material is placed in an evaporation chamber of the vacuum deposition device; The vacuum deposition equipment is evacuated to a vacuum degree of 0 to 3.5 Pa; The vacuum deposition equipment performs vacuum deposition based on set deposition parameters, with an evaporation chamber temperature of 120°C to 135°C, a cracking chamber temperature of 690°C to 720°C, and a deposition chamber temperature of 20°C to 30°C.

5. The method for manufacturing a circuit board protective film layer according to claim 4, It is characterized in that The removal of the protective tape and the Parylene film layer thereon comprises the following steps: Use an antistatic knife to cut the Parylene film layer along the border of the protective tape; The protective tape and the Parylene film layer thereon are peeled off.

6. The method for manufacturing a circuit board protective film layer according to any one of claims 1 to 5, It is characterized in that Before placing the circuit board into a vacuum deposition device to perform Parylene vacuum deposition so that the surface of the circuit board is covered with a Parylene film layer, the manufacturing method further comprises the following steps: The test piece is used to perform Parylene film deposition in a vacuum deposition device to adjust the deposition parameters of the vacuum deposition device.

7. The method for manufacturing a circuit board protective film layer according to claim 6, It is characterized in that The steps of performing Parylene film deposition in a vacuum deposition device using a test piece to adjust the deposition parameters of the vacuum deposition device include: Place a test piece of known thickness into a vacuum deposition device and perform Parylene film deposition based on preset parameters; Test the thickness, appearance and adhesion of the Parylene film on the test piece; The deposition parameters of the vacuum deposition equipment are adjusted based on the test results of the test piece.

8. The method for manufacturing a circuit board protective film layer according to any one of claims 1 to 5, It is characterized in that Before using the protective tape to cover the non-film-covered components on the circuit board, the manufacturing method further includes the following steps: Clean the surface of the circuit board.

9. The method for manufacturing a circuit board protective film layer according to claim 8, It is characterized in that Cleaning operations on the circuit board surface include: Plasma cleaning of the circuit board surface; and / or Wipe the circuit board with anhydrous ethanol.

10. A circuit board, It is characterized in that The invention comprises a Parylene film layer formed by the manufacturing method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Film removing method for Parylene film

    CN108925059A

  • Astronavigation-level Parylene-C-based thin film and preparation method thereof

    CN116641026A

  • High-frequency circuit board surface coating process

    CN117641751A

  • Circuit board having the method of coating and coating layer of circuit board

    KR1020100091368A