Device and method for diamond explosive extrusion growth

By using a diamond explosive extrusion growth device and method, and by utilizing low-explosive explosives and angle adjustment, large-particle micron-sized diamonds were successfully synthesized, solving the problem of uneven particle size distribution in existing technologies and achieving industrialized production and cost reduction.

CN107715799BActive Publication Date: 2024-11-12NANJING UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201610658090.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2016-08-11
Publication Date
2024-11-12
Estimated Expiration
2036-08-11

AI Technical Summary

Technical Problem

Existing technologies are insufficient for the effective synthesis of large-particle micron-sized diamonds, and the uneven particle size distribution makes industrial production difficult.

Method used

A diamond explosive extrusion growth device is used. By adjusting the angle of the base plate and the extrusion fly plate, the explosive force of low-velocity explosive is used to extrude diamond powder into large micron-sized diamond particles. A mixture of ammonium nitrate explosive and wood flour is used as the driving agent, combined with purification treatment with dilute nitric acid.

Benefits of technology

It achieves narrow particle size distribution and one-time molding of large micron-sized diamond particles, which is suitable for industrial production, reduces production costs and simplifies equipment structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN107715799B_ABST
    Figure CN107715799B_ABST
Patent Text Reader

Abstract

The present invention provides a device and method for diamond explosion extrusion growth. The device comprises a base plate, an extrusion fly plate, and a pulley; a groove for containing diamond powder is provided on the base plate, a connecting end of the extrusion fly plate is connected to one end of the base plate, a movable end of the extrusion fly plate is connected to the pulley and the angle between the extrusion fly plate and the base plate is adjusted by the pulley, a low-explosion velocity explosive is arranged on the extrusion fly plate, and a detonator is fixed at the bottom end of the low-explosion velocity explosive. The low-explosion velocity explosive is used to drive the extrusion fly plate to impact small-particle diamond powder, and the speed of the fly plate is as high as 7km / s. When the extrusion fly plate contacts the diamond powder, the high temperature and high pressure generated make the diamond powder melt and aggregate to form large-particle micron-sized diamond. The diamond explosion extrusion growth method adopted by the present invention has a high conversion rate of diamond particles, and can achieve more than 25% of small-particle diamonds into large particles; the production is carried out by using powdered emulsion explosives and wood powder, the process is simple, the cost is low, and the output is easy to enlarge, which is convenient for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of explosive welding and high temperature and high pressure synthesis, and in particular to a device and method for synthesizing large-particle micron diamond by explosive extrusion. Background Art

[0002] The polycrystalline diamond prepared by the present invention is a superhard material, a high-end product among diamonds, with ultra-high purity and ultra-precision polishing effect, and is widely used in ultra-precision polishing of magnetic heads, hard disks, gemstones, hard glass, ceramics and hard alloys; additives for lubricants or engine oils, coatings for metal molds, tools, parts, etc., reinforcing agents for rubber or plastics, packaging materials for IT products and magnetic recording systems; components of transmitting fields and CVD film materials.

[0003] At present, the main methods for artificially synthesizing diamonds include static pressure method and detonation method. The static pressure method synthesizes diamonds, that is, using the static high pressure generated by the hydraulic six-sided top press and the high temperature generated by the electric furnace to transform graphite into diamond under the action of a catalyst. Although the process is simple, it is costly and is mainly used in low-end markets such as sandpaper. The detonation method synthesizes diamonds by using the carbon in the negative oxygen balance explosive to undergo agglomeration and phase transformation under the thermodynamic conditions of the explosive detonation to generate nano-sized diamonds. Chinese patent CN01114454.8 proposes a method for synthesizing nano-diamonds by detonation method. The product characteristics are that the particle size is concentrated in the range of 1 to 100 nm, the particle shape is spherical, but it is easy to agglomerate. Patent CN101112678A proposes a method for synthesizing diamonds by detonation with an external carbon source in the explosive, and successfully produces micron diamonds, but the particle size distribution of the product is wide. Since the particle size of the product itself is relatively small, it is difficult to grade the product. Summary of the invention

[0004] The object of the present invention is to provide a device and method for diamond explosion extrusion growth, which can increase the diamond particle size.

[0005] The technical solution provided to achieve the purpose of the present invention is as follows:

[0006] A device for extruding and growing diamond by explosion, comprising a base plate, an extrusion fly plate, and a pulley; a groove for containing diamond powder is formed on the base plate, a connecting end of the extrusion fly plate is connected to one end of the base plate, a movable end of the extrusion fly plate is connected to the pulley and an angle between the extrusion fly plate and the base plate is adjusted by the pulley, low-detonation-velocity explosives are arranged on the extrusion fly plate, and a detonator is fixed to the bottom end of the low-detonation-velocity explosives.

[0007] Furthermore, the base plate is made of 45# steel and the extruded fly plate is made of 45# steel.

[0008] The method for synthesizing large-grain micron diamond of the present invention comprises the following steps in sequence:

[0009] (a) Spreading low detonation velocity explosives flat on the extruded flyer plate;

[0010] (b) Fill the groove with small diamond powder particles;

[0011] (c) adjusting the angle θ between the extrusion flyer plate and the base plate by pulling the pulley;

[0012] (d) starting the detonator to detonate the low-detonation-velocity explosive, so that the extrusion flyer plate extrudes the base plate under the action of the explosion force, thereby obtaining a crude product containing large-particle micron diamonds;

[0013] (e) Purifying the crude product obtained in (d) to obtain large-particle micron diamond.

[0014] Furthermore, in step (a), the drug layer thickness H2 is 20 mm.

[0015] Furthermore, in step (c), the angle θ is 30° to 45°.

[0016] The low-explosion-velocity explosive used in the present invention is 90% of powdered ammonium-titanium explosive and 10% of wood powder, and the low-explosion-velocity explosive (4) has an explosion velocity of 2000 m / s. The particle size of the powdered ammonium-titanium explosive is between 1 and 2 μm, and the particle size of the wood powder is between 5 and 10 μm.

[0017] The size of the small-particle micron diamond in the present invention is between 0.46 and 3.21 μm, and the size of the large-particle micron diamond is between 5 and 10 μm.

[0018] Compared with the prior art, the present invention has the following significant advantages:

[0019] (1) The product of the present invention is large-particle micron diamond with a narrow particle size distribution.

[0020] (2) The present invention adopts explosive extrusion growth technology, which is formed in one step, is simple in industry, and can realize industrial production.

[0021] (3) The driving explosive used in the present invention is a mixture of ammonium tantalum explosive and wood powder, which is cheap and widely available.

[0022] (4) The base plate and the extruded fly plate used in the present invention have a simple structure and can be made of ordinary stainless steel, which is cheap and easy to process. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the structure of the device for diamond explosion extrusion growth of the present invention;

[0024] Figure 2is the XRD diagram of the product when the angle between the extruded flying plate and the substrate is 30° in the present invention;

[0025] Figure 3 It is a particle size distribution diagram of the product when the angle between the extrusion flying plate and the base plate is 30° in the present invention;

[0026] Figure 4 This is a scanning electron microscope image of the product when the angle between the extruded flying plate and the substrate is 30° in the present invention;

[0027] Figure 5 is a particle size distribution diagram of the diamond raw material in the present invention;

[0028] Figure 6 This is a SEM image of the product when the angle between the extruded flying plate and the substrate is 45° in the present invention. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below in conjunction with the accompanying drawings.

[0030] The present invention is realized by the following means:

[0031] like Figure 1 As shown, a device for explosive extrusion growth of diamonds comprises a base plate 1, an extrusion flying plate 3, and a pulley 6; a groove 2 for containing diamond powder is formed on the base plate 1, a connecting end of the extrusion flying plate 3 is connected to one end of the base plate 1, a movable end of the extrusion flying plate 3 is connected to the pulley 6 and the angle between the extrusion flying plate 3 and the base plate 1 is adjusted by the pulley 6, a low-detonation-velocity explosive 4 is arranged on the extrusion flying plate 3, and a detonator 5 is fixed to the bottom end of the low-detonation-velocity explosive 4.

[0032] In the present invention, the angle between the squeezing flying plate 3 and the pulley 6 is controlled by the pulley. In addition, any device for achieving stretching can be used in the device, which will not be described in detail here.

[0033] The length×width×height dimensions of the base plate 1 are: 800×250×45mm; the length×width×height dimensions of the extruded fly plate 3 are: 490×190×10mm; the length×width×height dimensions of the groove 2 are: 500×200×2mm. The base plate 1 is 45# steel, and the extruded fly plate 3 is 45# steel.

[0034] Example 1: θ = 30°

[0035] Weigh 90g of ammonium nitrate explosive and 10g of wood powder and mix them evenly for use. Spread the mixed low-detonation-velocity explosive on the extrusion fly plate, with a thickness of 20mm; spread small-particle diamond powder in the groove, with a thickness of 2mm; place the extrusion fly plate against the base plate, pull the pulley to adjust the extrusion fly plate to 30° with the base plate; detonate the low-detonation-velocity explosive with a detonator at the connecting end of the extrusion fly plate to obtain a product containing large-particle micron diamonds. Collect the explosion products, pass them through a 100-mesh sieve, and remove larger impurities such as metal wires and adhesive tape fragments. Dry the solution to obtain the initial product of large-particle diamonds. Add dilute nitric acid to the initial product and react at 80°C for 3 hours, wash with deionized water until neutral, and put it in an oven for drying to obtain large-particle micron diamonds.

[0036] The samples were tested using a D8ADVANCE X-ray diffractometer. Figure 2 As shown in the figure, the characteristic peaks of the diffraction pattern of the sample are at 43°, 75°, and 91°, proving that the synthesized diamond is cubic diamond. The sample was observed using a JEOL JSM-6380LV field emission scanning electron microscope, as shown in the figure. Figure 3 As shown in the figure, its appearance has sharp edges and irregular shapes; the particle size is tested by BT-9300H laser particle size distribution analyzer, as shown in the figure. Figure 4 As shown, its particle size distribution range is in the range of 5 to 10 μm, and the median particle size is d 50 =6.18μm. However, for the test of small diamond powder, such as Figure 5 As shown in Figure 2, the particle size distribution range is between 0.46 and 3.21 μm, and the median particle size is d 50 =1.16μm.

[0037] The above tests have proven that the device and method can synthesize large-particle micron diamonds, and the product particle size distribution is narrow.

[0038] Example 2: θ = 45°

[0039] According to the formula ratio of low-explosion velocity explosives, 90g of ammonium-tetium explosive and 10g of wood powder are weighed and mixed evenly for standby use. The mixed low-explosion velocity explosive is spread on the extruded fly plate, and the thickness of the drug layer H2 is 20mm; the small-particle diamond powder is spread in the groove, and the thickness H4 is 2mm; the extruded fly plate is leaned against the base plate, and the pulley is pulled to adjust the extruded fly plate to 45° with the base plate; the low-explosion velocity explosive is detonated with a detonator at the connecting end of the extruded fly plate to obtain a product containing large-particle micron diamonds. The explosion products are collected and passed through a 100-mesh sieve to remove larger impurities, such as metal wires, adhesive tape fragments, etc. The solution is dried to obtain the initial product of large-particle diamonds. Dilute nitric acid is added to the initial product and reacted at 80°C for 3 hours, washed with deionized water until neutral, and placed in an oven for drying to obtain large-particle micron diamonds.

[0040] The sample was tested using a D8ADVANCE X-ray diffractometer. The characteristic peaks of the sample's diffraction pattern are at 43°, 75°, and 91°, proving that the synthesized diamond is a cubic diamond. The sample was observed using a JEOL JSM-6380LV field emission scanning electron microscope. Figure 6 As shown, its appearance has sharp edges and irregular shapes; tested by Bettersize2000 laser particle size distribution analyzer, its particle size distribution range is 1.48~3.94μm, and the median particle size is d 50 =2.23μm.

[0041] The above tests have proven that the device and method can synthesize large-particle micron diamonds, and the product particle size can be controlled by angle.

Claims

1. A device for diamond explosion extrusion growth, characterized in that: The device comprises a base plate (1), an extrusion flying plate (3), and a pulley (6); a groove (2) for containing diamond powder is formed on the base plate (1); a connecting end of the extrusion flying plate (3) is connected to one end of the base plate (1); a movable end of the extrusion flying plate (3) is connected to the pulley (6); and an angle between the extrusion flying plate (3) and the base plate (1) is adjusted by the pulley (6); a low-detonation-velocity explosive (4) is arranged on the extrusion flying plate (3); and a detonator (5) is fixed to the bottom end of the low-detonation-velocity explosive (4); The steps of the method for diamond explosion extrusion growth are as follows: (a) spreading low detonation velocity explosive (4) on the extruded flyer plate (3); (b) filling the groove (2) with small-grain micron diamond powder; (c) adjusting the angle θ between the extrusion flyer plate (3) and the base plate (1) by pulling the pulley (6); (d) starting the detonator (5) to detonate the low-detonation-velocity explosive (4), so that the extrusion flyer plate (3) extrudes the base plate (1) under the action of the explosion force, thereby obtaining a crude product containing large-particle micron diamonds; (e) purifying the crude product obtained in (d) to obtain large-grain micron diamond; In step (c), the angle θ is 30° to 45°; The low detonation velocity explosive (4) has a detonation velocity of 2000 m / s.

2. The device for diamond explosion extrusion growth according to claim 1, characterized in that: The length×width×height dimensions of the base plate (1) are: 800×250×45 mm; the length×width×height dimensions of the extruded fly plate (3) are: 490×190×10 mm; the length×width×height dimensions of the groove (2) are: 500×200×2 mm.

3. The device for diamond explosion extrusion growth according to claim 1, characterized in that: The base plate (1) is made of 45# steel, and the extruded fly plate (3) is made of 45# steel.

4. The device for diamond explosion extrusion growth according to claim 1, characterized in that: In step (a), the drug layer thickness H2 is 20 mm.

5. The device for diamond explosion extrusion growth according to claim 1, characterized in that: The low-detonation-velocity explosive (4) is 90% of powdered ammonium nitrate explosive and 10% of wood powder.

6. The device for diamond explosion extrusion growth according to claim 5, characterized in that: The particle size of the powdered ammonium nitrate explosive is between 1 and 2 μm, and the particle size of the wood powder is between 5 and 10 μm.

7. The device for diamond explosion extrusion growth according to claim 1, characterized in that: The size of the small-particle micron diamond is between 0.46 and 3.21 μm, and the size of the large-particle micron diamond is between 5 and 10 μm.