A preparation process of graphene composite carbon-based high-temperature membrane

Through the preparation process of graphene composite carbon-based high-temperature film, flake graphite and graphene oxide dispersant combined with methyl silicone oil, the problems of attenuation effect and high processing cost of carbon-based electrothermal materials at high temperatures are solved, and high conductivity is achieved. Graphene composite materials with high thermal conductivity, suitable for industrial and civil heating needs.

CN109495992BActive Publication Date: 2024-11-08HUNAN BUSHENG ELECTRIC APPLIANCES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201811336191.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-11-12
Publication Date
2024-11-08
Estimated Expiration
2038-11-12

AI Technical Summary

Technical Problem

Existing carbon-based electrothermal materials have a heating attenuation effect at high temperatures, which are costly and have strict processing requirements. As a conductive material, flake graphite is difficult to directly apply to electrically heated products, and there is a problem of high temperature accumulation and difficulty in dispersing.

Method used

The high-conductivity and high-thermal graphene film are prepared by selecting high-purity scale graphite and graphene oxide dispersant, combined with methyl silicone oil, and ball milling and high-speed fluidization mixing technology to prepare high-conductivity and high-thermal graphene. Composite material, forming a uniform and dense film-like material.

Benefits of technology

Improves the high temperature resistance, electrical conductivity and thermal conductivity of the material, reduces production costs, and achieves efficient electric heating conversion efficiency. The process is relatively simple, the energy consumption is low, and there is no emission of harmful pollutants. It is suitable for industrial and civil heating needs. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109495992B_ABST
    Figure CN109495992B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of preparation technology of graphene composite materials, and specifically relates to a preparation technology of graphene composite carbon-based high-temperature membrane. The process includes: (1) preparing flake graphite powder; (2) selecting raw materials; (3) mixing; (4) drying, fluidizing and mixing, and material molding. The present invention obtains high-conductivity and high-thermal conductivity materials through a specific process and a specific ratio. The preparation method is relatively simple, the energy consumption is low, and there is no emission of harmful pollutants. It is a clean and environmentally friendly production technology. The graphene composite carbon-based high-temperature membrane obtained by the present invention has an electric-to-thermal conversion efficiency of more than 99.5%, which can solve industrial and civilian heating problems with low power consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation technology of graphene composite materials, and specifically relates to a preparation technology of a graphene composite carbon-based high-temperature film. Background Art

[0002] With the progress of industrialization, more and more industrial equipment requires heating materials and products. Boiler steam, gas equipment, etc. are commonly used to provide heat sources. Electric heating equipment is generally not selected due to low thermoelectric conversion efficiency, high energy consumption, fragility, attenuation and other problems. As an electric heating material product, its high conversion efficiency, low energy consumption, high stability performance and other issues have become the key issues of electric heating products.

[0003] Currently, carbon-based electric heating materials mainly adopt carbon fiber, carbon crystal and other materials. Due to the organic components inside, there is a heating attenuation effect. The higher the temperature, the more obvious the attenuation. Judging from the market response in recent years, the long-term use effect is not ideal.

[0004] Whether producing carbon fiber or carbon crystal, if you want to make high-performance electric heating products, you must have very strict requirements on the processing and control of the raw silk materials to achieve high purification, high reinforcement, densification and smooth surface of the raw silk, which increases the product cost.

[0005] Graphite is generally used as a conductive material, flake graphite, which is a natural crystalline graphite, similar to fish phosphate, belonging to the hexagonal crystal system, and has a layered structure. It has good high temperature resistance, electrical conductivity, thermal conductivity, lubrication, plasticity, acid and alkali resistance, etc. However, flake graphite cannot be used directly as a conductive material. This is because the surface of the unprocessed carbon-based material contains a large number of polar groups, so it has the disadvantages of being difficult to disperse, easy to flocculate, and agglomerating at high temperatures. Summary of the invention

[0006] In order to solve the above-mentioned technical problems, the present invention provides a preparation process of a graphene composite carbon-based high-temperature membrane, which fully utilizes the conductivity, crystal structure, high temperature resistance, plasticity and other characteristics of high-quality graphite, adds graphene dispersant and methyl silicone oil, so that the product stability, high temperature resistance and conductivity are enhanced, the production process is simplified, and production costs can be effectively saved.

[0007] The present invention provides a preparation process for a graphene composite carbon-based high-temperature membrane, comprising the following steps: step (1), selecting flake graphite with a purity of 99.0-99.5% and a particle size of 1-2 mm for preparing flake graphite powder, ball-milling the flake graphite to a particle size of 20-40 μm under a room temperature dry environment to obtain fine-grained flake graphite powder; step (2), selecting a graphene dispersant, the selected material being a graphene oxide dispersion with a purity of 99wt%, a flake size of 1-5 μm and a concentration of 10 mg / ml.

[0008] Step (3), selecting methyl silicone oil with a specific gravity of 0.96-0.97 and a viscosity of 100±8mm2 / s; Step (4), adding the above-mentioned graphene dispersant at a mass ratio of 0.1-0.8% and methyl silicone oil at a mass ratio of 0.5-1.5% to the fine-grained flake graphite powder obtained in step (1), stirring at room temperature and pressure for 60 minutes at a stirring speed of 300-500r / min to obtain an incompletely mixed graphene composite carbon-based material.

[0009] Preferably, in the present invention: the mass percentage of flake graphite carbon is 99%, the mass percentage of graphene dispersant is 0.7%, and the mass percentage of methyl silicone oil is 0.3%; and the stirring speed is 300 r / min.

[0010] Or preferably, the carbon content of flake graphite is 99%, the graphene dispersant is 0.5%, the methyl silicone oil is 0.5%, and the stirring speed is 400r / min; or preferably, the carbon content of flake graphite is 99%, the graphene dispersant is 0.3%, the methyl silicone oil is 0.7%; the stirring speed is 500r / min.

[0011] The above-mentioned preparation process of a graphene composite carbon-based high-temperature membrane also includes step (5) S1 drying fluidized mixing: using a high-speed fluidized mixer, the lower part of the mixer is provided with a distribution plate, and the bottom is a compressed air and dry hot air mixing chamber, the composite material obtained in step (4) is fed to the distribution plate evenly through a sealed feeding device, and the wind pressure is gradually adjusted to: 0.25MPa-0.3Mpa, the temperature is 80°C, so that the composite material obtained in step (4) enters a continuous fluidized state, and a filter bag receiving device is provided at the upper outlet of the fluidized mixer, and the dried composite is fed to the bottom conveyor. The material is transported to the molding machine; S2 material molding adopts high-precision scraper flat material distribution and horizontal coating, and the scraper material thickness is adjusted to 30-50μm and the pressure is 15-18Mpa. The film is calendered to obtain a graphene composite carbon-based high-temperature film with a purity of 99%-99.9%. Its normal operating temperature is 40-350℃, and the inert gas protection temperature is controlled at 1000-1500℃. The thermal conductivity in the vertical direction is 500-800W / mK, the thermal conductivity in the horizontal direction is 1200-1950W / mK, and the specific gravity is 1.78-2.12g / cm 3 , electrothermal conversion efficiency ≥99.5%.

[0012] The structure of the high-speed fluidized mixer includes: a fluidizing chamber, a feed port is provided at the lower part of the fluidizing chamber, the feed port is communicated with the lower part of the fluidizing chamber, a distribution plate is provided at the lower part of the fluidizing chamber, the lower part of the feed port is inclined toward the distribution plate, and the lower part of the distribution plate is a hot air mixing chamber, and two air inlets and corresponding valves are arranged on the side wall of the hot air mixing chamber, hot air is introduced into the first air inlet located at the upper part, and fluidizing air is introduced into the second air inlet located at the lower part; the upper part of the fluidizing chamber is connected with the bag-type dust collector, the upper top part of the bag-type dust collector is provided with a blowing and exhaust device, the lower part of the bag-type dust collector is provided with a collecting device, the lower part of the collecting device is provided with a spiral feeding system, the lower part of the spiral feeding system is provided with a distribution bed, and the distribution bed is provided with a plurality of distribution rollers for rolling and forming the distribution rollers arranged in parallel above it.

[0013] The feed port is inclined at an angle of 45° to the horizontal plane, and the plane where the cross section of the lower part of the feed port is located is at an angle of 45° to the plane where the distribution plate is located.

[0014] The longitudinal section of the hot air mixing chamber is in the shape of an inverted triangular cone as a whole, and the angle between the first air inlet for hot air and the second air inlet for fluidizing air is 60°.

[0015] The longitudinal section of the material collecting device is an isosceles trapezoid that is small at the top and large at the bottom.

[0016] The lower part of the cloth plate is connected with a vibration device, and the vibration device is driven by a motor to vibrate.

[0017] The first air inlet and the second air inlet are respectively provided with a first partition plate, the first partition plate is provided with a plurality of first mesh holes of the same shape and uniform size, and the second partition plate is also provided with a plurality of second mesh holes of the same shape and uniform size.

[0018] The first air inlet and the second air inlet are located on the same side of a longitudinal plane passing through the center of the hot air mixing chamber.

[0019] The preparation method of the present invention is simple and can be realized under normal conditions. After the fine-grained flake graphite is electrified, the problem of overheating caused by aggregation of polar groups of large-particle graphite can be solved. The preparation method can greatly improve the friction resistance and plasticity of the material by adding methyl silicone oil and mixing by a fluidized bed solid phase method. The addition of a graphene dispersant can greatly improve the superconducting properties of the composite material, making the thermal effect of ions in the composite material more obvious, the heat conversion efficiency higher, and the electrical and thermal conductivity improved.

[0020] In this manufacturing method, the inorganic materials are used to the maximum extent, which can reduce the problems of electrical conductivity and thermal conductivity attenuation of previous fiber composite materials and enhance the stability of use.

[0021] The present invention makes full use of the molecular structural combination of graphite and graphene. Through the material preparation process mentioned in the present invention, a highly uniform, dense and highly adhesive film material with a thickness of 40-50 μm is formed, and a skeleton-type conductive network is built. Under the action of the electric field, ions rub and collide with each other in the composite material to generate a large amount of heat. In addition, because graphene is a superconducting material, the resistivity of the composite material can be reduced, thereby reducing power consumption.

[0022] The beneficial effects of the present invention are: (1) the present invention obtains high electrical conductivity and high thermal conductivity materials through a specific process and a specific ratio, the production method is relatively simple, the energy consumption is low, and no harmful pollutants are emitted. It is a clean and environmentally friendly production technology.

[0023] (2) The graphene composite carbon-based high-temperature membrane obtained by the present invention has an electric-to-thermal conversion efficiency of 99.5%, which can solve industrial and civilian heating problems with low power consumption.

[0024] (3) The graphene composite carbon-based high-temperature film obtained by the present invention can be combined with ceramics, microcrystalline plates, mica sheets and other materials for fixed-length compounding. By adjusting the formula ratio and size of the composite material, under normal environmental conditions, a heating material with a temperature of 40-350°C can be obtained after power is turned on, and it can be used at high temperatures within 350°C. Through inert gas protection, the heating temperature can reach 1500°C, and the market promotion and application effect is obvious. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a structural schematic diagram of a high-speed fluidized mixer of the present invention; Figure 2 It is a comparison diagram of thermal conductivity of Example 1 and Comparative Examples 1-5; Figure 3 It is a comparison diagram of thermal conductivity of Example 1 and Comparative Examples 6-8; Figure 4 It is an enlarged structural schematic diagram of the hot air mixing chamber in Example 4; Figure 5 is a schematic structural diagram of the first partition in Example 4; Figure 6 is a schematic structural diagram of the second partition in Example 4; Figure 7 It is a schematic diagram of the structure of the cloth plate in Example 5; in the figure, 1-fluidizing chamber, 2-feeding port, 3-cloth plate, 4-hot air, 5-hot air mixing chamber, 6-fluidizing air, 7-blowing exhaust device, 8-bag dust collector, 9-collecting device, 10-screw feeding system, 11-cloth rolling and forming roller, 12-cloth bed, 41-first air inlet, 61-second air inlet, 42-first partition, 62-second partition, 43-first mesh, 63-second mesh. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods so that those skilled in the art can better understand the present invention, but the present invention is not limited thereto.

[0027] The graphene dispersant used in the present invention is purchased from: Ningbo Institute of Materials, Chinese Academy of Sciences; methyl silicone oil is purchased from Shandong Longhui Chemical Co., Ltd.; Example 1 A process for preparing a graphene composite carbon-based high-temperature membrane comprises the following steps: Step (1), flake graphite with a purity of 99% and a particle size of 1-2 mm is selected for flake graphite powder, and ball-milled to a particle size of 20 μm under a room temperature dry environment to obtain fine-grained flake graphite powder; Step (2), selecting a graphene dispersant, the selected material is a graphene oxide dispersion, wherein the pure The method comprises the following steps: step (1) adding the graphene dispersant in a mass ratio of 0.8% and the methyl silicone oil in a mass ratio of 0.2%, and stirring for 60 minutes at room temperature and pressure at a stirring speed of 400 r / min to obtain an incompletely mixed graphite powder; step (2) adding the graphene dispersant in a mass ratio of 0.8% and the methyl silicone oil in a mass ratio of 0.2%, and stirring for 60 minutes at room temperature and pressure at a stirring speed of 400 r / min to obtain an incompletely mixed graphite powder; olefin composite carbon-based material; step (5), S1: drying fluidized mixing: the lower part of the mixer is provided with a distribution plate 3, and the bottom is a compressed air and dry hot air mixing chamber 5, the composite material obtained in step (4) is fed to the distribution plate 3 evenly through a sealed feeding device, and the wind pressure is gradually adjusted to: 0.25MPa-0.3Mpa, and the temperature is 80°C, so that the composite material obtained in step (4) enters a continuous fluidized state, and a filter bag receiving device is provided at the upper outlet of the fluidized mixer, and the dry The dried composite material is conveyed to the molding machine; S2: The material molding adopts high-precision scraper plane material distribution and horizontal coating, and the scraper material thickness is adjusted to 30μm and the pressure is 15Mpa. The film is calendered to obtain a graphene composite carbon-based material with a purity of 99.9%. Under the condition of the use temperature of 280℃, the inert gas protection temperature is controlled at 1200℃, the vertical thermal conductivity is 850W / mK, the horizontal thermal conductivity is 1950W / mK, and the specific gravity is 1.78g / cm 3 , the electric-thermal conversion efficiency is 99.5%.

[0028] A high-speed fluidized mixer is used for drying and fluidization, and the specific structure of the high-speed fluidized mixer includes: a fluidized chamber 1, a feed port 2 is provided at the lower part of the fluidized chamber 1, and the feed port 2 is communicated with the lower part of the fluidized chamber 1, a cloth plate 3 is provided at the lower part of the fluidized chamber 1, and the lower part of the feed port 2 is inclined toward the cloth plate 3, and below the cloth plate 3 is a hot air mixing chamber 5, and two air inlets and corresponding valves are provided on the side walls of the hot air mixing chamber 5, and hot air 4 is introduced into the first air inlet 41 located at the upper part, and fluidizing air 6 is introduced into the second air inlet 61 located at the lower part; the upper part of the fluidized chamber 1 is connected with the bag-type dust collector 8, and the upper top of the bag-type dust collector 8 is provided with a blowing exhaust device 7, and the lower part of the bag-type dust collector 8 is provided with a collecting device 9, and the lower part of the collecting device 9 is provided with a spiral feeding system 10, and a cloth bed 12 is provided below the spiral feeding system 10, and the cloth bed 12 is provided with a plurality of cloth rolling and forming rollers 11 arranged in parallel above it.

[0029] The feed port 2 is inclined at an angle of 45° to the horizontal plane, and the plane where the cross section of the lower part of the feed port 2 is located is at an angle of 45° to the plane where the distribution plate 3 is located.

[0030] The longitudinal section of the hot air mixing chamber 5 is in the shape of an inverted triangular cone as a whole, and the angle between the first air inlet 41 for hot air and the second air inlet 61 for fluidizing air is 60°.

[0031] The longitudinal section of the material collecting device 9 is an isosceles trapezoid that is smaller at the top and larger at the bottom. The material collecting device 9 may also be a common material collecting device available on the market, as long as the purpose of collecting materials in the present invention can be achieved.

[0032] The difference between Comparative Example 1 and Example 1 is that step (4) is specifically as follows: (4) adding the above-mentioned graphene dispersant at a mass ratio of 0.5% and methyl silicone oil at a mass ratio of 0.5% to the fine-grained flake graphite powder obtained in (1), stirring for 60 minutes at room temperature and pressure, and the stirring speed is 400r / min to obtain an incompletely mixed graphene composite carbon-based material; The difference between Comparative Example 2 and Example 1 is that step (4) is specifically as follows: (4) adding the above-mentioned graphene dispersant at a mass ratio of 0.3% and methyl silicone oil at a mass ratio of 0.5% to the fine-grained flake graphite powder obtained in (1), and stirring for 60 minutes at room temperature and pressure, and the stirring speed is 400r / min to obtain an incompletely mixed graphene composite carbon-based material. The above-mentioned graphene dispersant is added to the fine-grained flaky graphite powder obtained in (1) at a mass ratio of 0.7%, and stirred at room temperature and pressure for 60 minutes at a stirring speed of 400r / min to obtain an incompletely mixed graphene composite carbon-based material; the difference between Comparative Example 3 and Example 1 is that step (4) is specifically as follows: (4) the above-mentioned graphene dispersant is added to the fine-grained flaky graphite powder obtained in (1) at a mass ratio of 0.8% and the methylphenyl silicone oil is added to the fine-grained flaky graphite powder obtained in (1) at a mass ratio of 0.2%, and stirred at room temperature and pressure for 60 minutes at a stirring speed of 400r / min. min, to obtain an incompletely mixed graphene composite carbon-based material; the difference between Comparative Example 4 and Example 1 is that step (4) is specifically as follows: (4) the above-mentioned graphene dispersant is added at a mass ratio of 0.5% and methylphenyl silicone oil is added at a mass ratio of 0.5% to the fine-grained flake graphite powder obtained in (1), and stirred at room temperature and pressure for 60 minutes at a stirring speed of 400r / min to obtain an incompletely mixed graphene composite carbon-based material; the difference between Comparative Example 5 and Example 1 is that step (4) is specifically as follows: (4) the above-mentioned 0.3% of graphene dispersant and 0.7% of methylphenyl silicone oil by mass are added to the fine-grained flake graphite powder obtained in (1), and stirred at room temperature and pressure for 60 minutes at a stirring speed of 400 r / min to obtain an incompletely mixed graphene composite carbon-based material; the thermal conductivity of the thermal conductive material is tested respectively, and the thermal conductivity is measured by a quasi-equilibrium thermal conductivity meter; when measuring, the sheet-shaped thermal conductive material is first taken, and then placed at 100-120° C., dried for 6-8 hours, and then measured by a quasi-equilibrium thermal conductivity meter; Figure 2 The results of thermal conductivity of the materials in the embodiments and comparative examples 1-5 are as follows; Figure 2It can be seen that the thermal conductivities of the products in Example 1 and Comparative Examples 1-2 are similar. The only difference between Example 1 and Comparative Examples 1 and 2 is the amount of methyl silicone oil in (4). Adjusting the amount of methyl silicone oil has little effect on the final thermal conductivity. The thermal conductivity of the thermally conductive material in Example 1 of the present invention reaches a maximum of 1950 w / m·k, and the thermal conductivity of the products in Examples 2 and 3 is also around 1950 w / m·k. Comparative Examples 3-5 replace methylphenyl silicone oil with methyl silicone oil and adjust its amount. It can be found that adjusting the type of raw materials will have a certain effect on the thermal conductivity of the thermally conductive material. In comparison, the thermal conductivity of the solution in Example 1 of the present invention is higher.

[0033] The difference between Comparative Example 6 and Example 1 is that, in step (2), a graphene dispersant is selected, and the selected material is a graphene oxide dispersion liquid, wherein the purity is 99wt%, the flake diameter is 5μm, and the concentration is 10mg / ml; the dosage is 0.8%; the rest is exactly the same as in Example 1; The difference between Comparative Example 7 and Example 1 is that, in step (2), a graphene dispersant is selected, and the selected material is a graphene oxide dispersion liquid, wherein the purity is 99wt%, the flake diameter is 5μm, and the concentration is 10mg / ml; the dosage is 0.3%; the rest is exactly the same as in Example 1 Example 1 is exactly the same; the difference between Comparative Example 8 and Example 1 is that, in step (2), a graphene dispersant is selected, and the selected material is a graphene oxide dispersion liquid, wherein the purity is 99wt%, the flake diameter is 1μm, and the concentration is 10mg / ml; its dosage is 0.5%; the rest is exactly the same as Example 1; the thermal conductivity of the products in Example 1 and Comparative Examples 6-8 is significantly higher than that of the products in Comparative Examples 6-8, which indicates that the purity, dosage and selection of the dispersant will also have a significant impact on the thermal conductivity of the subsequent products.

[0034] Example 2 A process for preparing a graphene composite carbon-based high-temperature membrane comprises the following steps: (1) preparing flake graphite powder: selecting flake graphite with a purity of about 99% and a particle size of 1 mm, and ball-milling it to a particle size of 30 μm under a room temperature and dry environment to obtain fine-grained flake graphite powder; (2) selecting a graphene dispersant, the selected material being a graphene oxide dispersion liquid, wherein the purity is 99wt%, the flake size is 5 μm, and the concentration is 10 mg / ml; (3) selecting methyl silicone oil with a specific gravity of 0.96 and a viscosity of 100±8 mm2 / s; (4) adding the above-mentioned graphene dispersant at a mass ratio of 0.5% and the methyl silicone oil at a mass ratio of 0.5% to the fine-grained flake graphite powder obtained in (1), stirring at room temperature and pressure for 60 minutes at a stirring speed of 300 r / min to obtain an incompletely mixed graphene carbon-based composite material.

[0035] (4) S1: Drying and fluidizing mixing: Drying and fluidizing are performed by a high-speed fluidizing mixer. The specific structure of the high-speed fluidizing mixer is the same as that of Example 1. A distribution plate is provided at the bottom of the mixer, and a compressed air and dry hot air mixing chamber is provided at the bottom. The composite material obtained in step (3) is evenly fed to the distribution plate through a sealed feeding device, and the wind pressure is gradually adjusted to 0.25 MPa and the temperature is 80° C., so that the composite material obtained in step (3) enters a continuous fluidizing state. A filter bag receiving device is provided at the upper outlet of the fluidizing mixer, and a compressed air and dry hot air mixing chamber is provided at the bottom. The conveyor conveys the dried composite material to the molding machine; S2: Material molding adopts high-precision scraper plane cloth and horizontal coating, adjusts the scraper cloth thickness to 40μm, the pressure to 17Mpa, and calenders the film to obtain a graphene composite carbon-based high-temperature film with a purity of 99.5%. Its normal operating temperature is 40-350℃, and the inert gas protection temperature is controlled at 1000-1500℃. The thermal conductivity in the vertical direction is 600W / mK, the thermal conductivity in the horizontal direction is 1450W / mK, and the specific gravity is 1.95g / cm 3 , electrothermal conversion efficiency ≥99%.

[0036] Example 3 The preparation process of graphene composite carbon-based high-temperature membrane includes the following steps: (1) Select flake graphite powder with a purity of about 99% and a particle size of 2 mm, and ball-mill it to a particle size of 40 μm under room temperature and dry environment to obtain fine-grained flake graphite powder; (2) Select a graphene dispersant, and the selected material is a graphene oxide dispersion with a purity of 99wt%, a purity of 99wt%, a flake size of 5 μm, and a concentration of 10 mg / ml; (3) Select methyl silicone oil with a specific gravity of 0.96-0.97 and a viscosity of 100±8mm2 / s; (4) Add the above-mentioned graphene dispersant at a mass ratio of 0.5% and methyl silicone oil at a mass ratio of 0.5% to the fine-grained flake graphite powder obtained in (1), stir at room temperature and pressure for 60 minutes, and the stirring speed is 500r / min to obtain an incompletely mixed graphene composite carbon-based material.

[0037] (5) S1: Drying and fluidizing mixing: Drying and fluidizing are performed by a high-speed fluidizing mixer, the specific structure of which is the same as that of Example 1; a distribution plate is provided at the bottom of the mixer, and a compressed air and dry hot air mixing chamber is provided at the bottom. The composite material obtained in step (3) is evenly fed to the distribution plate through a sealed feeding device, and the wind pressure is gradually adjusted to 0.3 MPa and the temperature is 80° C., so that the composite material obtained in step (3) enters a continuous fluidizing state. A filter bag receiving device is provided at the upper outlet of the fluidizing mixer, and the composite material is transported through the bottom. The dry composite material is conveyed to the molding machine by the device; S2: Material molding adopts high-precision scraper plane material distribution and horizontal film coating, and the scraper material thickness is adjusted to 50μm and the pressure is 18Mpa. The film is calendered to obtain a graphene composite carbon-based high-temperature film with a purity of 99.5%. Its normal operating temperature is 40-300℃, and the inert gas protection temperature is controlled at 1000-1500℃. The thermal conductivity in the vertical direction is 560W / mK, the thermal conductivity in the horizontal direction is 1280W / mK, and the specific gravity is 2.12g / cm 3 , electrothermal conversion efficiency ≥99%.

[0038] Example 4 In order to prevent impurities from entering at the air inlet, the inventors designed a first partition 42 and a second partition 62, and the specific structure is as follows: a first partition 42 and a second partition 62 are respectively provided at the first air inlet 41 and the second air inlet 61, and a plurality of first mesh holes 43 of the same shape and uniform size are provided on the first partition 42, and a plurality of second mesh holes 63 of the same shape and uniform size are also distributed on the second partition 62.

[0039] The first air inlet 41 and the second air inlet 61 are located on the same side of a longitudinal plane passing through the center of the hot air mixing chamber 5. The remaining structure is the same as that of the first embodiment.

[0040] The difference between the embodiment 5 and the embodiment 1 is that the lower part of the material distribution plate 3 is connected to the vibration device 14 and the vibration device is driven by a motor to vibrate. In this way, the material can be evenly distributed in the material distribution plate 3 to prevent the material from agglomerating or unevenly distributed.

Claims

1. A process for preparing a graphene composite carbon-based high-temperature membrane, comprising the following steps: Step (1) preparing flake graphite powder, selecting flake graphite with a purity of 99.0-99.5% and a particle size of 1-2 mm, and ball-milling it to a particle size of 20-40 μm under a room temperature dry environment to obtain fine-grained flake graphite powder; Step (2) selecting a graphene dispersant with a purity of 99 wt%, a flake diameter of 1-5 μm, and a concentration of 10 mg / ml; Step (3) Select a specific gravity of 0.96-0.97 and a viscosity of 100±8mm 2 / s methyl silicone oil; Step (4) adding the graphene dispersant in a mass ratio of 0.2-0.8% and methyl silicone oil in a mass ratio of 0.2-0.8% to the fine-grained flake graphite powder obtained in step (1), stirring at room temperature and pressure for 60 minutes at a stirring speed of 300-500 r / min to obtain an incompletely mixed graphene carbon-based composite material. The mass percentage of flake graphite carbon is 99%, the mass percentage of graphene dispersant is 0.8%, and the mass percentage of methyl silicone oil is 0.2%; the stirring speed is 300r / min, Step (5): S1 drying fluidized mixing: A high-speed fluidized mixer is used, the lower part of the mixer is provided with a distribution plate, and the bottom is a compressed air and dry hot air mixing chamber. The composite material obtained in step (4) is evenly fed to the distribution plate through a sealed feeding device, and the wind pressure is gradually adjusted to: 0.25MPa-0.3Mpa, temperature is 80°C, so that the composite material obtained in step (4) enters a continuous fluidized state, a filter bag collecting device is set at the upper outlet of the fluidized mixer, and the dried composite material is conveyed to the molding machine through the bottom conveyor; S2 Material Forming The high-precision scraper plane cloth and horizontal lamination and calendering film are used to obtain a graphene composite carbon-based high-temperature film with a purity of 99%-99.9%. Its normal operating temperature is 40-350℃, and the inert gas protection temperature is controlled at 1000-1500℃. The vertical thermal conductivity is 500-800W / mK, the horizontal thermal conductivity is 1200-1950W / mK, the specific gravity is 1.78-2.12g / cm³, and the electrothermal conversion efficiency is ≥99%. The structure of the high-speed fluidized mixer is as follows: a fluidized chamber (1), wherein a feed port (2) is provided at the lower portion of the fluidized chamber (1), the feed port (2) being communicated with the lower portion of the fluidized chamber (1), a distribution plate (3) being provided at the lower portion of the fluidized chamber (1), the lower portion of the feed port (2) being inclined toward the distribution plate (3), a hot air mixing chamber (5) being provided below the distribution plate (3), two air inlets and corresponding valves being provided on the side wall of the hot air mixing chamber (5), the hot air (4) being introduced into the first air inlet (41) at the upper portion, and the fluidizing air (6) being introduced into the second air inlet (61) at the lower portion; The upper part of the fluidizing chamber (1) is connected to the bag dust collector (8), the upper part of the bag dust collector (8) is provided with a blowing exhaust device (7), the lower part of the bag dust collector (8) is provided with a collecting device (9), the lower part of the collecting device (9) is provided with a spiral feeding system (10), the lower part of the spiral feeding system (10) is provided with a material bed (12), and the material bed (12) is provided with a plurality of material rolling and forming rollers (11) arranged in parallel above the material bed. The feed port (2) is inclined at an angle of 45° to the horizontal plane, and the plane where the cross section of the lower part of the feed port (2) is located is at an angle of 45° to the plane where the distribution plate (3) is located. The longitudinal section of the hot air mixing chamber (5) is in the shape of an inverted triangular cone as a whole, and the angle between the first air inlet (41) for hot air and the second air inlet (61) for fluidizing air is 60 degrees. The longitudinal section of the material collecting device (9) is an isosceles trapezoid that is smaller at the top and larger at the bottom.