Bipolar ionomer membrane

By using a bipolar membrane in VRB in which sulfonated polymers are covalently bonded to heterocyclic molecules containing multiple nitrogens, the problems of high vanadium ion permeability and high cost in vanadium redox flow batteries are solved and improved Proton conductivity and oxidation stability improve battery efficiency and economy.

CN108779275BActive Publication Date: 2024-10-15CAMX POWER LLC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN201780015518.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2016-02-03
Filing Date
2017-02-03
Publication Date
2024-10-15
Estimated Expiration
2037-02-03

AI Technical Summary

Technical Problem

The existing vanadium redox flow battery (VRB) separator membrane has problems such as high vanadium ion permeability, high cost, high self-discharge rate and insufficient proton conductivity, which affects battery efficiency and life.

Method used

A bipolar membrane composed of sulfonated polymers and covalently bonded heterocyclic molecules containing multiple nitrogens is used to reduce the permeability of vanadium ions and simultaneously improve proton conductivity and oxidation by adjusting the pKa value and binding mode of the heterocyclic molecules. Stability, using low-cost microporous support membranes filled with bipolar compositions.

Benefits of technology

It achieves low vanadium ion permeability, improves proton conductivity and oxidation stability, reduces the self-discharge rate and cost of the battery, and improves the overall performance and economy of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN108779275B_ABST
    Figure CN108779275B_ABST
Patent Text Reader

Abstract

A membrane for an electrochemical cell or a fuel cell is provided. The membrane may be formed from or include a sulfonated polymer, whereby the sulfonated polymer is covalently or ionically bound to a heterocyclic molecule containing multiple nitrogen atoms. The resulting membrane has excellent ionic conductivity and selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application relies on and claims priority to U.S. Provisional Application No. 62 / 290,692, filed on February 3, 2016.

[0003] Statement of Government Rights

[0004] This invention was made with government support under Contract No. DE-SC0006457 awarded by the U.S. Department of Energy. The government has certain rights in this invention. Field of the Invention

[0005] The present disclosure relates to ion exchange membranes for electrochemical applications, such as use as separators in electrochemical cells. Background Art

[0006] Vanadium redox flow batteries (VRBs) are rugged, multi-KWh long-life flow batteries with an energy density of about 20Wh / liter that can economically store large amounts of renewable energy in liquid form and can be used as accumulators for intermittent renewable power plants, such as wind and solar, or to store off-peak power generation. VRBs work by pumping charged anolyte and catholyte from a storage tank into an electrochemical half-cell separated by an ion-permeable membrane (in contact with a carbon felt anode and cathode on both sides of the ion-permeable membrane). The battery discharges by electrons from the anolyte flowing across the electrical load into the catholyte, while ions (usually protons) flow through the ion-permeable membrane to maintain charge balance.

[0007] Negative half cell V 2+ ←→V 3+ +e - Eo=-0.255V

[0008] Positive half cell - +VO2 + +2H + ←→VO 2+ +H2O Eo=1.00V

[0009] VO2 Total + +2H + +V 2+ ←→VO 2+ +H2O+V 3+ Net Eo = 1.255V

[0010] Vanadium ions constitute the anolyte (V 3+ / V 2+ coupling) and catholyte (VO 2+ / VO2 +coupling), which greatly simplifies and improves battery life because, even if the separator leaks, there is no chemical cross contamination because the anolyte and catholyte leaking species are of the same composition; only the state of charge is different.

[0011] A key enabler of VRB applicability is the ionically conductive separator membrane. However, current VRBs have a round-trip charge / discharge efficiency of only 75-80% because the permeation of vanadium ions through currently known separators is unfavorable. An ideal membrane would have low vanadium ion permeability, be resistant to vanadium contamination, have high proton conductivity, good oxidation and acid chemical stability, good mechanical strength, and be low cost. Sulfonated tetrafluoroethylene-based fluoropolymer-copolymer cation exchange membranes, otherwise known as perfluorosulfonic acid (PFSA) membranes or having the trade name It has become the state-of-the-art separator for VRBs due to its relatively good chemical stability, long service life, good cycling stability, high mechanical strength, and high proton conductivity.

[0012] However, PFSA membranes have many drawbacks, including high cost, vanadium contamination, and, in particular, vanadium ion permeation. Vanadium-ion permeation can discharge a charged VRB at idle, as well as reduce coulombic efficiency during operation, resulting in self-discharge of almost 6% and low efficiency, depending on the discharge current. In addition, vanadium-ions carry bound water, and vanadium-ion permeation through the membrane can change the water balance of the VRB. Although contamination does not destroy the membrane, it requires regular cleaning and washing of the membrane. The relatively high membrane cost also poses a fundamental challenge to overall VRB cost reduction. Therefore, due to vanadium ion leakage, membrane contamination, and high cost, there is great interest in replacing PFSA membranes with alternative membranes that address these drawbacks.

[0013] Bipolar membranes consisting of a thin cation coating on an anion-cation exchange proton-conducting membrane have been shown to be cation selective based on the Coulombic repulsion of cations of different charges after protonation in acidic media (or the Donnan repulsion effect). The Donnan effect increases exponentially with the charge of the permeating cation, so that multivalent cations are repelled to a greater extent than monovalent protons.

[0014] Ogumi confirmed that the cation exchange PFSA Bipolar membrane composed of 4-vinylpyridine plasma polymerized on the surface of the membrane in acidic medium 2+ and one price Li +4-Vinylpyridine is protonated in acidic media to acquire a positive charge, which repels and inhibits divalent cation permeation more than monovalent cation permeation. Sata reported that bipolar membranes composed of aliphatic amines and polyamines such as polyethyleneimine chemically grafted on PFSA membranes have demonstrated monovalent cation permselectivity in continuous electrodialysis concentration of seawater.

[0015] This principle has also been confirmed in VRB membranes. Luo reported that when the ungrafted Nafion In comparison, the membrane composed of polyethyleneimine (PEI) grafted onto Nafion 117 made VO 2+ The transport is reduced by 20 times. The final result is that when comparing 5% grafted PEI-Nafion Compared with unmodified Nafion When the membrane was grafted with PEI, the coulombic efficiency increased from 93.8 to 97.3%. However, the proton conductivity of the PEI-grafted membrane was also unexpectedly reduced by about 30%.

[0016] The primary and secondary amines in the bipolar membrane may have relatively high basicity, e.g., pKa greater than about 9, and when protonated, may have a sufficiently strong Donnan effect to inhibit proton transport to an undesirable extent. Also, primary and secondary aliphatic amines and polyamines may be 5+ The ions are oxidatively unstable. Therefore, for the reasons stated above, it would be desirable to provide bipolar VRB membranes that do not contain primary or secondary amines or polyamines.

[0017] Direct methanol fuel cells use proton conducting membranes such as PFSA and other sulfonated polymers. These membranes suffer from self-discharge due to methanol crossing the membrane which reduces fuel cell efficiency.

[0018] Therefore, there is a need for new materials useful as separators in vanadium redox flow batteries or other applications requiring desirable ion perm selectivity and dielectric constants.

[0019] Brief description of the invention

[0020] The following brief description is provided to facilitate understanding of some of the unique innovative features of the present disclosure, rather than a comprehensive description. A comprehensive understanding of the various aspects of the present invention can be obtained by taking the entire specification, claims, drawings and abstract as a whole.

[0021] It is an object of the present invention to provide a bipolar membrane having a desired ion permeation selectivity and dielectric constant for a VRB having reduced vanadium-ion permeation while maintaining or improving proton conductivity. The bipolar membrane is optionally non-porous. Another object is to provide a bipolar membrane having greater oxidative stability than bipolar membranes containing primary or secondary non-cyclic aliphatic amines. Still another object is to provide a potentially lower cost optionally non-porous composite membrane comprising a low cost microporous support membrane wherein the membrane pores are filled with a sulfonated polymer. Still another object is to provide a potentially lower cost non-porous composite bipolar membrane comprising a low cost microporous support membrane wherein the membrane pores are filled with a bipolar composition.

[0022] According to one aspect of the present invention, there is provided a bipolar membrane comprising a sulfonated polymer, optionally a sulfonated polymer film and a heterocyclic molecule containing multiple nitrogen atoms, the heterocyclic molecule containing multiple nitrogen atoms comprising two or more nitrogen atoms, hereinafter referred to as the heterocyclic molecule containing multiple nitrogen atoms, chemically bonded to at least one surface of the sulfonated polymer. After bonding to the sulfonated polymer, the heterocyclic molecule containing multiple nitrogen atoms has a pKa of less than about 9.0. Prior to chemical bonding to the surface of the sulfonated polymer, the heterocyclic molecule containing multiple nitrogen atoms is optionally derived from a molecule selected from the group consisting of adenine, aminoisoquinoline, aminobenzimidazole, 4-aminopiperidine and aminoimidazole pyridine. Optionally, any combination of the above may be used.

[0023] According to another aspect of the present invention, there is provided a composite bipolar membrane comprising a microporous support membrane, wherein the pores of the microporous membrane are substantially filled with the aforementioned bipolar composition.

[0024] Another aspect of the present invention is a composite bipolar membrane comprising a microporous support membrane, wherein the pores of the microporous support membrane are less than about 10 microns and are substantially filled with the aforementioned bipolar composition, optionally wherein the microporous support membrane is composed of at least one polymer selected from the group consisting of polyolefins, polytetrafluoroethylene, polysulfones, polyethersulfones, polyesters, polyimides, polyamides, nitrocellulose and mixed cellulose esters.

[0025] Another aspect of the present invention is a non-porous composite bipolar membrane comprising a non-woven support membrane, wherein the pores of the non-woven support membrane are greater than about 10 microns and are substantially filled with the aforementioned bipolar composition, and the microporous support membrane is optionally composed of at least one polymer selected from the group consisting of polyolefins, polytetrafluoroethylene, polysulfones, polyethersulfones, polyesters, polyimides, polyamides, nitrocellulose and mixed cellulose esters.

[0026] The invention further relates to a method for producing the aforementioned membrane or composite membrane.

[0027] Another aspect of the present invention is a vanadium redox flow battery incorporating the aforementioned membrane.

[0028] In addition to incorporation into VRBs, the membranes or composite membranes provided herein may also be used in other flow batteries or fuel cells, in particular direct methanol fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The aspects described in the drawings are illustrative and exemplary in nature and are not intended to limit the subject matter defined in the claims. The detailed description of the various exemplary aspects described below can be understood when read in conjunction with the following drawings, in which like structures are indicated by like reference numerals, wherein:

[0031] Figure 1 is a schematic diagram of a membrane according to some aspects as provided herein.

[0032] Detailed description

[0033] The following description is merely exemplary in nature and is by no means meant to limit the scope of the present invention, its application or use, which can certainly vary. The present invention is described with reference to the non-limiting definitions and terms included herein. These definitions and terms are not intended to limit the scope or practice of the present invention, but are provided for exemplary and descriptive purposes only. Although the method or composition is described in a certain order of each step or using specific materials, it should be understood that steps or materials can be interchangeable so that the description can include multiple parts or steps arranged in many ways as those skilled in the art will readily appreciate.

[0034] It should be understood that when an element is referred to as being “on” another element, it can be directly on the other element or intervening elements may exist therebetween. In contrast, when an element is referred to as being “directly on” another element, there are no intervening elements present.

[0035] It should be understood that although the terms "first", "second", "third", etc. can be used to describe various elements, components, regions, layers and / or parts in this article, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of this article, the "first element", "component", "region", "layer" or "part" discussed below can be referred to as the second (or other) element, component, region, layer or part.

[0036] The terms used herein are only for the purpose of describing specific embodiments and are not intended to be limiting. Unless the content clearly indicates otherwise, the singular forms "one", "a kind" and "the" as used herein are meant to include plural forms, including "at least one (kind)". "Or" refers to "and / or". The term "and / or" as used herein includes any and all combinations of one or more of the relevant listed items. It should be further understood that the terms "comprises" and / or "comprising", or "includes" and / or "including" when used in this specification indicate the presence of the features, regions, wholes, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, regions, wholes, steps, operations, elements, components and / or their collections. The term "or a combination thereof" refers to a combination including at least one of the above elements.

[0037] Unless otherwise defined, all terms (including technical terms and scientific terms) used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the present invention belongs. It should be further understood that terms, such as those defined in commonly used dictionaries, should be understood to have the meaning consistent with their meaning in the context of the relevant art and the present disclosure, and should not be interpreted in an idealized or overly formal sense, unless so explicitly defined herein.

[0038] Provide a membrane, it includes the modification of the membrane polymer structure, thus the combination of membrane material and modifier significantly improves the ability of the membrane to be used as a separator between half cells in an electrochemical cell or a fuel cell. The membrane provided reduces unwanted ion transmembrane transport, while improving or substantially stabilizing the excellent proton transport capacity of the following polymer membrane material. Thus, an object of the present invention is to provide a membrane, it includes heterocyclic molecules containing multiple nitrogen covalently bonded to at least one surface or active group of a sulfonic acid polymer. The bipolar membrane can be used for any chemical process that is suitable for combining heterocyclic molecules containing multiple nitrogen, optionally covalently bonded to sulfonic acid polymers. In some aspects, heterocyclic molecules containing multiple nitrogen include amine or amide functional group substituents at one or more sites on the ring, so an amination method can be used, through the formation of sulfonamide coupling or acid-base salts, via the protonation of unbonded electron pairs in the amine to form a membrane. Thus, in some non-limiting aspects, in order to bond to sulfonic acid polymers, amine reagents or precursors optionally contain primary or secondary amine moieties. Although the following disclosure relates primarily to membranes for use in vanadium redox cells, it should be understood that this is for exemplary purposes only and is not limiting. The membranes may be used in other electrochemical cells or fuel cells, such as direct methanol fuel cells.

[0039] In certain aspects, the membrane is used as a separator in a vanadium redox battery. It has been found that although the vanadium ion permeability can be very low in surface aminated sulfonic acid polymers, if the amine is a polymerized primary or secondary amine such as polyethyleneimine or polyamidoamine hyperbranched dendrimers, and when the amine has a pKa greater than about 9.0 after bonding to the sulfonic acid polymer, the aforementioned bipolar membranes can have unacceptably low proton permeability. Through extensive research, the inventors have found that high proton permeability and low vanadium ion permeability can be obtained if the amine is a heterocyclic multiple nitrogen-containing molecule, optionally a heterocyclic multiple nitrogen-containing amine and / or has a pKa less than about 9.0 after bonding to the sulfonic acid polymer. While not being bound by any particular theory, it is believed that after protonation in an acidic VRB electrolyte, heterocyclic molecules bonded to a sulfonic acid polymer having a pKa less than about 9.0 will have weaker Donnan repulsion than modifier molecules having a pKa greater than about 9.0, thus, achieving lower proton permeability while maintaining low vanadium ion rejection. Further, while not wanting to be bound by any particular theory, by replacing sulfonic acid protons on the membrane surface with one or more heterocyclic molecules having a pKa less than 9.0, Grothaus proton "hopping" transport from one bonded heterocyclic site to another can be enhanced via a hydrogen bonding / breaking mechanism. Since hydrated vanadium ions may not participate in Grothaus transport, but rather are transported via the solvent, their permeation will not be enhanced, thereby favoring proton transport via vanadium cation transport.

[0040] Thus, a membrane is provided that includes a substrate (e.g., in the form of a film or membrane), wherein the substrate may be or may include one or more polysulfonic acid polymers, wherein one or more surfaces of the substrate may be coated on one or both sides with heterocyclic nitrogen-containing molecules as modifiers. A schematic diagram of an exemplary membrane is provided in Figure 1 In. As described, the substrate 2 is coated, contacted or otherwise combined with a modifier 4 so as to form heterocyclic nitrogen-containing molecules on the exposed surface of the substrate. The heterocyclic nitrogen-containing molecules optionally form a thin film layer on the surface, partially or completely penetrate the surface of the substrate, or a combination thereof. The heterocyclic nitrogen-containing molecular layer is optionally located on the substrate, optionally directly on the substrate. The heterocyclic nitrogen-containing molecular layer is optionally substantially continuous or discontinuous on the surface of the substrate. The reaction of the heterocyclic nitrogen-containing molecules with the sulfonic acid polymer causes a certain degree of substitution of the sulfonic acid protons by the heterocyclic amine. The degree of substitution of the heterocyclic molecule for the proton can be 0.01% to 100% or any value or range therebetween, optionally 0.1% to 80%, optionally 10% to 80%, optionally 10% to 50%.

[0041] Provide a membrane, it has one or more heterocyclic molecules containing multiple nitrogens that are covalently, ionically or otherwise combined with polysulfonic acid. The heterocyclic molecule containing multiple nitrogens includes carbon atoms and at least two nitrogen atoms in the ring structure. The heteroatom is optionally any heteroatom, thereby providing basicity to the heterocyclic ring. Illustrative examples of heteroatoms include nitrogen and phosphorous. In some aspects, other suitable heteroatoms may also be included in the ring structure. The heterocyclic molecule includes at least one heterocyclic structure. Optionally, the modifier is a non-cyclic molecule with at least one phosphorous substituent, optionally having a pKa of 9.0 or less after bonding polysulfonic acid. In some aspects, the heterocyclic molecule containing multiple nitrogens optionally includes multiple rings, optionally multiple heterocyclic rings, and optionally does not require each ring to contain one or more heteroatoms. In some aspects, 1,2,3,4,5 or more heterocyclic rings or non-heterocyclic rings may be included in the heterocyclic molecule containing multiple nitrogens. Optionally, the heterocyclic molecule containing multiple nitrogens is not a polymer.

[0042] The provided membranes optionally have a heterocyclic molecule containing multiple nitrogens, which has a pKa of or less than 9.0 after bonding to the sulfonic acid polymer. Optionally, the pKa is or less than 9.0, 8.5, 8.0, 7.5, 7.0, 6.5, 6.0, 5.5, 5.0, 4.5, 4.0, 3.5 or 3.0. In some aspects, the pKa is 3.0 to 9.0 or any value or range therebetween, optionally 6.0 to 8.0. In some aspects, the membrane does not contain a modifier on the sulfonic acid-containing polymer, which has a pKa greater than 9.0 after bonding to the polymer.

[0043] The resulting film is optionally a non-porous film. The non-porous film has a Gurly air permeability number greater than 86,400 sec / 10cc0.20in 2 In some aspects, the membrane has a Gurly air permeability of 3600sec / 10cc 0.20in 2 or greater, optionally 40,000sec / 10cc 0.20in 2 or larger.

[0044] The provided membranes have the same or reduced proton resistivity with the polymer-bound heterocyclic molecule modifier relative to a polymer system without the modifier. In certain aspects, the proton resistivity is 20 ohm cm or less. 2 , optionally 1ohm cm 2 In some aspects, the proton resistivity is 0.1 to 0.5 ohm cm 2 , optionally 0.2 to 0.4 ohm cm 2 .

[0045] The provided membranes have reduced or substantially equivalent vanadium ion transport relative to membranes not modified with heterocyclic molecule modifiers. In certain aspects, the vanadium ion transport is or is less than 1.1×10 -4 Mol / day cm 2 , optionally in 1.0 M vanadyl sulfate / 3 M sulfuric acid 1.0 × 10 -5 Mol / day cm 2 .

[0046] The present inventors have found that among heterocyclic multiple nitrogen-containing amines that satisfy or produce the aforementioned properties, some have much higher proton / vanadium ion permselectivity than others. In particular, protonated forms of perfluorosulfonic acid (PFSA) (e.g. Bipolar membranes prepared by direct reaction of ) with aqueous solutions of adenine, aminoisoquinoline, aminobenzimidazole, 4-aminopiperidine or aminoimidazopyridine have demonstrated high vanadium ion rejection, and in the case of adenine and aminoimidazopyridine, the desired proton conductivity has also been demonstrated. Combinations of the foregoing adenine, aminoisoquinoline, aminobenzimidazole, 4-aminopiperidine and aminoimidazopyridine can also be used as precursor heterocyclic multiple nitrogen containing molecules. In certain aspects, the sulfonic acid polymer is modified only with amine containing materials, and the amine containing materials are exclusively adenine, aminoisoquinoline, 4-aminopiperidine, aminobenzimidazole, aminoimidazopyridine and combinations thereof. In certain aspects, the sulfonic acid polymer is modified with amine containing molecules, and the amine containing molecules are exclusively adenine, aminoimidazopyridine, or combinations thereof.

[0047] The combination of heterocyclic molecules containing multiple nitrogen and sulfonic acid polymers, optionally with one or more surfaces of sulfonic acid polymer films, can be achieved by sulfonamide coupling or the formation of acid-base salts, hereinafter referred to as amination. This is a non-limiting example of the combination mechanism of heterocyclic molecules and sulfonic acid polymers. Exemplary combinations include those formed by or via sulfonamide, anhydride, ester, or a combination thereof. Similarly, heterocyclic molecules containing multiple nitrogen optionally include one or more substituents, which include functional groups suitable for combining sulfonic acid polymers. Such substituents exemplarily include, but are not limited to amines, optional primary or secondary amines, hydroxyls or carboxylic acids. In some aspects, the sulfonic acid polymer film is first modified in the sulfonate group to combine one or more heterocyclic molecules with different functional groups. For example, the polymer is optionally modified by the following: using such as PCl3 or PCl5 to convert the sulfonate group into an acid chloride, and then reacting with a substituent containing an acid, amine or alcohol moiety on the heterocyclic molecule. Other suitable combinations between heterocyclic molecules containing multiple nitrogen and polymers are similarly suitable.

[0048] In some aspects, the heterocyclic molecule containing multiple nitrogens can include substituents including primary or secondary amines with available unpaired nitrogen electrons for sulfonamide coupling or acid-base salt formation by protonation with sulfonic acid protons. Sulfonamide coupling can be obtained by a variety of methods including direct condensation, acyl chloride coupling or carbodiimide coupling. In some aspects, direct condensation can be used because of its lower cost, avoidance of toxic and corrosive reagents and fewer reaction steps. Direct condensation consists of the reaction between the proton form of the sulfonic acid polymer and the heterocyclic amine solution. The reaction can result in the formation of sulfonamide coupling and dehydration. The reaction can be illustrated as:

[0049] RSO3H+R'NH2→RSO2NHR'+H2O (wherein R is the part containing sulfonic acid polymer and R' is the heterocyclic amine part).

[0050] The formation of the acid-base salt can also be obtained by similar conditions to the sulfonamide coupling and results in the transfer of a proton from the acid form of the sulfonic acid polymer to an unpaired electron in the heterocyclic amine. The reaction can be shown as:

[0051] RSO3H+R'NH2→RSO3 -+ NH3R' (wherein R is a sulfonic acid polymer-containing moiety and R' is a heterocyclic amine moiety).

[0052] In direct condensation and acid-base salt formation, heterocyclic molecules containing multiple nitrogens with amine substituents are attached to the sulfonated polymer.

[0053] Furthermore, in the direct condensation and acid-base salt formation, the bipolar nitrogen-containing heterocyclic molecule-sulfonic acid polymer film can be prepared by coating a solution of nitrogen-containing heterocyclic molecules directly onto the sulfonic acid polymer film or by immersing the sulfonic acid polymer film in a bath of a solution containing nitrogen-containing heterocyclic molecules. In some aspects, in order to limit the binding of heterocyclic molecules to one side of the film, the side of the film can be temporarily blocked or masked. After the reaction has proceeded to the desired extent, the excess nitrogen-containing heterocyclic molecules can be washed from the sulfonated film.

[0054] The sulfonic acid polymer is optionally in the form of a film or membrane. In this case, the sulfonic acid polymer film or membrane may be optionally pre-swollen before contacting the heterocyclic molecule containing multiple nitrogens, wherein the pre-swelling may be by immersion in a pure solvent (i.e., not containing heterocyclic molecules containing multiple nitrogens) for dissolving the heterocyclic molecules containing multiple nitrogens before the reaction. This can prevent the sulfonic acid polymer film from being physically deformed when immersed in a solution of heterocyclic molecules containing multiple nitrogens.

[0055] The solvent for the heterocyclic molecule binding sulfonic acid polymer is optionally an alcohol, a ketone, an ester, water or a mixture thereof. In certain aspects, the solvent is water, optionally exclusively water.

[0056] The sulfonic acid polymer is optionally one or more selected from the following: per(fluorosulfonic acid / polytetrafluoroethylene) copolymer, sulfonated polystyrene, sulfonated trifluoropolystyrene, sulfonated polystyrene-divinylbenzene copolymer, sulfonated styrene-butadiene, sulfonated polyparaphenylene, sulfonated poly(etheretherketone), sulfonated poly(ether-ketone-ether-ketone-ketone), sulfonated polysulfone, sulfonated poly(ethersulfone), sulfonated 2,6-dimethyl-1,4-phenylene oxide, sulfonated poly(phthalazinone etherketone), sulfonated polyimide, sulfonated polyphosphazene, and sulfonated polybenzimidazole, sulfonated polyphenylsulfone, poly(vinylidene fluoride)-grafted-poly(styrenesulfonic acid), poly(arylene sulfide ketone), poly(arylene sulfide ketone ketone) and sulfonated polyfluorenyl ether ketone. In a specific aspect, the sulfonic acid polymer can be a per(fluorosulfonic acid / polytetrafluoroethylene) copolymer, otherwise known under the trade name or Well known.

[0057] In certain aspects, the sulfonic acid polymer film has a thickness of 5 microns to 500 microns, or any value or range therebetween. Optionally, the sulfonic acid polymer film has a thickness of 15 microns to 200 microns.

[0058] In certain aspects, the sulfonic acid polymer film is laminated to a nonwoven, optionally porous membrane, optionally to provide additional strength to the sulfonic acid polymer film. Optionally, the sulfonic acid polymer is not in the form of a film, but is instead combined with a nonwoven or porous membrane of a different material. Optionally, the sulfonic acid polymer is combined with a porous membrane, wherein some or all of the pores of the membrane are filled with the sulfonic acid polymer, resulting in a membrane that is substantially non-porous, as defined herein.

[0059] If the sulfonic acid polymer is fully swollen in the reaction solvent and given enough reaction time and temperature, the amination process can be carried out to a certain extent under the surface of the polymer. The degree of substitution of sulfonic acid protons by heterocyclic molecules containing multiple nitrogens is mainly controlled by the concentration of the heterocyclic molecules containing multiple nitrogens in the reaction solvent, the reaction time, the reaction temperature and the composition of the reaction solvent. In the process of using the impregnation method, the concentration of the heterocyclic amine containing multiple nitrogens in the solution can be less than 10%, optionally less than 1 weight%. Optionally, the impregnation time is 1 second to 24 hours, optionally 10 minutes to 10 hours. The reaction temperature is optionally greater than 0°C and less than the boiling point of the solvent at 1.0 atmospheres, optionally greater than 30°C and less than 100°C. The heterocyclic molecule solvent containing multiple nitrogens can include or be exclusively water, alcohol, ketone, ester, amide, cyclic amide or a mixture thereof. Optionally, the heterocyclic molecule solvent containing multiple nitrogens is water, optionally exclusively water.

[0060] The heterocyclic molecule containing multiple nitrogens is optionally combined with the membrane on one or both sides. In some aspects, the reaction between the heterocyclic molecule containing multiple nitrogens and the polymer can be provided on only one side of the membrane and can be obtained by masking or sealing one side of the membrane with a material that is impermeable to the reaction solution. The material providing the masking or sealing is optionally a polymer sheet or film, optionally selected from polyolefins, butyl rubber, silicone rubber and ethylene propylene rubber.

[0061] In certain aspects, a non-porous composite membrane is provided, which includes a non-woven or microporous support film, which can be prepared by impregnating the non-woven or microporous film with a solution of a sulfonated polymer, drying the solution, annealing the sulfonated polymer at a temperature above the glass transition temperature of the sulfonated polymer, and finally binding the heterocyclic molecule containing multiple nitrogen to the sulfonated polymer on at least one surface of the composite film. As a non-limiting example, a non-porous composite bipolar membrane can be prepared by dip-coating or soaking the microporous support film in a PFSA solution (such as available from Dupont tm D520 from Sigma-Aldrich The method comprises preparing a microporous support film of the present invention comprises preparing a microporous support film of the present invention and preparing the microporous support film of the present invention. The method ... The thickness of the support film is optionally from 5 to 500 microns, or any value or range therebetween, optionally from 15 to 200 microns.

[0062] Membranes as provided herein are optionally used in electrochemical cells, fuel cells, or for any other purpose where selective permeability is desired. In some aspects, membranes are introduced into electrochemical cells, such as vanadium redox cells. Electrochemical cells optionally include negative half-cells and positive half-cells. Negative half-cells include anodes and anolytes. Positive half-cells optionally include cathodes and catholytes. Membranes as provided herein are located between two half-cells to form a barrier between anolytes and catholytes. The selective permeability of the membrane improves the function and efficiency of the battery by maintaining or improving ionic conductivity while reducing the vanadium (or other reactants) permeability of the membrane from one half-cell to another.

[0063] In certain aspects, the membrane is bound to the heterocyclic molecule containing multiple nitrogen only on one side of the membrane. In such a case, the heterocyclic molecule containing multiple nitrogen is bound to the side that is optionally proximal to the negative half-cell side of the battery in order to improve membrane performance.

[0064] In certain aspects, the electrochemical cell is a vanadium redox cell or a portion thereof. Optionally, the anolyte and the catholyte comprise vanadium ions in different oxidation states. In a vanadium oxide cell, the connection between the sulfonic acid polymer and the heterocyclic ring containing multiple nitrogens is optionally an amide or amine-acid salt connection, optionally such as through a sulfonamide group.

[0065] In some aspects, the membrane as provided herein is included in a fuel cell. The fuel cell includes an anode, a cathode and a membrane separating the anode and the cathode as provided herein. In some aspects, the membrane is combined with a heterocyclic molecule containing multiple nitrogen only on one side of the membrane. In such a case, the heterocyclic molecule binding side containing multiple nitrogen is optionally the near end of the anode side of the battery to improve membrane performance.

[0066] In certain aspects, the fuel cell is a direct methanol fuel cell. In a direct methanol fuel cell, the connection between the sulfonic acid polymer and the multi-nitrogen containing heterocycle is optionally an amide or amine-acid salt combination, optionally such as through a sulfonamide group, optionally through an anhydride or ester bond.

[0067] Various aspects of the present invention are illustrated by the following non-limiting examples. The examples are for illustrative purposes only and are not intended to limit any implementation of the present invention.

[0068] Experimental

[0069] Proton resistivity

[0070] When using 2M sulfuric acid electrolyte, 1.3cm 2 Proton resistivity was measured in a thru-plane clamped conductivity cell with a 4-point detector of electrode area and platinum electrodes. AC impedance was measured using an EGG Princeton Applied Research Potentiostat / Galvanostat Model 273A using a 10mv signal scanned from 600KHz to 10Hz. The bulk resistance is derived from the low impedance intersect of the high frequency semicircle on the actual resistance axis of the complex impedance plane. The bulk resistance is then subtracted from the resistance of the test fixture without the membrane to obtain the resistance of the membrane. The resistivity is normalized to the area and reported in ohms cm 2 The area resistance of the meter.

[0071] Vanadium ion transport

[0072] Vanadium ion transport was measured in a clamped diffusion cell containing 1.0 M vanadyl sulfate (VO) in 3 M sulfuric acid on one side of the test membrane. 2+ ions) and 1.0 M Mg2SO4 in 3 M sulfuric acid on the other side to balance the osmotic pressure. After a period of time, the concentration of vanadium in the Mg2SO4 chamber was measured spectroscopically. Vanadium ion leakage is reported as moles vanadium / cm 2 sky.

[0073] Ion exchange capacity

[0074] The ion exchange capacity (IEC) of the bipolar membranes was determined by acid-base titration. The IEC provides useful information about the number of accessible proton exchange sites in the membrane. The anhydrous bipolar membranes were immersed in a saturated NaCl solution for 2 h / 60 °C and then for 24 h / 30 °C to + Ion exchange H + , the released H + Acid-base titration to determine the mequiv.g of protons-1 IEC is calculated by the following formula: IEC = (H + mequiv.) / anhydrous wt film = meq / gram.

[0075] Porosity

[0076] The film porosity is measured by Gurley air permeability device. The Gurley number is greater than 86,400 sec / 10cc0.20in 2 The membrane is considered to be non-porous.

[0077] Example 1

[0078] 0.470 g of perfluorosulfonic acid (PFSA) ( 117) Film blocked with butyl rubber: A butyl rubber membrane was mechanically fixed to one side of the film so that it was aminated only on one side of the film. To pre-swell the film, the blocked film was immersed in 50 g of distilled water at 80°C for 30 minutes. The water-pre-swollen film was then immersed in 50 g of a 0.05% aqueous solution of 5-aminoisoquinoline (Alfa Aesar L01223) at 80°C for 3 hours and then rinsed with distilled water. The film had a 2M sulfuric acid concentration of 0.30 ohm cm 2 The proton area resistivity is 0.821 meq / g, and the ion exchange capacity is 2.75×10 in 1.0 M vanadyl sulfate / 3 M sulfuric acid. -5 Mol / day cm 2 Compared to unmodified PFSA, the transport of vanadyl ions was 4 times slower, and the proton conductivity was comparable.

[0079] Example 2

[0080] 0.470 g of perfluorosulfonic acid (PFSA) ( 117) Film blocked with butyl rubber: A butyl rubber film was mechanically fixed to one side of the film so that it was aminated only on one side of the film. To pre-swell the film, the blocked film was immersed in 50 g of distilled water at 80° C. for 30 minutes. The water-swollen film was then immersed in 50 g of a 0.125% aqueous solution of 5-aminoisoquinoline (Alfa Aesar L01223) at 80° C. for 3 hours and then rinsed with distilled water. The film had a 1.0 ohm cm 2 The proton area resistivity is 0.749 meq / g, and the ion exchange capacity is 9.2×10 in 1.0 M vanadyl sulfate / 3 M sulfuric acid. -6 Mol / day cm 2Compared to unmodified PFSA, the vanadyl ion transport was 12 times slower.

[0081] Example 3

[0082] 0.470 g of perfluorosulfonic acid (PFSA) ( 117) Film blocked with butyl rubber: A butyl rubber film was mechanically fixed to one side of the film so that it was aminated only on one side of the film. To pre-swell the film, the blocked film was immersed in 50 g of distilled water at 80°C for 30 minutes. The water-swollen film was then immersed in 50 g of a 0.25% aqueous solution of 5-aminoisoquinoline (Alfa Aesar L01223) at 80°C for 3 hours and then rinsed with distilled water. The film had a 2M sulfuric acid resistance of 1.3 ohm cm 2 The proton area resistivity is 0.67 meq / g, and the ion exchange capacity is 5.7×10 in 1.0 M vanadyl sulfate / 3 M sulfuric acid. -6 Mol / day cm 2 Compared to unmodified PFSA, the vanadyl ion transport was 19 times slower.

[0083] Example 4

[0084] 0.470 g of perfluorosulfonic acid (PFSA) ( 117) The film was blocked with butyl rubber so that it was aminated only on one side of the film. To pre-swell the film, the blocked film was immersed in 50 g of distilled water at 80°C for 30 minutes. The water-swollen film was then immersed in 50 g of a 0.25% adenine aqueous solution (Aldrich A8626) at 80°C for 2 hours and then rinsed with distilled water. The film had a 2M sulfuric acid density of 0.34 ohm cm 2 The proton area resistivity is 0.869 meq / g, and the ion exchange capacity is 1.7×10 in 1.0 M vanadyl sulfate / 3 M sulfuric acid. -5 Mol / day cm 2 Compared with unmodified PFSA, the vanadyl ion transport is 6 times slower, and the proton conductivity is comparable.

[0085] Example 5

[0086] 0.470 g of perfluorosulfonic acid (PFSA) ( 117) The film was blocked with butyl rubber to allow amination on only one side of the film. To pre-swell the film, the blocked film was immersed in 50 g of distilled water at 80°C for 30 minutes. The water-swollen film was then immersed in 50 g of a 0.25% aqueous solution of 3-aminoimidazo(1,2)pyridine (SigmaAldrich 685755) at 80°C for 3 hours and then rinsed with distilled water. The film had a 2M sulfuric acid concentration of 0.30 ohm cm 2 The proton area resistivity is 0.702 meq / g, and the ion exchange capacity is 5.9×10 in 1.0 M vanadyl sulfate / 3 M sulfuric acid. -6 Mol / day cm 2 Compared with unmodified PFSA, the vanadyl ion transport is 19 times slower, and the proton conductivity is comparable.

[0087] Example 6

[0088] 0.470 g of perfluorosulfonic acid (PFSA) ( 117) The film was blocked with butyl rubber so that it was aminated only on one side of the film. To pre-swell the film, the blocked film was immersed in 50 g of distilled water at 80°C for 30 minutes. The water-pre-swollen film was then immersed in 50 g of a 0.25% aqueous solution of 2-aminobenzimidazole (Alfa-Aesar L02066) at 80°C for 3 hours and then rinsed with distilled water. The film had a 2M sulfuric acid density of 14.3 ohm cm 2 The proton area resistivity is 0.504 meq / g, and the ion exchange capacity is 3.6×10 in 1.0 M vanadyl sulfate / 3 M sulfuric acid. -7 Mol / day cm 2 Compared with unmodified PFSA, the vanadyl ion transport was 312 times slower.

[0089] Example 7

[0090] 0.470 g of perfluorosulfonic acid (PFSA) ( 117) The film was blocked with butyl rubber to allow amination on only one side of the film. To pre-swell the film, the blocked film was immersed in 50 g of distilled water at 80°C for 30 minutes. The water-swollen film was then immersed in 50 g of a 0.25% aqueous solution of 4-aminopiperidine (Alfa-Aesar L20127) at 80°C for 3 hours and then rinsed with distilled water. The film had a 2M sulfuric acid concentration of 0.21 ohm cm 2 The proton area resistivity is 0.0 meq / g and the ion exchange capacity is 2.3×10 in 1.0 M vanadyl sulfate / 3 M sulfuric acid.-5 Mol / day cm 2 Compared with unmodified PFSA, the vanadyl ion transport is 8 times slower.

[0091] Example 8 - Composite Bipolar Membrane

[0092] At room temperature, in a glass beaker, a 15 μm thick, 0.2 μm pore size, 2.2 sec / 100 cc Gurly permeability, 0.20 in 2 A 15 / 16 inch diameter polyester film disk (Sterlitech Corp., PET0247100) with a dry weight of 9 mg was immersed in 0.4 grams of a 15% perfluorosulfonic acid polymer solution (Ion Power Inc. EW1100) for 10 minutes. After immersion, the excess solution was poured off and the wet film was dried at 80°C for 20 minutes. After drying, 1.0 grams of water was added to release the film from the glass surface, and then, at 80°C, the film was dried for another 10 minutes. At 130°C and 1 kg / in 2 The dried membrane is placed in a polytetrafluoroethylene (PTFE) Annealing between sheets for 20 minutes. The film was immersed in 50 grams of 0.10% 3-aminoimidazo (1,2) pyridine aqueous solution at 80°C for 3 hours and then washed in distilled water. One side of the film was sealed with butyl rubber to allow amination on only one side of the film. The film had a weight of 26 mg, a thickness of 19 microns, and a thermal conductivity of >86,400 sec / 10 cc0.20 in 2 Gurly permeability and 0.83 ohm cm in 2M sulfuric acid 2 The proton area resistivity is 3.95×10 in 1.0M vanadyl sulfate / 3M sulfuric acid. -7 Mol / day cm 2 Compared with unmodified PFSA, the vanadyl ion transport was 278 times slower.

[0093] Comparative Example 1

[0094] 0.470 g of perfluorosulfonic acid (PFSA) ( 117) Film blocked with butyl rubber: A butyl rubber film was mechanically fixed to one side of the film so that only one side of the film was aminated. The blocked film was immersed in 50 g of distilled water at 80°C for 2 hours. The film had a 2M sulfuric acid concentration of 0.29 ohm cm 2 The proton area resistivity, ion exchange capacity of 0.849 meq / g and 1.1×10 -4 Mol / day cm 2Vanadium transport.

[0095] Comparative Example 2

[0096] 0.470 g of perfluorosulfonic acid (PFSA) ( 117) Film blocked with butyl rubber: A butyl rubber film was mechanically fixed to one side of the film so that only one side of the film was aminated. To pre-swell the film, the blocked film was immersed in 50 grams of distilled water at 80°C for 30 minutes. The water-swollen film was then immersed in 50 grams of a 0.25% 1200 MW polyethyleneimine aqueous solution (Polysciences Inc 24313) at 80°C for 3 hours and then rinsed with distilled water. The film had a 20 ohm cm in 2M sulfuric acid. 2 The proton area resistivity is 0.378 meq / g and the ion exchange capacity is 1.3×10 in 1.0 M vanadyl sulfate / 3 M sulfuric acid. -6 Mol / day cm 2 Compared to unmodified PFSA, the vanadyl ion transport was 87 times slower.

[0097] Comparative Example 3

[0098] 0.470 g of perfluorosulfonic acid (PFSA) ( 117) Film blocked with butyl rubber: A butyl rubber film was mechanically fixed to one side of the film so that only one side of the film was aminated. To pre-swell the film, the blocked film was immersed in 50 g of distilled water at 80°C for 30 minutes. The water-swollen film was then immersed in 50 g of a 0.25% aqueous solution of polyamidoamine hyperbranched dendritic polymer polyelectrolyte dendritic polymer, ethylenediamine core 4.0 generation (Aldrich 412449) at 80°C for 2 hours and then rinsed with distilled water. The film had a 3.1 ohm cm in 2M sulfuric acid. 2 The proton area resistivity and ion exchange capacity of 0.789 meq / g and 1.0×10 -5 Mol / day cm 2 Compared with unmodified PFSA, the vanadyl ion transport was 11 times slower.

[0099] Various modifications of the present disclosure in addition to those shown and described herein will be apparent to those skilled in the art from the foregoing description. Such modifications are also intended to fall within the scope of the appended claims.

[0100] It should be understood that unless otherwise specified, all reagents are obtainable from sources known in the art.

[0101] List of various aspects

[0102] 1. Membrane, including:

[0103] Sulfonated polymers; and

[0104] A heterocyclic molecule, optionally containing multiple nitrogen atoms, covalently bonded to the sulfonated polymer.

[0105] 2. The membrane of aspect 1, wherein the heterocyclic molecule has a pKa of less than 9.0, optionally between 3.0 and 9.0.

[0106] 3. The film of aspect 1, wherein the film has a Gurly Air Permeability Number greater than

[0107] 86,400sec / 10cc 0.20in 2 .

[0108] 4. The membrane of aspect 1, wherein the proton resistivity is or less than 20 ohm cm 2 .

[0109] 5. The membrane of aspect 1, wherein the vanadium transport in 1.0M vanadyl sulfate / 3M sulfuric acid is 1.1×10 -4 Mol / day cm 2 .

[0110] 6. The film of aspect 1, wherein the film has a thickness between 10 and 1000 microns.

[0111] 7. The film of aspects 1-6 in any combination, wherein the heterocyclic molecule is selected from adenine, aminoisoquinoline, aminobenzimidazole, aminoimidazopyridine, 4-aminopiperidine, and combinations thereof.

[0112] 8. The membrane of aspects 1-6 of any combination, wherein the sulfonated polymer comprises at least one polymer selected from the group consisting of per(fluorosulfonic acid / polytetrafluoroethylene) copolymer, sulfonated polystyrene, sulfonated trifluoropolystyrene, sulfonated polystyrene-divinylbenzene copolymer, sulfonated styrene-butadiene, sulfonated polyparaphenylene, sulfonated poly(etheretherketone), sulfonated poly(ether-ketone-ether-ketone-ketone), sulfonated polysulfone, sulfonated poly(ethersulfone), sulfonated 2,6-dimethyl-1,4-phenylene oxide, sulfonated poly(phthalazine ether ketone), sulfonated polyimide, sulfonated polyphosphazene, sulfonated polybenzimidazole, sulfonated polyphenylsulfone, poly(vinylidene fluoride)-grafted-poly(styrene sulfonic acid), poly(arylene sulfide ketone) poly(arylene sulfide ketone ketone) and sulfonated polyfluorenyl ether ketone, and combinations thereof.

[0113] 9. The film of aspects 1-6 in any combination, wherein the polymer is in the form of a non-porous film.

[0114] 10. The membrane of aspects 1-6 in any combination, wherein the sulfonated polymer is bonded to a nonwoven or microporous support film.

[0115] 11. The membrane of aspect 10, wherein the sulfonated polymer is located within a plurality of pores within a nonwoven or microporous support film.

[0116] 12. The membrane of aspect 10, wherein the support membrane comprises polytetrafluoroethylene, polysulfone, polyethersulfone, polyester, polyimide, polyamide, polyolefin, nitrocellulose, cellulose, mixed cellulose esters, or combinations thereof.

[0117] 13. The membrane of aspect 11, wherein the support membrane has a pore cross-sectional size of 0.01 to 1000 microns.

[0118] 14. Aspects 1, 7 and 8 combined.

[0119] 15. Combined aspects 2, 7 and 8.

[0120] 16. Aspects 1, 7, 8 and 9 combined.

[0121] 17. Combined aspects 2, 7, 8 and 9.

[0122] 18. Aspects 1, 7, 8 and 10 combined.

[0123] 19. Aspects 2, 7, 8 and 10 combined.

[0124] 20. A membrane comprising: a sulfonated polymer comprising perfluorosulfonic acid; and a heterocyclic molecule selected from adenine, aminoisoquinoline, aminobenzimidazole, aminoimidazopyridine, 4-aminopiperidine, and combinations thereof, wherein the heterocyclic molecule is covalently or ionically bonded to the sulfonated polymer.

[0125] 21. Aspect 20, wherein the film has a Gurly Air Permeability number greater than 86,400 sec / 10 cc 0.20 in 2 .

[0126] 22. Aspect 20, wherein the proton resistivity is or less than 20 ohm cm 2 .

[0127] 23. Aspect 20, wherein the vanadium transport is at or below 1.1×10 -4 Mol / day cm 2 .

[0128] 24. Aspect 20, 21, 22, 23 alone or in combination, wherein the film has a thickness between 10 and 1000 microns.

[0129] 25. A membrane comprising: a sulfonated polymer comprising perfluorosulfonic acid; and a heterocyclic molecule selected from adenine, aminoimidazopyridine, and combinations thereof, said heterocyclic molecule being covalently or ionically bonded to said sulfonated polymer.

[0130] 26. A membrane comprising: a sulfonated polymer comprising perfluorosulfonic acid; and a heterocyclic molecule selected from adenine, aminoimidazopyridine, and combinations thereof, the heterocyclic molecule being covalently or ionically bonded to the sulfonated polymer.

[0131] 27. Aspects 1-26 in any combination, wherein the membrane is an electrochemical cell or a fuel cell.

[0132] 28. Aspects 1-26 in any combination, wherein the membrane is a vanadium redox cell.

[0133] 29. Aspects 1-26 in any combination, wherein the membrane is a direct methanol fuel cell.

[0134] References

[0135] 1.M.Gattrell, J.Park, B.MacDougall, J.Apte, S.McCarthy, and CWWu, "Astudy of the mechanism of the vanadium 4+ / 5+redox reaction in acidicsolutions," Journal of the Electrochemical Society (J.Electrochem.Soc.), 2004, vol.151, no1, pp.A123-A130

[0136] 2.S.Eckroad Vanadium Redox Flow Batteries An In-Depth Analysis1014836Technical Update,March 2007,Electric Power Research Institute

[0137] 3.Zempachi Ogumi,Yoshiharu Uchimoto,Masanori Tsujikawa,Kazuaki Yasudaand Zen-Ichiro Takehara,Modification of ion exchange Membrane by PlasmaProcess.Journal of Membrane Science54,(1990),163-74

[0138] 4.Qingtao Luo,Huaming Zhang,Jian Chen,Peng Qian and Yunfeng Zhai’Modification of membrane using interfacial polymerization forvanadium redox flow battery applications.Journal of Membrane Science 311(2008)98–103

[0139] 5.Tongwen Xu,Ion exchange membranes:State of their development andperspective.Journal of Membrane Science 263(2005)1–29

[0140] 6.Toshikatsu Sata,Ryuji Izuo.Modification of transport properties ofion exchange membrane.XI.Electrodialytic properties of cation exchangemembranes having polyethyleneimine layer fixed by acid–amide bonding.Journalof Applied Polymer Science Volume 41Issues 9-10(1990)2349-2362

[0141] 7.Morihiro Saito,Naoko Arimura,Kikuko Hayamizu,Tatsuhiro Okada,Mechanisms of Ion and Water Transport in Perfluorosulfonated IonomerMembranes for Fuel Cells.J.Phys Chem B 2004,108,16064-70

[0142] 8. US 4,849,311, Itoh et al., July 18, 1989

[0143] 9. US 5,547,551, August 20, 1996

[0144] The patents, publications and applications mentioned in the specification illustrate the level of those skilled in the art to which the invention belongs. These patents, publications and applications are incorporated herein by reference to the same extent as if each individual patent, publication or application was specifically and separately incorporated herein by reference.

[0145] The foregoing description describes particular embodiments of the present invention, but is not intended to be limiting of its implementation. The following claims, including their equivalents, are intended to define the scope of the present invention.

Claims

1. A membrane for a vanadium redox flow battery (VRB), comprising: Sulfonated polymers; Nonwoven or microporous support films; and Heterocyclic molecules containing multiple nitrogen groups including primary amine substituents, The heterocyclic molecule is selected from adenine, aminoisoquinoline, aminobenzimidazole, aminoimidazopyridine, 4-aminopiperidine and a combination thereof, The heterocyclic molecule is covalently or ionically bonded to the sulfonic acid of the sulfonated polymer, and wherein the sulfonated polymer is located within a plurality of pores within a nonwoven or microporous support film.

2. The membrane of claim 1, wherein said heterocyclic molecule, after bonding to said sulfonated polymer, has a pKa of less than 9.

0.

3. The film of claim 1, wherein the film has a Gurly Air Permeability number greater than 86,400 sec / 10 cc 0.20 in 2 .

4. The membrane of claim 1, wherein the proton resistivity is at or below 20 ohm cm 2 .

5. The membrane of claim 1, wherein the vanadium transport in 1.0 M vanadyl sulfate / 3 M sulfuric acid is at or below 1.1 x 10 -4 Mol / day cm 2 .

6. The film of claim 1, wherein the film has a thickness between 10 and 1000 microns.

7. The membrane of any one of claims 1 to 6, wherein the heterocyclic molecule is selected from the group consisting of aminoisoquinoline, aminobenzimidazole, aminoimidazopyridine, and combinations thereof.

8. The membrane of any one of claims 1 to 6, wherein the sulfonated polymer comprises at least one polymer selected from the group consisting of per(fluorosulfonic acid / polytetrafluoroethylene) copolymers, sulfonated polystyrene, sulfonated trifluoropolystyrene, sulfonated polystyrene-divinylbenzene copolymers, sulfonated styrene-butadiene, sulfonated polyparaphenylene, sulfonated poly(etheretherketone), sulfonated poly(ether-ketone-ether-ketone-ketone), sulfonated 2,6-dimethyl-1,4-phenylene oxide, sulfonated poly(phthalazine ether ketone), sulfonated polyimide, sulfonated polyphosphazene, sulfonated polybenzimidazole, sulfonated polyphenylene sulfone, poly(vinylidene fluoride)-grafted-poly(styrene sulfonic acid), poly(arylene sulfide ketone) poly(arylene sulfide ketone ketone) and sulfonated polyfluorenyl ether ketone, and combinations thereof.

9. The membrane of claim 6, wherein the polymer is in the form of a non-porous membrane.

10. The membrane of claim 1, wherein the support film comprises polytetrafluoroethylene, polysulfone, polyethersulfone, polyester, polyimide, polyamide, polyolefin, nitrocellulose, cellulose, mixed cellulose esters, or combinations thereof.

11. The membrane of claim 1 wherein the support film has a pore cross-sectional size of 0.01 to 1000 microns.

12. Vanadium redox battery, comprising: a negative half-cell, including an anode and an anolyte; a positive half-cell including a cathode and a catholyte; and The membrane of any one of claims 1 to 6, located between a negative half-cell and a positive half-cell.

13. The vanadium redox cell of claim 12, wherein the membrane comprises a heterocycle on only one side.

14. The vanadium redox battery of claim 13, wherein the heterocyclic ring is located on the proximal side of the negative half-cell.

15. The vanadium redox battery of claim 12, wherein the heterocyclic molecule is selected from the group consisting of adenine, aminoisoquinoline, aminobenzimidazole, aminoimidazopyridine, 4-aminopiperidine, and combinations thereof.

16. The vanadium redox battery of claim 12, wherein the sulfonated polymer comprises at least one polymer selected from the group consisting of per(fluorosulfonic acid / polytetrafluoroethylene) copolymer, sulfonated polystyrene, sulfonated trifluoropolystyrene, sulfonated polystyrene-divinylbenzene copolymer, sulfonated styrene-butadiene, sulfonated polyparaphenylene, sulfonated poly(etheretherketone), sulfonated poly(ether-ketone-ether-ketone-ketone), sulfonated polysulfone, sulfonated poly(ethersulfone), sulfonated 2,6-dimethyl-1,4-phenylene oxide, sulfonated poly(phthalazine ether ketone), sulfonated polyimide, sulfonated polyphosphazene, sulfonated polybenzimidazole, sulfonated polyphenylene sulfone, poly(vinylidene fluoride)-grafted-poly(styrene sulfonic acid), poly(arylene sulfide ketone) poly(arylene sulfide ketone ketone) and sulfonated polyfluorenyl ether ketone, and combinations thereof.

17. The vanadium redox cell of claim 12, wherein the supported membrane comprises polytetrafluoroethylene, polysulfone, polyethersulfone, polyester, polyimide, polyamide, polyolefin, nitrocellulose, cellulose, mixed cellulose esters, or combinations thereof.

18. The vanadium redox battery of claim 12 in the form of a vanadium redox battery.

19. The vanadium redox cell of claim 12, wherein both the anolyte and the catholyte comprise vanadium.

20. The vanadium redox battery of claim 12, wherein the heterocycle is covalently linked to the sulfonated polymer via a sulfonamide.

21. A method for preparing a membrane according to any one of claims 1 to 6, comprising the steps of: contacting at least one surface of the sulfonated polymer with a solution comprising a heterocyclic molecule containing multiple nitrogen atoms, the heterocyclic molecule comprising a primary amine, for a reaction time and at a reaction temperature to form a film; removing the film from the solution; and The film was dried.

22. The method for preparing a membrane of claim 21, further comprising pre-swelling the sulfonated polymer in a swelling solvent.

23. The method of claim 22, wherein the swelling solvent comprises water, an alcohol, an amide, a cyclic amide, dichloromethane, or a mixture thereof.

24. The method of claim 21, wherein the reaction time is from 1 second to 24 hours.

25. The method of claim 21, wherein the contacting temperature is from 25°C to 150°C.

26. The method of claim 21, wherein the heterocyclic molecule solution solvent comprises water, alcohol, N-methylpyrrolidone, amides, esters, ketones, alkyl chlorides, methylene chloride, aromatic solvents, and mixtures thereof.

27. The method of claim 21, wherein the drying temperature is 30°C to 150°C.

28. The method of claim 21, wherein one side of the membrane is blocked to prevent access to the heterocyclic molecule.

29. The method of claim 28, wherein the membrane is enclosed by a porous membrane comprising polytetrafluoroethylene, polysulfone, polyethersulfone, polyester, polyimide, polyamide, polyolefin, nitrocellulose, cellulose, mixed cellulose esters, or combinations thereof.

30. The method of claim 29, wherein the porous membrane has a pore size of 0.01 to 1000 microns.

31. The method of claim 21, wherein the sulfonated polymer is selected from the group consisting of per(fluorosulfonic acid / polytetrafluoroethylene) copolymers, sulfonated polystyrene, sulfonated trifluoropolystyrene, sulfonated polystyrene-divinylbenzene copolymers, sulfonated styrene-butadiene, sulfonated poly(p-phenylene), sulfonated poly(ether ether ketone), sulfonated poly(ether-ketone-ether-ketone-ketone), sulfonated polysulfone, sulfonated poly(ether sulfone), sulfonated 2,6-dimethyl-1,4-phenylene oxide, sulfonated poly(phthalazine ether ketone), sulfonated polyimide, sulfonated polyphosphazene, sulfonated polybenzimidazole, sulfonated polyphenylene sulfone, poly(vinylidene fluoride)-grafted-poly(styrene sulfonic acid), poly(arylene sulfide ketone) poly(arylene sulfide ketone ketone) and sulfonated polyfluorenyl ether ketone, and combinations thereof.

32. The method of claim 21, wherein the heterocyclic molecule is selected from the group consisting of adenine, aminoisoquinoline, aminobenzimidazole, aminoimidazopyridine, 4-aminopiperidine, and combinations thereof.

33. The method of claim 21, wherein the heterocyclic molecule has a pKa of less than 9.

0.

34. A method for preparing a membrane according to any one of claims 1 to 6, comprising the steps of: filling the pores of the porous support membrane with a solution of the sulfonated polymer, drying the solution to form a solid film, annealing the solid film at high temperature, At least one surface of the solid film is contacted with a solution of the heterocyclic molecule for a reaction time and at a reaction temperature.

35. The method of claim 34, further comprising removing the solid film from the solution and drying the solid film at a drying temperature greater than 60°C and less than 130°C.

36. The method of claim 34, wherein the annealing step is at a temperature greater than 80°C and less than 250°C.

37. The method of claim 34, further comprising sealing one side of the porous support membrane to prevent contact with a solution of the heterocyclic molecule.

38. The method of claim 34, wherein the contacting step is from 1 second to 24 hours.

39. The method of claim 34, wherein the contacting step is at a temperature of 25°C to 150°C.

Citation Information

Patent Citations

  • Automatic forward feed of the electrode on spark erosion machines - using hydraulic circuit contg. servo-valve actuated by torque motor

    DE2632005A1

  • A device for measurement of the temperature at power lines

    EP0101483A1

  • Sound attenuating resonator

    US3112008A

  • Immobilized electrolyte membrane

    US4849311A

  • Heterocycle grafted monomers and related polymers and hybrid inorganic-organic polymer membranes

    CN1926131A