Methods of producing metals
Through high shear mixing and fluidized bed spray granulation technology, the problem of uneven distribution of metal alloy powder particles is solved, and efficient production of alloy powders such as Ti-6Al-4V is achieved, ensuring the consistency of stoichiometry and particle shape .
Patent Information
- Application Number
- CN201680014398.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2015-03-10
- Filing Date
- 2016-03-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2036-03-10
AI Technical Summary
It is difficult to effectively produce metal alloy powders with appropriate stoichiometric and uniform particle distribution in the prior art, especially when producing such as Ti-6Al-4V alloy powders, due to the differences in particle sizes of different metal oxide particles, the alloy elements are difficult to uniformly distribute.
By combining the liquid with metal oxide particles, high shear mixing is performed to form a uniform liquid suspension, and the particles are grown using a fluidized bed spray granulation process, controlling the particle diameter and distribution to form a predetermined size and stoichiometric The non-metallic raw material powder is then electrolytically reduced to form the metal powder.
The uniform distribution and predetermined size of metal alloy powder particles are achieved, the efficiency and yield of the production process are improved, and the consistency of the stoichiometric and particle shape of the alloy are ensured.
Smart Images

Figure CN107530783B_ABST
Abstract
Description
[0001] The present invention relates to a method for producing a raw powder for reduction to a metal, a raw powder, and a method for producing a metal by reduction of a raw powder. The present invention may be particularly advantageous for producing metal alloys, such as metal alloy powders or intermetallic compound powders. Background Art
[0002] The present invention relates to a method of forming a raw material powder and a metal forming method of forming a metal by reducing the raw material powder.
[0003] In recent years, there has been a great deal of interest in the direct production of metals by direct reduction of solid feedstocks (e.g., metal oxide feedstocks). One such direct reduction process is the Cambridge Electrolysis process (as described in WO 99 / 64638). In the FFC process, a solid compound (e.g., a metal oxide) is arranged to contact a cathode in an electrolytic cell containing a molten salt. A potential is applied between the cathode and anode of the cell so that the compound is reduced. In the FCC process, the potential for producing the solid compound is lower than the precipitation potential of the cations in the molten salt.
[0004] Other reduction methods have been proposed for reducing feedstocks in the form of solid non-metallic compounds connected cathodically, such as the polar TM Process and the process described in WO 03 / 048399. Non-metallic compounds, such as metal oxides, can also be directly reduced by metallothermic processes, such as the molten salt calcium thermal process described in EP1445350.
[0005] Conventional implementation of the FFC process and other solid-state electrolytic reduction processes typically includes the production of a porous preform or precursor of raw materials made from a sintered powder of the solid non-metallic compound to be reduced. The porous preform is then carefully connected to the cathode to allow reduction to occur. Once the plurality of preforms are connected to the cathode, the cathode can be sunk into a molten salt and the preform can be reduced.
[0006] WO 2013 / 050772 discloses a method for producing a metal powder, comprising the steps of placing a certain amount of a raw material comprising a plurality of non-metallic particles in an electrolytic cell, and applying an electric potential between a cathode and an anode to reduce the raw material to a metal powder. The raw material powder of WO 2013 / 050772 is disclosed as non-metallic particles derived from crushed stone or minerals, or derived from naturally occurring sand. Typically, the raw material powder needs to be screened, for example, sifted to select a non-metallic particle portion having a desired average particle diameter or a desired particle size distribution.
[0007] There are many disclosures that can produce metal alloys by direct reduction of preforms containing more than one different metal oxides. For example, WO 99 / 64638 discloses the production of titanium aluminum alloys by reducing preforms containing both titanium oxide and aluminum oxide. However, it may be difficult to prepare a preform with appropriate stoichiometry in a short range to produce a desired alloy. This may be partly due to the size of some oxide particles, or due to the size difference between some oxide particles of different compositions. For example, titanium dioxide powder is usually supplied as a fine powder with a low average particle diameter (usually 1 micron to 2 microns). In contrast, aluminum oxide powder can usually be obtained with a much larger average particle diameter (e.g., 8 microns to 10 microns). Other less commonly used metal oxides (e.g., vanadium oxide) may only be commercially available with extremely large particle diameters (e.g., an average particle diameter of about 100 microns). The difference in this particle size means that it is difficult to evenly distribute alloying elements in the preforms used to form metal alloys.
[0008] This problem is exacerbated in situations where it is desired to produce alloy powders. For example, it may be particularly desirable to produce metal alloy powders having an average particle diameter in the range of 100 microns to 250 microns, or possibly even less than 100 microns. It is difficult to produce, for example, a Ti-6Al-4V alloy powder having this desired particle size by reducing a raw powder formed from simple agglomerates of titanium oxide, aluminum oxide, and vanadium oxide particles. This is due to the large particle size of the vanadium oxide particles (about 100 microns) and the fact that vanadium should only account for 4% by weight of the resulting Ti-6Al-4V alloy powder.
[0009] Preforms of mixed oxides can be obtained by mixing different metal oxide powders with a solvent and subjecting them to a ball milling process. After ball milling, the solvent can be evaporated and the remaining powder pressed to form a preform. However, ball milling is a relatively gentle process, and preforms produced in this way are non-uniform and lack controlled short-range stoichiometry. Summary of the invention
[0010] The present invention provides a method of producing a non-metallic raw material powder, a non-metallic raw material powder and a method of forming a metal by reduction of a non-metallic raw material powder as defined in the appended independent claims to which reference should now be made. Preferred or advantageous features of the invention are set out in a number of the dependent claims.
[0011] Thus, a method for producing a non-metallic raw material powder suitable for reduction to a metal may include the steps of combining a liquid with solid metal oxide particles to form a mixture, subjecting the mixture to high shear mixing to form a liquid suspension of the metal oxide and the liquid, and drying the liquid suspension using a fluidized bed spray granulation process to grow a plurality of particles to form the non-metallic raw material powder. The spray granulation process grows the plurality of raw material particles layer by layer to a predetermined average particle diameter.
[0012] The liquid that is combined with the metal oxide particles to form a mixture may advantageously include water and an organic binder, such as an aqueous solution of polyvinyl alcohol (PVA). Many other suitable binders are known. For example, a suitable binder may include polyvinyl pyrrolidone (PVP) or hydroxyethyl cellulose (HEC). Regardless of any large particle size deviation that may exist before high shear mixing, the metal oxide particles can be ground to similar fineness by subjecting the mixture of the liquid and the metal oxide particles to a high shear mixing process. That is, if there is a wide particle size distribution in the metal oxide particles that are combined with the liquid to form a mixture, the high shear mixing process can advantageously grind the particles so that the overall average particle diameter is reduced and the overall particle size distribution is narrowed. Advantageously, by forming a liquid suspension containing uniformly distributed fine metal oxide particles, a spray granulation technique can be used to grow the particles so that the raw material powder forms a predetermined average particle diameter.
[0013] The ratio of liquid to metal oxide powder in the mixture can vary. However, a preferred mixture is 50% to 70% by weight of metal oxide, with the remainder being liquid. At oxide loadings greater than 70% by weight, it may be difficult to produce high shear mixing sufficient to form a uniform liquid suspension. Suspensions formed with loadings greater than 70% by weight are difficult to pump into a spray granulation device. At oxide loadings less than 50% by weight, the time spent forming the raw material particles may be too long. At lower oxide loadings, the particles produced may be more spherical. Therefore, it may be advantageous to maintain an oxide loading of 50% to 60% by weight of the mixture, or 50% to 55% by weight of the mixture.
[0014] The step of drying the liquid suspension may include the following steps: spraying a portion of the liquid suspension into a heating chamber of a fluidized bed spray granulation device so that liquid is removed from each droplet of the suspension to form a plurality of seed particles; maintaining the plurality of seed particles in the heating chamber by means of a fluidizing gas stream; and spraying another portion of the liquid suspension into the heating chamber so that the droplets of the liquid suspension are continuously adsorbed on the plurality of seed particles and dried thereon. In this way, the plurality of raw material particles can be grown layer by layer to a predetermined particle size.
[0015] Fluidized bed, spray granulation processes are known and have particular applications in the pharmaceutical industry. When a liquid feed is sprayed into the chamber, it is dried to form a seed particle or germ particle. The germ particle is maintained therein by the fluidizing gas stream. As additional liquid feed is sprayed into the chamber, it accumulates layer by layer on the seed particle. The seed particle grows larger, forming an onion-like structure. A roughly spherical particle is formed. The particle grows until it is too large to be maintained in the fluidizing gas stream, after which it falls out of the bottom of the heating chamber. The resulting particle is dry, roughly spherical and dust-free.
[0016] The process parameters that can be controlled include the fluidizing air flow rate and the air temperature (inlet temperature). For the purposes of the present invention, it may be preferred that the air flow during spray granulation is about 100 m / s. 3 / hour to 190m 3 / hour, preferably 130m 3 / hour to 170m 3 For the purposes of the present invention, it may be preferred that the air temperature is from 120°C to 190°C, preferably from 130°C to 150°C.
[0017] Control of the process parameters allows the production of particles with a predetermined average particle diameter in the range of about 10 microns to about 10 millimeters. Different parameters may need to be selected to form particles of the same particle size using oxides of different densities. The high degree of control of these processes allows the final particle size and particle size distribution to be controlled within extremely close tolerances. In addition, the process yield can be substantially in excess of 90%. For example, when the process is run continuously, a yield in excess of 95% or 98% can be achieved.
[0018] Control of the average particle diameter may allow the formation of non-metallic feedstock powders of specific sizes to produce metal powders with specific powder properties. WO2014 / 068267 discusses the production of metal powders with specific powder properties for use in specific powder metallurgy processes.
[0019] After the feedstock is reduced, the preferred size range of the metal powder may vary depending on the desired end use of the metal powder. For example, the following provides an indication of the ranges that are generally preferred for different powder metallurgy processes. In each case, the lower limit of the range represents the D10 particle size and the upper limit of the range represents the D90 particle size.
[0020] Metal Injection Molding (MIM) - Particle size is 5 microns to 30 microns.
[0021] Gas Driven Cold Spray (GDCS) - particle size ranges from 15 microns to 45 microns.
[0022] Selective Laser Melting (SLM) - Particle size is 20 microns to 50 microns.
[0023] Electron Beam Melting (EBM) - Particle size is 50 microns to 100 microns.
[0024] Laser Metal Deposition (LMD) – Particle size ranges from 50 microns to 125 microns.
[0025] Cold Isostatic Pressing (CIP) - Particle size is 45 microns to 150 microns.
[0026] Hot Isostatic Pressing (HIP) - Particle size is 45 microns to 200 microns.
[0027] The actual particle size range of the powder used for any of the processes specified above may vary beyond the ranges stated. These numbers are provided as a guide to indicate the preferred or ideal particle size range of the metal powders used for these processes.
[0028] The advantage of the spray granulation process is that roughly spherical raw material particles can be formed. A powder formed by a plurality of such particles can be reduced to a metal powder of roughly spherical metal particles. Roughly spherical particles are rounded rather than angular and have a low aspect ratio between the x, y and z axes. The aspect ratio is about 1:1:1. Spherical metal powder particles are advantageous in many powder processing technologies. Currently, spherical metal powders are only produced by processes such as atomization or spheroidization of metal particles. Advantageously, the raw material powder disclosed herein can be directly reduced to produce a metal powder consisting of a plurality of roughly spherical metal powder particles.
[0029] The method can be particularly advantageous for forming alloy metals and alloy metal powders. For the purposes of this application, intermetallic compounds are considered to be alloys. Therefore, a first group of metal oxide particles and a second group of metal oxide particles can be combined with a liquid to form a mixture. The first group of metal oxide particles has a composition different from that of the second group of metal oxide particles. Preferably, the first group of metal oxide particles comprises a first metal oxide, and the second group of metal oxide particles comprises a second metal oxide, and the first metal is a metal different from the second metal. High shear mixing of the mixture can grind the different groups of metal oxide particles into fine particle sizes, such as an average particle diameter of less than 2 microns. The liquid suspension formed by the high shear process contains metal oxides of uniform fineness. In addition, the distribution of each different metal oxide is uniform. By controlling the ratio of the first group of metal oxide particles to the second group of metal oxide particles, the stoichiometry of the raw material powder formed using the method can be controlled. The different metal oxide particles are evenly distributed in the raw material powder produced, and short-range stoichiometry can be achieved.
[0030] Advantageously, the process can be applied to particles in which the average particle size of the first group of metal oxide particles is substantially different from that of the second group of metal oxide particles. The average particle size of the first group of metal oxide particles and the second group of metal oxide particles can differ by more than 2 times. For example, the average particle diameter of the first group of metal oxide particles can be 5 microns, and the average particle diameter of the second group of metal oxide particles can be 10 microns. The average particle diameter of the first group of metal oxide particles and the second group of metal oxide particles can differ by more than 10 times. The average particle size of the first group of metal oxide particles and the second group of metal oxide particles can differ by more than 100 times. Whenever there is a large difference in particle size between two or more groups of mixed particles, it is difficult to produce a raw material with a substantially uniform particle size without losing a large amount of material. The same problem occurs in the case where a single group of particles has a wide particle size distribution. The proposed process solves these problems and enables the controllable formation of a raw material powder consisting of powder particles of substantially uniform size.
[0031] Raw material powders containing complex metal oxide compositions can be produced as described above by mixing more than two groups of different metal oxide particles and processing them. For example, a method for producing a raw material powder may include mixing three or more groups of metal oxide particles (three or more groups each having a different composition). It may be desirable to form a mixture that contains a liquid, a group of titanium dioxide particles having an average particle diameter of less than 2 microns, a group of aluminum oxide particles having an average particle diameter of about 8 microns, and a vanadium pentoxide powder having an average particle diameter of about 100 microns. Advantageously, the method disclosed herein allows the formation of a raw material composed of roughly spherical particles (each of the three oxides has a uniform distribution). Such a raw material can be used to form a titanium-aluminum-vanadium alloy.
[0032] It may be advantageous that the metal oxide particles combined with the liquid to form the mixture are synthetic or refined metal oxide particles. Such particles are typically agglomerates of much finer particles. For example, a vanadium oxide powder particle having a diameter of 100 microns may be an agglomerate of much finer sub-particles having a particle diameter of, for example, less than 1 micron. Such particles may be effectively ground using a high shear mixing process.
[0033] Preferably, the raw powder is grown to a predetermined average particle diameter. The predetermined average particle diameter of the raw powder may be any value in the range of 10 microns to 10 millimeters. A preferred range may be 50 microns to 5 millimeters, such as 50 microns to 200 microns. Advantageously, the process for forming the raw powder may be controlled so that the raw powder has a narrow particle size distribution. For example, the width of the particle size distribution may be less than 100 microns between the D10 diameter and the D90 diameter. For example, the particle size distribution may be 50 microns or less.
[0034] The average particle diameter or average particle size can be determined by a variety of different techniques. For example, the average particle diameter (average particle size) can be determined by screening, laser diffraction, dynamic light scattering or image analysis. Although the exact value of the average particle diameter of the powder particles may be slightly different according to the measurement technique used to determine the average value, in practice, as long as the particles do not have an excessively high aspect ratio, the value has the same magnitude. For example, the technician will understand that it may be found that if the same powder is analyzed by screening, the average particle diameter is assumed to be 150 microns, and if analyzed by different techniques (such as laser diffraction), the average particle diameter is 142 microns. The preferred technique for determining the average particle diameter is laser diffraction. For example, an analyzer such as Malvern Mastersizer Hydro 2000MU can be used to determine the average particle diameter. This analyzer can also be used to determine a particle size range or a particle size distribution.
[0035] One standard method of defining the particle size distribution in a powder involves the D10 and D90 values. The D10 is the particle size value below which 10% of the total number of particles lie. The D90 is the particle size value below which 90% of the total number of particles lie. A raw material powder with a broad particle size distribution will have a large difference between its D10 and D90 values. Similarly, a raw material powder with a narrow particle size distribution will have a small difference between its D10 and D90 values.
[0036] The high shear mixing step may preferably be performed in a high shear mixer having a rotor capable of rotating at more than 5000 rpm (e.g., more than 6000 rpm or about 6500 rpm). The rotor rotates relative to the stator in a tank containing the mixture. That is, the rotor and stator are in a tank containing a mixture of liquid and metal oxide particles. The difference in velocity of the liquid near the tip of the rotor and the liquid adjacent to the stator creates a very high shear zone in the liquid. The high shear grinds the metal oxide particles in the liquid and forms a suspension of the metal oxide and liquid.
[0037] Various high shear mixers are readily available on the market. For example, small amounts can be processed by high shear mixing using an IKA G45M dispersing mixer.
[0038] Preferably, the dried particles from the spray granulator are heat treated before being reduced to metal. Heat treatment by a suitable firing process can remove any traces of organic binder remaining in each particle. The loss of organic binder can introduce a certain degree of porosity into the particles, which may be particularly advantageous in some methods of reducing particles to metals (e.g., electrolytic reduction involving molten salts). For example, the raw powder may contain a plurality of particles having a porosity of 5% to 50%, such as 10% to 30%. In other words, the porosity of a single particle may be 5% to 50%. Heat treatment can also impart a certain degree of mechanical strength to each particle.
[0039] It may be advantageous to heat treat or sinter the particles at a relatively high temperature to produce uniformly mixed metal oxide particles. Thus, the metal oxide particles of the raw powder may be uniformly mixed metal oxide particles having both a predetermined particle size and a predetermined metal element stoichiometry. Thus, the raw powder may be reduced to form a uniform metal alloy having a predetermined alloy composition. Thus, it may be desirable to heat treat the raw particles at a temperature above 900°C (e.g., at about 1000°C to 1400°C).
[0040] The method of producing a metal may comprise the steps of forming a non-metallic feedstock using a method as described herein, and reducing a non-metallic feedstock powder to form a metal. The feedstock powder may be reduced directly to the metal as a powder, or may be formed into a preform for subsequent reduction. Preferably, the feedstock powder is reduced directly to form a metal powder as a powder. The feedstock powder may be reduced by any suitable method, such as by metallothermic reduction.
[0041] It is preferred that the raw material powder is reduced by electrolytic reduction of the raw material powder in contact with a molten salt. For example, a certain amount of raw material powder may be arranged in an electrolytic cell containing a molten salt, and an electric potential may be applied between the anode and the cathode to reduce the raw material to metal. It is particularly preferred that the reduction of the raw material powder is achieved by using an FFC process, in which the raw material powder is contacted with the cathode and the molten salt in the electrolytic cell, and an electric potential is applied between the anode and the cathode so that the raw material is reduced.
[0042] The method for producing metal powder may include the following steps: arranging a cathode and an anode to contact a molten salt in an electrolytic cell, the upper surface of the cathode is loaded with a certain amount of non-metallic raw material, and the lower surface of the anode is vertically separated from the raw material and the cathode; and applying an electric potential between the cathode and the anode so that the raw material is reduced into a plurality of independent metal particles.
[0043] Some reduction processes may only proceed when the molten salt or electrolyte used in the process contains a metal species (reactive metal) that forms an oxide that is more stable than the metal oxide or compound being reduced. This information is readily available in the form of thermodynamic data (specifically, Gibbs free energy data) and can be conveniently determined from a standard Ellingham diagram or predominance diagram or Gibbs free energy diagram. Thermodynamic data and Ellingham diagrams regarding oxide stability are available and understood by electrochemists and extractive metallurgists (in which case these data and information are well known to those skilled in the art).
[0044] Therefore, the preferred electrolyte for the electrolytic reduction process may include a calcium salt. Calcium forms a more stable oxide than most other metals, and therefore can serve to promote the reduction of any metal oxide that is not as stable as calcium oxide. In other cases, salts containing other reactive metals may be used. For example, a salt containing lithium, sodium, potassium, rubidium, cesium, magnesium, calcium, strontium, barium or yttrium may be used to carry out a reduction process according to any aspect of the invention described herein. Chlorides or other salts may be used, including mixtures of chlorides or other salts.
[0045] By selecting an appropriate electrolyte, almost any metal oxide particle can be reduced using the methods and apparatus described herein. Naturally occurring minerals containing one or more such oxides can also be reduced. In particular, it is preferred to use a molten salt containing calcium chloride to reduce oxides of beryllium, boron, magnesium, aluminum, silicon, scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, germanium, yttrium, zirconium, niobium, molybdenum, hafnium, tantalum, tungsten, and lanthanides (including lanthanum, cerium, praseodymium, neodymium, and samarium).
[0046] The skilled person will be able to select a suitable electrolyte for reducing a particular metal oxide, in most cases an electrolyte comprising calcium chloride will be suitable.
[0047] In a particularly advantageous embodiment, the metal produced may be a titanium-aluminum-vanadium alloy. Particles of titanium oxide, aluminum oxide, and vanadium oxide may be combined with a liquid in a suitable ratio to form a mixture, which is then subjected to high shear mixing to form a uniform suspension of the different metal oxides in the liquid. The reduction of the raw powder thus formed is a titanium-aluminum-vanadium alloy of a predetermined composition.
[0048] A raw material powder suitable for reduction to metal may also be provided. The raw material powder may include a plurality of raw material particles having a predetermined average particle diameter. Preferably, the raw material powder consists of substantially spherical particles. The raw material powder is formed by a process as described above. The average particle diameter of the raw material powder may be 50 microns to 500 microns, for example 100 microns to 250 microns.
[0049] In one embodiment, the raw material powder may include titanium oxide and at least one additional metal oxide. The at least one additional metal oxide may be aluminum oxide and / or vanadium oxide and / or niobium oxide, and / or chromium oxide. The composition of the titanium alloy powder formed may be or be close to Ti-6Al-4V. The composition of the titanium alloy powder formed may be or be close to Ti-6Al-6V-2Sn.
[0050] In one embodiment, the raw material powder may include tantalum oxide and at least one additional metal oxide. The at least one additional metal oxide may be aluminum oxide and / or tungsten oxide and / or titanium oxide.
[0051] The step of drying the liquid suspension may include the following additional steps: spraying a portion of the liquid suspension into a heating chamber of a fluidized bed spray granulation device so that liquid is removed from each droplet of the suspension to form a plurality of seed particles; maintaining the plurality of seed particles in the heating chamber by means of a fluidizing gas flow; spraying another portion of the liquid suspension into the heating chamber so that droplets of the liquid suspension are continuously adsorbed on the plurality of seed particles and dried thereon, thereby growing a plurality of raw material particles.
[0052] In this context, any of the additional processing features for forming the feedstock powder as disclosed above may be combined with this aspect of the invention of the feedstock powder.
[0053] The raw material powder may be suitable for reduction to form a metal alloy, such as a metal alloy powder. Advantageously, each non-metallic particle may be a solid solution mixed oxide. Such oxides may be reduced to form metal alloy particles having a uniform distribution of metallic elements. The raw material powder may be suitable for reduction to a Ti-Al-V alloy, the raw material powder comprising titanium, aluminum, vanadium and oxygen.
[0054] The raw material powder may be a uniformly mixed oxide powder. The raw material powder may contain titanium, aluminum and vanadium as well as oxygen, and the ratio of the metal elements in the oxide powder may be 5.5 to 8 weight % aluminum, 3.5 to 6 weight % vanadium, and the rest titanium.
[0055] Depending on the composition, the raw material powder may be suitable for reduction to a titanium-aluminide alloy powder or a titanium-tantalum alloy powder or a tantalum-tungsten alloy powder or a tantalum-aluminum alloy powder.
[0056] Titanium aluminide (48Ti-48Al-2Nb-2Cr) is a high temperature titanium intermetallic compound used in turbines, especially in aerospace.
[0057] Titanium-tantalum (70Ti-30Ta) is a biomedical alloy used in, for example, dental applications.
[0058] Tantalum tungsten (Ta-2.5W) exhibits excellent corrosion resistance at elevated temperatures and is used, for example, in pipes in the chemical industry.
[0059] Tantalum and aluminum are potential capacitor materials. The combination gives a higher dielectric constant than tantalum alone, thus providing higher capacitance. DETAILED DESCRIPTION
[0060] Specific embodiments of one or more aspects of the present invention will now be described with reference to the accompanying drawings, in which:
[0061] Figure 1 is a schematic diagram showing a high shear mixing apparatus suitable for one embodiment of the present invention,
[0062] Figure 2 is a schematic diagram showing a fluidized bed spray granulation apparatus that can be used in an embodiment of the present invention,
[0063] Figure 3 is a schematic diagram showing the use of a spray granulation process to form raw material powder particles,
[0064] Figure 4 is a photomicrograph showing particles of a raw material powder formed using one embodiment of the present invention,
[0065] Figure 5 yes Figure 4 Electron micrograph of a portion of the powder,
[0066] Figure 6 , 7 and 8 are shown Figure 5 The aluminum on the area depicted in the micrograph ( Figure 6 ),vanadium( Figure 7 ) and titanium ( Figure 8 ) distribution of energy dispersive X-ray spectroscopy (EDS) elemental map,
[0067] Fig. 9 is a schematic diagram showing an electrolysis device arranged to reduce a raw material powder according to one embodiment of the present invention,
[0068] Fig.10 It is shown Fig. 9 A schematic cross-sectional view of additional details of the cathode structure of the electrolysis device,
[0069] Fig.11 yes Fig.10 A top view of the cathode shown in FIG.
[0070] Fig.12 By restoring Figure 4 SEM micrograph of Ti-Al-V alloy powder particles produced from raw powder.
[0071] The present invention relates to a method of forming a raw powder suitable for reduction to a metal. The present invention also relates to a raw powder formed by the method, and a method of producing a metal comprising the step of reducing the raw powder formed by the method. The method of forming the raw powder comprises the steps of combining a liquid with metal oxide particles to form a mixture, preferably the mixture having an oxide ratio of 50% to 70% by weight; subjecting the mixture to high shear mixing to form a liquid suspension; and drying the liquid suspension using a fluidized bed spray granulation process. The method has high shear mixing and fluidized bed spray granulation and will be discussed in general terms.
[0072] Figure 11 is a schematic diagram of a high shear mixing device 10 that may be suitable for forming a liquid suspension in various embodiments of the present invention. The high shear mixing device 10 includes a tank 11 containing a mixture 12 of a liquid and metal oxide particles. A high shear mixer 20 is arranged to contact the liquid mixture 12. The high shear mixer includes a motor 21, a connecting shaft 22, a rotor 23, and a stator 24. The rotor 23 is separated from the stator 24 by a narrow gap 25. In use, the motor 21 rotates the rotor 23 at a speed of typically 5000 rpm to 10000 rpm. Due to the rotor rotating and the stator remaining stationary and the speed difference of the liquid in the rotor and stator regions, high shear in the liquid is caused.
[0073] Typically, the liquid mixture 12 consists of an aqueous solution of a binder such as polyvinyl alcohol (PVA) and a certain proportion of metal oxide particles. The high shear forces generated in the liquid mixture 12 result in grinding of the metal oxide particles. Multiple parameters can be changed to affect the final particle size of the ground oxide. For example, all parameters such as the speed of the rotor 23, the distance of the gap 25 between the rotor and the stator, the ratio of metal oxide to liquid in the liquid mixture 12, and the mixing time can be changed to affect the particle size of the metal oxide produced by the high shear mixing process. High shear mixing forms a suspension of finely ground metal oxide particles in a liquid (e.g., an aqueous solution of PVA).
[0074] Various suitable high shear mixers or batch mixers are known and commercially available. For example, A wide variety of batch mixers are manufactured for forming pharmaceutical suspensions. These high shear mixers may be suitable in various embodiments of the present invention.
[0075] Figure 2 31 is a schematic diagram of a fluidized bed spray granulation device 30. The device includes a heating chamber through which an upwardly directed hot air stream 32 passes. A nozzle 33 injects droplets 34 of a liquid suspension into the heating chamber 31. The droplets 34 of the liquid suspension may be supplied directly by the high shear mixing device 10, or may be transferred to a separate holding tank before injection. Once in the heating chamber 31, the droplets 34 of the liquid suspension are dried and form solid particles 35. These solid particles 35 are maintained in the heating chamber 31 by the fluidization of the heated air stream 32. As additional droplets 34 of the liquid suspension are injected into the heating chamber 31, the droplets are adsorbed on the existing particles 35 and dried, thereby increasing the diameter of the particles 35. As the particles grow, they eventually reach a mass that is too large for them to be maintained in the fluidized state in the chamber. Once the particles reach such a diameter, they fall toward the bottom of the chamber and are collected.
[0076] The size, shape and mass of the collected particles 36 and the size distribution of the collected particles 36 can be influenced by controlling parameters such as the oxide loading of the liquid suspension, the injection pressure and the initial droplet size and the flow rate of the fluidizing gas stream.
[0077] The use of spray granulation technology allows a great degree of flexibility in controlling particle size and particle size distribution. By controlling and optimizing the process parameters, particle sizes in the range of 10 microns to 10 millimeters can be achieved. The advantage of this system is that any undersized particles that pass through the spray granulator can be returned to the heating chamber 31 for further growth. In addition, any oversized particles can be returned to the high shear mixer. Therefore, the process yield should easily exceed 90%, preferably exceed 95%, or exceed 98%.
[0078] Figure 3 is a schematic diagram depicting particle growth in a fluidized bed spray granulation apparatus. Once droplets 34 of a liquid suspension are injected into the heated chamber of the spray granulation apparatus, they dry rapidly to form small seed particles 35. Figure 2 As discussed, these seed particles 35 are fluidized by a stream of hot air. Subsequent droplets 37 of the liquid suspension adhere to the surface of the seed particles 35. These additional droplets quickly cover the surface of the seed particles and dry to add a layer of thickness to the seed particles. Over time, more and more droplets adhere to the surface of the fluidized particles and form a layer of onion-like particles 36. Figure 3 A cross-section of a fully formed particle 36 is shown, illustrating the layered structure.
[0079] Once the particles reach a predetermined particle size, they are collected from the spray granulation device. Preferably, the particles are then heat treated to drive off any residual binder from the particles and provide some mechanical stability. The heat treatment may also have the result of homogenizing the composition of the particles. Thus, the collected particles 36 may be subjected to a heat treatment regimen. The heat treatment may be a two-step regimen, which includes, for example, heating to 500° C. and holding for a period of time, followed by heating to 1000° C. and holding for a further period of time.
[0080] After the particles are collected (and heat treated if necessary), the raw powder can be reduced to form the metal. Preferably, the raw powder is reduced directly in powder form to produce the metal powder. However, it may be desirable to form the raw powder into a preform shape or pellets before reducing it to the metal.
[0081] Fig. 9An electrolysis device 110 configured for reducing a raw material powder is shown. The device includes a stainless steel cathode 120 and a carbon anode 130 located within a housing 140 of an electrolytic cell. The anode 130 is disposed above the cathode 120 and is spatially separated from the cathode 120. In certain embodiments, the housing 140 may contain 500 kg of a molten salt electrolyte 150 based on calcium chloride, the electrolyte comprising CaCl2 and 0.4 wt% CaO. Both the anode 130 and the cathode 120 are arranged to contact the molten salt 150. Both the anode 130 and the cathode 120 are connected to a power supply 160 so that an electric potential can be applied between the cathode and the anode.
[0082] Both cathode 120 and anode 130 are substantially horizontally oriented, with an upper surface of cathode 120 facing a lower surface of anode 130 .
[0083] The cathode 120 includes a rim 170 extending upward from the outer edge of the cathode, which acts as a retaining barrier for the raw material powder 190 loaded on the upper surface of the cathode. The rim 170 is integral with the cathode and is formed of the same material as the cathode. In other embodiments, the rim may be formed of a different material from the cathode, such as an electrically insulating material.
[0084] Can be Fig.10 and Fig.11 The structure of the cathode can be seen in more detail in FIG. 1. The rim 170 is in the form of a ring having a diameter of 30 cm. A first support cross-member 175 extends across the diameter of the rim. The cathode also includes a mesh support member 171 which is in the form of a ring having a diameter equal to that of the rim 170. On the rim 170, the mesh support member has a second support cross-member 176 of the same size as the support cross-member 175. The mesh 180 is supported by being sandwiched between the rim 170 and the mesh support member 171 (at Fig.10 The mesh 180 is shown in dotted lines. The mesh 180 comprises a stainless steel fabric with a mesh size of 100, which is held taut by the edge 170 and the mesh support member. The crossbeam 175 is arranged to abut against the lower surface of the mesh 180 and serves to support the mesh. The upper surface of the mesh 180 serves as the upper surface of the cathode.
[0085] The stainless steel fabric forming the mesh 180 is made of 30 micron thick 304 stainless steel wire, which is woven to form a fabric with square holes of 150 micron holes. The mesh size can vary and should generally have a diameter smaller than the average particle diameter of the raw material powder being reduced. The mesh 180, beam 175 and edge 170 forming the cathode are all conductive. In other embodiments, the mesh can be the only conductive component in the cathode.
[0086] In use, the raw powder may be reduced by applying a potential between cathode 120 and anode 130 sufficient to remove oxygen from raw powder 190. After reduction, the remaining metal powder product may be removed and washed to separate the metal powder from any remaining salts.
[0087] Example 1
[0088] As a specific example, a Ti-Al-V alloy is formed using aspects of the invention disclosed herein. The initial oxide powders used to form the raw material powder for reduction are TiO2, Al2O3 and V2O5. The average particle size of the TiO2 oxide powder is 1.2 microns. The average particle size of the Al2O3 oxide powder is 8.2 microns. The average particle size of the V2O5 powder is 97.7 microns. Due to the large difference between the initial particle sizes of the starting oxides, it is extremely difficult to combine these three oxide powders in a suitable ratio to form an alloy containing a low proportion of Al and V (e.g., Ti-6Al-4V alloy powder). Although large pellets with a desired oxide ratio can be formed, it is obvious that it is unlikely to approach the short-range composition required to form a Ti-6Al-4V alloy.
[0089] A total of 4800 grams of mixed oxide powder was used. Of these 4800 grams, 4195 grams were TiO2, 402 grams were Al2O3 and 203 grams of V2O5. This corresponds to a metallic element ratio of 88.5% Ti, 7.5% Al and 4% V. This feedstock was produced as a preliminary proof of concept. It is expected that the oxide feedstock powder of this composition will produce an alloy with a composition close to Ti-6Al-4V after reduction by the FFC process. It should be noted that the proportion of aluminum in the feedstock powder was intentionally increased to above 6% to take into account the loss of aluminum during the reduction process.
[0090] The oxide powder is mixed with a liquid to form a slurry having 59.5% solid oxide. The liquid consists of an aqueous solution of demineralized water and PVA. The proportion of PVA depends on the total oxide loading. Therefore, the proportion of PVA is 2.5% by weight relative to the total oxide loading. The liquid mixture is then subjected to high shear mixing at 6500 rpm for 15 minutes. An IKA dispersing mixer model G45M is used to achieve shear mixing.
[0091] After shear mixing, the liquid and oxide mixture form a suspension of ground oxide particles in the liquid / binder. The particle size of the oxide is substantially uniform, with the diameter of the oxide particles in the suspension being in the range of 2 microns or less. The liquid suspension is then subjected to a fluidized bed spray granulation process to produce solid oxide particles. A Glatt Procell Labsystem spray granulator is used to form the metal oxide particles. The process parameters are set so that the fluidizing air flow through the device is 150 m / s. 3 / hour, the air temperature was 120°C. The liquid suspension was sprayed into the chamber at a spray pressure of 3 bar and a spray rate of 57 g / min. These parameters were selected to provide an average product particle size of 100 to 200 microns.
[0092] After spray granulation, the collected oxide particles are heat treated. The heat treatment is performed to remove the organic component PVA binder and to impart mechanical strength to each individual powder particle. The heat treatment scheme also homogenizes the composition of each particle forming a solid solution of a metal oxide mixture.
[0093] To heat treat the oxide particles produced by spray granulation, they were heated to a temperature of 550°C in an electrically heated furnace at a rate of 3°C / min. The particles were maintained at this temperature for a period of 1 hour to remove traces of organic binder. The particles were then heated to 1000°C at 3°C / min and maintained at this temperature for a further 2 hours before cooling to room temperature. The resulting raw powder is shown in Figure 4 middle.
[0094] Figure 4 A raw material powder for reduction to form a Ti-Al-V powder is shown. The raw material powder was analyzed using a Malvern Mastersizer 2000 and found to contain a plurality of raw material particles having an average particle diameter of about 160 microns. The D10 particle size was 119 microns and the D90 particle size was 225 microns. The raw material powder was generally spherical and had a mixed oxide composition comprising titanium, aluminum and vanadium.
[0095] A portion of the raw powder is fixed and polished. Figure 5 An SEM micrograph of the powder is shown. It can be seen that the powder particles are substantially the same size and are relatively porous. The porosity of the powder may enhance the reduction of the powder using a molten salt reduction process.
[0096] The distribution analysis of aluminum, vanadium and titanium was performed using elemental X-ray mapping in a scanning electron microscope (SEM). Figure 6 Shows Figure 5 The distribution of aluminum in the sample, Figure 7 shows the distribution of vanadium in the same sample, and Figure 8shows the distribution of titanium in the same sample. Figure 6 The distribution of aluminum is unclear (probably due to the low atomic weight of aluminum), but it can be seen that the distribution of vanadium and titanium in the particles appears uniform. Figure 5 There are no vanadium rich or depleted regions in the particles shown. Considering the initial vanadium particle size is about 100 microns, it can be seen that the high shear mixing followed by spray granulation steps produce uniform raw powder particles with the desired elemental distribution and an average particle size of about 160 microns.
[0097] Use the above Fig. 9 The type of apparatus discussed is used to reduce the raw material powder to a metal alloy powder. About 20 grams of the raw material powder is placed on the upper surface of the cathode 20 and contacts the molten salt 150. The raw material powder 190 is supported by the mesh 180 of the cathode. The depth of the raw material powder 190 is about 1 cm.
[0098] The molten salt 50 (CaCl2 and 0.4 wt% CaO) was maintained at a temperature of 950°C and an electric potential was applied between the anode and the cathode. The heat flow and gas lift offset generated by the buoyancy of the gas (mainly CO and CO2) generated at the anode caused the molten salt to circulate within the cell and form a molten salt flow through the raw material powder bed. The cell was run in a constant current mode (at a current of 5 amperes) for a period of 16 hours. After this time, the cell was cooled, and the cathode was removed and washed to release the salt from the reduced raw material powder.
[0099] The reduced raw powder was removed from the cathode as a friable mass of metal alloy powder particles. The mass was broken up with an agate pestle and mortar and the material was separated into individual powder particles. The particles were then dried and analyzed. The analysis showed that the powder particles were a homogeneous titanium alloy with a composition close to Ti-6Al-6V. Fig.12 is a SEM micrograph showing one of the metal powder particles. This preliminary experiment shows that common commercial alloys, such as Ti-6Al-4V or Ti-6Al-6V-2Sn, can be produced using embodiments of the present invention by varying the ratios or types of oxides used to form the feedstock.
[0100] Example 2
[0101] As another specific example, titanium-aluminide intermetallic compounds (Ti-Al-Nb-Cr intermetallic compounds) are formed using aspects of the invention disclosed herein. The initial oxide powders used to form the raw material powder for reduction are TiO2, Al2O3, Nb2O5, and Cr2O3. The average particle size of the TiO2 oxide powder is 1.2 microns. The average particle size of the Al2O3 oxide powder is 8.2 microns. The average particle size of the Nb2O5 powder is 0.5 microns to 2 microns, and the average particle size of the Cr2O3 powder is 1 micron to 5 microns.
[0102] A total of 5000 g of mixed oxide powder was used. Of this total amount, 2861.4 g were TiO2, 1826.7 g were Al2O3, 198.4 g were Nb2O5, and 113.5 g were Cr2O3.
[0103] The oxide powder was mixed with an aqueous solution of demineralized water and PVA to form a slurry having 59.5% solid oxide. The slurry was then subjected to high shear mixing and spray granulation as described in Example 1. The spray granulation parameters were selected to provide a particle size distribution in the range of 100 microns to 250 microns. The spray granulation product was a powder of free-flowing gray-green particles.
[0104] After spray granulation, the collected oxide particles were heat treated to form a raw powder as described above with respect to Example 1. The raw powder was then reduced using a reduction process as described with respect to Example 1. The reduced powder was then collected and washed. SEM-EDX analysis of a number of powder particles showed that the average composition of the metal alloy powder was 45.46 atomic % Al, 50.23 atomic % Ti, 2.09 atomic % Cr, and 2.22 atomic % Nb.
[0105] Example 3
[0106] As another specific example, titanium-tantalum alloy (Ti-Ta alloy) is formed using aspects of the invention disclosed herein. The initial oxide powders used to form the raw material powder for reduction are TiO2 and Ta2O5. The average particle size of the TiO2 oxide powder is 1.2 microns. The average particle size of the Ta2O5 oxide powder agglomerates is 300 microns.
[0107] A total of 5000 g of mixed oxide powder was used. Of this total amount, 3806.3 g were TiO2 and 1193.7 g were Ta2O5.
[0108] The oxide powder was mixed with an aqueous solution of demineralized water and PVA to form a slurry having 53.2% solid oxide. The slurry was then subjected to high shear mixing and spray granulation as described in Example 1. The spray granulation parameters were selected to provide a particle size distribution in the range of 100 microns to 250 microns. The spray granulation product was a powder of free-flowing gray-green particles.
[0109] After spray granulation, the collected oxide particles were heat treated to form a raw powder as described above with respect to Example 1. The raw powder was then reduced using a reduction process as described with respect to Example 1. The reduced powder was then collected and washed. SEM-EDX analysis of a number of powder particles showed that the average composition of the metal alloy powder was 70.19 wt % Ti and 29.81 wt % Ta.
[0110] Example 4
[0111] As another specific example, a tantalum-tungsten alloy (Ta-W alloy) is formed using the various aspects of the invention disclosed herein. The initial oxide powders used to form the raw material powder for reduction are Ta2O5 and W2O3. The average particle size of the Ta2O5 oxide powder agglomerates is 300 microns. The particle size distribution of the WO3 oxide powder is 0.5 microns to 5 microns.
[0112] A total of 5000 g of mixed oxide powder was used. Of this total amount, 4871 g were Ta2O5 and 129 g were WO3.
[0113] The oxide powder was mixed with an aqueous solution of demineralized water and PVA to form a slurry having 59.5% solid oxide. The slurry was then subjected to high shear mixing and spray granulation as described in Example 1. The spray granulation parameters were selected to provide a particle size distribution in the range of 100 microns to 250 microns. The spray granulation product was a powder of free-flowing gray-green particles.
[0114] As described above with respect to Example 1, after spray granulation, the collected oxide particles were heat treated to form a raw powder. The raw powder was then reduced using a reduction process as described with respect to Example 1. The reduced powder was then collected and washed. SEM-EDX analysis of a number of powder particles showed that the average composition of the metal alloy powder was 93.61 wt % Ta and 6.39 wt % W.
[0115] Example 5
[0116] As another specific example, a tantalum-aluminum alloy (Ta-Al alloy) is formed using the various aspects of the invention disclosed herein. The initial oxide powders used to form the raw material powder for reduction are Ta2O5 and Al2O3. The average particle size of the Ta2O5 oxide powder agglomerates is 300 microns. The average particle size of the Al2O3 oxide powder agglomerates is 120 microns.
[0117] A total of 5000 g of mixed oxide powder was used. Of this total amount, 4847 g were Ta2O5 and 153 g were Al2O3.
[0118] The oxide powder was mixed with an aqueous solution of demineralized water and PVA to form a slurry having 59.5% solid oxide. The slurry was then subjected to high shear mixing and spray granulation as described in Example 1. The spray granulation parameters were selected to provide a particle size distribution in the range of 100 microns to 250 microns. The spray granulation product was a powder of free-flowing gray-green particles.
[0119] After spray granulation, the collected oxide particles were heat treated to form a raw powder as described above with respect to Example 1. The raw powder was then reduced using a reduction process as described with respect to Example 1. The reduced powder was then collected and washed. SEM-EDX analysis of a number of powder particles showed that the average composition of the metal alloy powder was 97.84 wt % Ta and 2.16 wt % Al.
Claims
1. A method for producing a metal, the method comprising: The following steps are involved: Forming a non-metallic raw material powder suitable for reduction into metal, the steps of forming the non-metallic raw material powder include: combining a liquid with solid metal oxide particles to form a mixture, wherein the sum of all metal oxide particles combined with the liquid to form the mixture comprises 50% to 70% by weight of the mixture, subjecting the mixture to high shear mixing to form a liquid suspension of the metal oxide and the liquid, Drying the liquid suspension using a fluidized bed spray granulation process to grow a plurality of particles to form the non-metallic raw material powder, heat treating the non-metallic raw material powder so that the porosity of the plurality of particles is between 5% and 50%, wherein the non-metallic raw material powder is heat treated at a temperature between 1000 degrees Celsius and 1400 degrees Celsius, and The non-metal feedstock powder is reduced to form a metal.
2. The method according to claim 1, wherein the step of drying the liquid suspension comprises the following further steps: spraying a portion of the liquid suspension into a heated chamber of a fluidized bed spray granulation apparatus such that liquid is removed from individual droplets of the suspension to form a plurality of seed particles; maintaining the plurality of seed particles within the heating chamber by means of a fluidizing gas stream; and Another portion of the liquid suspension is sprayed into the heating chamber, and droplets of the liquid suspension are continuously adsorbed to the plurality of seed particles and dried thereon, thereby causing the particles to grow to form the non-metallic raw material powder.
3. The method according to claim 1 or 2, wherein the liquid comprises water and an organic binder.
4. The method according to claim 1 or 2, wherein the liquid comprises water and an organic binder, wherein the binder is an aqueous solution of polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP) or hydroxyethyl cellulose (HEC).
5. The method of claim 1 or 2, wherein a first group of metal oxide particles and a second group of metal oxide particles are combined with the liquid to form the mixture, the first group of metal oxide particles having a different composition than the second group of metal oxide particles. 6 . The method of claim 5 , wherein the first group of metal oxide particles and the second group of metal oxide particles have different average particle sizes. 7 . The method of claim 6 , wherein the average particle size of the first group of metal oxide particles differs from the average particle size of the second group of metal oxide particles by a factor of more than 2. 8 .
8. The method of claim 6, wherein the average particle size of the first group of metal oxide particles differs from the average particle size of the second group of metal oxide particles by a factor of more than 10.
9. The method of claim 6, wherein the average particle size of the first group of metal oxide particles differs from the average particle size of the second group of metal oxide particles by a factor of greater than 100.
10. The method of claim 5, comprising three or more groups of metal oxide particles, each of the three or more groups having a different composition.
11. The method according to claim 1 or 2, wherein a process of forming the raw material powder is controlled so that the raw material powder has a predetermined average particle diameter.
12. The method of claim 11, wherein the predetermined average particle diameter is from 10 microns to 10 millimeters.
13. The method of claim 11, wherein the predetermined average particle diameter is from 50 microns to 5 millimeters.
14. The method of claim 11, wherein the predetermined average particle diameter is 50 microns to 200 microns.
15. The method according to claim 1 or 2, wherein the process of forming the raw material powder is controlled so that the raw material powder has a particle size distribution of less than 100 microns between D10 diameter and D90 diameter.
16. The method according to claim 1 or 2, wherein a process of forming the raw material powder is controlled so that the raw material powder has a particle size distribution of 50 micrometers or less between a D10 diameter and a D90 diameter.
17. The method of claim 1 or 2, wherein high shear mixing is performed using a rotor rotating at more than 5000 rpm.
18. The method of claim 1 or 2, wherein high shear mixing is performed using a rotor rotating at more than 6000 rpm.
19. The method according to claim 1 or 2, wherein the reduction of the non-metallic raw material powder is carried out by electrolytic reduction of the raw material powder in contact with a molten salt.
20. The method of claim 19 wherein the metal produced is a titanium-aluminum-vanadium alloy and particles of titanium oxide, aluminum oxide and vanadium oxide are combined with the liquid to form the mixture.
21. The method of claim 19 wherein the metal produced is a titanium-aluminum-niobium-chromium intermetallic compound and particles of titanium oxide, aluminum oxide, niobium oxide and chromium oxide are combined with the liquid to form the mixture.
22. The method of claim 19 wherein the metal produced is a titanium-tantalum alloy and particles of titanium oxide and tantalum oxide are combined with the liquid to form the mixture.
23. The method of claim 19 wherein the metal produced is a tantalum-tungsten alloy and particles of tantalum oxide and tungsten oxide are combined with the liquid to form the mixture.
24. The method of claim 19 wherein the metal produced is a tantalum-aluminum alloy and particles of tantalum oxide and aluminum oxide are combined with the liquid to form the mixture.
Citation Information
Patent Citations
Removal of oxygen from metal oxides and solid solutions by electrolysis in a fused salt
WO1999064638A1
Materials processing method and apparatus
WO2003048399A2
Reduction of metal oxides in an electrolytic cell
WO2003076690A1
Method for preparing active metal titanium and boron carbide complex spherical hot spraying powder
CN101176920A
Preparation method of ozone catalytic oxidation catalyst used for treating oil refining waste water
CN101982237A