A perovskite solar cell structure and preparation method thereof

By setting up a multi-layer composite perovskite active precursor layer in a perovskite solar cell, a gradient distribution layer is formed to improve the bending of Fermi level, which solves the low exciton separation and collection efficiency in traditional perovskite solar cells. Problem, significantly improving battery performance.

CN109273611BActive Publication Date: 2024-11-12CHINA HUANENG GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201811435493.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-11-28
Publication Date
2024-11-12
Estimated Expiration
2038-11-28

AI Technical Summary

Technical Problem

Exciton separation and collection efficiency in traditional perovskite solar cell structures is low, affecting battery performance.

Method used

At least two composite perovskite active precursor layers are provided between the first electrode and the second electrode arranged at intervals, forming a gradient distribution layer to construct a directional bending of the Fermi energy level, and forming a certain gradient using a thermal diffusion process. The perovskite active layer with varying ratios improves exciton transport efficiency.

Benefits of technology

It improves exciton separation and collection efficiency, improves the overall performance of perovskite solar cells, and is manifested as higher open voltage, current density and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109273611B_ABST
    Figure CN109273611B_ABST
Patent Text Reader

Abstract

The present invention discloses a perovskite solar cell structure and a preparation method thereof, comprising a first electrode and a second electrode spaced apart; at least two layers of composite perovskite active precursor layers are arranged between the first electrode and the second electrode. The solar cell prepared by the present invention comprises a first electrode, a second electrode spaced apart from the first electrode, and at least two layers of active layers arranged between the first electrode and the second electrode; the two layers of active layers are prepared in a sequential and reverse preparation manner and then pressed together, thereby avoiding the solvent damage effect in the preparation process of perovskites of different components. The two layers of active layers of the present invention utilize a thermal diffusion process to form a perovskite active layer with a certain gradient ratio change, which constructs a directional gradual bend of the Fermi level, has the characteristics of a homojunction, is conducive to the directional conduction of excitons, can improve the transmission efficiency of excitons, and thus improve the performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solar cells, and in particular relates to a perovskite solar cell structure and a preparation method thereof. Background Art

[0002] Perovskite solar cells and light-emitting diodes discovered in recent years are gaining more and more attention due to their high conversion efficiency, low cost, environmental friendliness, and product flexibility. Among them, the photoelectric conversion efficiency of new perovskite solar cells has increased several times in just a few years, showing very excellent photoelectric performance. The generation, diffusion, and collection of excitons in perovskite solar cells directly affect the performance of the cell.

[0003] The conventional perovskite solar cell structure is as follows Figure 2 As shown, the corresponding thin film structures are prepared in sequence from left to right, and finally a single-layer organic-inorganic hybrid structure perovskite active layer containing a single component and a single crystal form is formed, and its exciton separation and collection efficiency is low, which affects the performance of the entire perovskite solar cell. Summary of the invention

[0004] The purpose of the present invention is to provide a perovskite solar cell structure and a preparation method thereof to solve the above technical problems. The present invention constructs a solar cell device with a perovskite active center with directional bending of the Fermi level, homojunction properties, and a specific direction and specific gradient change, which has better exciton separation and collection efficiency and helps to improve battery performance.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] A perovskite solar cell structure comprises a first electrode and a second electrode which are arranged at intervals; at least two composite perovskite active precursor layers are arranged between the first electrode and the second electrode.

[0007] Furthermore, the at least two composite perovskite active precursor layers include a composite first perovskite active precursor layer and a second perovskite active precursor layer; a gradient distribution layer is formed between the first perovskite active precursor layer and the second perovskite active precursor layer.

[0008] Furthermore, the at least two layers of composite perovskite active precursor layers include three layers or more, and a gradient distribution layer is formed between two adjacent layers of composite perovskite active precursor layers.

[0009] Furthermore, the gradient distribution layer forms a gradient distribution of the perovskite active precursor along the direction from the first electrode to the second electrode, thereby constituting a directional gradual bending of the Fermi level.

[0010] Furthermore, the first electrode is an ITO transparent electrode, and the second electrode is a nano silver wire electrode.

[0011] Furthermore, an electron transport layer is provided between the first electrode and at least two composite perovskite active precursor layers; and a hole transport layer is provided between the second electrode and at least two composite perovskite active precursor layers.

[0012] A method for preparing a perovskite solar cell structure, comprising:

[0013] 1) Preparation of the first electrode: depositing an ITO transparent electrode as the first electrode;

[0014] 2) preparing an electron transport layer on the first electrode;

[0015] 3) preparing a first perovskite active precursor layer on the surface of the electron transport layer to obtain an n-region multilayer structure;

[0016] 4) Preparation of the second electrode: Printing nano silver wires on a substrate and annealing to obtain the second electrode;

[0017] 5) preparing a hole transport layer on the second electrode;

[0018] 6) preparing a second perovskite active precursor layer on the surface of the hole transport layer to obtain a p-region multilayer structure;

[0019] 7) Physically pressing the n-region multilayer structure and the p-region multilayer structure under a vacuum environment to obtain a perovskite solar cell structure.

[0020] Furthermore, in step 7), physical pressing and annealing are performed under vacuum: vacuum degree ≤ 1×10 -5 Pa, composite pressure 0.001-1MPa, annealing in vacuum: 130-150℃ annealing for 10-30 minutes.

[0021] Furthermore, the structure of the perovskite active precursor used in the first perovskite active precursor layer in step 3) is (RNH3)AX n Y 3-n ; R = hydrocarbon group; A = Pb, Sn; X, Y = Cl, Br, I; n is a real number of 0-3; DMF is used as solvent during preparation to prepare a slurry with a mass fraction of 20-35%; after coating at room temperature, annealing is performed in nitrogen at 100-140°C for 5-10 minutes to obtain a first perovskite active precursor layer with a thickness of 200-500nm.

[0022] Furthermore, the structure of the perovskite active precursor used in the first perovskite active precursor layer in step 3) is (RNH3)AX n Y 3-n; R = hydrocarbon group; A = Pb, Sn; X, Y = Cl, Br, I; n is a real number of 0-3; DMF is used as solvent during preparation to form a slurry with a mass fraction of 20-35%; after coating at room temperature, annealing is performed in nitrogen at 100-140°C for 5-10 minutes to obtain a second perovskite active precursor layer with a thickness of 200-500nm; the structure of the perovskite active precursor used in the first perovskite active precursor layer is different from the chemical composition and energy level structure of the perovskite active precursor used in the second perovskite active precursor layer.

[0023] Compared with the prior art, the present invention has the following beneficial effects: the solar cell prepared by the present invention comprises a first electrode, a second electrode spaced apart from the first electrode, and at least two active layers arranged between the first electrode and the second electrode; the two active layers are prepared respectively by sequential and reverse preparation methods and then pressed together in the solid state, thus avoiding the problem of the traditional solution method that a multi-layer continuous gradient perovskite film cannot be formed due to the solvent destruction effect in the preparation process of perovskites of different components.

[0024] The two active layers of the present invention utilize a thermal diffusion process to form a perovskite active layer with a certain gradient ratio change. The active layer constructs a directional gradual bending of the Fermi level, has the characteristics of a homojunction, is conducive to the directional conduction of excitons, can improve the transmission efficiency of excitons, and thus improve the performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic structural diagram of a perovskite solar cell structure of the present invention;

[0026] Figure 2 For the traditional perovskite solar cell structure;

[0027] Figure 3 A schematic diagram of the energy band of a perovskite solar cell structure before thermal diffusion according to the present invention;

[0028] Figure 4 A schematic diagram comparing a perovskite solar cell structure prepared in accordance with a preferred embodiment 1 of the present invention and an existing structure. DETAILED DESCRIPTION

[0029] When describing embodiments of the present invention, for the sake of clarity, specific terms are used. However, the present invention is not intended to be limited to the selected specific terms. It should be understood that each specific element includes all technical equivalents that operate in a similar manner to achieve similar purposes.

[0030] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0031] See also Figure 1As shown, a perovskite solar cell structure of the present invention is a gradient perovskite solar cell device structure, comprising a transparent electrode substrate 102 and a second electrode 110 arranged at intervals; a first perovskite active precursor layer 105 and a second perovskite active precursor layer 107 are provided between the transparent electrode substrate 102 and the second electrode 110; a transition layer is formed by thermal diffusion between the first perovskite active precursor layer 105 and the second perovskite active precursor layer 107. The perovskite solar cell structure has a plurality of active material layers and / or material layers, such as an electron transport layer 104 and a hole transport layer 108, between the transparent electrode substrate 102 and the second electrode 110.

[0032] A transition layer is formed between the first perovskite active precursor layer 105 and the second perovskite active precursor layer 107 , so that a distribution gradient of the perovskite active precursor is formed between the first perovskite active precursor layer 105 and the second perovskite active precursor layer 107 , thereby improving the exciton transmission and collection efficiency.

[0033] See also Figure 1 As shown, a perovskite solar cell structure of the present invention is a gradient-graded perovskite solar cell device structure, and the preparation method includes:

[0034] 1) Preparation of transparent electrode substrate 102: ITO transparent electrode deposited on transparent ultra-white glass is used as transparent electrode substrate 102, with no limit on area (5×5 cm in this example). 2 ), such products are commercial products that are mass-produced and can be used directly. Before use, the electrode surface should be treated with deionized water, acetone, and isopropanol ultrasonic treatment in sequence, then cleaned with a UV cleaner, and dried with nitrogen flow for later use.

[0035] 2) Prepare the electron transport layer 104 on the transparent electrode substrate 102: the material is SnO2 nanosol, the sol mass is 20g / L aqueous solution; the scraper coating speed is 5-100mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 100μm; after coating, anneal and dry in nitrogen at 80-200℃. The final thickness is about 10-100nm.

[0036] 3) Prepare the first perovskite active precursor layer 105 on the surface of the electron transport layer 104 to obtain an n-region multilayer structure: the structure is (RNH3)AX n Y 3-n(R = hydrocarbon group; A = Pb, Sn; X, Y = Cl, Br, I; n is a real number of 0-3), preferably CH3NH3PbCl3, the solvent is DMF, and the mass fraction is 20-35% slurry; the scraper coating speed is 10-30mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, annealing is carried out in nitrogen at 100-140℃ for 5-10 minutes. The thickness of the finally obtained perovskite active precursor layer 105 is 200-500nm.

[0037] 4) Preparation of the second electrode 110: Print nano silver wires on the substrate material ultra-white glass. The material is commercial silver nanowire sol, the solvent is isopropanol, the concentration is 50g / L, the diameter of the silver nanowire is about 100nm, and the length is 50-100μm. The scraper coating speed is 10-20mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 70-100℃ in nitrogen for 10-20 minutes. Finally, the second electrode 110 with a thickness of about 40-100nm is obtained.

[0038] 5) Prepare the hole transport layer 108 on the second electrode 110: the slurry used is a commercial PEDOT:PSS (AI4083) aqueous solution (NiO, Spiro, etc. can also be used), which is diluted with isopropanol in a volume ratio of (PEDOT:PSS):isopropanol=1:3, with a scraper coating speed of 10-30mm / s; coating temperature of 45-70°C; the distance between the scraper and the substrate is 50μm; after coating, anneal at 80-100°C in nitrogen for 10-20 minutes. The thickness of the final hole transport layer 108 is 100nm.

[0039] 6) Prepare a second perovskite active precursor layer 107 on the surface of the hole transport layer 108 to obtain a p-region multilayer structure: the structure is (RNH3)AX n Y 3-n (R = hydrocarbon group; A = Pb, Sn; X, Y = Cl, Br, I; n is a real number of 0-3), the solvent is DMF, and the mass fraction is 20-35% of the slurry; the scraper coating speed is 10-20mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, it is annealed in nitrogen at 100-140°C for 5-10 minutes. The thickness of the finally obtained perovskite active precursor layer 107 is 200-500nm.

[0040] 7) Physically press the n-region multilayer structure prepared in step 1-3 and the p-region multilayer structure prepared in step 4-6 under vacuum, with a vacuum degree of ≤1×10 -5 Pa, a composite pressure of 0.001-1 MPa, and annealing at 130-150° C. for 10-30 minutes in vacuum to obtain a perovskite solar cell structure of the present invention.

[0041] Example 1

[0042] The present invention provides a method for preparing a perovskite solar cell structure, comprising:

[0043] 1) Preparation of transparent electrode substrate 102: An ITO transparent electrode deposited on transparent ultra-white glass is used as transparent electrode substrate 102, with an area of ​​5×5 cm 2 , such products are commercial products that are mass-produced and can be used directly. Before use, the electrode surface should be treated with deionized water, acetone, and isopropanol ultrasonic treatment in sequence, then cleaned with a UV cleaner, and dried with nitrogen flow for later use.

[0044] 2) Prepare the electron transport layer 104 on the transparent electrode substrate 102: the material is SnO2 nanosol, the sol mass is 20g / L aqueous solution; the scraper coating speed is 25mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 100μm; after coating, anneal and dry at 150℃ in nitrogen. The final thickness is about 20nm.

[0045] 3) Prepare the first perovskite active precursor layer 105 on the surface of the electron transport layer 104 to obtain the n-region multilayer structure: the material is CH3NH3PbCl3, the solvent is DMF, and the mass fraction is 20% of the slurry; the scraper coating speed is 15mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 135°C in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 105 is 300nm.

[0046] 4) Preparation of the second electrode 110: Print nano silver wires on the substrate material ultra-white glass. The material is commercial silver nanowire sol, the solvent is isopropanol, the concentration is 50g / L, the diameter of the silver nanowire is about 100nm, and the length is 50-100μm. The scraper coating speed is 10mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 80℃ in nitrogen for 15 minutes. Finally, the second electrode 110 with a thickness of about 70nm is obtained.

[0047] 5) Prepare the hole transport layer 108 on the second electrode 110: the slurry used is a commercial PEDOT:PSS (AI4083) aqueous solution (NiO, Spiro, etc. can also be used), which is diluted with isopropanol in a volume ratio of (PEDOT:PSS):isopropanol=1:3, with a scraper coating speed of 20mm / s; the coating temperature is 60°C; the distance between the scraper and the substrate is 50μm; after coating, anneal at 90°C in nitrogen for 15 minutes. The thickness of the final hole transport layer 108 is 100nm.

[0048] 6) Prepare the second perovskite active precursor layer 107 on the surface of the hole transport layer 108 to obtain a p-region multilayer structure: the material is CH3NH3PbI3, the solvent is DMF, and the mass fraction is 20% of the slurry; the scraper coating speed is 15mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 135°C in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 107 is 300nm.

[0049] 7) Physically press the n-region multilayer structure prepared in step 1-3 and the p-region multilayer structure prepared in step 4-6 under vacuum, with a vacuum degree of ≤1×10 -5 Pa, a composite pressure of 0.01 MPa, and annealing at 135° C. for 20 minutes in vacuum to obtain a perovskite solar cell structure of the present invention.

[0050] After testing, the perovskite solar cell structure prepared in Example 1 has an opening voltage of 1.11V, a current density of 23.1mA / cm2, and an efficiency of 19.2%.

[0051] Example 2

[0052] The present invention provides a method for preparing a perovskite solar cell structure, comprising:

[0053] 1) Preparation of transparent electrode substrate 102: An ITO transparent electrode deposited on transparent ultra-white glass is used as transparent electrode substrate 102, with an area of ​​5×5 cm 2 , such products are commercial products that are mass-produced and can be used directly. Before use, the electrode surface should be treated with deionized water, acetone, and isopropanol ultrasonic treatment in sequence, then cleaned with a UV cleaner, and dried with nitrogen flow for later use.

[0054] 2) Prepare the electron transport layer 104 on the transparent electrode substrate 102: the material is SnO2 nanosol, the sol mass is 20g / L aqueous solution; the scraper coating speed is 100mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 100μm; after coating, anneal and dry at 150℃ in nitrogen. The final thickness is about 10nm.

[0055] 3) Prepare the first perovskite active precursor layer 105 on the surface of the electron transport layer 104 to obtain the n-region multilayer structure: the material is CH3NH3PbCl3, the solvent is DMF, and the mass fraction is 20% of the slurry; the scraper coating speed is 15mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 135°C in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 105 is 300nm.

[0056] 4) Preparation of the second electrode 110: Print nano silver wires on the substrate material ultra-white glass. The material is commercial silver nanowire sol, the solvent is isopropanol, the concentration is 50g / L, the diameter of the silver nanowire is about 100nm, and the length is 50-100μm. The scraper coating speed is 10mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 80℃ in nitrogen for 15 minutes. Finally, the second electrode 110 with a thickness of about 70nm is obtained.

[0057] 5) Prepare the hole transport layer 108 on the second electrode 110: the slurry used is a commercial PEDOT:PSS (AI4083) aqueous solution (NiO, Spiro, etc. can also be used), which is diluted with isopropanol in a volume ratio of (PEDOT:PSS):isopropanol=1:3, with a scraper coating speed of 20mm / s; the coating temperature is 60°C; the distance between the scraper and the substrate is 50μm; after coating, anneal at 90°C in nitrogen for 15 minutes. The thickness of the final hole transport layer 108 is 100nm.

[0058] 6) Prepare the second perovskite active precursor layer 107 on the surface of the hole transport layer 108 to obtain a p-region multilayer structure: the material is CH3NH3PbI3, the solvent is DMF, and the mass fraction is 20% of the slurry; the scraper coating speed is 15mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 135°C in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 107 is 300nm.

[0059] 7) Physically press the n-region multilayer structure prepared in step 1-3 and the p-region multilayer structure prepared in step 4-6 under vacuum, with a vacuum degree of ≤1×10 -5 Pa, a composite pressure of 0.01 MPa, and annealing at 135° C. for 20 minutes in vacuum to obtain a perovskite solar cell structure of the present invention.

[0060] Example 3

[0061] The present invention provides a method for preparing a perovskite solar cell structure, comprising:

[0062] 1) Preparation of transparent electrode substrate 102: An ITO transparent electrode deposited on transparent ultra-white glass is used as transparent electrode substrate 102, with an area of ​​5×5 cm 2 , such products are commercial products that are mass-produced and can be used directly. Before use, the electrode surface should be treated with deionized water, acetone, and isopropanol ultrasonic treatment in sequence, then cleaned with a UV cleaner, and dried with nitrogen flow for later use.

[0063] 2) Prepare the electron transport layer 104 on the transparent electrode substrate 102: the material is SnO2 nanosol, the sol mass is 20g / L aqueous solution; the scraper coating speed is 100mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 100μm; after coating, anneal and dry at 150℃ in nitrogen. The final thickness is about 10nm.

[0064] 3) Prepare the first perovskite active precursor layer 105 on the surface of the electron transport layer 104 to obtain the n-region multilayer structure: the material is CH3NH3PbCl3, the solvent is DMF, and the mass fraction is 35% of the slurry; the scraper coating speed is 20mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 135℃ in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 105 is 400nm.

[0065] 4) Preparation of the second electrode 110: Print nano silver wires on the substrate material ultra-white glass. The material is commercial silver nanowire sol, the solvent is isopropanol, the concentration is 50g / L, the diameter of the silver nanowire is about 100nm, and the length is 50-100μm. The scraper coating speed is 10mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 80℃ in nitrogen for 15 minutes. Finally, the second electrode 110 with a thickness of about 70nm is obtained.

[0066] 5) Prepare the hole transport layer 108 on the second electrode 110: the slurry used is a commercial PEDOT:PSS (AI4083) aqueous solution (NiO, Spiro, etc. can also be used), which is diluted with isopropanol in a volume ratio of (PEDOT:PSS):isopropanol=1:3, with a scraper coating speed of 20mm / s; the coating temperature is 60°C; the distance between the scraper and the substrate is 50μm; after coating, anneal at 90°C in nitrogen for 15 minutes. The thickness of the final hole transport layer 108 is 100nm.

[0067] 6) Prepare the second perovskite active precursor layer 107 on the surface of the hole transport layer 108 to obtain a p-region multilayer structure: the material is CH3NH3PbI3, the solvent is DMF, and the mass fraction is 35% of the slurry; the scraper coating speed is 20mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 135℃ in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 107 is 400nm.

[0068] 7) Physically press the n-region multilayer structure prepared in step 1-3 and the p-region multilayer structure prepared in step 4-6 under vacuum, with a vacuum degree of ≤1×10 -5Pa, a composite pressure of 0.01 MPa, and annealing at 135° C. for 20 minutes in vacuum to obtain a perovskite solar cell structure of the present invention.

[0069] Example 4

[0070] The present invention provides a method for preparing a perovskite solar cell structure, comprising:

[0071] 1) Preparation of transparent electrode substrate 102: An ITO transparent electrode deposited on transparent ultra-white glass is used as transparent electrode substrate 102, with an area of ​​5×5 cm 2 , such products are commercial products that are mass-produced and can be used directly. Before use, the electrode surface should be treated with deionized water, acetone, and isopropanol ultrasonic treatment in sequence, then cleaned with a UV cleaner, and dried with nitrogen flow for later use.

[0072] 2) Prepare the electron transport layer 104 on the transparent electrode substrate 102: the material is SnO2 nanosol, the sol mass is 20g / L aqueous solution; the scraper coating speed is 100mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 100μm; after coating, anneal and dry at 150℃ in nitrogen. The final thickness is about 10nm.

[0073] 3) Prepare the first perovskite active precursor layer 105 on the surface of the electron transport layer 104 to obtain the n-region multilayer structure: the material is CH3NH3PbCl3, the solvent is DMF, and the mass fraction is 35% of the slurry; the scraper coating speed is 20mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 135℃ in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 105 is 400nm.

[0074] 4) Preparation of the second electrode 110: Print nano silver wires on the substrate material ultra-white glass. The material is commercial silver nanowire sol, the solvent is isopropanol, the concentration is 50g / L, the diameter of the silver nanowire is about 100nm, and the length is 50-100μm. The scraper coating speed is 20mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 100℃ in nitrogen for 15 minutes. Finally, the second electrode 110 with a thickness of about 40nm is obtained.

[0075] 5) Prepare the hole transport layer 108 on the second electrode 110: the slurry used is a commercial PEDOT:PSS (AI4083) aqueous solution (NiO, Spiro, etc. can also be used), which is diluted with isopropanol in a volume ratio of (PEDOT:PSS):isopropanol=1:3, with a scraper coating speed of 20mm / s; the coating temperature is 60°C; the distance between the scraper and the substrate is 50μm; after coating, anneal at 90°C in nitrogen for 15 minutes. The thickness of the final hole transport layer 108 is 100nm.

[0076] 6) Prepare the second perovskite active precursor layer 107 on the surface of the hole transport layer 108 to obtain a p-region multilayer structure: the material is CH3NH3PbI3, the solvent is DMF, and the mass fraction is 35% of the slurry; the scraper coating speed is 20mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 135℃ in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 107 is 400nm.

[0077] 7) Physically press the n-region multilayer structure prepared in step 1-3 and the p-region multilayer structure prepared in step 4-6 under vacuum, with a vacuum degree of ≤1×10 -5 Pa, a composite pressure of 0.1 MPa, and annealing at 135° C. for 20 minutes in vacuum to obtain a perovskite solar cell structure of the present invention.

[0078] Example 5

[0079] The present invention provides a method for preparing a perovskite solar cell structure, comprising:

[0080] 1) Preparation of transparent electrode substrate 102: An ITO transparent electrode deposited on transparent ultra-white glass is used as transparent electrode substrate 102, with an area of ​​5×5 cm 2 , such products are commercial products that are mass-produced and can be used directly. Before use, the electrode surface should be treated with deionized water, acetone, and isopropanol ultrasonic treatment in sequence, then cleaned with a UV cleaner, and dried with nitrogen flow for later use.

[0081] 2) Prepare the electron transport layer 104 on the transparent electrode substrate 102: the material is SnO2 nanosol, the sol mass is 20g / L aqueous solution; the scraper coating speed is 100mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 100μm; after coating, anneal and dry at 150℃ in nitrogen. The final thickness is about 10nm.

[0082] 3) Prepare the first perovskite active precursor layer 105 on the surface of the electron transport layer 104 to obtain the n-region multilayer structure: the material is CH3NH3PbCl3, the solvent is DMF, and the mass fraction is 20% of the slurry; the scraper coating speed is 15mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 135°C in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 105 is 300nm.

[0083] 4) Preparation of the second electrode 110: Print nano silver wires on the substrate material ultra-white glass. The material is commercial silver nanowire sol, the solvent is isopropanol, the concentration is 50g / L, the diameter of the silver nanowire is about 100nm, and the length is 50-100μm. The scraper coating speed is 20mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 100℃ in nitrogen for 15 minutes. Finally, the second electrode 110 with a thickness of about 40nm is obtained.

[0084] 5) Prepare the hole transport layer 108 on the second electrode 110: the slurry used is a commercial PEDOT:PSS (AI4083) aqueous solution (NiO, Spiro, etc. can also be used), which is diluted with isopropanol in a volume ratio of (PEDOT:PSS):isopropanol=1:3, with a scraper coating speed of 20mm / s; the coating temperature is 60°C; the distance between the scraper and the substrate is 50μm; after coating, anneal at 90°C in nitrogen for 15 minutes. The thickness of the final hole transport layer 108 is 100nm.

[0085] 6) Prepare the second perovskite active precursor layer 107 on the surface of the hole transport layer 108 to obtain a p-region multilayer structure: the material is CH3NH3PbI3, the solvent is DMF, and the mass fraction is 35% of the slurry; the scraper coating speed is 20mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 135℃ in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 107 is 400nm.

[0086] 7) Physically press the n-region multilayer structure prepared in step 1-3 and the p-region multilayer structure prepared in step 4-6 under vacuum, with a vacuum degree of ≤1×10 -5 Pa, a composite pressure of 0.01 MPa, and annealing at 135° C. for 20 minutes in vacuum to obtain a perovskite solar cell structure of the present invention.

[0087] Example 6

[0088] The present invention provides a method for preparing a perovskite solar cell structure, comprising:

[0089] 1) Preparation of transparent electrode substrate 102: An ITO transparent electrode deposited on transparent ultra-white glass is used as transparent electrode substrate 102, with an area of ​​5×5 cm 2 , such products are commercial products that are mass-produced and can be used directly. Before use, the electrode surface should be treated with deionized water, acetone, and isopropanol ultrasonic treatment in sequence, then cleaned with a UV cleaner, and dried with nitrogen flow for later use.

[0090] 2) Prepare the first perovskite active precursor layer 105 on the transparent electrode substrate 102 to obtain the n-region multilayer structure: the material is CH3NH3PbCl3, the solvent is DMF, and the mass fraction is 20% of the slurry; the scraper coating speed is 15mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 135℃ in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 105 is 300nm.

[0091] 3) Preparation of the second electrode 110: Print nano silver wires on the substrate material ultra-white glass. The material is commercial silver nanowire sol, the solvent is isopropanol, the concentration is 50g / L, the diameter of the silver nanowire is about 100nm, and the length is 50-100μm. The scraper coating speed is 10mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, anneal at 80℃ in nitrogen for 15 minutes. Finally, the second electrode 110 with a thickness of about 70nm is obtained.

[0092] 4) Prepare a second perovskite active precursor layer 107 on the surface of the second electrode 110 to obtain a p-region multilayer structure: the structure is (RNH3)AX n Y 3-n (R = hydrocarbon group; A = Pb, Sn; X, Y = Cl, Br, I; n is a real number of 0-3), the solvent is DMF, and the mass fraction is 20% slurry; the scraper coating speed is 15mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, it is annealed at 135℃ in nitrogen for 10 minutes. The thickness of the final perovskite active precursor layer 107 is 300nm.

[0093] 5) Physically press the n-region multilayer structure prepared in step 1-2 and the p-region multilayer structure prepared in step 3-4 under vacuum, with a vacuum degree of ≤1×10 -5 Pa, a composite pressure of 0.01 MPa, and annealing at 135° C. for 20 minutes in vacuum to obtain a perovskite solar cell structure of the present invention.

[0094] In this embodiment, compared with Embodiment 1, the electron transport layer 104 and the hole transport layer 108 are not prepared, which can simplify the process and reduce the cost, but the efficiency of the obtained solar cell is slightly lower than that of the embodiment.

[0095] Comparative Example 1

[0096] Compared with Example 1, the difference in the preparation process of Comparative Example 1 is: preparation is carried out according to steps 1-3 of Example 1, and then the second perovskite active precursor layer 107 (CH3NH3PbI3) is directly prepared on the first perovskite active precursor layer 105 (CH3NH3PbCl3), and then the electron transport layer and silver nanowire electrode are prepared; due to the corrosion of the solvent during the preparation of the second perovskite active precursor layer 107 (CH3NH3PbI3), it is difficult to form a CH3NH3PbI3 film with good morphology; at the same time, the preparation of the corresponding electron transport layer is also due to the presence of water, resulting in device damage, and ultimately the battery is inefficient.

[0097] The energy band schematic diagram of the present invention before thermal diffusion is as follows Figure 3 After diffusion, the left side of the perovskite layer is enriched with Cl phase and the right side is enriched with I phase. The Fermi level bends in the middle transition layer. Under this gradient, electrons are more likely to move to the left, and the corresponding holes move to the right, which increases the collection and separation of excitons and the collection efficiency. The final comparison results are as follows: Figure 4 As shown, compared with the existing single-layer perovskite solar cell structure, the opening voltage, current density and efficiency of the perovskite solar cell structure of the present invention are comprehensively improved; specifically: the opening voltage is increased to 1.11V, the current density is increased to 23.1mA / cm2, and the efficiency is increased to 19.2%.

Claims

1. A method for preparing a perovskite solar cell structure, characterized in that: include: 1) Preparation of transparent electrode substrate (102): An ITO transparent electrode deposited on transparent ultra-white glass is used as the transparent electrode substrate (102), with an area of ​​5×5 cm 2 ; 2) preparing an electron transport layer (104) on a transparent electrode substrate (102): the material is SnO2 nanosol, the sol mass is 20 g / L of aqueous solution; the scraper coating speed is 25 mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 100 μm; after coating, annealing and drying at 150° C. in nitrogen; the final thickness is about 20 nm; 3) preparing a first perovskite active precursor layer (105) on the surface of the electron transport layer (104) to obtain an n-region multilayer structure: the material is CH3NH3PbCl3, the solvent is DMF, and the mass fraction is 20% of the slurry; the scraper coating speed is 15mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, annealing is carried out at 135°C in nitrogen for 10 minutes; the thickness of the finally obtained perovskite active precursor layer (105) is 300nm; 4) Preparation of the second electrode (110): printing nano silver wires on ultra-white glass substrate material, the material is commercial silver nano wire sol, the solvent is isopropanol, the concentration is 50 g / L, the diameter of the silver nano wires is about 100 nm, and the length is 50-100 μm; the scraper coating speed is 10 mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50 μm; after coating, annealing is carried out at 80° C. in nitrogen for 15 minutes; finally, a second electrode (110) with a thickness of about 70 nm is obtained; 5) Preparing a hole transport layer (108) on the second electrode (110): the slurry used is a commercial PEDOT:PSS aqueous solution, which is diluted with isopropanol in a volume ratio of (PEDOT:PSS):isopropanol=1:3, with a scraper coating speed of 20 mm / s; the coating temperature is 60°C; the distance between the scraper and the substrate is 50 μm; after coating, annealing is performed at 90°C in nitrogen for 15 minutes9; the thickness of the hole transport layer (108) finally obtained is 100 nm; 6) A second perovskite active precursor layer (107) is prepared on the surface of the hole transport layer (108) to obtain a p-region multilayer structure: the material is CH3NH3PbI3, the solvent is DMF, and the mass fraction is 20% of the slurry; the scraper coating speed is 15mm / s; the coating temperature is room temperature; the distance between the scraper and the substrate is 50μm; after coating, it is annealed at 135°C in nitrogen for 10 minutes; the thickness of the finally obtained perovskite active precursor layer (107) is 300nm; 7) Physically press the n-region multilayer structure prepared in steps 1)-3) and the p-region multilayer structure prepared in steps 4)-6) under vacuum, with a vacuum degree of ≤1×10 -5 Pa, composite pressure 0.01MPa, annealing at 135°C in vacuum for 20 minutes to obtain a perovskite solar cell structure; The prepared perovskite solar cell structure has an opening voltage of 1.11V, a current density of 23.1mA / cm2, and an efficiency of 19.2%.

2. A perovskite solar cell structure, characterized in that: The perovskite solar cell structure is prepared by the preparation method of claim 1.